Preparation method and application of tungsten-molybdenum carbide nanosheet heterojunction catalyst

By preparing a tungsten-molybdenum carbide nanosheet heterojunction catalyst, the problems of high overpotential and large resistance in the process of hydrogen production by water electrolysis were solved, and efficient alkaline water electrolysis hydrogen evolution performance was achieved, with excellent electrocatalytic activity and stability.

CN118880388AActive Publication Date: 2024-11-01NINGBO GUANGMING RUBBER & PLASTIC

Patent Information

Application Number
CN202411380170.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-30
Publication Date
2024-11-01
Estimated Expiration
2044-09-30

AI Technical Summary

Technical Problem

In existing industrial water electrolysis hydrogen production processes, the cathode hydrogen evolution reaction requires a high overpotential and faces resistance. The performance of non-precious metal catalysts is still significantly inferior to that of precious metal catalysts, making it difficult to achieve efficient water electrolysis hydrogen production.

Method used

A heterojunction catalyst of tungsten-molybdenum carbide nanosheets was prepared by high-temperature carbonization of zinc salt, molybdate and tungstate in a reducing atmosphere to form tungsten-molybdenum carbide nanosheets, followed by removal of zinc metal by hot acid etching to construct a heterostructure to optimize the surface porosity and electronic interactions of the catalyst.

Benefits of technology

It exhibits high electrocatalytic activity and stability in alkaline water electrolysis, with low cathode overpotential and stable operation for a long time at high current density, which increases the possibility of non-precious metal catalysts replacing precious metal catalysts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118880388A_ABST
    Figure CN118880388A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of electrocatalysts, and discloses a preparation method and application of a tungsten-molybdenum carbide nanosheet heterojunction catalyst, the preparation method comprises the following steps: (1) mixing and stirring a zinc salt solution with a mixed solution of molybdate, tungstate and dimethylimidazole, reacting for a certain time, and drying to obtain a tungsten-molybdenum-zinc trimetal organic framework; (2) calcining the prepared tungsten-molybdenum-zinc trimetal organic framework in a tubular furnace, and performing high-temperature carbonization in a reducing atmosphere to generate a tungsten-molybdenum carbide nanosheet heterojunction catalyst containing zinc metal; (3) zinc metal on the surface of the carbide nanosheet heterojunction catalyst is removed through hot acid etching treatment, and the tungsten-molybdenum carbide nanosheet heterojunction catalyst is obtained. The prepared tungsten-molybdenum carbide nanosheet heterojunction catalyst has excellent alkaline electrolytic water hydrogen evolution performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of electrocatalysts, and in particular to a preparation method and application of a tungsten-molybdenum carbide nanosheet heterojunction catalyst. Background Art

[0002] Compared to traditional fossil-based hydrogen production processes, water electrolysis hydrogen production technology is currently considered an ideal green hydrogen production method because it not only can couple renewable energy sources but also produces high-purity hydrogen, with low subsequent separation and purification costs, and the entire hydrogen production process is pollution-free. However, the current voltage for industrial water electrolysis is generally between 1.8 and 2.0 V, compared to the theoretical bias potential of 1.23 V, leaving significant room for improvement. To reduce the required voltage, it is necessary to address the high overpotentials required for the cathode and anode reactions and the resistance in the water electrolysis system. Currently, precious metal materials, such as Pt, are commonly used as catalysts for the cathode hydrogen evolution reaction. Their high cost hinders the large-scale development of water electrolysis hydrogen production. Developing non-precious metal-based catalysts to replace precious metal catalysts for efficient water electrolysis hydrogen production remains a major challenge in water electrolysis hydrogen production.

[0003] Among the non-precious metal catalysts reported so far, transition metal-based compounds such as transition metal sulfides, hydroxides, and carbides have been widely studied as alternatives to precious metal catalysts. Transition metal carbides, including Mo2C, W2C, and WC, have been reported many times for use in water electrolysis to produce hydrogen due to their similar d-band electronic structure to the precious metal Pt. For example, Chinese patent document No. CN202210260511.1 discloses a tungsten carbide-tungsten sulfide composite catalytic material, in which the tungsten carbide-tungsten sulfide composite catalytic layer is grown on the surface of a tungsten foil substrate. This composite catalytic material uses tungsten foil as a substrate and tungsten source. First, a tungsten trioxide thin film precursor is formed on the tungsten foil. Then, a tungsten carbide-tungsten sulfide thin film with a vertical flake structure is synthesized in one step by chemical vapor deposition, exhibiting relatively good hydrogen evolution performance. Another example is Chinese patent publication CN202210233979.1, which discloses a self-supporting tungsten-based composite material. This tungsten-based composite material uses tungsten foil as a substrate, on which tungsten carbide is in situ synthesized. Ni(OH)2 is then electrochemically deposited on the WC surface. The composite material provides strong mechanical stability. Ni(OH)2 has a moderate adsorption capacity for intermediate hydroxides and enhances the water dissociation step. Furthermore, WC has excellent hydrogen adsorption capacity. The synergistic effect of WC and Ni(OH)2 significantly enhances the catalyst's hydrogen evolution capacity.

[0004] Although transition metal carbides have shown some catalytic activity in hydrogen evolution from water electrolysis, the performance of currently reported transition metal carbide electrocatalysts still lags far behind that of commercial noble metal catalysts such as Pt / C. Therefore, by preparing a tungsten-molybdenum carbide nanosheet catalyst, it is possible to effectively balance its adsorption and desorption of water molecules and hydrogen intermediates. At the same time, the tungsten-molybdenum heterostructure can strengthen the electronic interaction between the active sites of tungsten and molybdenum metals, improving electron utilization, thereby further improving the performance of hydrogen evolution from water electrolysis, breaking the performance limitations of single metal carbide hydrogen evolution and achieving a replacement for noble metal catalysts. Summary of the Invention

[0005] The present invention addresses the problem of low intrinsic activity of single transition metal carbides in water electrolysis for hydrogen evolution in the prior art and provides a method for preparing a tungsten-molybdenum carbide nanosheet heterojunction catalyst. The prepared carbide nanosheet heterojunction catalyst exhibits excellent electrocatalytic activity for hydrogen evolution in alkaline water electrolysis and has good hydrogen evolution stability.

[0006] To achieve the above object, the present invention provides the following technical solution: a method for preparing a tungsten-molybdenum carbide nanosheet heterojunction catalyst, comprising the following steps: (1) Dissolve zinc salt in deionized water to obtain solution A, then dissolve molybdate, tungstate and N-methylimidazole in deionized water to obtain solution B, slowly and uniformly pour solution A into solution B, continue stirring and react at a constant temperature for a certain period of time, then centrifuge and wash, and dry to obtain a tungsten-molybdenum-zinc trimetallic organic framework; (2) placing the tungsten-molybdenum-zinc trimetallic organic framework prepared in step (1) into a tubular furnace for calcination, and carbonizing it at high temperature under a reducing atmosphere to generate a tungsten-molybdenum carbide nanosheet heterojunction catalyst containing zinc metal; (3) The tungsten-molybdenum carbide nanosheet heterojunction catalyst containing zinc metal prepared in step (2) is subjected to a thermal acid etching treatment to remove the zinc metal, thereby obtaining the tungsten-molybdenum carbide nanosheet heterojunction catalyst.

[0007] Preferably, the molar ratio of the zinc salt to dimethylimidazole in step (1) is 1:1-4.

[0008] Preferably, in step (1), the molar ratio of zinc salt to tungstate to molybdate is 4:1-4:1-4, the reaction time is 12-24 h, and the reaction temperature is 20-25°C.

[0009] Preferably, in step (2), the calcination temperature is 700-1000° C., and the calcination time is 1-4 h.

[0010] Preferably, the calcination atmosphere in step (2) is a mixture of hydrogen and argon, with the hydrogen accounting for 3% to 20%.

[0011] Preferably, the acid concentration of the hot acid treatment in step (3) is 0.5 M to 3 M, the temperature of the hot acid treatment is 60 to 90 °C, and the hot acid treatment time is 10 to 20 h.

[0012] Preferably, the prepared tungsten-molybdenum carbide nanosheet heterojunction catalyst is used as a working electrode in the alkaline electrolysis of water for hydrogen evolution reaction.

[0013] Compared with the prior art, the present invention has the following beneficial effects: (1) The tungsten-molybdenum carbide nanosheet heterojunction catalyst provided by the present invention has high electrocatalytic activity and stability in the process of hydrogen production by alkaline water electrolysis. -2 When the cathode overpotential is only about 92 mV, it can withstand a current density of 10 mA cm -2 The catalyst worked stably for 30 h without obvious potential decay, which increases the possibility of non-precious catalysts replacing precious metal catalysts. (2) The tungsten-molybdenum carbide nanosheet heterojunction catalyst provided by the present invention utilizes two metal carbides to construct a heterostructure, utilizing the electronic interaction between the tungsten-molybdenum metal sites to enhance the adsorption and desorption of hydrogen intermediates by the metal sites; (3) The tungsten-molybdenum carbide nanosheet heterojunction catalyst provided by the present invention optimizes the mass transfer process between the catalyst and the electrolyte by regulating the porosity of the carbide surface, increases the active reaction area of ​​the catalyst, and improves the hydrogen evolution performance in alkaline water electrolysis. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 This is a scanning electron microscope (SEM) image of the catalyst Mo2C / WC NS prepared in Example 1; Figure 2 TEM image of the catalyst Mo2C / WC NS prepared in Example 1; Figure 3 XRD pattern of the catalyst Mo2C / WC NS prepared in Example 1; Figure 4 Polarization curves of the catalysts prepared in Example 1 and Comparative Examples 1 to 3 for hydrogen evolution in alkaline water electrolysis in application examples; Figure 5 This is a constant current timing curve of hydrogen evolution in alkaline water electrolysis using the catalyst Mo2C / WC NS prepared in Example 1. DETAILED DESCRIPTION

[0015] The following will clearly and completely describe the technical solutions in the embodiments of the present invention in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of the present invention.

[0016] like Figures 1 to 5 As shown, an embodiment of the present invention provides a method for preparing a tungsten-molybdenum carbide nanosheet heterojunction catalyst, comprising the following steps: (1) Dissolve zinc salt in deionized water to obtain solution A, and dissolve molybdate, tungstate, and dimethylimidazole in deionized water to obtain solution B. The molar ratio of zinc salt to dimethylimidazole is controlled to be 1:1-4, and the molar ratio of zinc salt to tungstate to molybdate is controlled to be 4:1-4:1-4. Pour solution A into solution B, stir and mix, and react. The reaction time is controlled to be 12-24 hours at 20-25°C to obtain a tungsten-molybdenum-zinc trimetallic organic framework. The zinc salt, molybdate, or tungstate used is a soluble salt. The zinc salt includes nitrate, chloride, acetate, sulfate, and hydrates of cobalt, such as zinc nitrate, zinc chloride, zinc acetate, zinc sulfate, etc. Molybdate includes sodium molybdate, ammonium molybdate, and hydrates thereof. Tungstate includes tungstate, ammonium tungstate, and hydrates thereof.

[0017] (2) The tungsten-molybdenum-zinc trimetallic organic framework precursor prepared in step (1) was placed in a tube furnace and calcined. The calcination temperature was controlled at 700-1000°C and the heating rate was controlled at 1-5°C / min. -1 The constant temperature calcination time is 1 to 4 hours, the calcination atmosphere is a mixture of hydrogen and argon, and the hydrogen accounts for 3% to 20%. The organic skeleton is converted into a carbon skeleton after high-temperature calcination. Dimethylimidazole is used as a carbon source to form carbides with metal tungsten and metal molybdenum. Metallic zinc is reduced and precipitated, and finally a tungsten-molybdenum carbide nanosheet heterojunction catalyst containing zinc metal is obtained.

[0018] (3) The tungsten-molybdenum carbide nanosheet heterojunction catalyst containing zinc metal prepared in step (2) is heat-treated in an acid solution of a certain concentration, wherein the acid concentration is selected to be 0.5 M to 3 M, the temperature of the heat acid treatment is 60 to 90 °C, and the heat acid treatment time is 10 to 20 h, so as to remove the surface zinc ions and finally obtain a tungsten-molybdenum carbide nanosheet heterojunction catalyst.

[0019] The preparation principle is as follows: zinc ions can coordinate with dimethylimidazole, molybdate ions, and tungstate ions. The coordination interaction between zinc ions, dimethylimidazole, molybdate ions, and tungstate ions reacts to form a tungsten-molybdenum-zinc trimetallic organic framework. Under a reducing atmosphere, the tungsten and molybdenum in the framework react with dimethylimidazole as a carbon source to form tungsten carbide and molybdenum carbide. Simultaneously, the zinc ions are reduced to form zinc metal particles. Acid-heat treatment is then used to remove the zinc metal particles from the carbide nanosheets, increasing the porosity of the catalyst surface, ultimately achieving the preparation of a tungsten-molybdenum carbide nanosheet heterojunction catalyst.

[0020] The tungsten-molybdenum carbide nanosheet heterojunction catalyst prepared according to the preparation method can be represented by the chemical formula: Mo2C / WC NS, where Mo2C represents molybdenum carbide; WC represents tungsten carbide; and NS represents the nanosheet structure. The catalyst is composed of molybdenum carbide and tungsten carbide, forming a heterogeneous carbide structure. After acid-heat treatment, the surface porosity is increased. The prepared tungsten-molybdenum carbide nanosheet heterojunction catalyst can be used as a working electrode in the hydrogen evolution reaction during alkaline water electrolysis.

[0021] In the alkaline water electrolysis hydrogen evolution reaction, a standard three-electrode system is used, specifically a glassy carbon electrode covered with a tungsten-molybdenum carbide nanosheet heterojunction catalyst provided by the present invention as the working electrode, a Hg / HgO electrode as the reference electrode, a carbon rod as the counter electrode, and a 1.0 M potassium hydroxide solution as the electrolyte.

[0022] Example 1 (1) Weigh 0.1 M zinc nitrate hexahydrate and dissolve it in 25 mL of deionized water to form solution A. Then weigh 0.1 M sodium tungstate, 0.1 M sodium molybdate, and 0.2 M dimethylimidazole and dissolve them in 25 mL of deionized water to form solution B. Slowly introduce solution A into solution B. The ratio of zinc salt and dimethylimidazole and tungstate to molybdate is selected because the ratio of zinc salt to dimethylimidazole has a significant effect on the formation of the organic skeleton. When the zinc salt concentration is too high, the zinc metal content in the generated organic skeleton is high, and particle agglomeration is likely to occur during the subsequent carbonization process. In addition, if the content of dimethylimidazole as a carbon source is too low, it will be detrimental to the formation of molybdenum carbide and tungsten carbide; when the zinc salt concentration is too low, the zinc metal content in the generated organic skeleton is low, which is detrimental to the further coordination of zinc metal with tungstate and molybdate, resulting in a low content of tungsten and molybdenum ions in the precursor, resulting in a subsequent decrease in the content of molybdenum carbide and tungsten carbide, and a decrease in the number of catalytic active sites; and the concentration ratio of tungstate to molybdate will affect the subsequent formation of tungsten carbide and molybdenum carbide heterojunctions.

[0023] (2) The mixed solution was stirred at 25 °C for 20 h to generate a tungsten-molybdenum-zinc trimetallic organic framework precursor. The reason for the reaction at a constant temperature of 25 °C is that the reaction temperature and time will affect the size of the organic framework. Adopting a constant moderate temperature and appropriate reaction time is conducive to ensuring the uniformity of the size of the tungsten-molybdenum-zinc trimetallic organic framework precursor nanosheet structure.

[0024] (3) The tungsten-molybdenum-zinc trimetallic organic framework precursor was calcined in a tube furnace. The temperature of the tube furnace was set to 900 °C and the heating rate was controlled at 3 °C min -1 The reaction was carried out in a hydrogen / argon mixture (5% / 95%) atmosphere, heated at a constant temperature of 900°C for 3 hours. After completion, the reaction was cooled to room temperature to produce a tungsten-molybdenum carbide nanosheet heterojunction catalyst containing zinc metal. Controlling the temperature and time of the carbide reaction is beneficial to the crystallinity of the tungsten carbide and molybdenum carbide and the dispersion of the active component. When the temperature is too low and the reaction time is too short, the carbide is poorly formed, resulting in no tungsten carbide and molybdenum carbide formation or poor crystallinity of the resulting carbides. When the temperature is too high and the reaction time is too long, the tungsten carbide and molybdenum carbide tend to agglomerate during the carbide process due to the high temperature, resulting in a decrease in the specific surface area of ​​the resulting carbide and poor dispersion of the active component. The appropriate heating rate is controlled to prevent structural collapse during the conversion of the organic framework to a carbon framework caused by excessive heating. The carbide reaction was carried out in a hydrogen / argon mixture (5% / 95%) atmosphere because a reducing atmosphere facilitates the formation of carbides and the precipitation of metallic zinc.

[0025] (4) The prepared tungsten-molybdenum carbide nanosheet heterojunction catalyst containing zinc metal was dissolved in a 1 M H2SO4 solution; the reaction was stirred at 70°C for 12 h, cooled to room temperature, washed three times with deionized water by centrifugation, and dried under vacuum to obtain a tungsten-molybdenum carbide nanosheet heterojunction catalyst, denoted as Mo2C / WC NS. The acid concentration, acid treatment temperature, and time were controlled to ensure the removal of zinc metal particles and increase the porosity and specific surface area of ​​the catalyst. Excessive acid concentration and treatment temperature, or prolonged treatment time, may lead to the destruction of the carbon structure and the dissolution of molybdenum carbide or tungsten carbide. Too low a temperature will not completely remove the zinc metal, affecting the specific surface area of ​​the catalyst and resulting in a decrease in hydrogen evolution activity.

[0026] The rich pore structure inside the catalyst is conducive to the contact reaction between the active sites and the electrolyte, which facilitates the subsequent hydrogen evolution reaction. At the same time, the heterogeneous structure composed of molybdenum carbide and tungsten carbide can further regulate the electronic environment around metal tungsten and molybdenum, which is conducive to balancing the binding and detachment of hydrogen with metal tungsten or molybdenum sites. Specifically, the rich pore structure can better transport water molecules to the catalyst surface, while the heterogeneous structure of molybdenum carbide and tungsten carbide can redistribute the electrons of the metal sites, thereby weakening the original metal sites' excessive adsorption of hydrogen, making the adsorption and desorption of hydrogen intermediates more reasonable, and accelerating the kinetics of the hydrogen evolution reaction. The construction of this catalyst also optimizes the mass transfer and kinetics of the reaction process, ultimately showing excellent hydrogen evolution performance.

[0027] The microstructure of the prepared tungsten-molybdenum carbide nanosheet heterojunction catalyst was observed by scanning electron microscopy (SEM) and transmission electron microscopy (TEM). Figure 1 As shown in the TEM image Figure 2 As shown. Figure 1-Figure 2 It can be seen that the tungsten-molybdenum carbide nanosheet heterojunction catalyst presents a nanosheet structure with a thickness of tens of nanometers, and the carbide particles are dispersed in the sheet-like carbon skeleton. The X-ray diffraction XRD pattern of the tungsten-molybdenum carbide nanosheet heterojunction catalyst prepared in this embodiment is as follows Figure 3 As shown, the characteristic peaks of tungsten carbide and molybdenum carbide can be seen in the catalyst, proving the successful synthesis of tungsten-molybdenum carbide nanosheet heterojunction catalyst.

[0028] Comparative Example 1 According to the process of Example 1, 0.1 M zinc nitrate hexahydrate was weighed and dissolved in 25 mL of deionized water to form solution A. Then, 0.1 M sodium tungstate, 0.1 M sodium molybdate, and 0.2 M dimethylimidazole were weighed and dissolved in 25 mL of deionized water to form solution B. Solution A was slowly introduced into solution B. The mixed solution was stirred at 25 ° C for 20 h, centrifuged three times with deionized water, and dried to obtain a tungsten-molybdenum-zinc trimetallic organic framework precursor. The tungsten-molybdenum-zinc trimetallic organic framework precursor was placed in a tube furnace and calcined. The tube furnace temperature was set to 900 ° C, and the heating rate was controlled to 3 ° C min -1 The reaction atmosphere was a hydrogen / argon mixture (5% / 95%), and the reaction was heated at 900°C for 3 hours. After completion of the reaction, the mixture was cooled to room temperature to obtain a zinc-containing tungsten-molybdenum carbide nanosheet heterojunction catalyst, designated Zn@Mo2C / WC NS. Without subsequent thermal acid treatment, the catalyst surface contained zinc nanoparticles and had relatively small pores. This was compared to the tungsten-molybdenum carbide nanosheet heterojunction catalyst prepared in Example 1, demonstrating the role of a highly porous surface in promoting hydrogen evolution during water electrolysis.

[0029] Comparative Example 2 According to the process of Example 1, 0.1 M zinc nitrate hexahydrate was weighed and dissolved in 25 mL of deionized water to form solution A. Then, 0.1 M sodium tungstate and 0.2 M dimethylimidazole were weighed and dissolved in 25 mL of deionized water to form solution B. Solution A was slowly introduced into solution B. The mixed solution was stirred at 25 ° C for 20 h, centrifuged three times with deionized water, and dried to obtain a tungsten-zinc organic framework precursor. The tungsten-zinc organic framework precursor was placed in a tube furnace and calcined. The tube furnace temperature was set to 900 ° C, and the heating rate was controlled to 3 ° C min -1 The reaction atmosphere was a hydrogen / argon mixture (5% / 95%), and the reaction was heated at 900°C for 3 hours. After completion, the reaction was cooled to room temperature to obtain a tungsten carbide nanosheet heterojunction catalyst containing zinc metal. The prepared tungsten carbide nanosheet catalyst containing zinc metal was dissolved in a 1 M H2SO4 solution and stirred at 70°C for 12 hours. The mixture was cooled to room temperature, washed three times with deionized water by centrifugation, and dried under vacuum to obtain the tungsten carbide nanosheet catalyst, designated WCNS. Single-component tungsten carbide was synthesized to compare the effect of the heterostructure composed of molybdenum carbide and tungsten carbide on hydrogen evolution performance in the composite carbide component.

[0030] Comparative Example 3 According to the process of Example 1, 0.1 M zinc nitrate hexahydrate was weighed and dissolved in 25 mL of deionized water to form solution A. 0.1 M molybdenum tungstate and 0.2 M dimethylimidazole were weighed and dissolved in 25 mL of deionized water to form solution B. Solution A was slowly introduced into solution B. The mixed solution was stirred at 25 ° C for 20 h, centrifuged three times with deionized water, and dried to obtain a molybdenum zinc organic framework precursor. The molybdenum zinc organic framework precursor was placed in a tube furnace and calcined. The tube furnace temperature was set to 900 ° C, and the heating rate was controlled to 3 ° C min -1 The reaction atmosphere was a hydrogen / argon mixture (5% / 95%), and the reaction was heated at 900°C for 3 hours. After completion, the reaction was cooled to room temperature to obtain a zinc-containing molybdenum carbide nanosheet heterojunction catalyst. The prepared zinc-containing molybdenum carbide nanosheet catalyst was dissolved in a 1 M H2SO4 solution and stirred at 70°C for 12 hours. The mixture was cooled to room temperature, washed three times with deionized water by centrifugation, and dried under vacuum to obtain the molybdenum carbide nanosheet catalyst, designated Mo2C NS. Single-component molybdenum carbide was synthesized to compare the effect of heterojunctions composed of molybdenum carbide and tungsten carbide on hydrogen evolution performance within the composite carbide component.

[0031] Application Examples (1) A three-electrode system was used, with a glassy carbon electrode coated with the catalyst prepared in Example 1 or Comparative Examples 1-3 as the working electrode, a carbon rod as the counter electrode, a saturated Hg / HgO electrode as the reference electrode, and 1.0 M KOH as the electrolyte; (2) CV activation: A Shanghai Chenhua CHI 760E electrochemical workstation was used. Argon was introduced into the electrolyte for 0.5 h before testing. The CV program was used with a test range of 0 to -0.8 V vs. RHE and a scan rate of 0.05 V s -1 , after 50 cycles, the electrode reaches a stable state.

[0032] The catalysts prepared in Example 1 and Comparative Examples 1-3 were subjected to linear sweep voltammetry (LSV) testing.

[0033] After activation, the program was switched to LSV program with a test range of 0 to -0.8 V vs. RHE, a scan rate of 5 mV / s, and an overpotential of 0 V and 10 mA cm relative to the reversible hydrogen electrode. -2 The potential difference is measured under Figure 4 As shown in the figure, the polarization curves of the Mo2C / WC NS and Zn@Mo2C / WC NS, Mo2C NS and WC NS in the electrolysis of water and hydrogen evolution in 1.0 M KOH solution provided in this embodiment are shown in the figure. Figure 4 As shown, from Figure 4 As can be seen in the figure, in an alkaline environment, the overpotential of the Mo2C / WC NS catalyst is approximately 92 mV, which is significantly better than single-component tungsten carbide and molybdenum carbide, as well as tungsten and molybdenum carbides containing zinc metal that have not been subjected to thermal acid etching. This proves that the optimization of heterogeneous structure and pore structure has a synergistic effect on hydrogen evolution from water electrolysis.

[0034] The catalyst prepared in Example 1 was subjected to a stability test.

[0035] After CV activation, the program was switched to ISTEP and the current was set to 0.0007 A, i.e., the current density was 10 mA cm -2 , the running time is set to 30 h. Figure 5 As shown, the potential of the tungsten-molybdenum carbide heterojunction catalyst is basically stable near the initial potential of 92 mV without any change, proving that it has good stability for hydrogen evolution in alkaline water electrolysis.

[0036] It should be noted that, in this document, relational terms such as first and second, etc., are used only to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any actual relationship or order between these entities or operations. Moreover, the terms "comprises," "comprising," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that includes a list of elements includes not only those elements but also other elements not explicitly listed, or elements inherent to such process, method, article, or apparatus.

[0037] While embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions, and variations may be made to these embodiments without departing from the principles and spirit of the invention, and that the scope of the invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing a tungsten-molybdenum carbide nanosheet heterojunction catalyst, characterized in that: The steps include: (1) dissolving zinc salt in deionized water to obtain solution A, then dissolving molybdate, tungstate and 2-methylimidazole in deionized water to obtain solution B, slowly and uniformly pouring solution A into solution B, reacting for a certain period of time, and obtaining a tungsten-molybdenum-zinc trimetallic organic framework; (2) placing the tungsten-molybdenum-zinc trimetallic organic framework prepared in step (1) into a tubular furnace for calcination, and carbonizing at high temperature under a reducing atmosphere to generate a tungsten-molybdenum carbide nanosheet heterojunction catalyst containing zinc metal; (3) The tungsten-molybdenum carbide nanosheet heterojunction catalyst containing zinc metal prepared in step (2) is subjected to thermal acid etching to remove the zinc metal, thereby obtaining the tungsten-molybdenum carbide nanosheet heterojunction catalyst.

2. The method for preparing the tungsten-molybdenum carbide nanosheet heterojunction catalyst according to claim 1, characterized in that: The molar ratio of zinc salt to dimethylimidazole is 1:1-4.

3. The method for preparing the tungsten-molybdenum carbide nanosheet heterojunction catalyst according to claim 1, characterized in that: The molar ratio of the zinc salt to tungstate and molybdate is 4:1-4:1-4.

4. The method for preparing the tungsten-molybdenum carbide nanosheet heterojunction catalyst according to claim 1, characterized in that: The reaction time in step (1) is 12-24 h, and the reaction temperature is 20-25°C.

5. The method for preparing the tungsten-molybdenum carbide nanosheet heterojunction catalyst according to claim 1, characterized in that: In step (2), the calcination temperature is 700-1000° C. and the calcination time is 1-4 hours.

6. The method for preparing the tungsten-molybdenum carbide nanosheet heterojunction catalyst according to claim 1, characterized in that: In step (2), the calcination atmosphere is a mixture of hydrogen and argon, with the hydrogen accounting for 3% to 20%.

7. The method for preparing the tungsten-molybdenum carbide nanosheet heterojunction catalyst according to claim 1, characterized in that: In step (3), the acid concentration of the hot acid treatment is 0.5 M to 3.0 M, the temperature of the hot acid treatment is 60 to 90° C., and the hot acid treatment time is 10 to 20 h.

8. The tungsten-molybdenum carbide nanosheet heterojunction catalyst prepared according to the preparation method according to any one of claims 1 to 7.

9. Use of the tungsten-molybdenum carbide nanosheet heterojunction catalyst according to claim 8 as a working electrode in a hydrogen evolution reaction by electrolysis of water in an alkaline electrolyte.

Citation Information

Patent Citations

  • Defect-rich molybdenum-doped cobalt selenide / nanocarbon electrocatalyst as well as preparation method and application of defect-rich molybdenum-doped cobalt selenide / nanocarbon electrocatalyst

    CN112481653A

  • Preparation method of nitrogen-doped molybdenum and tungsten carbide nano material electrocatalyst

    CN113122866A

  • Synthesis method of ZnMo-MOF-derived carbon-coated molybdenum carbide

    CN114100648A

  • Nano tungsten-molybdenum hydrogen evolution catalyst as well as preparation method and application thereof

    CN116145153A

  • Ruthenium-loaded molybdenum carbide catalyst, membrane electrode and preparation method and application of ruthenium-loaded molybdenum carbide catalyst and membrane electrode

    CN118007170A

Cited By

  • Two-dimensional tungsten carbide nanosheet loaded non-noble metal catalyst as well as preparation and application thereof

    CN119736662A