Green corrosion inhibitor for cooling water system

By using green corrosion inhibitors in the cooling water system, the problems of poor corrosion effect and environmental pollution of the corrosion inhibitors are solved, and excellent corrosion inhibition effect and environmental protection performance for a variety of materials are achieved. It is suitable for a variety of cooling water systems.

CN118880340APending Publication Date: 2024-11-01SUZHOU NUCLEAR POWER RES INST CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410907615.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The corrosion inhibitors used in existing cooling water systems have poor corrosion effects, high nitrogen and phosphorus content, and environmental pollution problems, and microbial corrosion and substances such as phosphate and chromium cause harm to the equipment and the environment.

Method used

A green corrosion inhibitor is used, and the composition includes bactericides, dispersants, alkaline amino acid derivatives, azoles and alkalizing agents. The preparation method is used to generate bactericides and dispersants to form a protective film to slow down corrosion and control pH. Values ​​to adapt to different cooling water systems and avoid the use of phosphorus and chromium.

Benefits of technology

Effectively reduce microbial corrosion, improve the corrosion inhibition effect of various materials, and reduce the negative impact on the environment. It is suitable for various cooling water systems, comply with environmental protection regulations, and improves the operation level of equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118880340A_ABST
    Figure CN118880340A_ABST
Patent Text Reader

Abstract

The invention provides a green corrosion inhibitor for a cooling water system, and particularly relates to the field of corrosion prevention of the cooling water system. Based on the total mass of the corrosion inhibitor, the corrosion inhibitor is prepared from the following raw material components in percentage by weight: 5 to 10 percent of bactericide, 1 to 2 percent of dispersant, 40 to 80 percent of alkaline amino acid derivative, 0.2 to 1.0 percent of azole substance, 0.6 to 3.0 percent of basifier and the balance of water. The phosphorus-free corrosion inhibitor does not contain phosphorus, introduction of microbial nutrient substances can be reduced, the added bactericide can inhibit the growth process of microorganisms and reduce microbial corrosion, and meanwhile, through the combined action of multiple mechanisms, the corrosion inhibitor has excellent compatibility and corrosion inhibition effect on multiple materials such as carbon steel and copper alloy. Furthermore, the corrosion inhibitor does not contain phosphate and chromium, and can effectively reduce negative effects on the environment and an ecological system, so that the corrosion inhibitor can be widely applied to various cooling water systems.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of cooling water system anticorrosion, and in particular to a green corrosion inhibitor for a cooling water system. Background Art

[0002] The closed cooling water system (CCW) of a nuclear power plant is an important part of the nuclear power plant. Its main function is to provide cooling water for the heat exchange equipment of the nuclear power plant to ensure that the temperature of these equipment is effectively controlled during operation, thereby ensuring the safe and stable operation of the nuclear power plant. The equipment of the closed cooling water system is mostly made of metal materials such as carbon steel, stainless steel, and copper alloy, with carbon steel being the main material. It is often corroded by cooling water during operation, so appropriate corrosion protection measures need to be taken.

[0003] At present, the cooling water systems of domestic nuclear power plants mostly adopt the method of adding composite corrosion inhibitors for corrosion protection. The corrosion inhibitor monomers include phosphates, nitrites, molybdates, chromates, etc., among which phosphates are the most widely used. Traditional corrosion inhibitors have the following problems: 1. As the operation time of nuclear power plants increases, the degree of equipment aging increases, and the loose corrosion products covering the surface of the equipment will become active oxygen adsorption sites, thereby aggravating the corrosion process and easily causing suspended matter and Fe and Cu content to exceed the standard during the operation stage. 2. The nitrogen and phosphorus in the corrosion inhibitor are nutrients for certain microorganisms. The metabolic activities of microorganisms on the metal surface interact with the corrosion process, endangering the structural integrity of nuclear power plant pipelines and components; and the phosphorus and chromium in phosphate and chromate corrosion inhibitors will also pollute the environment. Summary of the invention

[0004] In view of the above shortcomings of the prior art, the present invention provides a green corrosion inhibitor for a cooling water system to improve the problems of poor corrosion inhibition effect and high nitrogen and phosphorus content of the existing corrosion inhibitors.

[0005] To achieve the above-mentioned purpose and other related purposes, the present invention provides a green corrosion inhibitor for a cooling water system. Based on the total mass of the corrosion inhibitor, the corrosion inhibitor is composed of the following raw material components in weight percentage: 5-10% bactericide, 1%-2% dispersant, 40%-80% basic amino acid derivatives, 0.2%-1.0% azole substances, 0.6%-3% alkalizer, and the rest is water.

[0006] In one example of the present invention, for a copper-containing cooling water system, the content of the alkalizer is 0.6% to 1.5%; for a copper-free cooling water system, the content of the alkalizer is 0.6% to 3.0%.

[0007] In an example of the present invention, the fungicide includes a compound derived from o-hydroxycinnamic acid lactone.

[0008] In an example of the present invention, the dispersant includes a polyacrylic acid dispersant.

[0009] In one example of the present invention, the basic amino acid derivative includes any one or both of a histidine derivative and a lysine derivative.

[0010] In one example of the present invention, the alkalizing agent includes any one or more of ammonia water, ethanolamine and sodium hydroxide.

[0011] In an example of the present invention, the azole substance includes any one or more of 4-methyl-2-phenylimidazole, 5-methyl-benzotriazole, and methylbenzotriazole.

[0012] In one example of the present invention, the bactericide is prepared by:

[0013] adding a solvent and a coumarin derivative into a container, wherein the coumarin derivative is dissolved in the solvent;

[0014] Add chitosan to the solvent in which the coumarin derivative is dissolved and start stirring;

[0015] Introducing an inert gas into the container and performing a reaction at a set temperature;

[0016] After the reaction is completed, the solvent is removed to obtain the fungicide.

[0017] In an example of the present invention, the mass ratio of the coumarin derivative to the chitosan is 2:1 to 4:1.

[0018] In one example of the present invention, the reaction temperature of the coumarin derivative and the chitosan is 0-5° C., and the reaction time is 4-10 h.

[0019] The green corrosion inhibitor for cooling water system of the present application does not contain phosphorus, which can not only reduce the introduction of microbial nutrients, but also the added bactericide can inhibit the growth process of microorganisms, reduce microbial corrosion, and simultaneously act together through multiple mechanisms (film formation, increase in corrosion reaction energy barrier, synergistic effect), and has excellent compatibility and corrosion inhibition effect on various materials such as carbon steel and copper alloy. Further, the corrosion inhibitor of the present invention does not contain phosphate and chromium, which can effectively reduce the negative impact on the environment and ecosystem, so the corrosion inhibitor of the present application can be widely used in various cooling water systems. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 The macroscopic morphology of 20# carbon steel after corrosion inhibition performance test in different cooling waters: a is without corrosion inhibitor; b is with the corrosion inhibitor prepared in the comparative example; c is with the corrosion inhibitor prepared in Example 1; d is with the corrosion inhibitor prepared in Example 2;

[0021] Figure 2 The scanning electron microscope images of 20# carbon steel after the corrosion inhibition performance test in different cooling waters; a is without corrosion inhibitor; b is with the corrosion inhibitor prepared in the comparative example; c is with the corrosion inhibitor prepared in Example 1; d is with the corrosion inhibitor prepared in Example 2;

[0022] Figure 3 The macroscopic morphology of T2 copper alloy after corrosion inhibition performance test in different cooling waters: a is without corrosion inhibitor; b is with corrosion inhibitor prepared in comparative example; c is with corrosion inhibitor prepared in Example 1; d is with corrosion inhibitor prepared in Example 2;

[0023] Figure 4 These are scanning electron microscope images of T2 copper alloy after corrosion inhibition performance tests in different cooling waters: a is without corrosion inhibitor; b is with the addition of corrosion inhibitor prepared in comparative example; c is with the addition of corrosion inhibitor prepared in Example 1; d is with the addition of corrosion inhibitor prepared in Example 2. DETAILED DESCRIPTION

[0024] The following is an explanation of the embodiments of the present invention by specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention. It should be noted that the features in the following embodiments and the embodiments can be combined with each other without conflict. It should also be understood that the terms used in the embodiments of the present invention are intended to describe specific embodiments, rather than to limit the scope of protection of the present invention. The test methods for which specific conditions are not specified in the following examples are usually carried out under conventional conditions or according to the conditions recommended by the manufacturers.

[0025] In this article, when it comes to numerical ranges, unless otherwise specified, the distribution of optional values ​​within the numerical range is considered continuous and includes the two numerical endpoints (i.e., the minimum value and the maximum value) of the numerical range, as well as every value between the two numerical endpoints. When multiple numerical ranges are provided to describe features or characteristics, these numerical ranges can be combined.

[0026] It should be noted that, unless otherwise specified, "%" herein represents mass percentage.

[0027] The invention provides a green corrosion inhibitor for a cooling water system. Based on the total mass of the corrosion inhibitor, the corrosion inhibitor is composed of the following raw material components in weight percentage: 5-10% of a bactericide, 1%-2% of a dispersant, 40%-80% of a basic amino acid derivative, 0.2%-1.0% of an azole substance, 0.6%-3.0% of an alkalizer, and the remainder being water.

[0028] The role of the bactericide in the present application is as follows: microorganisms in cooling water are prone to form microbial corrosion on metal surfaces, that is, the secretions of intermediate products and / or final products of microbial cell metabolism will cause corrosion to the metal surface. Adding a bactericide to the corrosion inhibitor can inhibit the growth of microorganisms and reduce the corrosion rate of the metal surface. The amount of bactericide added to the corrosion inhibitor of the present application is 5-10%, for example, 5%, 8% or 10%. In one embodiment, the bactericide is selected from o-hydroxycinnamic acid lactone derivative compounds, which have good antioxidant properties and help reduce oxidative corrosion on metal surfaces. In addition, o-hydroxycinnamic acid lactone derivative compounds are environmentally friendly due to their natural origin and biodegradability.

[0029] Exemplarily, the o-hydroxycinnamic acid lactone derivative compound is prepared by reacting a coumarin derivative with chitosan, and the preparation method thereof comprises the following steps:

[0030] S1. Adding a coumarin derivative and a solvent into a container, wherein the coumarin derivative is dissolved in the solvent;

[0031] S2, adding chitosan to the solvent in which the coumarin derivative is dissolved and starting stirring;

[0032] S3, introducing an inert gas into the container and reacting at a set temperature;

[0033] S4. After the reaction is completed, the solvent is removed to obtain an o-hydroxycinnamic acid lactone derivative compound.

[0034] In step S1, the solvent is an organic solvent with high solubility for coumarin derivatives. For example, the solvent is 5% acetone. In other embodiments, the solvent may also be other organic solvents that meet the reaction requirements.

[0035] In step S2, the mass ratio of the coumarin derivative to chitosan is 2:1 to 4:1, for example, 2:1, 3:1 or 4:1.

[0036] In step S3, the reaction temperature of the coumarin derivative and chitosan is 0-5°C, for example, 0°C, 2°C, 4°C or 5°C; the reaction time is 4-10h, for example, 4h, 6h, 8h or 10h. In one embodiment, nitrogen is selected as the inert gas, and in other embodiments, any other inert gas that can meet the reaction requirements can also be selected, such as argon or helium.

[0037] In step S4, the solvent may be removed by evaporation, such as rotary evaporation.

[0038] The o-hydroxycinnamic acid lactone derivative compounds prepared with coumarin derivatives and chitosan as raw materials contain a large number of hydroxyl (-OH) and amino (-NH2), which can form strong chemical adsorption on the metal surface, help to form a protective film on the metal surface, thereby slowing down the corrosion process.

[0039] In one embodiment, the coumarin derivative is 7-methyl acyl chloride coumarin, and the specific reaction between the coumarin derivative and chitosan is as follows:

[0040]

[0041] In one embodiment, the dispersant is an ionic polymer dispersant rich in carboxyl groups. Under alkaline conditions, the carboxyl groups (-COOH) in the dispersant bind to the active sites on the surface of the iron oxide particles to establish a charged layer around the oxide particles to reduce the aggregation and deposition of corrosion products. Exemplarily, the dispersant is a polyacrylic acid dispersant, including polyacrylic acid (PAA). The dispersant may also be other carboxyl-rich compounds that can achieve the effect of forming a charged layer around the metal oxide.

[0042] In one embodiment, the alkalizer includes any one or more of ammonia water, ethanolamine and sodium hydroxide. The alkalizer can be any one of the above-mentioned alkalizers, such as ammonia water, ethanolamine or sodium hydroxide, or any two or three combinations of the above-mentioned alkalizers, such as a combination of ammonia water and ethanolamine, a combination of ammonia water and sodium hydroxide, a combination of ethanolamine and ammonia water, and a combination of ammonia water, ethanolamine and sodium hydroxide. When the alkalizer is added in a combined form, the ratio of its components is not limited and can be mixed in any proportion. In other embodiments, the alkalizer can also be an alkaline chemical substance not listed above, which meets the use requirements.

[0043] For copper-containing cooling water systems, if the pH of the cooling water is too high, NH3 in the cooling water will combine with copper ions to form a complex, accelerating the corrosion of copper. Therefore, in this application, for copper-containing cooling water systems, the content of the alkalizer in the corrosion inhibitor is 0.6% to 1.5%, such as 0.6%, 0.9%, 1.2% or 1.5%, and the pH of the copper-containing cooling water system is controlled at 9.0 to 10.5, such as 9.0, 10.0 or 10.5 when used; for copper-free cooling water systems, the content of the alkalizer in the corrosion inhibitor is 0.6% to 3.0%, such as 0.6%, 1%, 2% or 3%; when used, the pH of the copper-free cooling water system is controlled at 9.0 to 11.0, such as 9.0, 10.0 or 11.0.

[0044] The role of the basic amino acid derivatives in the present application is as follows: the basic amino acid derivatives include polar groups (-COOH, -NH2) with high electronegativity and strong affinity for metals and hydrophobic non-polar groups (-CH2). The polar groups adsorb on the metal surface, change the double electrical layer structure, and increase the activation energy of the metal ionization process; the non-polar groups are arranged in a directional manner away from the metal surface to form a hydrophobic film, which becomes a barrier to the diffusion of substances related to the corrosion reaction and inhibits the corrosion reaction. In the present application, the content of the basic amino acid derivatives in the corrosion inhibitor is 40% to 80%, for example 40%, 50%, 60% or 80%. The basic amino acid derivatives include derivatives of histidine (C6H9N3O2) and lysine (C6H 14 In other embodiments, other basic amino acid derivatives that can achieve the above functions can also be selected.

[0045] The effects of azoles in this application are as follows: azoles can form a hydrophobic polymer composite film on the copper surface to prevent the release of copper ions; by increasing the energy barrier for the diffusion of dissolved oxygen to the metal surface, the corrosion tendency of copper materials is reduced. In this application, the content of azole compounds in the corrosion inhibitor is 0.2% to 1.0%, such as 0.2%, 0.4%, 0.6%, 0.8% or 1.0%. Azoles include but are not limited to any one or more of 4-methyl-2-phenylimidazole, 5-methyl-benzotriazole, and methylbenzotriazole. For example, azoles can be selected from 4-methyl-2-phenylimidazole, 5-methyl-benzotriazole, or a combination of 4-methyl-2-phenylimidazole and methylbenzotriazole, or a combination of 4-methyl-2-phenylimidazole, 5-methyl-benzotriazole and methylbenzotriazole. When azoles are added in combination, the proportion of each component is not limited and can be mixed in any proportion. In other embodiments, the azole substance may also be selected from substances containing azole rings not listed above, as long as they can exert the above effects. Among them, the structural formula of methylbenzotriazole is as follows:

[0046]

[0047] Tolyltriazole

[0048] Furthermore, for cooling water systems containing stainless steel, since chloride ions can penetrate the passivation film on the surface of the stainless steel and combine with cations in the film to form soluble chlorides, leading to the destruction of the passivation film and promoting the occurrence of local corrosion, azole substances should be chlorine-free compounds.

[0049] The technical scheme of the present invention is described in detail below through several specific examples. Unless otherwise specified, the raw materials and reagents used in the following examples are all commercially available products, or can be prepared by conventional methods in the art, and the instruments used in the examples are all commercially available.

[0050] Example 1

[0051] In this embodiment, the corrosion inhibitor is composed of the following raw material components in weight percentage: 5% bactericide, 1% dispersant, 80% basic amino acid derivative, 0.5% azole substance, 1.2% alkalizer, and the rest is water. The above components are mixed uniformly at room temperature and pressure to obtain the corrosion inhibitor.

[0052] Wherein, the bactericide is an o-hydroxycinnamic acid lactone derivative compound, the dispersant is polyacrylic acid, the basic amino acid derivative is N-acetyl-L-histidine, the azole substance is 4-methyl-2-phenylimidazole, and the alkalizer is ammonia water. The o-hydroxycinnamic acid lactone derivative compound is prepared by the following method: 5% acetone and coumarin derivatives are added to a container, and the coumarin derivatives are dissolved in acetone; chitosan is added to the acetone solution in which the coumarin derivatives are dissolved and stirring is started, and the mass ratio of the coumarin derivatives to the chitosan is 3:1; nitrogen is introduced into the container as a protective gas, and the reaction is carried out at 0°C for 10 hours; after the reaction is completed, the acetone is removed to obtain the o-hydroxycinnamic acid lactone derivative compound.

[0053] Example 2

[0054] In this embodiment, the corrosion inhibitor is composed of the following raw material components in weight percentage: 7.5% bactericide, 1.5% dispersant, 40% basic amino acid derivative, 1.0% azole substance, 0.6% alkalizer, and the rest is water. The above components are mixed uniformly at normal temperature and pressure to obtain the corrosion inhibitor.

[0055] Wherein, the bactericide is an o-hydroxycinnamic acid lactone derivative compound, the dispersant is polyacrylic acid, the basic amino acid derivative is N-acetyl-L-histidine, the azole substance is methyl benzotriazole, and the alkalizing agent is sodium hydroxide. The o-hydroxycinnamic acid lactone derivative compound is prepared by the following method: 5% acetone and coumarin derivatives are added to a container, and the coumarin derivatives are dissolved in acetone; chitosan is added to the acetone solution in which the coumarin derivatives are dissolved and stirring is started, and the mass ratio of the coumarin derivatives to the chitosan is 4:1; nitrogen is introduced into the container as a protective gas, and the reaction is carried out at 5°C for 4 hours; after the reaction is completed, the acetone is removed to obtain the o-hydroxycinnamic acid lactone derivative compound.

[0056] Example 3

[0057] In this embodiment, the corrosion inhibitor is composed of the following raw material components in weight percentage: 10% bactericide, 2% dispersant, 60% basic amino acid derivative, 0.2% azole substance, 3.0% alkalizer, and the rest is water. The above components are mixed uniformly at room temperature and pressure to obtain the corrosion inhibitor.

[0058] Wherein, the bactericide is an o-hydroxycinnamic acid lactone derivative compound, the dispersant is polyacrylic acid, the basic amino acid derivative is 5-hydroxy-L-lysine, the azole substance is 5-methyl-benzotriazole, and the alkalizing agent is ethanolamine. The o-hydroxycinnamic acid lactone derivative compound is prepared by the following method: 5% acetone and coumarin derivatives are added to a container, and the coumarin derivatives are dissolved in acetone; chitosan is added to the acetone solution in which the coumarin derivatives are dissolved and stirring is started, and the mass ratio of the coumarin derivatives to the chitosan is 2:1; nitrogen is introduced into the container as a protective gas, and the reaction is carried out at 3°C ​​for 8 hours; after the reaction is completed, the acetone is removed to obtain the o-hydroxycinnamic acid lactone derivative compound.

[0059] Example 4

[0060] In this embodiment, the corrosion inhibitor is composed of the following raw material components in weight percentage: 8% bactericide, 1.5% dispersant, 65% basic amino acid derivative, 0.2% azole substance, 1.9% alkalizer, and the rest is water. The above components are mixed uniformly at room temperature and pressure to obtain the corrosion inhibitor.

[0061] Wherein, the bactericide is an o-hydroxycinnamic acid lactone derivative compound, the dispersant is polyacrylic acid, the basic amino acid derivative is N-acetyl-L-histidine, the azole substance is 4-methyl-2-phenylimidazole, and the alkalizer is sodium hydroxide. The o-hydroxycinnamic acid lactone derivative compound is prepared by the following method: 5% acetone and coumarin derivatives are added to a container, and the coumarin derivatives are dissolved in acetone; chitosan is added to the acetone solution in which the coumarin derivatives are dissolved and stirring is started, and the mass ratio of the coumarin derivatives to the chitosan is 2:1; nitrogen is introduced into the container as a protective gas, and the reaction is carried out at 3°C ​​for 7 hours; after the reaction is completed, the acetone is removed to obtain the o-hydroxycinnamic acid lactone derivative compound.

[0062] Example 5

[0063] In this embodiment, the corrosion inhibitor is composed of the following raw material components in weight percentage: 10% bactericide, 1.8% dispersant, 40% basic amino acid derivative, 1% azole substance, 2.1% alkalizer, and the rest is water. The above components are mixed uniformly at room temperature and pressure to obtain the corrosion inhibitor.

[0064] Wherein, the bactericide is an o-hydroxycinnamic acid lactone derivative compound, the dispersant is polyacrylic acid, the basic amino acid derivative is 5-hydroxy-L-lysine, the azole substance is 4-methyl-2-phenylimidazole, and the alkalizing agent is ethanolamine. The o-hydroxycinnamic acid lactone derivative compound is prepared by the following method: 5% acetone and coumarin derivatives are added to a container, and the coumarin derivatives are dissolved in acetone; chitosan is added to the acetone solution in which the coumarin derivatives are dissolved and stirring is started, and the mass ratio of the coumarin derivatives to the chitosan is 4:1; nitrogen is introduced into the container as a protective gas, and the reaction is carried out at 5°C for 4 hours; after the reaction is completed, the acetone is removed to obtain the o-hydroxycinnamic acid lactone derivative compound.

[0065] Example 6

[0066] In this embodiment, the corrosion inhibitor is composed of the following raw material components in weight percentage: 7% bactericide, 1.8% dispersant, 80% basic amino acid derivative, 0.2% azole substance, 1.0% alkalizer, and the rest is water. The above components are mixed uniformly at room temperature and pressure to obtain the corrosion inhibitor.

[0067] Wherein, the bactericide is an o-hydroxycinnamic acid lactone derivative compound, the dispersant is polyacrylic acid, the basic amino acid derivative is 5-hydroxy-L-lysine, the azole substance is methyl benzotriazole, and the alkalizing agent includes 0.1% ammonia water, 0.3% sodium hydroxide and 0.6% ethanolamine. The o-hydroxycinnamic acid lactone derivative compound is prepared by the following method: 5% acetone and coumarin derivatives are added to a container, and the coumarin derivatives are dissolved in acetone; chitosan is added to the acetone solution in which the coumarin derivatives are dissolved and stirring is started, and the mass ratio of the coumarin derivatives to the chitosan is 2.5:1; nitrogen is introduced into the container as a protective gas, and the reaction is carried out at 5°C for 5 hours; after the reaction is completed, the acetone is removed to obtain the o-hydroxycinnamic acid lactone derivative compound.

[0068] Example 7

[0069] In this embodiment, the corrosion inhibitor is composed of the following raw material components in weight percentage: 7% bactericide, 2% dispersant, 75% basic amino acid derivative, 0.7% azole substance, 1.5% alkalizer, and the rest is water. The above components are mixed uniformly at room temperature and pressure to obtain the corrosion inhibitor.

[0070] Wherein, the bactericide is an o-hydroxycinnamic acid lactone derivative compound, the dispersant is polyacrylic acid, the basic amino acid derivative is 5-hydroxy-L-lysine, the azole substance is methyl benzotriazole, and the alkalizing agent is ammonia water. The o-hydroxycinnamic acid lactone derivative compound is prepared by the following method: 5% acetone and coumarin derivatives are added to a container, and the coumarin derivatives are dissolved in acetone; chitosan is added to the acetone solution in which the coumarin derivatives are dissolved and stirring is started, and the mass ratio of the coumarin derivatives to the chitosan is 3:1; nitrogen is introduced into the container as a protective gas, and the reaction is carried out at 0°C for 10 hours; after the reaction is completed, the acetone is removed to obtain the o-hydroxycinnamic acid lactone derivative compound.

[0071] Example 8

[0072] In this embodiment, the corrosion inhibitor is composed of the following raw material components in weight percentage: 10% bactericide, 1.9% dispersant, 50% basic amino acid derivative, 0.4% azole substance, 1.5% alkalizer, and the rest is water. The above components are mixed uniformly at room temperature and pressure to obtain the corrosion inhibitor.

[0073] Wherein, the bactericide is an o-hydroxycinnamic acid lactone derivative compound, the dispersant is polyacrylic acid, the basic amino acid derivative includes 20% N-acetyl-L-histidine and 30% 5-hydroxy-L-lysine, the azole substance is 5-methyl-benzotriazole, and the alkalizing agent is sodium hydroxide. The o-hydroxycinnamic acid lactone derivative compound is prepared by the following method: 5% acetone and coumarin derivatives are added to a container, and the coumarin derivatives are dissolved in acetone; chitosan is added to the acetone solution in which the coumarin derivatives are dissolved and stirred, and the mass ratio of the coumarin derivatives to the chitosan is 3.5:1; nitrogen is introduced into the container as a protective gas, and the reaction is carried out at 4°C for 6 hours; after the reaction is completed, the acetone is removed to obtain the o-hydroxycinnamic acid lactone derivative compound.

[0074] Example 9

[0075] In this embodiment, the corrosion inhibitor is composed of the following raw material components in weight percentage: 6% bactericide, 1.7% dispersant, 70% basic amino acid derivative, 1% azole substance, 1% alkalizer, and the rest is water. The above components are mixed uniformly at room temperature and pressure to obtain the corrosion inhibitor.

[0076] Wherein, the bactericide is an o-hydroxycinnamic acid lactone derivative compound, the dispersant is polyacrylic acid, the basic amino acid derivative includes 50% N-acetyl-L-histidine and 20% 5-hydroxy-L-lysine, the azole substance is 5-methyl-benzotriazole, and the alkalizer includes 0.4% sodium hydroxide and 0.6% ethanolamine. The o-hydroxycinnamic acid lactone derivative compound is prepared by the following method: 5% acetone and coumarin derivatives are added to a container, and the coumarin derivatives are dissolved in acetone; chitosan is added to the acetone solution in which the coumarin derivatives are dissolved and stirring is started, and the mass ratio of the coumarin derivatives to the chitosan is 2:1; nitrogen is introduced into the container as a protective gas, and the reaction is carried out at 3°C ​​for 8 hours; after the reaction is completed, the acetone is removed to obtain the o-hydroxycinnamic acid lactone derivative compound.

[0077] Example 10

[0078] In this embodiment, the corrosion inhibitor is composed of the following raw material components in weight percentage: 9% bactericide, 1.5% dispersant, 80% basic amino acid derivative, 0.7% azole substance, 1.1% alkalizer, and the rest is water. The above components are mixed uniformly at room temperature and pressure to obtain the corrosion inhibitor.

[0079] Wherein, the bactericide is an o-hydroxycinnamic acid lactone derivative compound, the dispersant is polyacrylic acid, the basic amino acid derivative includes 10% N-acetyl-L-histidine and 70% 5-hydroxy-L-lysine, the azole substance includes 0.3% 4-methyl-2-phenylimidazole, 0.2% methylbenzotriazole and 0.2% 5-methyl-benzotriazole, and the alkalizer includes 0.4% ammonia water and 0.7% sodium hydroxide. The o-hydroxycinnamic acid lactone derivative compound is prepared by the following method: 5% acetone and coumarin derivatives are added to a container, and the coumarin derivatives are dissolved in acetone; chitosan is added to the acetone solution in which the coumarin derivatives are dissolved and stirring is started, and the mass ratio of the coumarin derivatives to the chitosan is 2:1; nitrogen is introduced into the container as a protective gas, and the reaction is carried out at 3°C ​​for 8 hours; after the reaction is completed, the acetone is removed to obtain the o-hydroxycinnamic acid lactone derivative compound.

[0080] Comparative Example

[0081] In this comparative example, the corrosion inhibitor is composed of the following raw material components in weight percentage: 1% dispersant, 80% alkaline amino acid derivative, 0.5% azole substance, 1.2% alkalizer, and the rest is water, and the above components are mixed uniformly at room temperature and pressure to obtain the corrosion inhibitor. Among them, the dispersant is polyacrylic acid, the alkaline amino acid derivative is N-acetyl-L-histidine, the azole substance is 4-methyl-2-phenylimidazole, the alkalizer is ammonia water, and the rest is water, and the above components are mixed uniformly at room temperature and pressure to obtain the corrosion inhibitor.

[0082] The corrosion inhibitor formulation compositions of Examples 1 to 10 and the comparative examples in this application are shown in Table 1:

[0083]

[0084] The corrosion inhibitors prepared in Examples 1 to 10 and the comparative examples were tested for corrosion inhibition performance. The standard corrosion coupons were made of 20# carbon steel and T2 copper alloy, and the test process was carried out in accordance with GB / T18175-2014. In order to evaluate the corrosion inhibition performance of the corrosion inhibitor on 20# carbon steel and T2 copper alloy, the two materials were placed in experimental water with corrosion inhibitors added for experiments. In order to be closer to actual applications, the experimental water used cooling water from a pressurized water reactor nuclear power plant. Specifically, the 20# carbon steel / T2 copper alloy test piece was wiped, cleaned, and dried, then weighed, and then fixed on the coupon instrument and placed in cooling water with corrosion inhibitor added. The corrosion inhibitor content in the cooling water was 300 mg / kg, and the temperature was kept constant at 40°C for 336 hours. After the test coupons were cleaned, dried, weighed, and the average corrosion rate was calculated. The corrosion inhibition performance test results are shown in Table 2:

[0085]

[0086]

[0087] It can be seen from the test results in Table 1 that the corrosion rate is greatly reduced after the corrosion inhibitors prepared in Examples 1 to 10 and the comparative example are added to the cooling water. Furthermore, the corrosion inhibition rate of the corrosion inhibitor with the addition of the bactericide is greatly improved compared with the corrosion inhibitor without the bactericide.

[0088] The more representative test cases in the above corrosion inhibition performance test were selected to characterize the macroscopic and microscopic morphologies of the corrosion coupons after the test. The characterization results are as follows: Figures 1 to 4 As shown. Figures 1 to 4 It can be seen that after adding the corrosion inhibitor of the present application to the cooling water, the macroscopic morphology and microstructure of the metal are well protected.

[0089] Furthermore, in actual use, there are generally 20# carbon steel and T2 copper alloy in the cooling water system. In order to more accurately simulate the actual application environment and evaluate the comprehensive protective performance of the corrosion inhibitor, 20# carbon steel and T2 copper alloy are placed together in the cooling water with the corrosion inhibitor added. Such an experimental setting can more realistically reflect the actual effect of the corrosion inhibitor under the coexistence of multiple materials. The test method is the same as that for testing the anti-corrosion performance of 20# carbon steel and T2 copper alloy, and will not be repeated here. The corrosion inhibition performance test results are shown in Table 3:

[0090]

[0091] It can be seen from the test results in Table 2 that for a system containing both 20# carbon steel and T2 copper alloy, the corrosion rate is greatly reduced after the corrosion inhibitor prepared in Example 1 and the comparative example is added to the cooling water. Furthermore, the corrosion inhibition rate of the corrosion inhibitor with the addition of a bactericide is greatly improved compared with the corrosion inhibitor without a bactericide. Therefore, the corrosion inhibitor prepared in this application has good practical value.

[0092] The green corrosion inhibitor for cooling water system of the present application does not contain phosphorus, which can not only reduce the introduction of microbial nutrients, but also the added bactericide can inhibit the growth process of microorganisms, reduce microbial corrosion, and simultaneously act together through multiple mechanisms (film-forming effect, increase of corrosion reaction energy barrier, synergistic effect), and has excellent compatibility and corrosion inhibition effect on various materials such as carbon steel and copper alloy. Further, the corrosion inhibitor of the present invention does not contain phosphate and chromium, which can effectively reduce the negative impact on the environment and ecosystem, so the corrosion inhibitor of the present application can be widely used in various cooling water systems. Further, the corrosion inhibitor formula of the present invention can help power plants solve the current application dilemma of corrosion inhibitors, meet relevant environmental protection laws and regulations, and improve the operation level of power plants. Therefore, the present invention effectively overcomes some practical problems in the prior art and has high utilization value and use significance.

[0093] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.

Claims

1. A green corrosion inhibitor for a cooling water system, characterized in that: Based on the total mass of the corrosion inhibitor, the corrosion inhibitor is composed of the following raw material components in weight percentage: Fungicide 5% to 10%; Dispersant 1% to 2%; Basic amino acid derivatives 40% to 80%; Azoles 0.2% to 1.0%; Alkalizing agent 0.6% to 3.0%; The rest is water.

2. The green corrosion inhibitor for cooling water system according to claim 1, characterized in that: For a copper-containing cooling water system, the content of the alkalizer is 0.6% to 1.5%; for a copper-free cooling water system, the content of the alkalizer is 0.6% to 3.0%.

3. The green corrosion inhibitor for cooling water system according to claim 1, characterized in that: The bactericide includes o-hydroxycinnamic acid lactone derivative compounds.

4. The green corrosion inhibitor for cooling water system according to claim 1, characterized in that: The dispersant includes a polyacrylic acid dispersant.

5. The green corrosion inhibitor for cooling water system according to claim 1, characterized in that: The basic amino acid derivatives include any one or both of histidine derivatives and lysine derivatives.

6. The green corrosion inhibitor for cooling water system according to claim 1, characterized in that: The alkalizing agent includes any one or more of ammonia water, ethanolamine and sodium hydroxide.

7. The green corrosion inhibitor for cooling water system according to claim 1, characterized in that: The azole substances include any one or more of 4-methyl-2-phenylimidazole, 5-methyl-benzotriazole, and methylbenzotriazole.

8. The green corrosion inhibitor for cooling water system according to claim 1, characterized in that: The bactericide is prepared by the following method: adding a solvent and a coumarin derivative into a container, wherein the coumarin derivative is dissolved in the solvent; Add chitosan to the solvent in which the coumarin derivative is dissolved and start stirring; Introducing an inert gas into the container and performing a reaction at a set temperature; After the reaction is completed, the solvent is removed to obtain the fungicide.

9. The green corrosion inhibitor for cooling water system according to claim 8, characterized in that: The mass ratio of the coumarin derivative to the chitosan is 2:1 to 4:

1.