Titanium alloy wear-resistant and ablation-resistant composite strengthening layer and preparation method thereof
The titanium alloy wear-resistant and ablation-resistant composite reinforcement layer is prepared through shot peening and plasma nitriding technology, which solves the problem of titanium alloy being easily combustible and ablated at high temperatures, and achieves high-strength, wear-resistant and impact-resistant ablation properties. Improves reliability and safety of hot-end components.
Patent Information
- Application Number
- CN202410982574.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-07-22
AI Technical Summary
Titanium alloys are prone to combust and ablation at high temperatures, resulting in the failure of hot-end components in aerospace and weapons equipment, and the existing coating technology is costly and has limited protection effect.
The titanium alloy wear-resistant and ablation-resistant composite reinforcement layer is prepared by shooting peening and plasma nitriding technology to form a nanocrystalline structure and compound layer, with high binding strength and excellent fatigue resistance. The surface nano-layer is formed by shooting peening for 40 seconds, and the plasma is in the form of Nitrogen and hydrogen are introduced into the bulk nitriding furnace to form a composite reinforcement layer.
The high strength, wear resistance and impact ablation effect of titanium alloy surface is achieved, which significantly improves the wear resistance and ablation resistance of the material, ensures the reliability and safety of hot-end components, and has a low cost in the preparation method. Easy to control operation.
Smart Images

Figure CN118880225A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of titanium alloy surface treatment, and in particular to a titanium alloy wear-resistant and ablation-resistant composite strengthening layer and a preparation method thereof. Background Art
[0002] Titanium alloys are sensitive to combustion environments. Oxides produced by oxidation at high temperatures have low density and a loose oxide film, which cannot protect the substrate: the heat released by combustion is much greater than the heat dissipation rate, which increases the metal temperature and accelerates combustion. This makes it easy to catch fire and burn under high temperature, high pressure or severe impact when used as hot-end components in power systems of aerospace and weapons, resulting in combustion, melting, and burn-through of hot-end components, causing equipment failure and even safety accidents. Titanium alloys used as hot-end components must withstand high-temperature and high-speed gas erosion, and the flame retardancy and erosion-resistant ablation problems of titanium alloys must be solved. At present, coating technology has become the main technology for the application of titanium alloy hot-end components due to its good protective effect and low cost. In order to achieve flame retardancy and erosion-resistant ablation of titanium alloys by applying coating technology, the designed and prepared coating must meet the following requirements: self-flammability can isolate gas; resistance to gas erosion, small difference in thermal expansion coefficient with the substrate; high bonding strength with the substrate and tight bonding.
[0003] In view of the above-mentioned defects, the inventors of the present invention finally obtained the present invention after a long period of research and practice. Summary of the invention
[0004] The purpose of the present invention is to solve the flame retardancy and erosion erosion resistance problems of titanium alloy used as hot end components to withstand high temperature and high speed gas erosion, and provide a titanium alloy wear-resistant and ablation-resistant composite strengthening layer and a preparation method thereof.
[0005] In order to achieve the above object, the present invention discloses a titanium alloy wear-resistant and ablation-resistant composite strengthening layer and a preparation method thereof, comprising the following steps:
[0006] S1, grinding the titanium alloy material, further polishing it to a low roughness state, and cleaning it in acetone or alcohol solution;
[0007] S2, clamping the titanium alloy obtained in step S1 on a tool, and presetting the Almon strength using an arc height meter;
[0008] S3, adjust the horizontal distance between the tooling and the shot peening gun muzzle, select the shot peening material, the incident angle of the muzzle, the flow rate and the pressure of the shot peening gun muzzle, and shot peen for 40 seconds to obtain the surface nano-crystallized titanium alloy sample;
[0009] S4, cleaning the titanium alloy sample obtained in step S3 in acetone or an alcohol solution;
[0010] S5, placing the material obtained in step S4 in a plasma nitriding furnace, evacuating the furnace, and turning on the voltage;
[0011] S6, introducing nitrogen, hydrogen / argon, adjusting the temperature and pressure in the furnace, and performing heat preservation nitriding to obtain a composite strengthening layer;
[0012] S7, then the sample is cooled to room temperature in the furnace and the sample is taken out.
[0013] In the step S1, the titanium alloy material is a high-strength TC11 alloy.
[0014] In step S2, the titanium alloy material is further polished to a mirror surface.
[0015] In step S2, Almon is a type A test piece.
[0016] In step S3, the horizontal distance is 120 mm, the shot peening shot is AZB425 ceramic shot, the incident angle is 90°, the flow rate is 3 kg / min, and the key parameter pressure is 0.25-0.50 MPa.
[0017] In step S5, the voltage is 600-700V.
[0018] In the step S6, the amount of nitrogen gas introduced is 100 to 300 sccm, and the amount of hydrogen gas / argon gas introduced is 100 to 300 sccm.
[0019] In the step S6, the nitriding temperature is 750-850°C, the nitriding time is more than 10 hours, and the gas pressure in the furnace is 200-250Pa.
[0020] The invention also discloses a titanium alloy wear-resistant and ablation-resistant composite strengthening layer prepared by the preparation method.
[0021] Compared with the prior art, the beneficial effects of the present invention are:
[0022] 1. The present invention provides a wear-resistant and ablation-resistant composite strengthening layer suitable for titanium alloys. The surface strengthening layer is prepared by spraying composite technology, which has excellent bonding strength, the coating will not peel off, and has good impact and ablation resistance effect;
[0023] 2. The present invention provides a wear-resistant and ablation-resistant composite strengthening layer suitable for titanium alloys. The surface layer has a nanocrystalline structure, which can significantly improve the wear resistance and erosion resistance of the material; the diffusion layer introduces residual stress to ensure that there is no cracking during the deformation process, and has excellent fatigue resistance; the aluminum-rich layer is located between the compound layer and the diffusion layer, and can form aluminum oxide after high-temperature oxidation to prevent high-temperature gases, especially oxygen, from contacting the matrix, thereby further improving the ablation resistance;
[0024] 3. The present invention provides a wear-resistant and ablation-resistant composite strengthening layer suitable for titanium alloys. Through the coordinated cooperation of a compound layer, an aluminum-rich layer and a diffusion layer with a specific structure, the composite strengthening layer has good high-temperature wear resistance and high-temperature flame ablation resistance, and can effectively improve the wear and ablation characteristics of the hot end components of the titanium alloy, and improve the reliability and safety of the use of the hot end components of the titanium alloy;
[0025] 4. The preparation method of the present invention is easy to control and operate, has low cost and is pollution-free, and ensures excellent effect of the composite layer. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 The cross-sectional morphology after shot peening in the embodiment of the present invention;
[0027] Figure 2 The cross-sectional morphology of the spraying composite layer in the embodiment of the present invention;
[0028] Figure 3 This is the cross-sectional morphology after shot peening in Comparative Example 1 of the present invention;
[0029] Figure 4 This is the cross-sectional morphology of the nitrided layer in Comparative Example 5 of the present invention;
[0030] Figure 5 Schematic diagram of the structure of the composite strengthening layer in an embodiment of the present invention;
[0031] Figure 6 is the surface hardness of the embodiment of the present invention and the comparative example;
[0032] Figure 7 The wear rate test results of the embodiments of the present invention and the comparative examples are shown in FIG.
[0033] Figure 8 The mass ablation rate test results of the embodiments of the present invention and the comparative examples are shown in FIG. DETAILED DESCRIPTION
[0034] The above and other technical features and advantages of the present invention are described in more detail below in conjunction with the accompanying drawings.
[0035] Example
[0036] S1: Grind the TC11 titanium alloy material with sandpaper, and further polish it to a low roughness state (mirror state is best), and clean it in acetone or alcohol solution;
[0037] S2: The TC11 titanium alloy sample obtained in S1 is clamped on the fixture, and the Almon strength is pre-set using an arc height meter;
[0038] S3: Adjust the horizontal distance between the sample and the shot peening gun muzzle to 120mm, select AZB425 ceramic shot peening shot, the muzzle incident angle is 90°, the flow rate is 3kg / min, the shot peening gun muzzle pressure is 0.25-0.50MPa, and start preparing the titanium alloy deformation layer;
[0039] S4: Clean the titanium alloy sample obtained in S3 in acetone or alcohol solution;
[0040] S5: placing the material obtained in step 4 in a plasma nitriding furnace, evacuating the vacuum to 50 Pa, and turning on the voltage, the voltage is 700 V;
[0041] S6: 200 sccm of nitrogen and 200 sccm of hydrogen were introduced in a ratio of 1:1, the temperature in the furnace was adjusted to 800°C, the gas pressure was 200 Pa, and the temperature was kept for 10 hours to obtain a composite strengthening layer;
[0042] S7: The sample is then cooled to room temperature in the furnace and taken out.
[0043] The cross section of the titanium alloy deformation layer obtained in step S3 is as follows Figure 1 As shown in the figure, it can be seen that the grains are refined and diffusion channels of Al and N elements are formed. The composite strengthening layer obtained in step S6 is shown in Figure 2 As shown, it can be seen that a compound layer, an aluminum-rich layer and a diffusion layer are formed. The schematic diagram of the composite strengthening layer structure is shown in Figure 5 The surface hardness of the strengthening layer is shown in Figure 6 As shown in Figure 2, a high temperature friction and wear test (800°C) was conducted. The test results are shown in Figure 2. Figure 7 As shown in the figure, a flame ablation test was carried out at 1100℃ for 300s. The mass ablation rate is shown in Figure 8 shown.
[0044] Comparative Example 1
[0045] S1: Grind the TC11 titanium alloy material with sandpaper, and further polish it to a low roughness state (mirror state is best), and clean it in acetone or alcohol solution;
[0046] S2: The TC11 titanium alloy sample obtained in S1 is clamped on the fixture, and the Almon strength is pre-set using an arc height meter;
[0047] S3: Adjust the horizontal distance between the sample and the shot peening gun muzzle to 120mm, select AZB425 ceramic shot peening shot, the muzzle incident angle is 90°, the flow rate is 3kg / min, the shot peening gun muzzle pressure is 0.10-0.25MPa, and start preparing the titanium alloy deformation layer;
[0048] S4: Clean the titanium alloy sample obtained in S3 in acetone or alcohol solution;
[0049] S5: placing the material obtained in step 4 in a plasma nitriding furnace, evacuating the vacuum to 50 Pa, and turning on the voltage, the voltage is 700 V;
[0050] S6: 200 sccm of nitrogen and 200 sccm of hydrogen were introduced in a ratio of 1:1, the temperature in the furnace was adjusted to 800°C, the gas pressure was 200 Pa, and the temperature was kept for 10 hours to obtain a composite strengthening layer;
[0051] S7: The sample is then cooled to room temperature in the furnace and taken out.
[0052] Due to insufficient pressure at the shot peening gun muzzle, Figure 3 It shows that the surface grain refinement of Comparative Example 1 is not as good as that of the embodiment, which affects the diffusion channel, and the corresponding hardness, wear and ablation test results are not as good as those of the embodiment. Figure 6 , 7 and 8.
[0053] Comparative Example 2
[0054] S1: Grind the TC11 titanium alloy material with sandpaper, and further polish it to a low roughness state (mirror state is best), and clean it in acetone or alcohol solution;
[0055] S2: The TC11 titanium alloy sample obtained in S1 is clamped on the fixture, and the Almon strength is pre-set using an arc height meter;
[0056] S3: Adjust the horizontal distance between the sample and the shot peening gun muzzle to 120mm, select AZB425 ceramic shot peening shot, the muzzle incident angle is 90°, the flow rate is 3kg / min, the shot peening gun muzzle pressure is 0.50-0.60MPa, and start preparing the titanium alloy deformation layer;
[0057] S4: Clean the titanium alloy sample obtained in S3 in acetone or alcohol solution;
[0058] S5: placing the material obtained in step 4 in a plasma nitriding furnace, evacuating the vacuum to 50 Pa, and turning on the voltage, the voltage is 700 V;
[0059] S6: 200 sccm of nitrogen and 200 sccm of hydrogen were introduced in a ratio of 1:1, the temperature in the furnace was adjusted to 800°C, the gas pressure was 200 Pa, and the temperature was kept for 10 hours to obtain a composite strengthening layer;
[0060] S7: The sample is then cooled to room temperature in the furnace and taken out.
[0061] Due to the high pressure at the shot peening gun muzzle, the surface deformation of Comparative Example 2 was serious, the surface roughness was large, microcracks appeared, and the corresponding hardness, wear and ablation test results were not as good as those of the embodiment. Figure 6 , 7and 8.
[0062] Comparative Example 3
[0063] S1: Grind the TC11 titanium alloy material with sandpaper, and further polish it to a low roughness state (mirror state is best), and clean it in acetone or alcohol solution;
[0064] S2: The TC11 titanium alloy sample obtained in S1 is clamped on the fixture, and the Almon strength is pre-set using an arc height meter;
[0065] S3: Adjust the horizontal distance between the sample and the shot peening gun muzzle to 120mm, select AZB425 ceramic shot peening shot, the muzzle incident angle is 90°, the flow rate is 3kg / min, the shot peening gun muzzle pressure is 0.25-0.50MPa, and start preparing the titanium alloy deformation layer;
[0066] S4: Clean the titanium alloy sample obtained in S3 in acetone or alcohol solution;
[0067] S5: placing the material obtained in step 4 in a plasma nitriding furnace, evacuating the vacuum to 50 Pa, and turning on the voltage, the voltage is 700 V;
[0068] S6: 200 sccm of nitrogen and 200 sccm of hydrogen were introduced in a ratio of 1:1, the temperature in the furnace was adjusted to 700°C, the gas pressure was 200 Pa, and the temperature was kept for 10 hours to obtain a composite strengthening layer;
[0069] S7: The sample is then cooled to room temperature in the furnace and taken out.
[0070] Due to the low nitriding temperature, the surface strengthening effect of Comparative Example 3 is poor, and no thick strengthening protective layer is formed. The corresponding hardness, wear and ablation test results are not as good as those of the embodiment. Figure 6 , 7 and 8.
[0071] Comparative Example 4
[0072] S1: Grind the TC11 titanium alloy material with sandpaper, and further polish it to a low roughness state (mirror state is best), and clean it in acetone or alcohol solution;
[0073] S2: The TC11 titanium alloy sample obtained in S1 is clamped on the fixture, and the Almon strength is pre-set using an arc height meter;
[0074] S3: Adjust the horizontal distance between the sample and the shot peening gun muzzle to 120mm, select AZB425 ceramic shot peening shot, the muzzle incident angle is 90°, the flow rate is 3kg / min, the shot peening gun muzzle pressure is 0.25-0.50MPa, and start preparing the titanium alloy deformation layer;
[0075] S4: Clean the titanium alloy sample obtained in S3 in acetone or alcohol solution;
[0076] S5: placing the material obtained in step 4 in a plasma nitriding furnace, evacuating the vacuum to 50 Pa, and turning on the voltage, the voltage is 700 V;
[0077] S6: 200 sccm of nitrogen and 200 sccm of hydrogen were introduced in a ratio of 1:1, the temperature in the furnace was adjusted to 900°C, the gas pressure was 200 Pa, and the temperature was kept for 10 hours to obtain a composite strengthening layer;
[0078] S7: The sample is then cooled to room temperature in the furnace and taken out.
[0079] Due to the high nitriding temperature, the surface grains of Comparative Example 4 were coarsened, which affected the formation of the continuous aluminum-rich layer, and the corresponding ablation test results were not as good as those of the embodiment. Figure 8 shown.
[0080] Comparative Example 5
[0081] S1: Grind the TC11 titanium alloy material with sandpaper, and further polish it to a low roughness state (mirror state is best), and clean it in acetone or alcohol solution;
[0082] S2: Place the material obtained in step 1 in a plasma nitriding furnace, evacuate the furnace, and turn on the voltage, which is 700V.
[0083] S3: 200 sccm of nitrogen and 200 sccm of hydrogen are introduced in a ratio of 1:1, the temperature in the furnace is adjusted to 800°C, the gas pressure is 200 Pa, and the temperature is kept for 10 hours to obtain a nitriding layer;
[0084] S4: The sample is then cooled to room temperature in the furnace and taken out.
[0085] Comparative Example 5 is a single nitriding strengthening treatment, and there is no continuous aluminum-rich layer on the secondary surface. Figure 4 As shown, the ablation resistance is affected, and the corresponding hardness, wear and ablation test results are not as good as those in the embodiment. Figure 6 , 7 and 8.
[0086] Comparative Example 6
[0087] TC11 titanium alloy, without any treatment.
[0088] Comparative Example 6 is TC11 titanium alloy, without any treatment, and the corresponding hardness, wear and ablation test results are not as good as those of the embodiment. Figure 6 , 7 and 8.
[0089] The above description is only a preferred embodiment of the present invention, which is only illustrative and not restrictive of the present invention. Those skilled in the art understand that many changes, modifications, and even equivalences may be made to the present invention within the spirit and scope defined by the claims of the present invention, but all of them will fall within the scope of protection of the present invention.
Claims
1. A titanium alloy wear-resistant and ablation-resistant composite strengthening layer and a preparation method thereof, It is characterized in that The following steps are involved: S1, grinding the titanium alloy material, further polishing it to a low roughness state, and cleaning it in acetone or alcohol solution; S2, clamping the titanium alloy obtained in step S1 on a tool, and presetting the Almon strength using an arc height meter; S3, adjust the horizontal distance between the tooling and the shot peening gun muzzle, select the shot peening material, the incident angle of the muzzle, the flow rate and the pressure of the shot peening gun muzzle, and shot peen for 40 seconds to obtain the surface nano-crystallized titanium alloy sample; S4, cleaning the titanium alloy sample obtained in step S3 in acetone or an alcohol solution; S5, placing the material obtained in step S4 in a plasma nitriding furnace, evacuating the furnace, and turning on the voltage; S6, introducing nitrogen, hydrogen / argon, adjusting the temperature and pressure in the furnace, and performing heat preservation nitriding to obtain a composite strengthening layer; S7, then the sample is cooled to room temperature in the furnace and the sample is taken out.
2. A titanium alloy wear-resistant and ablation-resistant composite strengthening layer and a preparation method thereof according to claim 1, It is characterized in that In the step S1, the titanium alloy material is a high-strength TC11 alloy.
3. A titanium alloy wear-resistant and ablation-resistant composite strengthening layer and a preparation method thereof according to claim 1, It is characterized in that In step S2, the titanium alloy material is further polished to a mirror surface.
4. A titanium alloy wear-resistant and ablation-resistant composite strengthening layer and a preparation method thereof as claimed in claim 1, It is characterized in that In step S2, Almon is a type A test piece.
5. A titanium alloy wear-resistant and ablation-resistant composite strengthening layer and a preparation method thereof as claimed in claim 1, It is characterized in that In step S3, the horizontal distance is 120 mm, the shot peening shot is AZB425 ceramic shot, the incident angle is 90°, the flow rate is 3 kg / min, and the key parameter pressure is 0.25-0.50 MPa.
6. A titanium alloy wear-resistant and ablation-resistant composite strengthening layer and a preparation method thereof according to claim 1, It is characterized in that In step S5, the voltage is 600-700V.
7. A titanium alloy wear-resistant and ablation-resistant composite strengthening layer and a preparation method thereof as claimed in claim 1, It is characterized in that In the step S6, the amount of nitrogen gas introduced is 100 to 300 sccm, and the amount of hydrogen gas / argon gas introduced is 100 to 300 sccm.
8. A titanium alloy wear-resistant and ablation-resistant composite strengthening layer and a preparation method thereof as claimed in claim 1, It is characterized in that In the step S6, the nitriding temperature is 750-850°C, the nitriding time is more than 10 hours, and the gas pressure in the furnace is 200-250Pa.
9. A titanium alloy wear-resistant and ablation-resistant composite strengthening layer prepared by the preparation method according to any one of claims 1 to 8.
Citation Information
Patent Citations
Titanium alloy blisk blade machining process method
CN112404913A
Helicon wave plasma nitriding method
CN115927999A
Preparation method of titanium alloy latticed gradient surface modification layer
CN117587356A
Cited By
TC4 titanium alloy surface strengthening layer based on ion implantation and ion nitriding treatment as well as treatment method and application of TC4 titanium alloy surface strengthening layer
CN121046773A
A surface strengthening layer of TC4 titanium alloy based on ion implantation and ion nitriding treatment, a treatment method and application thereof
CN121046773B