Acid etching solution for etching copper foil and preparation method thereof
By using inorganic acid, oxidant, fluorine source, heterocyclic compound and amino compound in the acid etching solution, the etching rate caused by the increase in copper ion concentration in the existing acid etching solution is solved. The problems of dropping and side corrosion achieve efficient and precise etching effects.
Patent Information
- Application Number
- CN202411141506.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-08-20
AI Technical Summary
During the etching process, the increase in copper ion concentration of existing acid etching liquid leads to a decrease in the etching rate and increase in the side etching, which affects the etching accuracy and efficiency, and the precipitation generation affects the effect.
Using inorganic acids, oxidants, fluorine sources, heterocyclic compounds, amino compounds and corrosion inhibitors, the stable complexes are formed through heterocyclic compounds and amino compounds, the side corrosion is restricted, the copper ion load concentration and etching efficiency are improved, and the copper ion load concentration and etching efficiency are improved, and the The stabilizer forms a protective film to reduce precipitation.
The copper ion load concentration and etching rate of the etching liquid are improved, the degree of side etching and precipitation content are reduced, the etching accuracy and efficiency are ensured, and the temperature range is adapted to a certain market prospect.
Abstract
Description
Technical Field
[0001] The present application relates to the field of etching liquid, and in particular to an acidic etching liquid for etching copper foil and a preparation method thereof. Background Art
[0002] Acidic etching solution is a commonly used etching medium and is widely used in the manufacturing process of printed circuit boards (PCBs). In PCB manufacturing, it is necessary to accurately etch away the unwanted parts of the copper foil to form the desired circuit pattern.
[0003] At present, etching solutions for etching the copper foil covered on the substrate include acid copper chloride, alkaline copper chloride, sulfuric acid / hydrogen peroxide, ferric chloride, sulfuric acid / chromic acid and other etching systems. Although the above etching solutions have a faster etching rate and better etching uniformity, there are still some problems. For example, as the etching process proceeds, the copper ion concentration in the etching solution gradually increases. After reaching a certain level, the etching rate will drop significantly, affecting the etching efficiency; increasing the degree of side etching, affecting the etching accuracy; precipitation will be generated on the substrate surface and in the solution, thereby affecting the etching effect, etc., all of which limit the effect of the above etching solutions in practical applications.
[0004] The present application aims to provide an excellent acidic etching solution for copper foil to solve the above-mentioned problems. The etching solution can effectively increase the copper ion loading concentration of the etching solution without significantly affecting the etching efficiency, and at the same time avoids the problems of increasing the degree of side etching and reducing the etching accuracy, and greatly reduces the precipitation content on the substrate surface and in the solution. On the other hand, the etching solution of the present application also has an excellent etching rate and can adapt to a certain degree of etching temperature, and has very excellent market and application prospects. Summary of the invention
[0005] In order to solve the above problems, the first aspect of the present application provides an acidic etching solution for etching copper foil. The raw materials are, by mass percentage, 20-40% inorganic acid, 4-6% oxidant, 0.1-0.3% fluorine source, 0.2-0.4% heterocyclic compound, 1.2-2.4% amino compound, 1.5-4% corrosion inhibitor, 0.1-0.2% stabilizer, and deionized water to make up the balance.
[0006] As a preferred solution, the mass ratio of the fluorine source, the heterocyclic compound and the amino compound is (0.1-0.25): (0.25-0.35): (1.5-2.2).
[0007] As a preferred solution, the mass ratio of the fluorine source, the heterocyclic compound and the amino compound is (0.15-0.2): (0.28-0.3): (1.8-2).
[0008] As a preferred solution, the inorganic acid is a combination of nitric acid and hydrochloric acid.
[0009] As a preferred solution, the mass ratio of nitric acid to hydrochloric acid is (5-8):(0.5-1).
[0010] As a preferred solution, the mass ratio of nitric acid to hydrochloric acid is (6-7):(0.6-0.8).
[0011] As a preferred solution, the concentration of the inorganic acid is 30-95wt%.
[0012] As a preferred solution, the oxidant is at least one of hydrogen peroxide, perbenzoic acid, sodium hypochlorite and ferric chloride.
[0013] As a preferred solution, the oxidant is a combination of hydrogen peroxide, sodium hypochlorite and ferric chloride.
[0014] As a preferred solution, the mass ratio of hydrogen peroxide, sodium hypochlorite and ferric chloride is (3-4): (1-1.5): (0.2-0.3).
[0015] As a preferred solution, the mass ratio of hydrogen peroxide, sodium hypochlorite and ferric chloride is (3.2-3.5): (1.2-1.3): (0.2-0.25).
[0016] As a preferred solution, the fluorine source is hydrofluoric acid.
[0017] As a preferred solution, the heterocyclic compound is at least one of 3-amino-1,2,4-triazole, 2-aminothiazole, 6-nitrobenzimidazole, methylbenzotriazole, and 2-mercaptobenzothiazole.
[0018] As a preferred solution, the heterocyclic compound is a combination of 2-mercaptobenzothiazole and 6-nitrobenzimidazole.
[0019] As a preferred solution, the mass ratio of 2-mercaptobenzothiazole to 6-nitrobenzimidazole is (4-4.5):(1-2).
[0020] As a preferred solution, the mass ratio of 2-mercaptobenzothiazole to 6-nitrobenzimidazole is (4.2-4.4):(1.4-1.6).
[0021] As a preferred solution, the amino compound is at least one of trishydroxymethylaminomethane, diethanolamine, tetramethylammonium oxide, triethanolamine, diethylaminopropylamine, dimethylethanolamine, and propylenediamine.
[0022] As a preferred solution, the amino compound is a combination of trishydroxymethylaminomethane, diethylaminopropylamine and propylenediamine.
[0023] As a preferred solution, the mass ratio of trishydroxymethylaminomethane, diethylaminopropylamine and propylenediamine is (3-4): (0.5-1): (1.2-1.8).
[0024] As a preferred solution, the mass ratio of trishydroxymethylaminomethane, diethylaminopropylamine and propylenediamine is (3.2-3.5): (0.6-0.8): (1.4-1.6).
[0025] In this application, by selecting the above-mentioned heterocyclic compounds and amino compounds to act together with hydrofluoric acid, the etching accuracy and efficiency of the acidic etching solution are greatly improved, and the side etching degree and precipitation content are reduced. Through the joint action of the above-mentioned heterocyclic compounds and amino compounds, the contact of the oxidant and the fluorine source with the metal is accelerated. At the same time, a good complex is formed between the heteroatoms in the heterocyclic compounds and the metal surface, thereby limiting the influence of the etching solution on the side, and as the etching process proceeds, the stable complex inside the etching solution system formed by the heterocyclic compounds and amino compounds stabilizes the chemical balance in the etching solution, thereby reducing the overall precipitation content while ensuring etching accuracy and efficiency.
[0026] As a preferred solution, the corrosion inhibitor is a combination of imidazolines and azoles.
[0027] As a preferred solution, the mass ratio of the imidazolines to the azoles is (1.5-2):(3-3.5).
[0028] As a preferred solution, the imidazoline is oleyl hydroxyethyl imidazoline or oleyl aminoethyl imidazoline.
[0029] As a preferred solution, the imidazoline is oleylaminoethyl imidazoline.
[0030] As a preferred solution, the azole is at least one of tolyltriazole, 3-aminotriazole and mercaptobenzotriazole.
[0031] As a preferred solution, the azole is a combination of toluene triazole and mercaptobenzotriazole.
[0032] As a preferred solution, the mass ratio of methylbenzotriazole to mercaptobenzotriazole is (6-8):(2-3).
[0033] As a preferred solution, the mass ratio of methylbenzotriazole to mercaptobenzotriazole is (7-7.5):(2-2.5).
[0034] As a preferred solution, the stabilizer is at least one of sodium hydroxysulfonate, ammonium chloride, citric acid, and ethylenediaminetetraacetic acid.
[0035] As a preferred solution, the stabilizer is a combination of sodium hydroxysulfonate and ethylenediaminetetraacetic acid.
[0036] As a preferred solution, the mass ratio of the sodium hydroxysulfonate to ethylenediaminetetraacetic acid is (1-1.5): (0.5-1).
[0037] In the present application, the above-mentioned stabilizer and corrosion inhibitor are used in combination to form a protective film of suitable thickness by combining with the metal atoms on the surface, thereby limiting the contact degree between the etching solution and the panel, thereby protecting the local structure and avoiding excessive corrosion and side corrosion caused by excessive penetration of the etching solution. Moreover, through the complexation of the etching solution system, the stable complex formed can greatly improve its absorption degree for metal particles, thereby greatly improving its etching efficiency during etching operation, thereby obtaining good etching accuracy and reducing unnecessary precipitation content.
[0038] The second aspect of the present application provides a method for preparing the above-mentioned acidic etching solution for etching copper foil, which specifically comprises the following steps: slowly adding inorganic acid to deionized water and stirring evenly, then adding the remaining raw materials in sequence, heating to 45-55°C, stirring at 40-60rpm until the solution is uniform, and then naturally cooling the solution to 25°C.
[0039] The beneficial effects of this application are:
[0040] 1. The present application provides an acidic etching solution for etching copper foil, which can effectively increase the copper ion loading concentration of the etching solution without significantly affecting the etching efficiency, and at the same time avoids the problems of increasing the degree of side etching and reducing the etching accuracy, and greatly reduces the precipitation content on the substrate surface and in the solution. On the other hand, the etching solution of the present application also has an excellent etching rate and can adapt to a certain degree of etching temperature, and has very excellent market and application prospects.
[0041] 2. The acidic etching solution for etching copper foil provided in the present application accelerates the contact of the oxidant and the fluorine source with the metal through the joint action of the heterocyclic compound and the amino compound. At the same time, the heteroatoms in the heterocyclic compound form a good complex with the metal surface, thereby limiting the influence of the etching solution on the side. As the etching process proceeds, the stable complex inside the etching solution system formed by the heterocyclic compound and the amino compound stabilizes the chemical balance in the etching solution, thereby reducing the overall precipitation content while ensuring the etching accuracy and efficiency.
[0042] 3. The acidic etching solution for etching copper foil provided in the present application, the compound use of its specific stabilizer and corrosion inhibitor, can combine with the metal atoms on the surface to form a protective film of suitable thickness, limit the contact degree between the etching solution and the panel, thereby protecting the local structure, avoiding excessive corrosion and side corrosion caused by excessive penetration of the etching solution, and through the complexation of the etching solution system, the stable complex formed can greatly improve its absorption degree of metal particles, thereby greatly improving its etching efficiency during etching operation, thereby obtaining good etching accuracy and reducing unnecessary precipitation content. DETAILED DESCRIPTION
[0043] The following will further explain and demonstrate the technical solutions in the above invention content of this application in the form of specific implementation schemes. The following embodiments are only practical examples used to illustrate and explain the contents of the technical solutions in the specification, and should not limit the scope of the claims to be protected by this application. All technical products based on the technical solutions described in the invention content of this application should be included in the scope to be protected by this application.
[0044] In the following examples, unless otherwise specified, the raw materials are all commercially available products, or can be prepared by methods well known to those skilled in the art.
[0045] Example 1
[0046] Embodiment 1 The first aspect provides an acidic etching solution for etching copper foil. The raw materials are, by mass percentage, 30% inorganic acid, 4.5% oxidant, 0.18% fluorine source, 0.28% heterocyclic compound, 1.95% amino compound, 2.2% corrosion inhibitor, 0.18% stabilizer, and deionized water to make up the balance.
[0047] The inorganic acid is a composition of nitric acid and hydrochloric acid, the mass ratio of the two is 6.5:0.8, the concentration of nitric acid is 68wt%, and the concentration of hydrochloric acid is 36.5wt%.
[0048] The oxidant is a combination of hydrogen peroxide, sodium hypochlorite and ferric chloride, and the mass ratio of the three is 3.4:1.2:0.2.
[0049] The fluorine source is hydrofluoric acid.
[0050] The heterocyclic compound is a composition of 2-mercaptobenzothiazole and 6-nitrobenzimidazole, and the mass ratio of the two is 4.2:1.5.
[0051] The amino compound is a composition of trishydroxymethylaminomethane, diethylaminopropylamine and propylenediamine, and the mass ratio of the three is 3.4:0.7:1.5.
[0052] The corrosion inhibitor is a composition of imidazolines and azoles, and the mass ratio of the two is 1.8:3.2.
[0053] The imidazoline is oleylaminoethyl imidazoline; the azole is a combination of toluene triazole and mercapto benzotriazole, and the mass ratio of the two is 7.4:2.1.
[0054] The stabilizer is a composition of sodium hydroxysulfonate and ethylenediaminetetraacetic acid, and the mass ratio of the two is 1.2:0.8.
[0055] The second aspect of the present embodiment provides a method for preparing the above-mentioned acidic etching solution for etching copper foil, which specifically includes the following steps: slowly adding inorganic acid to deionized water and stirring evenly, then adding the remaining raw materials in sequence, heating to 50°C, stirring at 50 rpm until the solution is uniform, and then naturally cooling the solution to 25°C.
[0056] Example 2
[0057] Example 2 The first aspect provides an acidic etching solution for etching copper foil. The raw materials are, by mass percentage, 30% inorganic acid, 4.5% oxidant, 0.12% fluorine source, 0.32% heterocyclic compound, 2.2% amino compound, 2.2% corrosion inhibitor, 0.18% stabilizer, and deionized water to make up the balance.
[0058] The inorganic acid is a composition of nitric acid and hydrochloric acid, the mass ratio of the two is 5.5:1, the concentration of nitric acid is 68wt%, and the concentration of hydrochloric acid is 36.5wt%.
[0059] The oxidant is a combination of hydrogen peroxide, sodium hypochlorite and ferric chloride, and the mass ratio of the three is 3.8:1.1:0.3.
[0060] The fluorine source is hydrofluoric acid.
[0061] The heterocyclic compound is a composition of 2-mercaptobenzothiazole and 6-nitrobenzimidazole, and the mass ratio of the two is 4.2:1.5.
[0062] The amino compound is a composition of trishydroxymethylaminomethane, diethylaminopropylamine and propylenediamine, and the mass ratio of the three is 3.4:0.7:1.5.
[0063] The corrosion inhibitor is a composition of imidazolines and azoles, and the mass ratio of the two is 1.8:3.2.
[0064] The imidazoline is oleylaminoethyl imidazoline; the azole is a combination of toluene triazole and mercapto benzotriazole, and the mass ratio of the two is 7.4:2.1.
[0065] The stabilizer is a composition of sodium hydroxysulfonate and ethylenediaminetetraacetic acid, and the mass ratio of the two is 1.2:0.8.
[0066] The second aspect of the present embodiment provides a method for preparing the above-mentioned acidic etching solution for etching copper foil, which specifically includes the following steps: slowly adding inorganic acid to deionized water and stirring evenly, then adding the remaining raw materials in sequence, heating to 50°C, stirring at 50 rpm until the solution is uniform, and then naturally cooling the solution to 25°C.
[0067] Comparative Example 1
[0068] The specific implementation of this comparative example is basically the same as that of Example 1, except that the acidic etching solution for etching the copper foil has the following raw materials, by mass percentage: 30% inorganic acid, 4.5% oxidant, 0.18% fluorine source, 0.12% heterocyclic compound, 4.2% amino compound, 2.2% corrosion inhibitor, 0.18% stabilizer, and the balance is supplemented by deionized water.
[0069] Comparative Example 2
[0070] The specific implementation of this comparative example is basically the same as that of Example 1, except that the acidic etching solution for etching the copper foil has the following raw materials, by mass percentage: 30% inorganic acid, 4.5% oxidant, 0.18% fluorine source, 0.45% heterocyclic compound, 0.85% amino compound, 2.2% corrosion inhibitor, 0.18% stabilizer, and the balance is supplemented by deionized water.
[0071] Comparative Example 3
[0072] The specific implementation of this comparative example is substantially the same as that of Example 1, except that the heterocyclic compound is a composition of 2-mercaptobenzothiazole and 6-nitrobenzimidazole, and the mass ratio of the two is 6:0.5.
[0073] Comparative Example 4
[0074] The specific implementation of this comparative example is basically the same as that of Example 1, except that the heterocyclic compound is a combination of 4-dimethylaminopyridine and 3-methylpyrrole, with a mass ratio of 4.2:1.5.
[0075] Comparative Example 5
[0076] The specific implementation of this comparative example is basically the same as that of Example 1, except that the amino compound is a composition of trishydroxymethylaminomethane, diethylaminopropylamine and propylenediamine, and the mass ratio of the three is 1:1:0.2.
[0077] Comparative Example 6
[0078] The specific implementation of this comparative example is basically the same as that of Example 1, except that the amino compound is a combination of formamide and isopropylamine, with a mass ratio of 3.4:0.7.
[0079] Comparative Example 7
[0080] The specific implementation of this comparative example is basically the same as that of Example 1, except that the azole is a combination of toluene triazole and mercapto benzotriazole, and the mass ratio of the two is 8:0.5.
[0081] Comparative Example 8
[0082] The specific implementation of this comparative example is substantially the same as that of Example 1, except that the mass ratio of sodium hydroxysulfonate to ethylenediaminetetraacetic acid is 1:3.
[0083] Comparative Example 9
[0084] The specific implementation of this comparative example is basically the same as that of Example 1, except that the stabilizer is a combination of sodium bisulfite and sodium toluenesulfonate, with a mass ratio of 1.2:0.8.
[0085] Comparative Example 10
[0086] The specific implementation of this comparative example is substantially the same as that of Example 1, except that the mass ratio of imidazolines to azoles is 3:1.
[0087] Performance Evaluation
[0088] The etching solutions prepared in the examples and comparative examples were tested by static suspension test. The size of the copper foil of the test circuit board was 7.8 cm × 10 cm × 0.01 cm, (ρ = 9.11 g / cm 3 ), etching time is 4 min, and etching temperature is 45 °C.
[0089] 1. Use the weight loss method to calculate the etching rate of the etching solution on the copper foil of the circuit board, record the thickness of the copper etched by the etching solution per unit time, and take the average value of 10 tests and record it in Table 1.
[0090] 2. Calculate the cross section of the etched copper foil by SEM observation and calculate the etching factor, etching factor = 2 × copper line width / (bottom width of circuit pattern - top width of circuit pattern). Take the average value of 10 tests and record it in Table 1.
[0091] 3. After etching is completed, observe by SEM whether there is any obvious residue left.
[0092] Table 1 Performance test results
[0093] Example Etching rate (μm / min) Etching Factor Residue Retention Example 1 24.98 8.12 No retention Example 2 24.44 8.07 No retention Comparative Example 1 22.64 6.24 Small amount of retention Comparative Example 2 21.98 7.17 Micro-retention Comparative Example 3 22.61 7.54 No retention Comparative Example 4 22.17 7.39 No retention Comparative Example 5 21.91 6.62 Small amount of retention Comparative Example 6 21.64 6.74 Small amount of retention Comparative Example 7 22.07 7.07 Micro-retention Comparative Example 8 20.7 6.98 Micro-retention Comparative Example 9 22.2 6.91 Micro-retention Comparative Example 10 21.9 7.01 Micro-retention
[0094] It can be seen from the examples and comparative examples of the present application and the data results in Table 1 that Examples 1 and 2 of the present application have obvious advantages over comparative examples 1 to 10 in terms of etching rate, side etching degree and precipitation content performance. This is mainly due to the combined effect of the raw material scheme specified in the present application. Comparative examples 1 to 10 did not adopt the technical scheme specified in the present application, resulting in obvious disadvantages in the above-mentioned performance tests. This further proves the necessity of the technical scheme specified in the present application for the technical effect of the present application and solving technical problems.
Claims
1. An acidic etching solution for etching copper foil, characterized in that: The acidic etching solution for etching copper foil comprises, by mass percentage, 20-40% of inorganic acid, 4-6% of oxidant, 0.1-0.3% of fluorine source, 0.2-0.4% of heterocyclic compound, 1.2-2.4% of amino compound, 1.5-4% of corrosion inhibitor, 0.1-0.2% of stabilizer, and the balance is supplemented by deionized water; The mass ratio of the fluorine source, the heterocyclic compound and the amino compound is (0.1-0.25): (0.25-0.35): (1.5-2.2); The inorganic acid is a combination of nitric acid and hydrochloric acid; the mass ratio of the nitric acid to the hydrochloric acid is (5-8): (0.5-1); The concentration of the inorganic acid is 30 to 95 wt %; The oxidant is at least one of hydrogen peroxide, perbenzoic acid, sodium hypochlorite, and ferric chloride; The heterocyclic compound is at least one of 3-amino-1,2,4-triazole, 2-aminothiazole, 6-nitrobenzimidazole, methylbenzotriazole, and 2-mercaptobenzothiazole; The amino compound is at least one of trishydroxymethylaminomethane, diethanolamine, tetramethylammonium oxide, triethanolamine, diethylaminopropylamine, dimethylethanolamine, and propylenediamine; The corrosion inhibitor is a composition of imidazolines and azoles; the mass ratio of the imidazolines to the azoles is (1.5-2): (3-3.5); The imidazoline is oleyl hydroxyethyl imidazoline or oleyl aminoethyl imidazoline; The azole is at least one of toluene triazole, 3-amino triazole and mercapto benzotriazole; The stabilizer is at least one of sodium hydroxysulfonate, ammonium chloride, citric acid, and ethylenediaminetetraacetic acid.
2. The acidic etching solution for etching copper foil according to claim 1, characterized in that: The oxidant is a combination of hydrogen peroxide, sodium hypochlorite and ferric chloride.
3. The acidic etching solution for etching copper foil according to claim 2, characterized in that: The mass ratio of hydrogen peroxide, sodium hypochlorite and ferric chloride is (3-4): (1-1.5): (0.2-0.3).
4. The acidic etching solution for etching copper foil according to claim 3, characterized in that: The fluorine source is hydrofluoric acid.
5. The acidic etching solution for etching copper foil according to claim 4, characterized in that: The heterocyclic compound is a combination of 2-mercaptobenzothiazole and 6-nitrobenzimidazole.
6. The acidic etching solution for etching copper foil according to claim 5, characterized in that: The mass ratio of the 2-mercaptobenzothiazole to the 6-nitrobenzimidazole is (4-4.5):(1-2).
7. The acidic etching solution for etching copper foil according to claim 6, characterized in that: The amino compound is a composition of tris(hydroxymethyl)aminomethane, diethylaminopropylamine and propylenediamine; the mass ratio of tris(hydroxymethyl)aminomethane, diethylaminopropylamine and propylenediamine is (3-4):(0.5-1):(1.2-1.8).
8. The acidic etching solution for etching copper foil according to claim 7, characterized in that: The azoles are a combination of toluene triazole and mercaptobenzotriazole; the mass ratio of toluene triazole to mercaptobenzotriazole is (6-8):(2-3).
9. The acidic etching solution for etching copper foil according to claim 8, characterized in that: The stabilizer is a composition of sodium hydroxysulfonate and ethylenediaminetetraacetic acid; the mass ratio of the sodium hydroxysulfonate and ethylenediaminetetraacetic acid is (1-1.5): (0.5-1).
10. A method for preparing an acidic etching solution for etching copper foil according to any one of claims 1 to 9, characterized in that: The specific steps include: Slowly add the inorganic acid into the deionized water and stir evenly, then add the remaining raw materials in sequence, raise the temperature to 45-55°C, stir at 40-60 rpm until the solution is uniform, and then naturally cool the solution to 25°C to obtain the product.
Citation Information
Patent Citations
Etchant composition for copper / molybdenum alloy film
CN103890232A
Acid etching liquid for copper-titanium film of advanced flat
CN106086891A
Etching liquid composition and application thereof
CN113106453A
Etching liquid composition, preparation method and etching method
CN116162934A
Etchant composition and method
US20100252530A1
Cited By
Metal etching preparation process
CN119506883A
Metal etching fabrication process
CN119506883B
Etching solution and preparation method thereof
CN121203666A