Growth device and growth method for growing gallium oxide single crystal by edge-defined film-fed growth method
By using thermal radiation heating and specific power control in the device for growing gallium oxide single crystals in the mode guide method, the controllable width and thickness in the same furnace are achieved, and the thermal field design and process incompatibility in the prior art are solved. The problem of this paper improves the yield rate of single crystals and reduces waste of raw materials.
Patent Information
- Application Number
- CN202411185614.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-01
AI Technical Summary
The existing method of growing gallium oxide single crystals in mode guide method requires two furnaces, and the thermal field design and process are incompatible, resulting in low growth and yield of hetero crystals.
A growth device including crucible, mold, crucible cover, heating body and cover plate is designed. The crucible and mold are heated more uniformly by heat radiation, reducing the surface temperature gradient of the mold, and realizing the same furnace through specific power control steps. The controllable width and thickness within the time of the shoulder-release process.
It effectively avoids the growth of hetero crystals, improves the yield of large-thick gallium oxide single crystals, and reduces raw material waste.
Smart Images

Figure CN118880463A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of gallium oxide single crystal growth, and in particular to a growth device and a growth method for growing gallium oxide single crystal using a guided mode method. Background Art
[0002] The methods for growing single crystals (such as gallium oxide single crystals) include the guided mold method, the crucible descent method, etc. Among them, the guided mold method is a growth method that uses a mold to transport the raw material melt to the top of the mold through capillary action to grow into a crystal. When the guided mold method grows thick gallium oxide single crystals, there are shoulder release processes in both the horizontal width and thickness directions. Due to the anisotropic growth habits of gallium oxide, uncontrolled random direction growth will occur. This process greatly increases the probability of random small face growth, resulting in the subsequent crystals growing unexpected impurities, polycrystals, etc., which greatly reduces the yield rate.
[0003] In order to solve the problem of impure crystals, a multi-step method for preparing large-thickness single crystals has been proposed. However, this method requires that after a crystal of a certain width is grown in the first step, it is used as a large-size seed crystal to grow thicker crystals again, which requires two furnaces. In addition, the thermal field design and process between these two steps are not completely compatible.
[0004] Therefore, the prior art still needs to be improved and developed. Summary of the invention
[0005] In view of the above-mentioned deficiencies in the prior art, an object of the present invention is to provide a growth device and a growth method for growing gallium oxide single crystals by a guided mode method, aiming to solve the problem that the existing method requires two furnaces and the thermal field design and process between the two times are not fully compatible.
[0006] The technical solution of the present invention is as follows:
[0007] A growth device for growing gallium oxide single crystals by a guided mold method, the growth device comprising a crucible, a mold, a crucible cover, a heating element and a cover plate, characterized in that the mold is arranged in the crucible, the cover plate and the crucible cover are respectively provided with a first large-size through hole and a second large-size through hole at the center, the horizontal distance difference between the edge of the first large-size through hole at the center of the cover plate and the edge of the mold is 5 to 20 mm, and the horizontal distance difference between the second large-size through hole at the center of the crucible cover and the edge of the mold is 1 to 2 mm; the crucible cover covers the upper edge of the crucible; the cover plate covers the upper edge of the heating element; the heating element surrounds the periphery of the crucible in an annular shape, and the upper edge of the heating element is 10-15 mm higher than the upper edge of the crucible;
[0008] Optionally, the diameter of the heating element is 10-20 mm larger than the diameter of the crucible.
[0009] Preferably, the heating element is made of metal iridium.
[0010] Optionally, the through hole of the cover plate is in a square or playground track shape.
[0011] Preferably, the heating element, the crucible, the mold, the crucible cover and the cover plate are arranged in an axisymmetric manner.
[0012] The above device is used to grow a gallium oxide single crystal, and the method steps include:
[0013] S1. Melting the raw materials: The power of the heating element is increased by electromagnetic induction, and then the heat is transferred to the crucible by thermal radiation, so that the temperature of the crucible is increased and the gallium oxide raw materials therein are completely melted. When the raw material melt rises to the upper surface of the mold and reaches a stable state, the power is stopped;
[0014] S2. Seeding: Use cubic columnar gallium oxide seed crystals for seeding, slowly lower the seed crystals at a speed of 5-10 μm / s, so that the cubic columnar gallium oxide seed crystals contact the melt on the upper surface of the mold, and melt the end of the seed crystal 5 to 10 mm and then connect with the melt;
[0015] S3. Neck shrinking: slightly increase the power of the entire heating element 3 by 50-100w, slowly pull the seed crystal vertically upward at a speed of 5-10μm / s, so that the cross-section of the newly grown seed crystal end is smaller than the cross-section of its original cubic column, and the neck shrinking is completed after pulling for 3 to 5mm. The surface of the seed crystal parallel to the width of the mold, that is, the long side, is used as the main growth surface;
[0016] S4. Width shoulder release: reduce the total power of the heating element 3 by less than 100w / h, and stop reducing the power when a shoulder release trend is observed; the crystal will remain parallel to the crystal plane during the shoulder release process; pull the seed crystal vertically upward at a speed of 10-20μm / s to gradually expand the width of the crystal at the end of the seed crystal;
[0017] S5. Thickness shoulder release: After the S4 width shoulder release step is completed, the total power of the heating element 3 is continued to be reduced at a rate of 50-100W / h to increase the temperature gradient between the cover plate and the mold; the seed crystal is continued to be pulled vertically upward at a speed of 10-40μm / s to make the seed crystal end crystal evenly expand in the thickness direction;
[0018] S6. Equal-diameter growth: When the S5 thickness shoulder release step is completed, all shoulder release processes are completed and the equal-diameter growth stage is entered. According to the growth situation, the existing power of the heating element is maintained or the total power of the heating element 3 is appropriately reduced at a rate of 50-100W / h. The seed crystal is continued to be pulled vertically upward at a speed of 10-40μm / s to achieve equal-diameter growth and obtain a thick gallium oxide single crystal.
[0019] Preferably, the cross-sectional dimensions of the cubic columnar seed crystal rod are 4 mm×4 mm to 5 mm×5 mm.
[0020] Beneficial effects: The present invention adds a heating element to the growth device of the conventional guided mold method for growing gallium oxide single crystals, and makes its upper edge higher than the upper edge of the crucible by 10-15mm. After adding the heating element, the crucible is first heated by thermal radiation, and then the raw materials are heated by the crucible. The increased thermal radiation process makes the crucible and the mold heated more evenly, thereby reducing the temperature gradient on the mold surface. In addition, the portion of the heating element that is higher than the upper surface of the crucible can heat the space above the mold and reduce the temperature gradient above the mold. The use of the growth device is conducive to realizing a controllable growth process in the same furnace in which the shoulders are first placed only in the width direction and then the thickness is expanded, which effectively avoids the growth of impure crystals and improves the yield of large-thickness gallium oxide single crystals. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 A schematic diagram of a structure in which a heating element and a cover plate are arranged on the periphery of a crucible provided in an embodiment of the present invention.
[0022] Figure 2 This is a schematic diagram of releasing the shoulders in the width direction first during the shoulder release process.
[0023] Figure 3 This is a schematic diagram of placing the shoulder in the thickness direction after the shoulder is placed in the width direction.
[0024] Figure 4 Schematic diagram of the gallium oxide single crystal prepared by the method of Example 1.
[0025] Figure 5 This is a schematic diagram of the gallium oxide crystal prepared by the method of Comparative Example 1. DETAILED DESCRIPTION
[0026] The present invention provides a growth device and a growth method for growing gallium oxide single crystals by a guided mode method. In order to make the purpose, technical solution and effect of the present invention clearer and more specific, the present invention is further described in detail below. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0027] The embodiment of the present invention provides a growth device for growing gallium oxide single crystals by a guided mode method, such as Figure 1 As shown, the growth device includes a crucible 5, a mold 4 located in the crucible 5, and a crucible cover 2 located on the crucible 5, wherein the growth device also includes:
[0028] A heating element 3, wherein the heating element 3 is located outside the crucible 5, and the upper edge of the heating element 3 is 10-15 mm higher than the upper edge of the crucible 5;
[0029] A cover plate 1 is provided on the heating element 3 , and a through hole 6 is provided at the center of the cover plate 1 .
[0030] In the embodiment of the present invention, based on the conventional growth device for growing gallium oxide single crystal by guided mold method (growth device for single crucible), a heating element 3 is added, and its upper edge is higher than the upper edge of the crucible by 10-15 mm.
[0031] Conventional heat field directly heats the internal raw materials through the crucible 5 to melt. After adding the heating element 3, the crucible 5 is first heated by heat radiation, and then the raw materials are heated by the crucible 5. The added heat radiation process makes the crucible 5 and the mold 4 heated more evenly, thereby reducing the temperature gradient on the surface of the mold 4. In addition, the portion of the heating element 3 that is higher than the upper surface of the crucible 5 can be used as a post-heating structure to reduce the temperature gradient of the mold 4, that is, the space above the mold 4 can be heated to reduce the vertical temperature gradient above the mold 4.
[0032] In addition, in the embodiment of the present invention, a cover plate 1 with a through hole 6 at the center is covered on the heating element 3. The shape of the through hole 6 can be square or a playground runway shape, etc. The cover plate 1 is provided to form a large vertical temperature gradient range near the cover plate 1. By combining with the above-mentioned post-heating structure, a combined temperature field range of small gradient-large gradient is realized, thereby further reducing the temperature gradient of the mold 4.
[0033] In one embodiment, the diameter of the heating element 3 is 10-20 mm larger than the diameter of the crucible 5 . An appropriate distance can evenly transfer heat and reduce the radial temperature gradient of the crucible 5 and the mold 4 .
[0034] In one embodiment, the heating element 3 is made of metal iridium or other materials that can provide the same effect.
[0035] In one embodiment, a first large-sized through hole 6 and a second large-sized through hole 6' are respectively provided at the center of the cover plate 1 and the crucible cover 2. The horizontal distance difference between the edge of the first large-sized through hole 6 and the edge of the mold 4 is between 5 and 20 mm, such as 5 mm, 15 mm, 20 mm, etc., and the horizontal distance difference between the edge of the second large-sized through hole 6' and the edge of the mold 4 is between 1 and 2 mm.
[0036] In one embodiment, the heating element 3, the crucible 5, the mold 4, the crucible cover 2 and the cover plate 1 are arranged in an axisymmetric manner.
[0037] The embodiment of the present invention provides a method for growing a gallium oxide single crystal using the growth device described in the embodiment of the present invention, which comprises the steps of:
[0038] The seeding and necking are performed sequentially;
[0039] like Figure 2-Figure 3As shown, the power is then reduced, and after a shoulder release trend is observed, the power reduction is stopped, and shoulder release in the width direction is performed. After the shoulder release in the width direction is completed, shoulder release in the thickness direction is performed;
[0040] Then, isodiametric growth is carried out to obtain gallium oxide single crystal.
[0041] In one embodiment, the power is reduced at a rate of less than 100 w / h.
[0042] In one embodiment, the shouldering in the thickness direction is performed under the condition of cooling. Specifically, the cooling effect can be achieved by reducing the power. Preferably, the power is reduced at a rate of 50 to 100 w / h.
[0043] Specifically, the (100) plane is selected as the main growth plane, and the pulling direction is <010> During the growth process, after the conventional steps such as seeding and necking, the power is first reduced slightly. After observing the trend of shoulder release, the power reduction is stopped. Due to the characteristics of the (100) plane growth habit, the crystal will maintain the shoulder release process in the width direction parallel to the (100) plane during the pulling process. After the width shoulder release is completed, the temperature is continued to be lowered to provide sufficient supercooling, and the shoulder will be evenly expanded in the thickness direction. After the shoulder release is completed, it can be pulled with equal diameter to obtain a thick gallium oxide single crystal.
[0044] In the embodiment of the present invention, by adopting the growth device of the embodiment of the present invention and combining it with the power control process, a controllable growth process of first placing shoulders in one dimension and then placing shoulders in the thickness direction is achieved in the same furnace, which effectively avoids the growth of impure crystals and improves the yield of large-thickness gallium oxide single crystals.
[0045] The unidirectional growth of the crystal (100) plane does not require a large growth driving force, so the thermal field temperature gradient is required to be small and rapid cooling is not allowed in the process. By adopting the embodiment of the present invention, the thermal field and process are coordinated to achieve one-dimensional direction controllable shoulder release.
[0046] Specifically, by adopting the thermal field of the embodiment of the present invention, the temperature gradient in the space above the mold 4 is easier to control. When the shoulder is released, the space above the mold 4 under the cover plate 1 has a smaller temperature gradient, and the power is controlled to achieve the growth of the crystal only in the radial direction of the mold 4. After the shoulder is released, the process is adjusted to achieve growth in the thickness direction of the mold 4.
[0047] The shoulder release process of the embodiment of the present invention is controllable in steps, avoiding wide and thick two-dimensional random shoulder release, and the single crystal yield is high; all processes are completed in a single continuous process, and the process is simple; usually the shoulder release triangle part is a non-machinable part, which will cause waste of raw materials. This method greatly reduces the waste rate of raw materials.
[0048] The present invention is further described in detail below through several embodiments.
[0049] Example 1
[0050] like Figure 1 As shown, on the basis of the conventional single crucible 5, a heating element 3 with a diameter greater than 10-20 mm is added, and its upper edge is 10-15 mm higher than the crucible 5. The raised portion serves as a post-heating structure, which greatly reduces the surface gradient of the mold 4.
[0051] 1. If Figure 1 As shown, a cover plate 1 with a middle through hole 6 is placed on the heating element 3, and the through hole is square in shape, so as to achieve the function of segmented regulation of the axial gradient.
[0052] 2. If Figure 2 As shown, the crystal plane 9 is the main growth plane, which is the (100) plane, and the pulling direction is the
[010] crystal direction 10.
[0053] 3. During the growth process, first increase the total power of the heating element 3. After the heating element 3 is heated by electromagnetic induction, the heat is transferred from the heating element 3 to the crucible 5 through the thermal radiation process, so that its temperature continues to rise. When the gallium oxide raw material in the crucible 5 is completely melted into a melt and rises to the upper surface of the mold 4, stop increasing the power. Then, the seed crystal 7 is seeded and inoculated. The seed crystal 7 is a gallium oxide seed crystal with a size of 5mm×5mm×50mm. The seed crystal 7 is slowly lowered and contacted with the melt on the upper surface of the mold 4, so that the end 5 to 10mm of the seed crystal 7 is partially melted and connected to the melt, and the seeding and inoculation operation is completed. Then, necking is performed, and the total power of the heating element 3 is slightly increased by 25-50w, and it is slowly pulled upward by 5-10μm / s, so that the cross-section of the grown crystal is 2mm×2mm to 3mm×3mm, which is smaller than the cross-section of the seed crystal 7. The necking process is completed after pulling for about 5mm. After these processes are completed, first reduce the total power of the heating element 3 slightly (<100w / h), and stop reducing the power after observing a shouldering trend. At this time, due to the presence of the heating element 3 and the cover plate 1, a smaller temperature gradient can be ensured between the cover plate 1 and the mold 4. The upper surface of the mold 4 also has a smaller temperature gradient. Therefore, combined with the characteristics of the growth habit of the (100) plane, it is not easy to grow in the direction perpendicular to the (100) plane, and tends to expand the area of the (100) plane during growth. Therefore, during the pulling process, the crystal 8 will maintain a lateral shouldering process parallel to the (100) plane, that is, it will grow in the form of increasing the crystal plane 9. At this time, the morphology of the crystal 8 is as follows: Figure 2 The pulling speed can be 10-20μm / s.
[0054] 4. When the width shoulder is completed, continue to reduce the power by 50-100w / h to increase the temperature gradient between the cover plate 1 and the mold 4, provide sufficient supercooling, and the pulling speed can remain unchanged. The pulling speed can be 10-20μm / s, or it can be appropriately increased by 10-40μm / s. At this time, the thickness direction will be evenly expanded, such as Figure 3 .
[0055] 5. After the shoulder is released, the pulling can be performed in equal diameter. The pulling speed can remain unchanged at 10-20 μm / s, or can be appropriately increased to 10-40 μm / s. The obtained crystal 8 is a large thickness gallium oxide single crystal. The structural diagram is shown in Figure 4 shown.
[0056] Comparative Example 1
[0057] The purpose of Comparative Example 1 is to compare the crystal quality obtained by the existing shoulder release process and the step-by-step shoulder release process. The difference is that Comparative Example 1 does not control the shoulder release morphology and allows the shoulder to be released in all directions, while Example 1 requires shoulder release in the radial direction parallel to the (100) plane first, and then shoulder release in the thickness direction after the radial shoulder release is completed. Operation process of Comparative Example 1:
[0058] 1. If Figure 2 As shown, the crystal plane 9 is the main growth plane, which is the (100) plane, and the pulling direction is the
[010] crystal direction 10.
[0059] 2. During the growth process, first increase the total power of the heating element 3. After the heating element 3 is heated by electromagnetic induction, the heat is transferred from the heating element 3 to the crucible 5 through the thermal radiation process, so that its temperature continues to rise. When the gallium oxide raw material in the crucible 5 is completely melted into a melt and rises to the upper surface of the mold 4, stop increasing the power. Then, the seed crystal 7 is seeded and inoculated. The seed crystal 7 is a gallium oxide seed crystal with a size of 5mm×5mm×50mm. The seed crystal 7 is slowly lowered and contacted with the melt on the upper surface of the mold 4, so that the end 5 to 10mm of the seed crystal 7 is partially melted and connected to the melt, and the seeding and inoculation operation is completed. Then, necking is performed, and the total power of the heating element 3 is slightly increased by 25-50w, and it is slowly pulled upward by 5-10μm / s, so that the cross-section of the grown crystal is 2mm×2mm to 3mm×3mm, which is smaller than the cross-section of the seed crystal 7. The necking process is completed after pulling for about 5mm.
[0060] 3. Reduce the power by 50-100w / h and release the shoulders. The pulling speed can remain unchanged or be appropriately increased by 10-40μm / s.
[0061] 4. After shoulder release, equal diameter pulling is completed. The pulling speed can remain unchanged or be appropriately increased by 10-40μm / s. The structural schematic diagram of the obtained crystal 8 is as follows Figure 5 shown.
[0062] In summary, the present invention provides a growth device and a growth method for growing gallium oxide single crystals by a guided mode method. By adopting a specific thermal field structure and combining a specific power control process, a controllable growth process of first placing shoulders in one dimension and then placing shoulders in the thickness direction in the same furnace is realized, which effectively avoids the growth of impurity crystals and improves the yield of large-thickness gallium oxide single crystals. The shoulder placing process of the embodiment of the present invention is controllable in steps, avoiding wide and thick two-dimensional random shoulder placing, and the single crystal yield is high; all processes are completed in a single continuous process, and the process is simple; usually the shoulder placing triangle part is a non-machinable part, which will cause waste of raw materials, and this method greatly reduces the waste rate of raw materials.
[0063] It should be understood that the application of the present invention is not limited to the above examples. For ordinary technicians in this field, improvements or changes can be made based on the above description. All these improvements and changes should fall within the scope of protection of the claims attached to the present invention.
Claims
1. A growth device for growing gallium oxide single crystals by a guided mold method, the growth device comprising a crucible (5), a mold (4), a crucible cover (2), a heating element (3) and a cover plate (1), It is characterized in that The mold (4) is arranged in the crucible (5); the cover plate (1) and the crucible cover (2) are both provided with large-sized through holes at their centers, namely, a first large-sized through hole (6) and a second large-sized through hole (6'); the horizontal distance difference between the edge of the first large-sized through hole (6) and the edge of the mold (4) is 5 to 20 mm, and the horizontal distance difference between the edge of the second large-sized through hole (6') and the edge of the mold (4) is 1 to 2 mm; the crucible cover (2) covers the upper edge of the crucible (5); the cover plate (1) covers the upper edge of the heating element (3); the heating element (3) surrounds the outer periphery of the crucible (5) in a ring shape, and the upper edge of the heating element (3) is 10 to 15 mm higher than the upper edge of the crucible (5).
2. A growth device for growing gallium oxide single crystals by a guided mode method according to claim 1, It is characterized in that The diameter of the heating element (3) is 10-20 mm larger than the diameter of the crucible (5).
3. The growth device for growing gallium oxide single crystal by guided mode method according to claim 1, It is characterized in that The heating element (3) is made of metal iridium.
4. The growth device for growing gallium oxide single crystal by guided mode method according to claim 1, It is characterized in that The through hole of the cover plate (1) is in the shape of a square or a playground track.
5. The growth device for growing gallium oxide single crystal by guided mode method according to claim 1, It is characterized in that The heating element (3), the crucible (5), the mold (4), the crucible cover (2) and the cover plate (1) are arranged in an axisymmetric manner.
6. A method for growing a gallium oxide single crystal by using the growth device for growing a gallium oxide single crystal by the guided mode method according to any one of claims 1 to 5, It is characterized in that The method mainly comprises the following steps: S1. Melting the raw materials: The power of the heating element (3) is increased by electromagnetic induction, and then the heat is transferred to the crucible (5) by thermal radiation, so that the temperature of the crucible (5) is increased, and the gallium oxide raw material therein is completely melted. When the raw material melt rises to the upper surface of the mold (4) and reaches a stable state, the power is stopped; S2. Seeding: Seeding is performed using a seed crystal (7), wherein the seed crystal (7) is a cubic columnar gallium oxide material, and the seed crystal (7) is slowly lowered at a speed of 5-10 μm / s so that the seed crystal (7) contacts the melt on the upper surface of the mold (4), and the end portion of the seed crystal (7) is melted by 5 to 10 mm and then connected to the melt; S3. Perform necking: slightly increase the power of the entire heating element (3) by 50-100w, slowly pull the seed crystal (7) vertically upward at a speed of 5-10μm / s, so that the end cross-section of the newly grown seed crystal (7) is smaller than the cross-section of its original cubic column, and the necking is completed after pulling for 3 to 5mm. The surface of the seed crystal (7) parallel to the width of the mold (4), that is, the long side, is used as the main growth surface, that is, the crystal surface (9); S4. Width shouldering: Reduce the total power of the heating element 3 by less than 100w / h, and stop reducing the power when a shouldering trend is observed; the crystal will remain parallel to the crystal plane (9) during the shouldering process; pull the seed crystal (7) vertically upward at a speed of 10-20μm / s, so that the width of the crystal at the end of the seed crystal (7) gradually expands; S5. Thickness shouldering: After the width shouldering step S4 is completed, the total power of the heating element 3 is continued to be reduced at a rate of 50-100W / h to increase the temperature gradient between the cover plate (1) and the mold (4); the seed crystal (7) is continued to be pulled vertically upward at a speed of 10-40μm / s, so that the end crystal of the seed crystal (7) is uniformly expanded in the thickness direction; S6. Equi-diameter growth: When the S5 thickness shoulder release step is completed, all shoulder release processes are completed and the equi-diameter growth stage is entered. According to the growth situation, the existing power of the heating element (3) is maintained or the total power of the crystal growth furnace is appropriately reduced at a rate of 50-100W / h. The seed crystal (7) is continuously pulled vertically upward at a speed of 10-40μm / s to achieve equi-diameter growth and obtain a thick gallium oxide single crystal (8).