Method for designing multi-pass reducing spinning track of corrugated pipe

By obtaining the characteristic size and wall thickness forming quality indicators during the corrugated diameter spinning process, a finite element model was designed and simulation experiments were conducted to determine the corrugated diameter spinning trajectory, and the corrugated diameter spinning in the existing technology was solved. Trajectory design problems realize the quantitative characterization and design of trajectories and improve the wall thickness forming quality.

CN118886128APending Publication Date: 2024-11-01NORTHWESTERN POLYTECHNICAL UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410867346.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-01
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The prior art cannot perform quantitative characterization and design of corrugated diameter spinning trajectory, which makes it difficult to control the wall thickness forming quality, and lacks clear trajectory quantization design principles and procedures, resulting in time-consuming and laborious design and poor results.

Method used

By obtaining the target feature size and wall thickness forming quality indicators during the representative period of the shrinkage spinning process of the target bellows, a finite element model is designed and simulation experiments are carried out to determine the feasible window in the form of the shrinkage spinning trajectory for each passage. , and determine the loading trajectory according to the wall thickness forming quality control targets to realize the quantitative design of the trajectory.

Benefits of technology

The trajectory design regulations and quantitative design basis were clarified, the uniformity of the wall thickness of the bellows was improved, the degree of wall thickness variation in the thinning and thickening areas was reduced, and the quality of the shrink-diameter spinning wall thickness was improved, which was highly operable and Universality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118886128A_ABST
    Figure CN118886128A_ABST
Patent Text Reader

Abstract

The invention discloses a corrugated pipe multi-pass reducing spinning track design method. The method comprises the steps that the target feature size of a target corrugated pipe component in a representative period of the reducing spinning process and the wall thickness forming quality regulation and control target and the wall thickness forming quality index of a target corrugated pipe in the reducing spinning process are obtained; designing a reducing spinning finite element model of the target corrugated pipe according to the target feature size; performing a diameter-reducing spinning simulation experiment on the finite element model, and determining a feasible window of a diameter-reducing spinning track form of each pass of the target corrugated pipe in a representative period based on a simulation experiment result and a wall thickness forming quality index; and according to the wall thickness forming quality regulation and control target, the loading track of each pass is determined from the feasible window, and the hole shrinkage spinning track of the target corrugated pipe is obtained. In this way, quantitative characterization and design of the corrugated pipe reducing spinning track can be achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of parts forming and manufacturing, and in particular to a method for designing a multi-pass shrinking spinning trajectory for a bellows. Background Art

[0002] The shrinkage spinning process controls the loading trajectory and loading parameters of the spinning wheel, and gradually applies local point loading deformation to the rotating tube blank to produce continuous local deformation accumulation to achieve the forming of variable diameter special-shaped pipe fittings. This process has the advantages of small forming load, high process flexibility and overall forming, and is widely used in the forming and manufacturing of special-shaped pipe fittings for advanced equipment such as aerospace.

[0003] The bellows is a typical type of variable diameter special-shaped pipe fittings with a complex structure. The generatrix consists of concave arc segments, convex arc segments and straight segments. When the bellows are formed by shrinking spinning, the loading trajectory of the roller is often a multi-pass complex curve. The loading conditions and boundary constraints of different structural feature segments are constantly changing. The forming wall thickness law changes in a complex way, and it is easy to produce defects such as excessive thinning, excessive thickening and uneven wall thickness, which restricts the precise forming quality and service performance of the bellows. Therefore, how to design a multi-pass shrinking spinning trajectory to improve the wall thickness forming quality is an important challenge faced by the precise forming of bellows.

[0004] The existing methods for designing the shrinking spinning trajectory are all aimed at forming the end variable diameter special-shaped tubes. For example, by adding a reverse return spinning pass between the forward spinning passes, the wall thickness quality of the end closing cylinder shrinking spinning can be controlled. Alternatively, the end closing cylinder is formed by shrinking spinning with multiple arc trajectories, and the curvature of the arc trajectory is optimized by the response surface method, so as to improve the uniformity of the wall thickness distribution of the formed part.

[0005] However, the existing trajectory design methods are all aimed at the forming of end-sealed special-shaped tubes, and cannot be used for bellows shrinking spinning with multiple sections of complex wave-shaped shrinkage; and the existing methods lack clear trajectory quantitative design principles and procedures, and can only design trajectories through empirical trial and error, which is time-consuming and labor-intensive and has poor results. The trajectory of bellows shrinking spinning is a complex curve, generally composed of multiple arcs and straight lines, which cannot be quantitatively characterized by existing methods. In addition, due to the different wall thickness variation laws in different structural feature areas during bellows shrinking spinning, the design of the loading trajectory must take into account both the local structural characteristics and the wall thickness forming requirements, which makes it difficult to achieve quantitative design through existing methods. Summary of the invention

[0006] The embodiment of the present application solves the problem in the prior art that the trajectory of the bellows shrinking spinning cannot be quantitatively characterized and designed by providing a method for designing the trajectory of the bellows shrinking spinning with multiple passes.

[0007] In order to achieve the above object, the technical solution of the embodiment of the present invention is:

[0008] In the first aspect, an embodiment of the present invention provides a method for designing a multi-pass diameter reduction spinning trajectory for a corrugated tube, comprising: obtaining a target characteristic dimension within a representative cycle of a diameter reduction spinning process of a target corrugated tube component, as well as a wall thickness forming quality control target and a wall thickness forming quality index of the target corrugated tube during the diameter reduction spinning process; designing a diameter reduction spinning finite element model of the target corrugated tube according to the target characteristic dimension; applying the finite element model to conduct a diameter reduction spinning simulation experiment, and determining a feasible window of the diameter reduction spinning trajectory form of each pass of the target corrugated tube within the representative cycle based on the results of the simulation experiment and the wall thickness forming quality index; determining the loading trajectory of each pass from the feasible window according to the wall thickness forming quality control target to obtain the diameter reduction spinning trajectory of the target corrugated tube.

[0009] In some possible implementations, the target characteristic dimensions include at least the total diameter reduction required for the target corrugated tube forming, the total axial length of the representative cycle, the axial length of the descending segment in the representative cycle, the convex arc radius of the descending segment in the representative cycle, the concave arc radius of the descending segment in the representative cycle, the length of the straight line segment in the representative cycle, the axial length of the rising segment in the representative cycle, the concave arc radius of the rising segment in the representative cycle, and the convex arc radius of the rising segment in the representative cycle.

[0010] In some possible implementations, the wall thickness forming quality control objectives include at least: improving the uniformity of the target bellows wall thickness, reducing the average wall thickness thinning degree of the target bellows thinning area, and reducing the average thickening degree of the target bellows thickening area; the wall thickness forming quality indicators include at least: the wall thickness mean square error value, the average thinning rate, and the average thickening rate; among them, the wall thickness mean square error value is an indicator for measuring the uniformity of the overall wall thickness distribution of the target bellows wall, the average thinning rate is an indicator for measuring the degree of wall thickness change in the target bellows wall thickness over-thinning area, and the average thickening rate is an indicator for measuring the degree of wall thickness change in the target bellows wall thickness over-thickening area.

[0011] In some possible implementations, the mean square error of the wall thickness is expressed as:

[0012]

[0013] The average thinning rate is expressed as:

[0014]

[0015] The average thickening rate is expressed as:

[0016]

[0017] Among them, t i Indicates the wall thickness of the bellows at different locations. Indicates the average wall thickness of the bellows; S drepresents the area enclosed by the wall thickness change rate of the excessive thinning area and the zero value, x d Represents the axial length of the excessive thinning area; S i represents the area enclosed by the wall thickness change rate of the excessive thickening area and the zero value, x i Represents the axial length of the excessive thickening area.

[0018] In some possible implementations, before designing a finite element model of the target bellows for shrinkage spinning according to the target characteristic dimensions, the method further includes: determining the shrinkage spinning trajectory form of the target bellows within a representative period, and quantitatively characterizing the trajectory form; wherein the trajectory form includes at least a descending convex arc, a descending concave arc, a straight line, an ascending concave arc, and an ascending convex arc within the representative period; the trajectory form is quantitatively characterized by the amount of shrinkage, the radius of the convex arc of the descending section, the transition angle of the arc trajectory of the descending section, the length of the straight line section, the radius of the convex arc of the ascending section, and the transition angle of the arc trajectory of the ascending section.

[0019] In some possible implementations, a finite element model is used to perform a reduction spinning simulation experiment, and based on the results of the simulation experiment and the wall thickness forming quality index, a feasible window of the reduction spinning trajectory form of the target corrugated tube in each pass within a representative cycle is determined, including: designing a first single factor experiment according to the finite element model and performing a simulation to obtain the wall thickness values ​​at different positions in the first simulation results; based on the wall thickness value, determining the reduction amount, the transition angle of the descending arc trajectory, and the transition angle of the ascending arc trajectory, and the quantitative relationship with the wall thickness forming quality index and the extreme value of the wall thickness forming quality index allowed for each pass; based on the quantitative relationship and combined with the extreme value, determining the feasible window of the reduction amount, the transition angle of the descending arc trajectory, and the transition angle of the ascending arc trajectory for each pass.

[0020] In some possible implementations, according to the wall thickness forming quality control target, the loading trajectory of each pass is determined from the feasible window to obtain the diameter reduction spinning trajectory of the target corrugated tube, including: determining the number of diameter reduction spinning passes according to the total diameter reduction amount and the determined feasible window of the diameter reduction amount of each pass; designing a second single factor experiment and performing simulation based on the finite element model, and determining the influence of the transition angle of the arc trajectory of the descending segment and the transition angle of the arc trajectory of the ascending segment on the wall thickness change of the thinning area and the thickening area according to the second simulation results; according to the wall thickness forming quality control target, based on the influence law, determining the transition angle of the arc trajectory of the descending segment and the transition angle of the arc trajectory of the ascending segment of each pass from the feasible window. The convex arc radius of the descending section of the target bellows component in the representative cycle is determined as the convex arc radius of the descending section of each pass, and the convex arc radius of the ascending section of the target bellows component in the representative cycle is determined as the convex arc radius of the ascending section of each pass; according to the limit value of the diameter reduction amount of each pass, the transition angle of the descending arc trajectory and the transition angle of the ascending arc trajectory, the radius of the concave arc of the descending section and the radius of the concave arc of the ascending section are determined respectively by a preset radius calculation formula; according to the total axial length of the representative cycle of the target bellows and the axial length of the descending arc of each pass and the axial length of the ascending arc, the length of the straight line segment of the spinning trajectory of each pass is determined.

[0021] In some possible implementations, the preset radius calculation formula is expressed as:

[0022]

[0023] Among them, d all Indicates the total reduction, d i represents the reduction amount of the first i passes, β i It represents the transition angle of the descending arc trajectory or the transition angle of the ascending arc trajectory of the i-th pass.

[0024] In some possible implementations, after obtaining the diameter reduction spinning trajectory of the target bellows, the method also includes: inputting the obtained diameter reduction spinning trajectory of the target bellows into a finite element model to obtain a simulation result of a spun component; the simulation result of the spun component includes a multi-pass spinning simulation forming result and a single-pass spinning simulation forming result; and verifying the effectiveness of the diameter reduction spinning trajectory of the target bellows by performing a quality comparison between the multi-pass spinning simulation forming result and the single-pass spinning simulation forming result.

[0025] In the second aspect, an embodiment of the present invention provides a device for designing a multi-pass diameter reduction spinning trajectory for a corrugated tube, comprising: an acquisition module, used to acquire a target characteristic dimension within a representative cycle of the diameter reduction spinning process of a target corrugated tube component, as well as a wall thickness forming quality control target and a wall thickness forming quality index of the target corrugated tube during the diameter reduction spinning process; a model construction module, used to design a diameter reduction spinning finite element model of a target corrugated tube according to the target characteristic dimension; a first determination module, used to perform a diameter reduction spinning simulation experiment on the finite element model, and determine a feasible window of the diameter reduction spinning trajectory form of each pass of the target corrugated tube within the representative cycle based on the results of the simulation experiment and the wall thickness forming quality index; a second determination module, used to determine the loading trajectory of each pass from the feasible window according to the wall thickness forming quality control target, and obtain the diameter reduction spinning trajectory of the target corrugated tube.

[0026] One or more technical solutions provided in the embodiments of the present invention have at least the following technical effects or advantages:

[0027] In the embodiment of the present invention, the target characteristic size in the representative cycle of the shrinking spinning process of the target bellows component, as well as the wall thickness forming quality control target and wall thickness forming quality index of the target bellows in the shrinking spinning process are obtained; the shrinking spinning finite element model of the target bellows is designed according to the target characteristic size; the shrinking spinning simulation experiment is carried out on the finite element model, and based on the results of the simulation experiment and the wall thickness forming quality index, the feasible window of the shrinking spinning trajectory of each pass of the target bellows in the representative cycle is determined; according to the wall thickness forming quality control target, the loading trajectory of each pass is determined from the feasible window, and the shrinking spinning trajectory of the target bellows is obtained. In this way, the trajectory design regulations and quantitative design basis are clearly given, which has strong operability and solves the problem of quantitative characterization and design difficulty of the shrinking spinning trajectory; at the same time, the structural requirements and wall thickness forming quality constraints of the target bellows are comprehensively considered, which can be used to design reasonable shrinking spinning trajectories of bellows with different structural parameters, and has strong versatility. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] In order to more clearly illustrate the embodiments of the present invention, the accompanying drawings required for use in the embodiments of the present invention will be briefly introduced below. Obviously, the accompanying drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying any creative work.

[0029] Figure 1 A schematic flow chart of an embodiment of a method for designing a trajectory for multi-pass diameter-reducing spinning of a bellows provided for the implementation of the present invention;

[0030] Figure 2 A schematic structural diagram of target features within a representative period of a target bellows component in an embodiment of the present invention;

[0031] Figure 3 Schematic diagram of the target bellows shrinking spinning trajectory in an embodiment of the present invention;

[0032] Figure 4a It is a schematic diagram of the quantitative relationship between the reduction amount, the transition angle of the arc trajectory of the descending section, the transition angle of the arc trajectory of the ascending section and the mean square error value of the wall thickness;

[0033] Figure 4b It is a schematic diagram of the quantitative relationship between the diameter reduction, the transition angle of the arc trajectory of the descending section, the transition angle of the arc trajectory of the ascending section and the average thinning rate;

[0034] Figure 4c It is a schematic diagram of the quantitative relationship between the diameter reduction, the transition angle of the arc trajectory of the descending section, the transition angle of the arc trajectory of the ascending section and the average thickening rate;

[0035] Figure 5 Schematic diagram of transition angle of wheel selection trajectory in an embodiment of the present invention;

[0036] Figure 6 A schematic diagram of a multi-pass trajectory in an embodiment of the present invention;

[0037] Figure 7 is a comparison diagram of simulation results of a spinning component in an embodiment of the present invention;

[0038] Figure 8 A comparison diagram of the effects of multi-pass shrinking spinning and single-pass shrinking spinning in an embodiment of the present invention;

[0039] Fig. 9 It is a schematic structural diagram of a device for designing a trajectory for multi-pass diameter reduction spinning of a bellows in an embodiment of the present invention. DETAILED DESCRIPTION

[0040] The technical solutions in the embodiments of the present application will be described clearly and completely below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0041] In the relevant description of this embodiment, the terms "including, containing, having" and the like are open terms and are generally understood to include but not be limited to; the term "at least one" is generally understood to mean one or more, where "plurality" refers to two or more; the term "at least one of the following" or similar expressions refers to any combination of these items, including any combination of single or plural items, for example, "at least one of a, b or c", or "at least one of a, b and c", can all represent: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or multiple, respectively; the symbol "A / B" is used to describe the selection relationship of associated objects, generally indicating an "or" relationship before and after.

[0042] In the following description of the present embodiment, the terms used in the embodiments of the present application are only for the purpose of describing specific embodiments, and are not intended to limit the present application. The singular forms "a" and "the" used in the embodiments of the present application and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.

[0043] Those skilled in the art should understand that in the following description of the embodiments of the present application, the order of serial numbers does not mean the order of execution, some or all of the steps can be executed in parallel or sequentially, and the execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.

[0044] Those skilled in the art will appreciate that the numerical ranges in the embodiments of the present application are to be construed as also specifically disclosing each intermediate value between the upper and lower limits of the scope. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the range is also included in the present invention. The upper and lower limits of these smaller ranges may be independently included or excluded in the scope.

[0045] Unless otherwise specified, the technical / scientific terms used herein have the same meanings as those generally understood by those skilled in the art to which this application belongs. Although this application only describes preferred methods and materials, any methods and materials similar or equivalent to these may also be used in the implementation or testing of this application. All documents mentioned in this specification are incorporated by reference to disclose and describe methods and / or materials related to the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0046] In order to illustrate the technical solution of the present invention, specific embodiments are provided below for illustration.

[0047] Based on the fact that existing methods lack clear trajectory quantitative design principles and procedures and are difficult to achieve quantitative design problems, an embodiment of the present invention provides a method for designing a multi-pass diameter reduction spinning trajectory for a bellows, which is used to solve the problem that the diameter reduction spinning trajectory of the bellows cannot be quantitatively characterized and designed in the prior art.

[0048] Figure 1 A schematic diagram of an embodiment of a method for designing a multi-pass shrinking spinning trajectory for a bellows provided for the implementation of the present invention, see Figure 1 As shown, the above-mentioned method for designing the trajectory of multi-pass shrinking spinning of bellows may include:

[0049] S101, obtaining a target characteristic dimension in a representative cycle of a target bellows component during a diameter reduction spinning process, and a wall thickness forming quality control target and a wall thickness forming quality index of the target bellows during the diameter reduction spinning process;

[0050] It should be noted that the target features are the key dimensions and parameters used to describe and / or evaluate the quality of bellows forming. These features are usually related to the design requirements, functional requirements and forming process of the bellows. By measuring and analyzing these target features, the specific parameters of the target bellows obtained by shrink spinning can be clarified to ensure that the bellows meet the predetermined performance standards and quality requirements.

[0051] In some embodiments, the target characteristic dimensions include at least the total reduction required for the target bellows forming, the total axial length of the representative cycle, the axial length of the descending section in the representative cycle, the convex arc radius of the descending section in the representative cycle, the concave arc radius of the descending section in the representative cycle, the length of the straight line section in the representative cycle, the axial length of the ascending section in the representative cycle, the concave arc radius of the ascending section in the representative cycle, and the convex arc radius of the ascending section in the representative cycle. Figure 2 Schematic diagram of the target feature of the target bellows component in a representative cycle in the embodiment of the present invention. The target feature size specifically included in the representative cycle during the shrinking spinning process of the target bellows component can be found in Figure 2 shown.

[0052] In some embodiments, the wall thickness forming quality control objectives may at least include: improving the uniformity of the target bellows wall thickness, reducing the average wall thickness thinning degree of the target bellows thinning area, and reducing the average thickening degree of the target bellows thickening area.

[0053] In some embodiments, the wall thickness forming quality index may include at least: a wall thickness mean square error value, an average thinning rate, and an average thickening rate.

[0054] Among them, the mean square error value of wall thickness is an indicator to measure the uniformity of the overall wall thickness distribution of the target corrugated pipe wall, the average thinning rate is an indicator to measure the degree of wall thickness change in the excessively thinned area of ​​the target corrugated pipe wall, and the average thickening rate is an indicator to measure the degree of wall thickness change in the excessively thickened area of ​​the target corrugated pipe wall.

[0055] It should be noted that in the manufacturing process of components such as bellows, the control of wall thickness forming quality is to ensure that the wall thickness of the bellows reaches the predetermined standard to meet the performance requirements and use environment of the product. The specific contents of the wall thickness forming quality control target and wall thickness forming quality index can be determined by referring to past experience, such as consulting relevant industry standards, technical literature or research reports, etc., to understand the general requirements and control methods for wall thickness forming quality in the industry, so as to determine different wall thickness forming quality control targets and wall thickness forming quality indexes suitable for corresponding components.

[0056] In some embodiments, the mean square error of the wall thickness can be expressed by the following formula (1):

[0057]

[0058] The average thinning rate can be expressed by the following formula (2):

[0059]

[0060] The average thickening rate can be expressed by the following formula (3):

[0061]

[0062] In the above formulas (1) to (3), t i Indicates the wall thickness of the bellows at different locations. Indicates the average wall thickness of the bellows; S d represents the area enclosed by the wall thickness change rate of the excessive thinning area and the zero value, x d Represents the axial length of the excessive thinning area; S i represents the area enclosed by the wall thickness change rate of the excessive thickening area and the zero value, x i Represents the axial length of the excessive thickening area.

[0063] S102, designing a finite element model of a target bellows according to a target characteristic size;

[0064] It can be understood that the purpose of designing the shrinkage spinning finite element model of the target bellows is to simulate the shrinkage spinning process of the target bellows, so as to determine the trajectory of the shrinkage spinning. However, due to the structural complexity of the bellows, the bellows usually has different trajectory forms at different positions during the shrinkage spinning process. Based on this, in some embodiments, before executing the above step S102, the above method may also include: determining the shrinkage spinning trajectory form of the target bellows in a representative cycle, and quantitatively characterizing the trajectory form;

[0065] The trajectory form includes at least a descending convex arc, a descending concave arc, a straight line, a rising concave arc and a rising convex arc within a representative period.

[0066] In some embodiments, the trajectory form can be quantitatively characterized by the reduction amount, the radius of the convex arc of the descending section, the transition angle of the arc trajectory of the descending section, the length of the straight section, the radius of the convex arc of the ascending section, and the transition angle of the arc trajectory of the ascending section. Figure 3 Schematic diagram of the target bellows shrinking spinning trajectory in the embodiment of the present invention. The various types of structures included in the above trajectory can be obtained by Figure 3 The various parameters of the target bellows shown in are quantitatively characterized.

[0067] In some embodiments, the design and implementation of the finite element model can be accomplished with the aid of various existing finite element analysis software, which provides engineers and scientists with powerful tools to simulate and analyze complex physical phenomena. For example, ABAQUS, which is a powerful tool that can be used to simulate and analyze the behavior of bellows during the shrink spinning process, thereby optimizing the design and improving production efficiency and guiding the actual production process.

[0068] In some embodiments, the above step S102 may include:

[0069] S1021, the S4R unit in ABAQUS is used to discretize the blank into grids;

[0070] S1022, inputting stress-strain data of material tensile deformation into a material model;

[0071] S1023, selecting a Coulomb friction model to describe the contact friction conditions at the interface between the workpiece and the mold;

[0072] S1024, setting the wheel loading boundary condition through the amplitude curve.

[0073] In this way, through the above steps S1021 to S1024, it is possible to construct a finite element model of the target bellows by reducing the diameter of the bellows.

[0074] S103, performing a spin shrinking simulation experiment on the finite element model, and determining a feasible window of the spin shrinking trajectory of each pass of the target bellows in a representative cycle based on the results of the simulation experiment and the wall thickness forming quality index;

[0075] In some embodiments, the above step S103 may include:

[0076] S1031, designing a first single factor test according to the finite element model and performing simulation to obtain wall thickness values ​​at different positions in the first simulation result;

[0077] S1032, determining the reduction amount, the transition angle of the descending arc trajectory, and the transition angle of the ascending arc trajectory based on the wall thickness value, the quantitative relationship between the wall thickness forming quality index, and the extreme value of the wall thickness forming quality index allowed for each pass;

[0078] S1033, according to the quantitative relationships obtained above, combined with the extreme value of the wall thickness forming quality index allowed for each pass, the feasible windows of the diameter reduction amount, the transition angle of the descending arc trajectory, and the transition angle of the ascending arc trajectory of each pass are determined.

[0079] Specifically, by taking each key factor affecting wall thickness forming (such as the above-mentioned reduction, the transition angle of the arc trajectory of the descending section, and the transition angle of the arc trajectory of the ascending section) as the experimental variable, setting different levels (i.e., different values) for each experimental variable, and running the simulation, the wall thickness values ​​that can be reached at different positions, such as the crest and trough of the corrugation, are extracted from the simulation results. By analyzing the wall thickness values ​​obtained by the simulation, the relationship between them and the experimental variables such as the reduction and the transition angle is found out respectively. Then, statistical methods such as regression analysis can be used to establish a mathematical model between the experimental variables and the above-mentioned wall thickness forming quality indicators, so as to obtain the quantitative relationship between the reduction, the transition angle of the arc trajectory of the descending section, and the transition angle of the arc trajectory of the ascending section, and the wall thickness forming quality indicators. Afterwards, according to the established mathematical model, the experimental variable values ​​that make the wall thickness forming quality indicators reach the optimal or meet the preset conditions such as specific requirements can be found, that is, the extreme values ​​of the above-mentioned wall thickness mean square error value, the average thinning rate, and the average thickening rate.

[0080] Finally, according to the quantitative relationship obtained above, with the above extreme values ​​as the boundary range, the feasible windows of the diameter reduction, the transition angle of the descending arc trajectory and the transition angle of the ascending arc trajectory can be determined respectively. Among them, the feasible window of the diameter reduction can be the value range of the specific diameter reduction length value, and the feasible windows of the transition angle of the descending arc trajectory and the transition angle of the ascending arc trajectory can be the value range of the corresponding angle values.

[0081] For example, FIG4 is a schematic diagram of a quantitative relationship between the diameter reduction, the transition angle of the descending arc trajectory, and the transition angle of the ascending arc trajectory and the wall thickness forming quality index in an embodiment of the present invention. Among them, FIG4(a) is a schematic diagram of the quantitative relationship between the diameter reduction, the transition angle of the descending arc trajectory, and the transition angle of the ascending arc trajectory and the mean square error value of the wall thickness; FIG4(b) is a schematic diagram of the quantitative relationship between the diameter reduction, the transition angle of the descending arc trajectory, and the transition angle of the ascending arc trajectory and the average thinning rate; FIG4(c) is a schematic diagram of the quantitative relationship between the diameter reduction, the transition angle of the descending arc trajectory, and the transition angle of the ascending arc trajectory and the average thickening rate.

[0082] It should be noted that the values ​​of the parameters specifically determined in FIG. 4 are only exemplary descriptions, and the determined parameter values ​​are different under different requirements for target bellows parameters.

[0083] S104, according to the wall thickness forming quality control target, determine the loading trajectory of each pass from the feasible window to obtain the shrinking spinning trajectory of the target corrugated tube.

[0084] In some embodiments, the above step S104 may include:

[0085] S1041, determining the number of diameter reduction spinning passes according to the total diameter reduction amount and the determined feasible window of the diameter reduction amount for each pass;

[0086] Specifically, the number of spinning passes and the diameter reduction amount of each pass can be obtained based on the allocation principle that the diameter reduction amount of each pass does not exceed the feasible window and the number of passes is as small as possible. The calculation formula of the number of passes n can be expressed by the following formula (4):

[0087]

[0088] Among them, d all Indicates the total reduction, d max Indicates the maximum reduction allowed in each pass.

[0089] S1042, based on the finite element model, design a second single factor test and perform simulation, and determine the influence of the arc trajectory transition angle of the descending section and the arc trajectory transition angle of the ascending section of each pass on the wall thickness change of the thinning area and the thickening area according to the second simulation results;

[0090] In the embodiment of the present invention, the second single factor test can use the transition angle of the descending arc trajectory and the transition angle of the ascending arc trajectory as single factor variables, and then design a series of different transition angle values ​​as test variables. For each transition angle value, run the finite element simulation, monitor and record the wall thickness change data of the thinning area and the thickening area, so as to summarize and determine the influence of the transition angle on the wall thickness change. For example, the increase of the transition angle may make the thinning area thinner and the thickening area thicker, or vice versa.

[0091] S1043, according to the wall thickness forming quality control target and based on the influencing law, the transition angle of the arc trajectory of the descending section and the transition angle of the arc trajectory of the ascending section of each pass are determined from the feasible window;

[0092] Specifically, in order to meet the goal of reducing the average wall thickness thinning degree in the excessive thinning area and the average wall thickness thickening degree in the excessive thickening area, based on the influence law, the transition angle is as small as possible in the excessive thinning area, and the transition angle is as large as possible in the excessive thickening area.

[0093] S1044, determining the convex arc radius of the descending section of the target bellows component in the representative cycle as the convex arc radius of the descending section of each pass, and determining the convex arc radius of the ascending section of the target bellows component in the representative cycle as the convex arc radius of the ascending section of each pass;

[0094] It is understandable that in the spinning process, the formation of the convex arc is directly affected by the contact surface between the spinning wheel and the workpiece. In order to ensure that the spinning wheel can evenly apply force and move smoothly along the workpiece surface, the radius of the convex arc can be designed to be equal to the radius of the spinning wheel.

[0095] S1045, according to the limit value of the diameter reduction amount of each pass, the transition angle of the arc trajectory of the descending section and the transition angle of the arc trajectory of the ascending section, the radius of the concave arc of the descending section and the radius of the concave arc of the ascending section of each pass are determined by a preset radius calculation formula;

[0096] In some embodiments, the above preset radius calculation formula can be expressed by the following formula (5):

[0097]

[0098] Among them, d all Indicates the total reduction, d i represents the reduction amount of the first i passes, β i represents the transition angle of the descending arc track or the transition angle of the ascending arc track of the i-th pass. For example, the variables of the transition angle of the wheel track can be referred to Figure 5 As shown, Figure 5 Schematic diagram of the transition angle of the wheel selection trajectory in an embodiment of the present invention.

[0099] In addition, since the concave arc radius needs to match the wheel radius: if the wheel radius is smaller than the calculated concave arc radius, the calculated concave arc radius is used to draw the trajectory; if the wheel radius is larger than the calculated wheel radius, the wheel radius can be used directly to draw the trajectory due to tooling limitations. Therefore, after determining the corresponding ascending or descending concave arc radius through the above formula (5), the concave arc radius r of the descending and ascending sections of each pass can be compared respectively. i The radius of the roller corner R rIf r i <R r , then the radius of the roller corner is used as the concave arc radius of the descending or ascending section of the i-th pass; if r i >R r , then the calculated r i Determine the concave arc radius of the descending or ascending section of the i-th pass.

[0100] S1046, determining the length of the straight line segment of each spinning trajectory according to the total axial length of the representative cycle of the target bellows and the axial length of the descending arc of each pass and the axial length of the ascending arc of each pass.

[0101] It can be understood that each pass in a representative cycle of the bellows includes the entire length from the trough to the peak and back to the trough. Therefore, the sum of the lengths of all the parts that make up this cycle must be equal to the total axial length of this representative cycle. When the total axial length of a representative cycle of the target bellows (i.e. the axial length of a complete corrugation) and the axial lengths of the descending arc and the ascending arc in each pass are known, based on this information, the length of the straight line segment of each pass spinning trajectory can be calculated.

[0102] By repeatedly executing the above steps S1042 to S1045, until the loading trajectories of the other passes except the last pass are determined, the last pass can be formed according to the target bellows component contour. In this way, the loading trajectory of each pass of the target bellows can be determined, thereby determining the shrinking spinning trajectory of the target bellows.

[0103] For example, see Figure 6 As shown, Figure 6 Through the above steps S101 to S104, the specific loading trajectory of each pass in the target bellows shrinking spinning process can be determined. In the actual spinning process, it is only necessary to load according to the determined trajectory, thus realizing the quantitative characterization of the spinning trajectory.

[0104] In the embodiment of the present invention, the design procedure and quantitative design basis of the target bellows shrinking spinning trajectory are clearly given, which has strong operability and solves the problem of quantitative characterization and design difficulty of the shrinking spinning trajectory; moreover, the method comprehensively considers the structural requirements and wall thickness forming quality constraints of the target bellows, and can be used to design reasonable shrinking spinning trajectories of bellows with different structural parameters, with strong versatility. At the same time, it also improves the uniformity of the overall wall thickness of the bellows, and further reduces the wall thickness thinning degree of the thinning area and the wall thickness thickening degree of the thickening area, effectively improving the wall thickness forming quality of the bellows shrinking spinning.

[0105] In some embodiments, after obtaining the shrinking spinning trajectory of the target bellows, the above method may further include validating the obtained spinning trajectory. Specifically, the method may include the following steps:

[0106] S11, inputting the obtained diameter reduction spinning trajectory of the target bellows into the finite element model to obtain a spinning component simulation result; the spinning component simulation result includes a multi-pass spinning simulation forming result and a single-pass spinning simulation forming result;

[0107] S12, by comparing the quality of multi-pass spinning simulation forming results and single-pass spinning simulation forming results, the effectiveness of the diameter reduction spinning trajectory of the target bellows is verified.

[0108] Specifically, the obtained trajectory is input into the shrinkage spinning finite element model to obtain the simulation results of the spinning component. Figure 7 As shown, Figure 7 The following is a comparison chart of the simulation results of the spinning component in the embodiment of the present invention. Then, by comparing the results of the multi-pass shrinking spinning of the bellows with the single-pass shrinking spinning, it is determined whether the maximum wall thickness thinning rate and the maximum wall thickness thickening rate of the multi-pass shrinking spinning are reduced or whether the reduction range meets the preset conditions. Figure 8 As shown, Figure 8 This is a comparison diagram of the effects of multi-pass shrinking spinning and single-pass shrinking spinning in an embodiment of the present invention. The horizontal axis is the normalized position after each pass of loading in a representative cycle, and the vertical axis is the wall thickness change rate. Figure 8 As shown, compared with single-pass, the maximum wall thickness reduction rate of multi-pass shrinkage spinning is reduced by about 15%, and the maximum wall thickness increase rate is reduced by about 3%.

[0109] It should be noted that Figure 7 and Figure 8 The values ​​of the parameters in the embodiment of the present invention are only an exemplary description, and the specific parameter values ​​can be specifically determined based on different parameter values ​​such as the target bellows specifications.

[0110] Finally, the wall thickness forming quality indicators of the multi-pass shrink spinning and single-pass shrink spinning of the bellows can be compared to determine whether the wall thickness forming quality indicators of the multi-pass shrink spinning are optimized compared to the single-pass, or whether the optimization effect meets the preset conditions. In this way, by comparing the optimization results of the maximum wall thickness reduction rate, the maximum wall thickness increase rate, and the wall thickness forming quality indicators of the multi-pass shrink spinning, it can be determined whether the obtained spinning trajectory is effective.

[0111] The process of steps S101 to S104 is described in detail below using a specific embodiment.

[0112] In the embodiment of the present invention, it is first determined that the total axial length of the representative cycle of the target component is 66.96 mm, the axial length of the descending section in the representative cycle is 25.98 mm, the convex arc radius of the descending section in the representative cycle is 15 mm, the concave arc radius of the descending section in the representative cycle is 15 mm, the length of the straight line segment in the representative cycle is 15 mm, the axial length of the ascending section in the representative cycle is 25.98 mm, the convex arc radius of the ascending section in the representative cycle is 15 mm, and the concave arc radius of the ascending section in the representative cycle is 15 mm.

[0113] Secondly, the quality control targets of bellows shrinkage spinning wall thickness forming are to improve the uniformity of bellows wall thickness, reduce the average wall thickness thinning degree in the excessive thinning area and the average thickness in the excessive thickening area, and the mean square error of wall thickness t MSE , average thinning rate The average thickening rate As a wall thickness forming quality indicator.

[0114] The form of the shrinkage spinning trajectory in a representative cycle of the bellows is descending convex arc-descending concave arc-straight line-ascending concave arc-ascending convex arc, and the shrinkage amount, the transition angle of the descending arc trajectory, the length of the straight line segment, and the transition angle of the ascending arc trajectory are used to quantitatively characterize the shrinkage spinning trajectory.

[0115] The ABAQUS bellows shrinkage spinning model was established, a single factor experiment was designed and the model was carried out, the wall thickness values ​​at different positions in the simulation results were extracted, and the quantitative relationship between the shrinkage amount and the transition angle of the arc trajectory of the descending section, the transition angle of the arc trajectory of the ascending section and the wall thickness forming quality index was obtained according to the above formulas (1) to (3). For details, please refer to Figure 4. At the same time, combined with literature, experience, etc., the extreme values ​​of the forming quality indicators are determined to be: t MSE ≤0.01,

[0116] Then, according to the quantitative relationship between the diameter reduction amount, the transition angle of the descending arc trajectory, the transition angle of the ascending arc trajectory and the wall thickness forming quality index, combined with the extreme value of the forming quality index, the feasible window of the diameter reduction amount and the transition angle of the descending arc trajectory and the transition angle of the ascending arc trajectory of each pass is determined, which can be shown in the following Table 1:

[0117] Table 1:

[0118]

[0119] Among them, the limit reduction of each pass is d max =4mm, the trajectory transition angle range is 35°≤β≤45°;

[0120] Then, according to the principle that the diameter reduction amount of each pass does not exceed the feasible window and the number of passes is as small as possible, the calculation formula of the number of passes can be shown in the above formula (4). In the embodiment of the present invention, the number of passes can be calculated according to formula (4), and the diameter reduction amount of each pass is 4mm-4mm-4mm-3mm respectively.

[0121] Afterwards, based on the established finite element model of bellows shrinkage spinning, a single factor experiment was designed and simulated, and the influence of the transition angle on the wall thickness change in the thinning area and the thickening area was obtained;

[0122] Then, in order to meet the goal of reducing the average wall thickness thinning degree in the over-thinning area and the average wall thickness thickening degree in the over-thickening area, based on the influencing law, the transition angle is as small as possible in the over-thinning area, and the transition angle is as large as possible in the over-thickening area. Therefore, 35° is preferentially selected as the transition angle of the descending arc trajectory, and 45° is preferentially selected as the transition angle of the ascending arc trajectory.

[0123] In the embodiment of the present invention, the radius of the selected wheel fillet can be 7mm, and the calculation of the concave arc radius of the descending section and the ascending section of each pass can be obtained by the above formula (5). First, determine the loading trajectory of the descending section and the ascending section of the first pass. The convex arc radius of the descending section and the ascending section is consistent with the convex arc radius of the descending section and the ascending section in the representative cycle of the target component, both of which are 15mm. When the transition angle of the arc trajectory of the descending section is 35°, the concave arc radius of the descending section is determined to be 7mm by the above formula (5); when the transition angle of the arc trajectory of the ascending section is 45°, it is determined that the concave arc radius of the ascending section is less than 7mm, so the concave arc radius of the ascending section and the descending section of the first pass is taken as 7mm.

[0124] Next, the loading trajectories of the second descending section and ascending section are determined. The convex arc radii of the descending section and ascending section are both 15 mm. When the arc trajectory transition angle of the descending section is 35°, the concave arc radius of the descending section is determined to be 29 mm by the above formula (5); when the arc trajectory transition angle of the ascending section is 45°, the concave arc radius of the ascending section is determined to be 12 mm. Both meet the requirement of not less than the radius of the rotary wheel corner. Therefore, the arc radius of the second descending section is determined to be 29 mm, and the arc radius of the ascending section is determined to be 12 mm.

[0125] Then, the loading trajectory of the descending section and the ascending section of the third pass is determined. The convex arc radii of the descending section and the ascending section are both 15 mm. When the transition angle of the arc trajectory of the descending section is 35°, the concave arc radius of the descending section is determined to be 51 mm; when the transition angle of the arc trajectory of the ascending section is 45°, the concave arc radius of the ascending section is determined to be 26 mm. Both meet the requirement of not being less than the corner radius of the rotating wheel; therefore, the arc radius of the descending section of the third pass is determined to be 51 mm, and the arc radius of the ascending section is determined to be 26 mm.

[0126] Finally, the fourth pass is the final pass, which needs to be formed according to the contour of the component. Therefore, the trajectory transition angles of the descending arc and the ascending arc are both 60°, and the radius of the concave arc is 15 mm.

[0127] The specific target bellows shrinking spinning multi-pass trajectory can be as follows Figure 6 shown.

[0128] Finally, the obtained trajectory is input into the above finite element model to obtain the spinning component, as shown in Figure 7 As shown in the figure, by comparing the results of bellows multi-pass shrinking spinning and single-pass shrinking spinning, it can be found that the maximum wall thickness reduction rate of multi-pass shrinking spinning is reduced by about 15%, and the maximum wall thickness increase rate is reduced by about 3%. Figure 8 Then, by comparing the wall thickness forming quality indicators of the bellows multi-pass shrinking spinning and single-pass shrinking spinning, it can be found that compared with the single-pass forming results, the wall thickness uniformity variance, average thinning rate, and average thickening rate of the bellows components formed by multi-pass forming are reduced by 73%, 55%, and 35%, respectively, as shown in the following Table 2:

[0129] Table 2:

[0130]

[0131] Through comparative analysis and measurement, the multi-pass trajectory design method for bellows shrinking spinning is effective in improving the wall thickness forming quality.

[0132] In the embodiment of the present invention, the target characteristic size in the representative cycle of the shrinking spinning process of the target bellows component, as well as the wall thickness forming quality control target and wall thickness forming quality index of the target bellows in the shrinking spinning process are obtained; the shrinking spinning finite element model of the target bellows is designed according to the target characteristic size; the shrinking spinning simulation experiment is carried out on the finite element model, and based on the results of the simulation experiment and the wall thickness forming quality index, the feasible window of the shrinking spinning trajectory of each pass of the target bellows in the representative cycle is determined; according to the wall thickness forming quality control target, the loading trajectory of each pass is determined from the feasible window, and the shrinking spinning trajectory of the target bellows is obtained. In this way, the trajectory design regulations and quantitative design basis are clearly given, which has strong operability and solves the problem of quantitative characterization and design difficulty of the shrinking spinning trajectory; at the same time, the structural requirements and wall thickness forming quality constraints of the target bellows are comprehensively considered, which can be used to design reasonable shrinking spinning trajectories of bellows with different structural parameters, and has strong versatility. At the same time, the uniformity of the overall wall thickness of the bellows is improved, and the degree of wall thinning in the thinning area and the degree of wall thickening in the thickening area are further reduced, effectively improving the forming quality of the bellows' wall thickness by reducing the diameter and spinning.

[0133] Based on the same inventive concept, an embodiment of the present application also provides a device for designing a multi-pass diameter-reducing spinning trajectory for a corrugated tube. Fig. 9 FIG. 1 is a schematic diagram of a structure of a multi-pass shrinking spinning trajectory design device for a corrugated pipe in an embodiment of the present invention, see Fig. 9 As shown, the bellows multi-pass shrinking spinning trajectory design device 900 may include:

[0134] An acquisition module 901 is used to acquire a target characteristic dimension in a representative cycle of a target bellows component during a shrinking spinning process, as well as a wall thickness forming quality control target and a wall thickness forming quality index of the target bellows during the shrinking spinning process;

[0135] A model building module 902 is used to design a finite element model of a target bellows according to a target characteristic size;

[0136] The first determination module 903 is used to perform a spin shrinking simulation experiment on the finite element model, and determine a feasible window of the spin shrinking trajectory of each pass of the target bellows in a representative cycle based on the results of the simulation experiment and the wall thickness forming quality index;

[0137] The second determination module 904 is used to determine the loading trajectory of each pass from the feasible window according to the wall thickness forming quality control target, and obtain the shrinking spinning trajectory of the target corrugated tube.

[0138] The various embodiments in this specification are described in a progressive manner, and the same or similar parts between the various embodiments can be referenced to each other. Each embodiment focuses on the differences from other embodiments.

[0139] The above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit the present application. Although the present application has been described in detail with reference to the aforementioned embodiments, a person of ordinary skill in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some or all of the technical features thereof may be replaced by equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the present application.

Claims

1. A method for designing a multi-pass shrinking spinning trajectory for a bellows, characterized in that: include: Obtaining target characteristic dimensions in a representative cycle of a target bellows component during a diameter reduction spinning process, as well as a wall thickness forming quality control target and a wall thickness forming quality index of the target bellows during the diameter reduction spinning process; Designing a finite element model of the target bellows according to the target characteristic dimensions; Performing a spin shrinking simulation experiment on the finite element model, and determining a feasible window of the spin shrinking trajectory of each pass of the target bellows in the representative cycle based on the results of the simulation experiment and the wall thickness forming quality index; According to the wall thickness forming quality control target, the loading trajectory of each pass is determined from the feasible window to obtain the diameter reduction spinning trajectory of the target corrugated pipe.

2. The method according to claim 1, characterized in that The target characteristic dimensions include at least the total diameter reduction required for the target corrugated tube forming, the total axial length of the representative cycle, the axial length of the descending segment in the representative cycle, the convex arc radius of the descending segment in the representative cycle, the concave arc radius of the descending segment in the representative cycle, the length of the straight line segment in the representative cycle, the axial length of the rising segment in the representative cycle, the concave arc radius of the rising segment in the representative cycle, and the convex arc radius of the rising segment in the representative cycle.

3. The method according to claim 2, characterized in that The wall thickness forming quality control objectives at least include: improving the uniformity of the wall thickness of the target bellows, reducing the average wall thickness thinning degree of the target bellows thinning area, and reducing the average thickening degree of the target bellows thickening area; The wall thickness forming quality index includes at least: wall thickness mean square error value, average thinning rate and average thickening rate; wherein, the wall thickness mean square error value is an index to measure the uniformity of the overall wall thickness distribution of the target corrugated pipe wall, the average thinning rate is an index to measure the degree of wall thickness change in the excessively thinned area of ​​the target corrugated pipe wall, and the average thickening rate is an index to measure the degree of wall thickness change in the excessively thickened area of ​​the target corrugated pipe wall.

4. The method according to claim 3, characterized in that The wall thickness mean square error value is expressed as: The average thinning rate is expressed as: The average thickening rate is expressed as: Among them, t i Indicates the wall thickness of the bellows at different locations. Indicates the average wall thickness of the bellows; S d represents the area enclosed by the wall thickness change rate of the excessive thinning area and the zero value, x d Represents the axial length of the excessive thinning area; S i represents the area enclosed by the wall thickness change rate of the excessive thickening area and the zero value, x i Represents the axial length of the excessive thickening area.

5. The method according to claim 4, characterized in that Before designing the shrink-spinning finite element model of the target bellows according to the target characteristic dimensions, the method further includes: Determine the shrinkage spinning trajectory form of the target corrugated tube within the representative period, and quantitatively characterize the trajectory form; wherein the trajectory form at least includes a descending convex arc, a descending concave arc, a straight line, an ascending concave arc, and an ascending convex arc within the representative period; the trajectory form is quantitatively characterized by the reduction amount, the radius of the descending convex arc, the transition angle of the descending arc trajectory, the length of the straight line segment, the radius of the ascending convex arc, and the transition angle of the ascending arc trajectory.

6. The method according to claim 5, characterized in that The step of performing a spin reduction simulation experiment on the finite element model and determining a feasible window of the spin reduction trajectory of each pass of the target bellows in the representative cycle based on the result of the simulation experiment and the wall thickness forming quality index comprises: Designing a first single factor test according to the finite element model and performing simulation to obtain wall thickness values ​​at different positions in the first simulation result; Based on the wall thickness value, respectively determine the reduction amount, the transition angle of the descending arc trajectory and the transition angle of the ascending arc trajectory, the quantitative relationship between the wall thickness forming quality index and the extreme value of the wall thickness forming quality index allowed in each pass; According to the quantitative relationship and in combination with the extreme value, the feasible window of the diameter reduction amount, the transition angle of the descending arc trajectory and the transition angle of the ascending arc trajectory of each pass is determined.

7. The method according to claim 6, characterized in that The step of determining the loading trajectory of each pass from the feasible window according to the wall thickness forming quality control target to obtain the shrinking spinning trajectory of the target bellows includes: Determine the number of shrinkage spinning passes according to the total shrinkage amount and the determined feasible window of the shrinkage amount in each pass; Based on the finite element model, a second single factor test is designed and simulated, and according to the second simulation results, the influence of the arc trajectory transition angle of the descending section and the arc trajectory transition angle of the ascending section on the wall thickness change of the thinning area and the thickening area is determined; According to the wall thickness forming quality control target and based on the influencing law, the transition angle of the arc trajectory of the descending section and the transition angle of the arc trajectory of the ascending section of each pass are determined from the feasible window; Determine the convex arc radius of the descending section of the target bellows component in the representative cycle as the convex arc radius of the descending section of each pass, and determine the convex arc radius of the ascending section of the target bellows component in the representative cycle as the convex arc radius of the ascending section of each pass; According to the limit value of the diameter reduction amount of each pass, the transition angle of the arc trajectory of the descending section and the transition angle of the arc trajectory of the ascending section, the radius of the concave arc of the descending section and the radius of the concave arc of the ascending section of each pass are determined by a preset radius calculation formula; The length of the straight line segment of each spinning trajectory is determined according to the total axial length of the representative cycle of the target bellows and the axial length of the descending arc of each pass and the axial length of the ascending arc of each pass.

8. The method according to claim 7, characterized in that The preset radius calculation formula is expressed as: Among them, d all Indicates the total reduction, d i represents the reduction amount of the first i passes, β i It represents the transition angle of the descending arc trajectory or the transition angle of the ascending arc trajectory of the i-th pass.

9. The method according to claim 1, characterized in that: After obtaining the diameter reduction spinning trajectory of the target bellows, the method further includes: Input the obtained diameter reduction spinning trajectory of the target bellows into the finite element model to obtain a spinning component simulation result; the spinning component simulation result includes a multi-pass spinning simulation forming result and a single-pass spinning simulation forming result; The effectiveness of the diameter-reducing spinning trajectory of the target bellows is verified by comparing the quality of the multi-pass spinning simulation forming results with the single-pass spinning simulation forming results.

10. A device for designing the trajectory of multi-pass shrinking spinning of a bellows, characterized in that: include: An acquisition module, used to acquire a target characteristic size in a representative cycle of a target bellows component during a shrinking spinning process, and a wall thickness forming quality control target and a wall thickness forming quality index of the target bellows during the shrinking spinning process; A model building module, used for designing a finite element model of the target bellows according to the target characteristic size; A first determination module is used to perform a diameter reduction spinning simulation experiment on the finite element model, and determine a feasible window of the diameter reduction spinning trajectory form of each pass of the target corrugated pipe in the representative cycle based on the results of the simulation experiment and the wall thickness forming quality index; The second determination module is used to determine the loading trajectory of each pass from the feasible window according to the wall thickness forming quality control target, and obtain the shrinking spinning trajectory of the target corrugated tube.

Citation Information

Cited By

  • Machining process method of super-flexible pipe

    CN120023228A