A nickel oxide-based target material, a method for preparing the same, and an application thereof
By doping strontium oxide into nickel oxide targets and using a specific process to prepare high-density nickel oxide-based targets, the problem of difficult sintering of nickel oxide targets was solved, the target quality and thin film performance were improved, and the performance of perovskite solar cells was enhanced.
Patent Information
- Application Number
- CN202410898224.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2044-07-05
AI Technical Summary
Existing technologies make it difficult to prepare high-density, high-quality nickel oxide targets, leading to nodules and defects during magnetron sputtering, which affects the performance of thin films.
By using strontium oxide as a dopant for nickel oxide-based targets, high-density nickel oxide-based targets were prepared through ball milling, spray granulation, molding, cold isostatic pressing, and sintering processes, thereby improving their sintering activity and thin film performance.
This improved the sinterability and density of the nickel oxide target, reduced the resistivity and roughness of the thin film, and enhanced the efficiency of the perovskite solar cell.
Abstract
Description
Technical Field
[0001] This invention relates to the field of metal target technology, and in particular to a nickel oxide-based target, its preparation method, and its application. Background Technology
[0002] Magnetron sputtering is a primary process for mass production of NiOx thin films due to its ease of industrial-scale production and the excellent and stable properties of the deposited films. As a raw material for magnetron sputtering, a good nickel oxide target needs high density and uniform, fine grains to avoid nodules and defects generated during magnetron sputtering. However, nickel oxide itself has low sintering reactivity, making sintering difficult and hindering the preparation of high-density nickel oxide targets.
[0003] Therefore, it is necessary to develop a nickel oxide-based target material that can improve sintering performance and target material quality. Summary of the Invention
[0004] The present invention aims to at least solve one of the technical problems existing in the prior art. To this end, the first aspect of the present invention provides a nickel oxide-based target material that can effectively improve the sinterability and density of the nickel oxide target material, and also improve the performance of the nickel oxide-based thin film.
[0005] A second aspect of the present invention also provides a method for preparing a nickel oxide-based target.
[0006] A third aspect of the present invention also provides an application of a nickel oxide-based target.
[0007] According to a first aspect of the present invention, a nickel oxide-based target material is provided, comprising nickel oxide and strontium oxide, wherein the strontium oxide accounts for 0.1% to 20% of the total mass of the nickel oxide-based target material.
[0008] The nickel oxide-based target material according to embodiments of the present invention has at least the following beneficial effects:
[0009] This invention uses strontium oxide as a dopant for nickel oxide-based targets. The introduction of strontium oxide can improve the sinterability and quality of nickel oxide targets, as well as enhance the performance of NiOx films, making them applicable to hole transport layers in perovskite solar cells.
[0010] This is because the strontium oxide of the present invention can undergo a eutectic reaction with nickel oxide, thereby improving its sintering activity and target quality. Furthermore, it can reduce the resistivity and roughness of the nickel oxide film, thus improving the efficiency of perovskite solar cells.
[0011] According to some embodiments of the invention, the strontium oxide accounts for 1% to 20% of the total mass. This includes all values from 1% to 20% and sub-ranges thereof, such as 1%, 5%, 10%, 15%, 20%, or subsets of any two thereof. Thus, within the aforementioned range, the quality of the nickel oxide film prepared by the target material is better.
[0012] According to some embodiments of the present invention, the strontium oxide accounts for 3% to 5% of the total mass. Therefore, when the strontium oxide content is within the above range, the nickel oxide film prepared therefrom has lower resistivity and lower roughness.
[0013] A method for preparing a nickel oxide-based target material according to a second aspect embodiment of the present invention includes the following steps:
[0014] S1. Nickel oxide powder and strontium oxide powder are mixed, ball-milled, and spray-granulated to obtain powder particles;
[0015] S2. The powder particles are molded and then cold isostatically pressed to obtain the raw target material.
[0016] S3. The raw target material is sintered to obtain the target material.
[0017] According to some embodiments of the present invention, the compression molding pressure is 0.1 MPa to 0.8 MPa.
[0018] According to some embodiments of the present invention, the cold isostatic pressure is 200MPa to 250MPa.
[0019] According to some embodiments of the present invention, the sintering step is as follows:
[0020] Heat to 500-750℃ for heat preservation I, then heat to 1400-1700℃ for heat preservation II.
[0021] According to some embodiments of the present invention, the heat preservation time I is 20h to 30h.
[0022] According to some embodiments of the present invention, the heat preservation II time is 24 to 48 hours.
[0023] According to some embodiments of the present invention, the sintering is carried out in an oxygen atmosphere.
[0024] A third aspect of the present invention provides the application of the nickel oxide-based target material described above in the fabrication of optical semiconductor devices.
[0025] Other features and advantages of the invention will be set forth in the description which follows, and will be apparent in part from the description, or may be learned by practicing the invention. Detailed Implementation
[0026] The following are specific embodiments of the present invention, and the technical solutions of the present invention will be further described in conjunction with the embodiments, but the present invention is not limited to these embodiments.
[0027] Unless otherwise specified, the reagents, methods and equipment used in this invention are all conventional reagents, methods and equipment in this technical field.
[0028] Nickel oxide and strontium oxide: Powders must be 4N pure and have a particle size of <100nm; commercially available.
[0029] Example 1
[0030] This example provides a nickel oxide-based target material, the component amounts and preparation method of which are as follows:
[0031] Pure water was added to 5 parts of strontium oxide and 95 parts of nickel oxide powder, then ball-milled and spray-granulated to obtain spherical particles. These particles were then molded at 0.5 MPa and cold isostatically pressed at 230 MPa to obtain a raw target. Finally, the target was heated from room temperature to 600 °C at a rate of 2 °C / min and held for 24 h in an oxygen atmosphere, followed by a heating to 1500 °C at a rate of 5 °C / min and held for 36 h. After natural cooling to room temperature, a strontium-doped nickel oxide-based target was obtained.
[0032] Example 2
[0033] This example provides a nickel oxide-based target material, the component amounts and preparation method of which are as follows:
[0034] Pure water was added to 5 parts of strontium oxide and 95 parts of nickel oxide powder, then ball-milled and spray-granulated to obtain spherical particles. These particles were then molded at 0.1 MPa and cold isostatically pressed at 200 MPa to obtain a raw target. Finally, the target was heated from room temperature to 500 °C at a rate of 2 °C / min and held for 24 h in an oxygen atmosphere, followed by a heating to 1500 °C at a rate of 5 °C / min and held for 24 h. After natural cooling to room temperature, a strontium-doped nickel oxide target was obtained.
[0035] Example 3
[0036] This example provides a nickel oxide-based target material, the component amounts and preparation method of which are as follows:
[0037] Pure water was added to 5 parts of strontium oxide and 95 parts of nickel oxide powder, then ball-milled and spray-granulated to obtain spherical particles. These particles were then molded at 0.8 MPa and cold isostatically pressed at 250 MPa to obtain a raw target. Finally, the target was heated from room temperature to 750 °C at a rate of 2 °C / min and held for 30 h in an oxygen atmosphere, followed by a heating to 1700 °C at a rate of 5 °C / min and held for 48 h. After natural cooling to room temperature, a strontium-doped nickel oxide target was obtained.
[0038] Example 4
[0039] This example provides a nickel oxide-based target material, the component amounts and preparation method of which are as follows:
[0040] Pure water was added to 1 part strontium oxide and 99 parts nickel oxide powder, then ball-milled and spray-granulated to obtain spherical particles. These particles were then molded at 0.5 MPa and cold isostatically pressed at 230 MPa to obtain a raw target. Finally, the target was heated from room temperature to 600 °C at a rate of 2 °C / min and held for 24 h in an oxygen atmosphere, followed by a heating to 1500 °C at a rate of 5 °C / min and held for 36 h. After natural cooling to room temperature, a strontium-doped nickel oxide target was obtained.
[0041] Example 5
[0042] This example provides a nickel oxide-based target material, the component amounts and preparation method of which are as follows:
[0043] Pure water was added to 20 parts of strontium oxide and 80 parts of nickel oxide powder, and then the mixture was ball-milled and spray-granulated to obtain spherical particles. These particles were then molded at 0.5 MPa and cold isostatically pressed at 230 MPa to obtain a raw target. Finally, the target was heated from room temperature to 600 °C at a rate of 2 °C / min and held for 24 h in an oxygen atmosphere, followed by a heating to 1500 °C at a rate of 5 °C / min and held for 36 h. The target was then naturally cooled to room temperature to obtain a strontium-doped nickel oxide target.
[0044] Example 6
[0045] This example provides a nickel oxide-based target material, which is prepared in a manner similar to that of Example 1, except that it contains 10 parts of strontium oxide and 90 parts of nickel oxide.
[0046] Example 7
[0047] This example provides a nickel oxide-based target material, which is prepared in a manner similar to that of Example 1, except that it contains 3 parts of strontium oxide and 97 parts of nickel oxide.
[0048] Comparative Example 1
[0049] This example provides a nickel oxide-based target material, the component amounts and preparation method of which are as follows:
[0050] Pure water was added to 100 parts of nickel oxide powder, then ball-milled and spray-granulated to obtain spherical particles. These particles were then molded at 0.5 MPa and cold isostatically pressed at 230 MPa to obtain a raw target. Finally, the target was heated from room temperature to 600℃ at a rate of 2℃ / min and held for 24 hours in an oxygen atmosphere, followed by a heating to 1500℃ at a rate of 5℃ / min and held for 36 hours. The target was then naturally cooled to room temperature to obtain the nickel oxide target.
[0051] Comparative Example 2
[0052] This example provides a nickel oxide-based target material, the preparation method of which is basically the same as in Example 1. The difference is that, calculated by the total mass of the nickel oxide-based target material, strontium oxide accounts for 0.05% of the total mass, namely 0.05 parts of strontium oxide and 99.95 parts of nickel oxide.
[0053] Comparative Example 3
[0054] This example provides a nickel oxide-based target material, the preparation method of which is basically the same as in Example 1. The difference is that, calculated by the total mass of the nickel oxide-based target material, strontium oxide accounts for 25% of the total mass, namely 25 parts of strontium oxide and 75 parts of nickel oxide.
[0055] Performance testing
[0056] The relative density of the nickel oxide-based targets prepared in Examples 1-7 and the comparative examples of the present invention was tested, and the data are shown in Table 1.
[0057] The nickel oxide-based targets prepared in Examples 1-7 and the comparative examples of this invention were subjected to radio frequency magnetron sputtering (sputtering power 1 kW, cavity vacuum 6.5 × 10⁻⁶). -4 Thin films were prepared by Pa, and the resistivity and root mean square roughness of the prepared films were tested. The data are shown in Table 1.
[0058] Relative density: measured using Archimedes' displacement method;
[0059] Resistivity: Measured using a four-probe DC resistance meter;
[0060] Root mean square roughness of thin film: measured using atomic force microscopy.
[0061] Table 1 Examples 1-7 and Comparative Examples 1-3
[0062] Relative density (%) Resistivity (Ω·cm) Root mean square roughness (nm) Example 1 98.5 <![CDATA[3.8×10 4 ]]> 5.99 Example 2 96.4 <![CDATA[4.8×10 5 ]]> 6.04 Example 3 97.8 <![CDATA[4.5×10 5 ]]> 6.03 Example 4 94.6 <![CDATA[7.7×10 6 ]]> 7.64 Example 5 95.7 <![CDATA[3.6×10 6 ]]> 6.98 Example 6 96.3 <![CDATA[2.4×10 6 ]]> 7.32 Example 7 97.2 <![CDATA[6.2×10 5 ]]> 6.24 Comparative Example 1 90.3 <![CDATA[8.4×10 6 ]]> 8.01 Comparative Example 2 90.5 <![CDATA[8.4×10 6 ]]> 7.96 Comparative Example 3 86.8 <![CDATA[7.3×10 6 ]]> 8.60
[0063] As can be seen from the data in Table 1, by introducing strontium oxide doping into the nickel oxide target, the present invention can improve the relative density of the target and reduce the resistivity and roughness of the thin film produced by the target through magnetron sputtering.
[0064] The present invention has been described in detail above with reference to the embodiments of the present invention. However, the present invention is not limited to the above embodiments. Within the scope of knowledge possessed by those skilled in the art, various changes can be made without departing from the spirit of the present invention.
Claims
1. A nickel oxide-based target material, characterized in that, Composed of nickel oxide and strontium oxide, the strontium oxide accounts for 3% to 5% of the total mass of the nickel oxide-based target material. The nickel oxide-based target material is prepared by the following method: S1. Nickel oxide powder and strontium oxide powder are mixed, ball-milled, and spray-granulated to obtain powder particles; S2. The powder particles are molded and then cold isostatically pressed to obtain the raw target material. S3. The raw target material is sintered to obtain the target material; The sintering steps are as follows: Heat to 500-750℃ and hold for heat I, then heat to 1400-1700℃ and hold for heat II; The sintering is carried out in an oxygen atmosphere.
2. The nickel oxide-based target material according to claim 1, characterized in that, The compression molding pressure is 0.1MPa~0.8MPa.
3. The nickel oxide-based target material according to claim 1, characterized in that, The cold isostatic pressure is 200MPa~250MPa.
4. The nickel oxide-based target material according to claim 1, characterized in that, The heat preservation time is 20 h to 30 h.
5. The nickel oxide-based target material according to claim 1, characterized in that, The heat preservation time II is 24~48h.
6. The application of the nickel oxide-based target according to any one of claims 1 to 5 in the fabrication of optical semiconductor devices.
Citation Information
Patent Citations
NMO oxide semiconductor material and preparation method and application thereof
CN116332623A
Hole transport layer, preparation method thereof and perovskite solar cell
CN117794268A
High-density nickel oxide-based rotating target material and preparation method thereof
CN118206360A