Ultrathin water-based solid electrolyte diaphragm, preparation method and application
By using ultra-thin aqueous solid electrolyte separator in lithium-ion batteries, combined with silicon-doped titanium aluminum lithium phosphate material and appropriate additives, the mechanical and cyclic performance problems of oxide solid electrolyte materials in lithium-ion batteries are solved, and the battery is improved Energy density and safety.
Patent Information
- Application Number
- CN202410955882.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The oxide solid electrolyte materials have problems in lithium-ion batteries with poor mechanical properties, high contact interface impedance, and poor magnification and cycling performance, resulting in insufficient battery safety and energy density.
Ultra-thin water-based solid electrolyte membranes, including base film and coatings, are used in the coatings to use silicon-doped solid electrolyte materials, which combines thickeners by adjusting porosity, particle size and coating thickness. Dispersants and lithium salt additives to improve ionic conductivity and battery cycling performance.
Suppresses the reduction of titanium, improves the transmission speed of lithium ions, enhances the circulation performance and energy density of the battery, and improves the safety and power performance of the battery.
Smart Images

Figure CN118888972A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of battery separators, and more specifically to an ultra-thin aqueous solid electrolyte separator, a preparation method and an application thereof. Background Art
[0002] In recent years, the research on solid-state batteries and solid-state electrolyte materials has been highly valued and widely studied. This is because solid-state batteries and solid-state electrolytes are expected to fundamentally solve the safety problems of lithium-ion batteries, while making it possible to use metallic lithium as a negative electrode, thereby further improving the energy density of the battery. Solid-state electrolytes mainly include organic polymer solid electrolytes, inorganic solid electrolytes and composite solid electrolytes, while inorganic solid electrolytes can be further divided into oxide solid electrolytes and sulfide solid electrolytes. Among them, oxide solid electrolytes are widely studied due to their good thermal stability and mechanical strength, high ionic conductivity and low cost.
[0003] However, oxide solid electrolyte materials currently have problems such as poor mechanical properties, high interface impedance with positive and negative electrodes, poor rate and cycle performance, and uncertain industrial system and preparation process, which prevent them from being applied on a large scale. There may be a transition state in the transition from the traditional polyolefin diaphragm plus liquid electrolyte to the final all-solid electrolyte. During the transition, what kind of technology and materials need to be used so that the diaphragm can not only complete its basic functions of insulating electrons and conducting ions, but also continue to improve the safety of the battery, optimize the interface with the positive and negative electrode materials, thereby improving the battery's cyclability, power, high and low temperature performance and even energy density, which are all worthy of our deep consideration and discussion. At present, the industry has combined the existing diaphragm technology and the solid electrolyte materials of cutting-edge research to propose a solid electrolyte coating diaphragm.
[0004] Among many solid electrolyte materials, lithium aluminum titanium phosphate (LATP) has high ionic conductivity and wide electrochemical window, stable performance and low price, and has been widely used in high-energy batteries. However, after LATP comes into contact with the metal lithium negative electrode, Ti 4+ Reduced to Ti 3+ , which deforms the LATP structure and slows down the lithium ion transmission, thus degrading the battery performance. Secondly, the ionic conductivity of the current oxide solid electrolyte coating diaphragm is relatively low. On the one hand, this is because the lithium ion ionization of the electrolyte itself is limited. On the other hand, it is related to the porosity and tortuosity of the base membrane, and the coating thickness also has a great influence. When the diaphragm pores are ideal parallel column channels, lithium ions can easily shuttle through, and the internal resistance of the battery is the lowest at this time; when the diaphragm pores are tortuous, the lithium ion shuttle path in the diaphragm becomes longer, reducing the rate at which lithium ions travel back and forth between the positive and negative electrode materials. Therefore, the internal resistance of the battery increases, and it is also easy to induce the growth of lithium ion dendrites and puncture the diaphragm, causing safety hazards. Summary of the invention
[0005] The present application provides an ultra-thin aqueous solid electrolyte diaphragm, a preparation method and an application thereof, which can inhibit the reduction of titanium, improve the battery cycle performance, improve the ion conductivity, and thus improve the energy density of the lithium battery.
[0006] The present application provides an ultra-thin aqueous solid electrolyte membrane, comprising a base membrane and a coating disposed on at least one surface of the base membrane, wherein the coating comprises a solid electrolyte; the solid electrolyte comprises Li 1.3+x Al 0.3 Ti 1.7 (PO4)3(SiO4) x ; Among them, 0≤X≤0.7.
[0007] In an alternative embodiment, the solid electrolyte comprises Li 1.4 Al 0.3 Ti 1.7 (PO4)3(SiO4) 0.1 , Li 1.5 Al 0.3 Ti 1.7 (PO4)3(SiO4) 0.2 , Li 1.6 Al 0.3 Ti 1.7 (PO4)3(SiO4) 0.3 , Li 1.7 Al 0.3 Ti 1.7 (PO4)3(SiO4) 0.4 , Li 1.8 Al 0.3 Ti 1.7 (PO4)3(SiO4) 0.5 , Li 1.9 Al 0.3 Ti 1.7 (PO4)3(SiO4) 0.6 、Li2Al 0.3 Ti 1.7 (PO4)3(SiO4) 0.7 One of them.
[0008] In an optional embodiment, the base film satisfies at least one of the conditions (1)-(2):
[0009] (1) The porosity of the base film is 30%-60%;
[0010] (2) The base film is a polypropylene film.
[0011] In an optional embodiment, the solid electrolyte satisfies at least one of the conditions (1)-(2):
[0012] (1) The particle size of the solid electrolyte is 300nm-900nm;
[0013] (2) In the slurry for preparing the coating, the mass percentage of the solid electrolyte is 20%-40%.
[0014] In an optional embodiment, the coating satisfies at least one of the conditions (1)-(2):
[0015] (1) The coating further comprises a thickener, a dispersant, an adhesive and a wetting agent;
[0016] Optionally, the thickener includes at least one of sodium carboxymethyl cellulose, lithium carboxymethyl cellulose, carboxyethyl cellulose, sodium alginate or polyacrylamide;
[0017] Optionally, in the slurry for preparing the coating, the mass percentage of the thickener is 1%-10%;
[0018] Optionally, the dispersant includes at least one of sodium polyacrylate, ammonium polyacrylate copolymer or polyvinyl alcohol;
[0019] Optionally, in the slurry for preparing the coating, the mass percentage of the dispersant is 0.1%-2%;
[0020] Optionally, the adhesive includes at least one of the copolymers formed by one or more monomers selected from the group consisting of lithium polymethacrylate, sodium polymethacrylate, polymethacrylate, styrene acrylic emulsion, polyvinyl alcohol, ethylene vinyl acetate copolymer, polyvinyl acetate, polyurethane, methyl methacrylate, methacrylic acid, ethacrylic acid, ethyl acrylate, ethyl methacrylate, propyl methacrylate or butyl methacrylate;
[0021] Optionally, in the slurry for preparing the coating, the mass percentage of the adhesive is 1%-10%;
[0022] Optionally, the wetting agent includes at least one of sodium dodecylbenzene sulfonate, polyoxyethylene alkylamine or sodium perfluorooctanoate;
[0023] Optionally, in the slurry for preparing the coating, the mass percentage of the wetting agent is 0.1%-2%;
[0024] (2) The total thickness of the coating is 1 μm-9 μm.
[0025] In an optional embodiment, the coating further comprises a lithium salt additive;
[0026] Optionally, the lithium salt additive includes one or more of LiTFSI, LiPF6 and LiFSI;
[0027] Optionally, in the slurry for preparing the coating, the mass percentage of the lithium salt additive is 1%-10%.
[0028] The present application provides a method for preparing an ultra-thin aqueous solid electrolyte membrane, which is used to prepare the solid electrolyte membrane as described above, and the steps include:
[0029] Preparing a coating slurry raw material for a solid electrolyte separator according to a ratio, wherein the coating slurry raw material includes a solid electrolyte, a solvent, a thickener, a dispersant, an adhesive and a wetting agent;
[0030] The solid electrolyte, the solvent, the thickener and the dispersant are stirred and mixed uniformly to obtain a premixed solution;
[0031] Sand-grinding the premixed solution, adding the adhesive and the wetting agent, and stirring thoroughly to obtain a coating slurry;
[0032] The coating slurry is applied on at least one surface of a base film to form a coating layer, and the solid electrolyte separator is formed after baking.
[0033] In an optional embodiment, the mass percentage of the solvent in the coating slurry is 30%-80%.
[0034] In an optional embodiment, the coating slurry raw material further includes a lithium salt additive, the premixed solution is sand-milled, and then the adhesive, the wetting agent and the lithium salt additive are added, and the coating slurry is obtained after fully stirring.
[0035] The present application provides a lithium-ion battery, comprising the solid electrolyte separator as described above; or the solid electrolyte prepared by the preparation method as described above.
[0036] According to the ultra-thin aqueous solid electrolyte membrane in the above embodiment, it includes a base film and a coating disposed on at least one surface of the base film, the coating includes a solid electrolyte, and the solid electrolyte includes Li 1.3+x Al 0.3 Ti 1.7 (PO4)3(SiO4) x Since the solid electrolyte is a silicon-doped lithium aluminum titanium phosphate solid electrolyte material, namely LATSP, when Si is doped with LATP, Si does not completely enter the P site but partially enters the Ti site, thereby improving the Ti 4+ The reduction stability of titanium can be inhibited, the battery cycle performance can be improved, and at the same time, the lithium ion transmission can be accelerated and the ion conductivity can be improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1A schematic diagram of the structure of an ultra-thin aqueous solid electrolyte membrane in an embodiment;
[0038] Figure 2 is a scanning electron microscope image of a coating in an embodiment;
[0039] Figure 3 A flowchart of a method for preparing an ultra-thin aqueous solid electrolyte membrane in an embodiment;
[0040] Figure 4 It is a flow chart of a method for preparing an ultra-thin aqueous solid electrolyte membrane in another embodiment.
[0041] Wherein: 1. base film; 2. coating; 21. first coating; 22. second coating. DETAILED DESCRIPTION
[0042] The present application is further described in detail below by specific embodiments in conjunction with the accompanying drawings. Wherein similar elements in different embodiments adopt associated similar element numbers. In the following embodiments, many detailed descriptions are intended to enable the present application to be better understood. However, those skilled in the art can easily recognize that some of the features can be omitted in different situations, or can be replaced by other elements, materials, and methods. In some cases, some operations related to the present application are not shown or described in the specification, in order to avoid the core part of the present application being overwhelmed by too much description, and for those skilled in the art, it is not necessary to describe these related operations in detail, and they can fully understand the related operations based on the description in the specification and the general technical knowledge in the art.
[0043] In addition, the features, operations or characteristics described in the specification can be combined in any appropriate manner to form various implementations, and the operation steps involved in each embodiment can also be replaced or adjusted in a sequence in a manner that is obvious to those skilled in the art. Therefore, the specification and drawings are only for the purpose of clearly describing a certain embodiment and do not mean that the composition and / or sequence are necessary.
[0044] The serial numbers of the components in this document, such as "first", "second", etc., are only used to distinguish the objects described and do not have any order or technical meaning. The "connection" and "coupling" mentioned in this application, unless otherwise specified, include direct and indirect connections (couplings).
[0045] See also Figure 1 The present application provides an ultra-thin aqueous solid electrolyte membrane (hereinafter referred to as "membrane"), comprising a base membrane 1 and a coating 2 disposed on at least one surface of the base membrane 1, wherein the coating 2 comprises a solid electrolyte; the solid electrolyte comprises Li 1.3+x Al 0.3 Ti1.7 (PO4)3(SiO4) x ; Among them, 0≤X≤0.7.
[0046] Since the solid electrolyte is a silicon (Si) doped lithium aluminum titanium phosphate (LATP) solid electrolyte material, namely LATSP, when Si is doped with LATP, Si does not completely enter the P site but partially enters the Ti site, thereby improving the Ti 4+ The solid electrolyte includes Li 1.4 Al 0.3 Ti 1.7 (PO4)3(SiO4) 0.1 , Li 1.5 Al 0.3 Ti 1.7 (PO4)3(SiO4) 0.2 , Li 1.6 Al 0.3 Ti 1.7 (PO4)3(SiO4) 0.3 , Li 1.7 Al 0.3 Ti 1.7 (PO4)3(SiO4) 0.4 , Li 1.8 Al 0.3 Ti 1.7 (PO4)3(SiO4) 0.5 , Li 1.9 Al 0.3 Ti 1.7 (PO4)3(SiO4) 0.6 、Li2Al 0.3 Ti 1.7 (PO4)3(SiO4) 0.7 The morphology of the prepared membrane is as follows Figure 2 shown.
[0047] The solid electrolyte is a silicon (Si) doped lithium aluminum titanium phosphate (LATP) solid electrolyte material, also known as modified lithium aluminum titanium phosphate. The preparation method is to dissolve the water-soluble precursors LiNO3, NH4H2PO4, (NH2)2CO in deionized water according to the stoichiometric ratio, then add Al2O3, TiO2, SiO2, stir at 70°C for 12 hours and then dry, and preheat the obtained mixture at 120°C for 1 hour to melt the urea in the mixture. Then a two-step annealing heat treatment is performed: first, react at 400°C for 6 hours to remove gaseous byproducts such as NO2, NH3 and H2O; second, calcined at 800°C for 8 hours to complete the synthesis of crystalline LATP. The obtained semi-finished material is crushed and ground at a preset speed for a preset time in a high-energy ball mill at room temperature to obtain a modified lithium aluminum titanium phosphate powder that meets the particle size requirements, that is, a solid electrolyte for preparing coating 2 is obtained. The preset speed ranges from 300rpm to 600rpm, and the preset grinding time ranges from 0.5h to 2h.
[0048] In an optional embodiment, the porosity of the base film 1 is 30%-60%. Further, the porosity of the base film 1 is 45%-55%. The combination of the coating 2 including the solid electrolyte and the base film 1 with high porosity can improve the wettability of the separator with the electrolyte, accelerate the lithium ion transmission rate, thereby improving the ion conductivity, and ultimately improving the energy density of the lithium battery.
[0049] In an optional embodiment, the base film 1 is a polypropylene porous film, which has a mature process and is a mature product used in existing diaphragms, and can effectively control the cost of diaphragm preparation and utilize control and optimization of diaphragm performance. Specifically, the polypropylene porous film can be prepared by a dry stretching process or a wet stretching process.
[0050] In an optional embodiment, the particle size of the solid electrolyte is 300nm-900nm. Optionally, the particle size of the solid electrolyte is one of 300nm, 400nm, 500nm, 600nm, 700nm, 800nm or 900nm, or a range between any of the above values. The particle size of the solid electrolyte is selected in the above range, which can effectively control the thickness of the subsequent coating 2, facilitate thinning the thickness of the coating 2, so as to reduce the effect of the thickness on the ion transmission rate, thereby improving the ionic conductivity of the diaphragm.
[0051] In an optional embodiment, the coating 2 further includes a lithium salt additive, and the lithium salt additive includes one or more of LiTFSI, LiPF6 and LiFSI. The lithium salt in the lithium salt additive can form a stable solution system with the solvent in the electrolyte, improve the conductivity of the electrolyte and the diffusion rate of lithium ions, thereby improving the ionic conductivity, energy density, capacity and other properties of the battery.
[0052] In an optional embodiment, the coating slurry for preparing the coating 2 further includes a solvent, and the solvent includes deionized water. The solvent facilitates the mixing and dispersion of solid substances in the solution.
[0053] In an optional embodiment, the coating 2 further includes a thickener, which includes at least one of sodium carboxymethyl cellulose, lithium carboxymethyl cellulose, carboxyethyl cellulose, sodium alginate or polyacrylamide; the dispersant includes at least one of sodium polyacrylate, ammonium polyacrylate copolymer or polyvinyl alcohol; the wetting agent includes at least one of sodium dodecylbenzene sulfonate, polyoxyethylene alkylamine or sodium perfluorooctanoate. The thickener is used to increase the viscosity and consistency of the slurry, improve the adhesion and coating properties of the slurry, and when used as a thickener for improving ionic conductivity (containing lithium carboxymethyl cellulose), it can not only make the coating 2 uniformly coated, but also replenish lithium and improve ionic conductivity.
[0054] In an optional embodiment, the coating 2 further includes a dispersant, which includes at least one of sodium polyacrylate, ammonium polyacrylate copolymer or polyvinyl alcohol. The dispersant is used to promote uniform dispersion of the slurry so that the diaphragm is evenly coated.
[0055] In an optional embodiment, the coating 2 further includes an adhesive, and the adhesive includes at least one of the copolymers formed by one or more monomers of lithium polymethacrylate, sodium polymethacrylate, polymethacrylate, styrene acrylic emulsion, polyvinyl alcohol, ethylene vinyl acetate copolymer, polyvinyl acetate, polyurethane, methyl methacrylate, methacrylic acid, ethyl acrylate, ethyl methacrylate, propyl methacrylate or butyl methacrylate. The adhesive is used to increase the adhesion between the base film 1 and the slurry. When the adhesive (containing lithium polymethacrylate) is used to improve the ionic conductivity, it can not only achieve the lithium supplementation effect, but also because of the large number of carboxyl functional groups it contains, it can use its complexation-decomplexation with lithium ions to transport lithium ions, thereby improving the ionic conductivity of the separator.
[0056] In an optional embodiment, the coating 2 further includes a wetting agent. The wetting agent includes at least one of sodium dodecylbenzene sulfonate, polyoxyethylene alkylamine or sodium perfluorooctanoate. The wetting agent is used to reduce the surface tension of the slurry, improve the affinity between the base film 1 and the slurry, and make it easier for the slurry to be coated on the base film 1.
[0057] In an optional embodiment, the mass percentage of the solid electrolyte in the slurry for preparing the coating 2 is 20%-40%. Optionally, the mass percentage of the solid electrolyte is one of 20%, 25%, 30%, 35% or 40%, or a range between any of the above values.
[0058] In an optional embodiment, the mass percentage of the solvent in the slurry for preparing the coating 2 is 30%-80%. Optionally, the mass percentage of the solvent is one of 30%, 35%, 40%, 45%, 50%, 60%, 70% or 80%, or a range between any of the above values.
[0059] In an optional embodiment, the mass percentage of the thickener in the slurry for preparing the coating 2 is 1%-10%. Optionally, the mass percentage of the thickener is one of 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9% or 10%, or a range between any of the above values.
[0060] In an optional embodiment, the mass percentage of the dispersant in the slurry for preparing the coating 2 is 0.1%-2%. Optionally, the mass percentage of the dispersant is one of 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.5% or 2%, or a range between any of the above values.
[0061] In an optional embodiment, the mass percentage of the lithium salt additive in the slurry for preparing the coating 2 is 1%-10%. Optionally, the mass percentage of the lithium salt additive is one of 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9% or 10%, or a range between any of the above values.
[0062] In an optional embodiment, the mass percentage of the binder in the slurry for preparing the coating 2 is 1%-10%. Optionally, the mass percentage of the lithium binder is one of 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9% or 10%, or a range between any of the above values.
[0063] In an optional embodiment, the mass percentage of the wetting agent in the slurry for preparing the coating 2 is 0.1%-2%. Optionally, the mass percentage of the wetting agent is 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.2%, 1.5%, 1.7%, 1.8% or 2%, or a range between any of the above values.
[0064] In an optional embodiment, the total thickness of the coating 2 is 1 μm-9 μm. Optionally, the total thickness of the coating 2 is one of 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm or 9 μm, or a range between any of the above values. The coating 2 can be disposed on one side of the base film 1.
[0065] In an optional embodiment, the coating 2 includes a first coating 21 and a second coating 22, the first coating 21 and the second coating 22 are disposed on both sides of the base film 1, and the total thickness of the first coating 21 and the second coating 22 is 1 μm-9 μm. Optionally, the total thickness of the first coating 21 and the second coating 22 is one of 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm or 9 μm, or a range between any of the above values. Preferably, the first coating 21 and the second coating 22 have the same thickness.
[0066] See also Figure 3 The present application also provides a method for preparing an ultra-thin aqueous solid electrolyte membrane, which is used to prepare the solid electrolyte membrane as described above, and the steps include:
[0067] S101: Prepare solid electrolyte, solvent, thickener, dispersant, adhesive and wetting agent according to the proportion, and the solid electrolyte is prepared according to the modified lithium aluminum titanium phosphate preparation method mentioned above. The mass percentage of solid electrolyte in coating 2 is 20%-40%, the mass percentage of solvent is 30%-80%, the mass percentage of thickener is 1%-10%, the mass percentage of dispersant is 0.1%-2%, the mass percentage of adhesive is 1%-10%, and the mass percentage of wetting agent is 0.1%-2%.
[0068] S102: The solid electrolyte, solvent, thickener and dispersant are stirred and mixed thoroughly to obtain a premixed solution.
[0069] S103: sand-grind the premixed solution, add an adhesive and a wetting agent, and stir thoroughly to obtain a coating slurry. The purpose of sand-grinding is to achieve sufficient mixing of the slurry so that the performance of the coating 2 prepared subsequently is uniform.
[0070] S104: coating the coating slurry on at least one surface of the base film 1 to form a coating 2, and then baking to form a solid electrolyte membrane. The uniformly mixed coating slurry is coated on the base film 1 using a gravure roller, and then baking to form a solid electrolyte membrane.
[0071] See also Figure 4 In some embodiments, the coating slurry further comprises a lithium salt additive, and the preparation method thereof comprises:
[0072] S101: Prepare solid electrolyte, lithium salt additive, solvent, thickener, dispersant, adhesive and wetting agent according to the proportion.
[0073] S102: The solid electrolyte, solvent, thickener and dispersant are stirred and mixed thoroughly to obtain a premixed solution.
[0074] S103: sand-grind the premixed solution, add adhesive, wetting agent and lithium salt additive, and stir thoroughly to obtain coating slurry. The purpose of sand-grinding is to achieve thorough mixing of the slurry so that the performance of the subsequently prepared coating 2 is uniform. The mass percentage of lithium salt additive is 1%-10%.
[0075] S104: coating the coating slurry on at least one surface of the base film 1 to form a coating 2, and then baking to form a solid electrolyte membrane.
[0076] The present application also provides a lithium-ion battery, comprising the above-mentioned solid electrolyte membrane; or the solid electrolyte membrane prepared by the above-mentioned preparation method.
[0077] In order to illustrate the effects of the present application, the present application also provides the following several more specific embodiments.
[0078] Embodiment 1
[0079] According to the modified lithium aluminum titanium phosphate preparation method, a solid electrolyte Li with a particle size of 700 nm was prepared at a preset speed of 300 rpm and a grinding time of 2 h. 1.4 Al 0.3 Ti 1.7 (PO4)3(SiO4) 0.1 , according to the mass percentage, 30% solid electrolyte, 7% thickener containing lithium carboxymethyl cellulose, 1% dispersant and 55% deionized water are fully stirred and sanded, and then 4.2% adhesive containing lithium polymethacrylate, 0.8% wetting agent and 2% LiTFSI are added, and the slurry is fully stirred again, and the slurry is coated on both surfaces of the polypropylene base film 1 by a double-sided roller of a gravure coating machine, and baked at 80°C to form a solid electrolyte coating 2 diaphragm, the thickness of the first coating 21 and the second coating 22 are 1μm each, and the total thickness of the coating 2 is 2μm. It is then used to assemble lithium batteries, and the battery structure is NCM│Li metal.
[0080] Embodiment 2
[0081] According to the modified lithium aluminum titanium phosphate preparation method, a solid electrolyte Li with a particle size of 700 nm was prepared at a preset speed of 300 rpm and a grinding time of 2 h. 1.5 Al 0.3 Ti 1.7 (PO4)3(SiO4) 0.2, according to the mass percentage, 30% solid electrolyte, 7% thickener containing lithium carboxymethyl cellulose, 1% dispersant and 55% deionized water are fully stirred and sanded, and then 4.2% adhesive containing lithium polymethacrylate, 0.8% wetting agent and 2% LiTFSI are added, and the slurry is fully stirred again, and the slurry is coated on both surfaces of the polypropylene base film 1 by a double-sided roller of a gravure coating machine, and baked at 80°C to form a solid electrolyte coating 2 diaphragm, the thickness of the first coating 21 and the second coating 22 are 1μm each, and the total thickness of the coating 2 is 2μm. It is then used to assemble lithium batteries, and the battery structure is NCM│Li metal.
[0082] Embodiment 3
[0083] According to the modified lithium aluminum titanium phosphate preparation method, a solid electrolyte Li with a particle size of 700 nm was prepared at a preset speed of 300 rpm and a grinding time of 2 h. 1.6 Al 0.3 Ti 1.7 (PO4)3(SiO4) 0.3 , according to the mass percentage, 30% solid electrolyte, 7% thickener containing lithium carboxymethyl cellulose, 1% dispersant and 55% deionized water are fully stirred and sanded, and then 4.2% adhesive containing lithium polymethacrylate, 0.8% wetting agent and 2% LiTFSI are added, and the slurry is fully stirred again, and the slurry is coated on both surfaces of the polypropylene base film 1 by a double-sided roller of a gravure coating machine, and baked at 80°C to form a solid electrolyte coating 2 diaphragm, the thickness of the first coating 21 and the second coating 22 are 1μm each, and the total thickness of the coating 2 is 2μm. It is then used to assemble lithium batteries, and the battery structure is NCM│Li metal.
[0084] Embodiment 4
[0085] According to the modified lithium aluminum titanium phosphate preparation method, a solid electrolyte Li with a particle size of 700 nm was prepared at a preset speed of 300 rpm and a grinding time of 2 h. 1.7 Al 0.3 Ti 1.7 (PO4)3(SiO4) 0.4 , according to the mass percentage, 30% solid electrolyte, 7% thickener containing lithium carboxymethyl cellulose, 1% dispersant and 55% deionized water are fully stirred and sanded, and then 4.2% adhesive containing lithium polymethacrylate, 0.8% wetting agent and 2% LiTFSI are added, and the slurry is fully stirred again, and the slurry is coated on both surfaces of the polypropylene base film 1 by a double-sided roller of a gravure coating machine, and baked at 80°C to form a solid electrolyte coating 2 diaphragm, the thickness of the first coating 21 and the second coating 22 are 1μm each, and the total thickness of the coating 2 is 2μm. It is then used to assemble lithium batteries, and the battery structure is NCM│Li metal.
[0086] Embodiment 5
[0087] According to the modified lithium aluminum titanium phosphate preparation method, a solid electrolyte Li with a particle size of 700 nm was prepared at a preset speed of 300 rpm and a grinding time of 2 h. 1.8 Al 0.3 Ti 1.7 (PO4)3(SiO4) 0.5 , according to the mass percentage, 30% solid electrolyte, 7% thickener containing lithium carboxymethyl cellulose, 1% dispersant and 55% deionized water are fully stirred and sanded, and then 4.2% adhesive containing lithium polymethacrylate, 0.8% wetting agent and 2% LiTFSI are added, and the slurry is fully stirred again, and the slurry is coated on both surfaces of the polypropylene base film 1 by a double-sided roller of a gravure coating machine, and baked at 80°C to form a solid electrolyte coating 2 diaphragm, the thickness of the first coating 21 and the second coating 22 are 1μm each, and the total thickness of the coating 2 is 2μm. It is then used to assemble lithium batteries, and the battery structure is NCM│Li metal.
[0088] Embodiment 6
[0089] According to the modified lithium aluminum titanium phosphate preparation method, a solid electrolyte Li with a particle size of 700 nm was prepared at a preset speed of 300 rpm and a grinding time of 2 h. 1.9 Al 0.3 Ti 1.7 (PO4)3(SiO4) 0.6 , according to the mass percentage, 30% solid electrolyte, 7% thickener containing lithium carboxymethyl cellulose, 1% dispersant and 55% deionized water are fully stirred and sanded, and then 4.2% adhesive containing lithium polymethacrylate, 0.8% wetting agent and 2% LiTFSI are added, and the slurry is fully stirred again, and the slurry is coated on both surfaces of the polypropylene base film 1 by a double-sided roller of a gravure coating machine, and baked at 80°C to form a solid electrolyte coating 2 diaphragm, the thickness of the first coating 21 and the second coating 22 are 1μm each, and the total thickness of the coating 2 is 2μm. It is then used to assemble lithium batteries, and the battery structure is NCM│Li metal.
[0090] Embodiment 7
[0091] According to the modified lithium aluminum titanium phosphate preparation method, the solid electrolyte Li2Al with a particle size of 700 nm was prepared at a preset speed of 600 rpm and a grinding time of 2 h. 0.3 Ti 1.7 (PO4)3(SiO4) 0.7, according to the mass percentage, 30% solid electrolyte, 7% thickener containing lithium carboxymethyl cellulose, 1% dispersant and 55% deionized water are fully stirred and sanded, and then 4.2% adhesive containing lithium polymethacrylate, 0.8% wetting agent and 2% LiTFSI are added, and the slurry is fully stirred again, and the slurry is coated on both surfaces of the polypropylene base film 1 by a double-sided roller of a gravure coating machine, and baked at 80°C to form a solid electrolyte coating 2 diaphragm, the thickness of the first coating 21 and the second coating 22 are 1μm each, and the total thickness of the coating 2 is 2μm. It is then used to assemble lithium batteries, and the battery structure is NCM│Li metal.
[0092] Embodiment 8
[0093] The difference between this embodiment and the fifth embodiment is that the particle size of the solid electrolyte is 300 nm.
[0094] According to the modified lithium aluminum titanium phosphate preparation method, a solid electrolyte Li with a particle size of 300 nm was prepared at a preset speed of 600 rpm and a grinding time of 2 h. 1.8 Al 0.3 Ti 1.7 (PO4)3(SiO4) 0.5 , according to the mass percentage, 30% solid electrolyte, 7% thickener containing lithium carboxymethyl cellulose, 1% dispersant and 55% deionized water are fully stirred and sanded, and then 4.2% adhesive containing lithium polymethacrylate, 0.8% wetting agent and 2% LiTFSI are added, and the slurry is fully stirred again, and the slurry is coated on both surfaces of the polypropylene base film 1 by a double-sided roller of a gravure coating machine, and baked at 80°C to form a solid electrolyte coating 2 diaphragm, the thickness of the first coating 21 and the second coating 22 are 1μm each, and the total thickness of the coating 2 is 2μm. It is then used to assemble lithium batteries, and the battery structure is NCM│Li metal.
[0095] Embodiment 9
[0096] The difference between this embodiment and the fifth embodiment is that the particle size of the solid electrolyte is 500 nm.
[0097] According to the modified lithium aluminum titanium phosphate preparation method, a solid electrolyte Li with a particle size of 500 nm was prepared at a preset speed of 500 rpm and a grinding time of 2 h. 1.8 Al 0.3 Ti 1.7 (PO4)3(SiO4) 0.5, according to the mass percentage, 30% solid electrolyte, 7% thickener containing lithium carboxymethyl cellulose, 1% dispersant and 55% deionized water are fully stirred and sanded, and then 4.2% adhesive containing lithium polymethacrylate, 0.8% wetting agent and 2% LiTFSI are added, and the slurry is fully stirred again, and the slurry is coated on both surfaces of the polypropylene base film 1 by a double-sided roller of a gravure coating machine, and baked at 80°C to form a solid electrolyte coating 2 diaphragm, the thickness of the first coating 21 and the second coating 22 are 1μm each, and the total thickness of the coating 2 is 2μm. It is then used to assemble lithium batteries, and the battery structure is NCM│Li metal.
[0098] Embodiment 10
[0099] The difference between this embodiment and the fifth embodiment is that the particle size of the solid electrolyte is 900 nm.
[0100] According to the modified lithium aluminum titanium phosphate preparation method, a solid electrolyte Li with a particle size of 900 nm was prepared at a preset speed of 300 rpm and a grinding time of 1 h. 1.8 Al 0.3 Ti 1.7 (PO4)3(SiO4) 0.5 , according to the mass percentage, 30% solid electrolyte, 7% thickener containing lithium carboxymethyl cellulose, 1% dispersant and 55% deionized water are fully stirred and sanded, and then 4.2% adhesive containing lithium polymethacrylate, 0.8% wetting agent and 2% LiTFSI are added, and the slurry is fully stirred again, and the slurry is coated on both surfaces of the polypropylene base film 1 by a double-sided roller of a gravure coating machine, and baked at 80°C to form a solid electrolyte coating 2 diaphragm, the thickness of the first coating 21 and the second coating 22 are 1μm each, and the total thickness of the coating 2 is 2μm. It is then used to assemble lithium batteries, and the battery structure is NCM│Li metal.
[0101] Embodiment 11
[0102] The difference between this embodiment and the fifth embodiment is that the coating 2 is arranged on the side of the base film 1 facing the positive electrode of the battery, and the thickness of the coating 2 is 2 μm.
[0103] According to the modified lithium aluminum titanium phosphate preparation method, a solid electrolyte Li with a particle size of 700 nm was prepared at a preset speed of 300 rpm and a grinding time of 2 h. 1.8 Al 0.3 Ti 1.7 (PO4)3(SiO4) 0.5, according to the mass percentage, 30% solid electrolyte, 7% thickener containing lithium carboxymethyl cellulose, 1% dispersant and 55% deionized water are taken, fully stirred and sanded, and then 4.2% adhesive containing lithium polymethacrylate, 0.8% wetting agent and 2% LiTFSI are added, and the slurry is fully stirred again, and the slurry is coated on one surface of the polypropylene base film 1 by a single-sided roller of a gravure coating machine, and baked at 80°C to form a solid electrolyte coating 2 diaphragm, and the thickness of the coating 2 is 2μm. It is then used to assemble a lithium battery, the battery structure is NCM│Li metal, and the side of the diaphragm coated with the coating 2 containing the solid electrolyte faces the positive electrode side of the battery.
[0104] Embodiment 12
[0105] The difference between this embodiment and the fifth embodiment is that the coating 2 is arranged on the side of the base film 1 facing the negative electrode of the battery, and the thickness of the coating 2 is 2 μm.
[0106] According to the modified lithium aluminum titanium phosphate preparation method, a solid electrolyte Li with a particle size of 700 nm was prepared at a preset speed of 300 rpm and a grinding time of 2 h. 1.8 Al 0.3 Ti 1.7 (PO4)3(SiO4) 0.5 , according to the mass percentage, 30% solid electrolyte, 7% thickener containing lithium carboxymethyl cellulose, 1% dispersant and 55% deionized water are taken, fully stirred and sanded, and then 4.2% adhesive containing lithium polymethacrylate, 0.8% wetting agent and 2% LiTFSI are added, and the slurry is fully stirred again, and the slurry is coated on one surface of the polypropylene base film 1 by a single-sided roller of a gravure coating machine, and baked at 80°C to form a solid electrolyte coating 2 diaphragm, and the thickness of the coating 2 is 2μm. It is then used to assemble a lithium battery, the battery structure is NCM│Li metal, and the side of the diaphragm coated with the coating 2 containing the solid electrolyte faces the negative electrode side of the battery.
[0107] Embodiment 13
[0108] The difference between this embodiment and the fifth embodiment is that the thickness of the first coating 21 and the second coating 22 are both 2 μm, and the total thickness of the coating 2 is 4 μm.
[0109] According to the modified lithium aluminum titanium phosphate preparation method, a solid electrolyte Li with a particle size of 700 nm was prepared at a preset speed of 300 rpm and a grinding time of 2 h. 1.8 Al 0.3 Ti 1.7 (PO4)3(SiO4) 0.5, according to the mass percentage, 30% solid electrolyte, 7% thickener containing lithium carboxymethyl cellulose, 1% dispersant and 55% deionized water are fully stirred and sanded, and then 4.2% adhesive containing lithium polymethacrylate, 0.8% wetting agent and 2% LiTFSI are added, and the slurry is fully stirred again, and the slurry is coated on both surfaces of the polypropylene base film 1 by a double-sided roller of a gravure coating machine, and baked at 80°C to form a solid electrolyte coating 2 diaphragm, the thickness of the first coating 21 and the second coating 22 are both 2μm, and the total thickness of the coating 2 is 4μm. It is then used to assemble lithium batteries, and the battery structure is NCM│Li metal.
[0110] Embodiment 14
[0111] The difference between this embodiment and the fifth embodiment is that the thickness of the first coating 21 and the second coating 22 are both 3 μm, and the total thickness of the coating 2 is 6 μm.
[0112] According to the modified lithium aluminum titanium phosphate preparation method, a solid electrolyte Li with a particle size of 700 nm was prepared at a preset speed of 300 rpm and a grinding time of 2 h. 1.8 Al 0.3 Ti 1.7 (PO4)3(SiO4) 0.5 , according to the mass percentage, 30% solid electrolyte, 7% thickener containing lithium carboxymethyl cellulose, 1% dispersant and 55% deionized water are fully stirred and sanded, and then 4.2% adhesive containing lithium polymethacrylate, 0.8% wetting agent and 2% LiTFSI are added, and the slurry is fully stirred again, and the slurry is coated on both surfaces of the polypropylene base film 1 by a double-sided roller of a gravure coating machine, and baked at 80°C to form a solid electrolyte coating 2 diaphragm, the thickness of the first coating 21 and the second coating 22 are both 3μm, and the total thickness of the coating 2 is 6μm. It is then used to assemble lithium batteries, and the battery structure is NCM│Li metal.
[0113] Embodiment 15
[0114] The difference between this embodiment and the fifth embodiment is that the thickness of the first coating 21 and the second coating 22 are both 4 μm, and the total thickness of the coating 2 is 8 μm.
[0115] According to the modified lithium aluminum titanium phosphate preparation method, a solid electrolyte Li with a particle size of 700 nm was prepared at a preset speed of 300 rpm and a grinding time of 2 h. 1.8 Al 0.3 Ti 1.7 (PO4)3(SiO4) 0.5, according to the mass percentage, 30% solid electrolyte, 7% thickener containing lithium carboxymethyl cellulose, 1% dispersant and 55% deionized water are fully stirred and sanded, and then 4.2% adhesive containing lithium polymethacrylate, 0.8% wetting agent and 2% LiTFSI are added, and the slurry is fully stirred again, and the slurry is coated on both surfaces of the polypropylene base film 1 by a double-sided roller of a gravure coating machine, and baked at 80°C to form a solid electrolyte coating 2 diaphragm, the thickness of the first coating 21 and the second coating 22 are both 4μm, and the total thickness of the coating 2 is 8μm. It is then used to assemble lithium batteries, and the battery structure is NCM│Li metal.
[0116] Embodiment 16
[0117] The difference between this embodiment and the fifth embodiment is that lithium polymethacrylate is replaced by sodium polymethacrylate.
[0118] According to the modified lithium aluminum titanium phosphate preparation method, a solid electrolyte Li with a particle size of 700 nm was prepared at a preset speed of 300 rpm and a grinding time of 2 h. 1.8 Al 0.3 Ti 1.7 (PO4)3(SiO4) 0.5 , according to the mass percentage, 30% solid electrolyte, 7% thickener containing lithium carboxymethyl cellulose, 1% dispersant and 55% deionized water are fully stirred and sanded, and then 4.2% adhesive containing sodium polymethacrylate, 0.8% wetting agent and 2% LiTFSI are added, and the slurry is fully stirred again, and the slurry is coated on both surfaces of the polypropylene base film 1 by a double-sided roller of a gravure coating machine, and baked at 80°C to form a solid electrolyte coating 2 diaphragm, the thickness of the first coating 21 and the second coating 22 are 1μm each, and the total thickness of the coating 2 is 2μm. It is then used to assemble lithium batteries, and the battery structure is NCM│Li metal.
[0119] Embodiment 17
[0120] The difference between this embodiment and the fifth embodiment is that the lithium carboxymethyl cellulose is replaced by sodium carboxymethyl cellulose.
[0121] According to the modified lithium aluminum titanium phosphate preparation method, a solid electrolyte Li with a particle size of 700 nm was prepared at a preset speed of 300 rpm and a grinding time of 2 h. 1.8 Al 0.3 Ti 1.7 (PO4)3(SiO4) 0.5, according to the mass percentage, 30% solid electrolyte, 7% thickener containing sodium carboxymethyl cellulose, 1% dispersant and 55% deionized water are fully stirred and sanded, and then 4.2% adhesive containing lithium polymethacrylate, 0.8% wetting agent and 2% LiTFSI are added, and the slurry is fully stirred again, and the slurry is coated on both surfaces of the polypropylene base film 1 by a double-sided roller of a gravure coating machine, and baked at 80°C to form a solid electrolyte coating 2 diaphragm, the thickness of the first coating 21 and the second coating 22 are 1μm each, and the total thickness of the coating 2 is 2μm. It is then used to assemble lithium batteries, and the battery structure is NCM│Li metal.
[0122] Embodiment 18
[0123] The difference between this embodiment and the fifth embodiment is that the lithium salt additive LiTFSI is not added.
[0124] According to the modified lithium aluminum titanium phosphate preparation method, a solid electrolyte Li with a particle size of 700 nm was prepared at a preset speed of 300 rpm and a grinding time of 2 h. 1.8 Al 0.3 Ti 1.7 (PO4)3(SiO4) 0.5 , according to the mass percentage, 30% solid electrolyte, 7% thickener containing lithium carboxymethyl cellulose, 1% dispersant and 57% deionized water are fully stirred and sanded, and then 4.2% adhesive containing lithium polymethacrylate and 0.8% wetting agent are added, and the slurry is fully stirred again, and the slurry is coated on both surfaces of the polypropylene base film 1 by a double-sided roller of a gravure coating machine, and baked at 80°C to form a solid electrolyte coating 2 diaphragm, the thickness of the first coating 21 and the second coating 22 are 1μm each, and the total thickness of the coating 2 is 2μm. It is then used to assemble lithium batteries, and the battery structure is NCM│Li metal.
[0125] Comparative Example 1
[0126] The difference between this comparative example and Example 1 is that the solid electrolyte does not contain Si.
[0127] According to the preparation method of modified lithium aluminum titanium phosphate, 700 nm Li 1.3 Al 0.3 Ti 1.7 (PO4)3 particles, take 30% Li by mass percentage 1.3 Al 0.3 Ti 1.7(PO4)3 particles, 7% thickener containing lithium carboxymethyl cellulose, 1% dispersant and 55% deionized water are fully stirred and sanded, and then 4.2% adhesive containing lithium polymethacrylate, 0.8% wetting agent and 2% LiTFSI are added, and the slurry is fully stirred again, and the slurry is coated on both surfaces of the polypropylene base film 1 by a double-sided roller of a gravure coating machine, and baked at 80°C to form a coating 2 diaphragm, the thickness of the first coating 21 and the second coating 22 are 1μm each, and the total thickness of the coating 2 is 2μm. It is then used to assemble lithium batteries, and the battery structure is NCM│Li metal.
[0128] Comparative Example 2
[0129] The difference between this comparative example and comparative example 1 is that the particle size of the solid electrolyte is 300 nm.
[0130] According to the preparation method of modified lithium aluminum titanium phosphate, 300 nm Li 1.3 Al 0.3 Ti 1.7 (PO4)3 particles, take 30% Li by mass percentage 1.3 Al 0.3 Ti 1.7 (PO4)3 particles, 7% thickener containing lithium carboxymethyl cellulose, 1% dispersant and 55% deionized water are fully stirred and sanded, and then 4.2% adhesive containing lithium polymethacrylate, 0.8% wetting agent and 2% LiTFSI are added, and the slurry is fully stirred again, and the slurry is coated on both surfaces of the polypropylene base film 1 by a double-sided roller of a gravure coating machine, and baked at 80°C to form a coating 2 diaphragm, the thickness of the first coating 21 and the second coating 22 are 1μm each, and the total thickness of the coating 2 is 2μm. It is then used to assemble lithium batteries, and the battery structure is NCM│Li metal.
[0131] Comparative Example 3
[0132] The difference between this comparative example and comparative example 1 is that the particle size of the solid electrolyte is 500 nm.
[0133] According to the preparation method of modified lithium aluminum titanium phosphate, 500 nm Li 1.3 Al 0.3 Ti 1.7 (PO4)3 particles, take 30% Li by mass percentage 1.3 Al 0.3 Ti 1.7(PO4)3 particles, 7% thickener containing lithium carboxymethyl cellulose, 1% dispersant and 55% deionized water are fully stirred and sanded, and then 4.2% adhesive containing lithium polymethacrylate, 0.8% wetting agent and 2% LiTFSI are added, and the slurry is fully stirred again, and the slurry is coated on both surfaces of the polypropylene base film 1 by a double-sided roller of a gravure coating machine, and baked at 80°C to form a coating 2 diaphragm, the thickness of the first coating 21 and the second coating 22 are 1μm each, and the total thickness of the coating 2 is 2μm. It is then used to assemble lithium batteries, and the battery structure is NCM│Li metal.
[0134] Comparative Example 4
[0135] The difference between this comparative example and comparative example 1 is that the particle size of the solid electrolyte is 900 nm.
[0136] According to the preparation method of modified lithium aluminum titanium phosphate, 900 nm Li 1.3 Al 0.3 Ti 1.7 (PO4)3 particles, take 30% Li by mass percentage 1.3 Al 0.3 Ti 1.7 (PO4)3 particles, 7% thickener containing lithium carboxymethyl cellulose, 1% dispersant and 55% deionized water are fully stirred and sanded, and then 4.2% adhesive containing lithium polymethacrylate, 0.8% wetting agent and 2% LiTFSI are added, and the slurry is fully stirred again, and the slurry is coated on both surfaces of the polypropylene base film 1 by a double-sided roller of a gravure coating machine, and baked at 80°C to form a coating 2 diaphragm, the thickness of the first coating 21 and the second coating 22 are 1μm each, and the total thickness of the coating 2 is 2μm. It is then used to assemble lithium batteries, and the battery structure is NCM│Li metal.
[0137] Comparative Example 5
[0138] The difference between this comparative example and comparative example 1 is that the coating 2 is arranged on the side of the base film 1 facing the positive electrode of the battery, and the thickness of the coating 2 is 2 μm.
[0139] According to the preparation method of modified lithium aluminum titanium phosphate, 700 nm Li 1.3 Al 0.3 Ti 1.7 (PO4)3 particles, take 30% Li by mass percentage 1.3 Al 0.3 Ti 1.7(PO4)3 particles, 7% thickener containing lithium carboxymethyl cellulose, 1% dispersant and 55% deionized water are fully stirred and sanded, and then 4.2% adhesive containing lithium polymethacrylate, 0.8% wetting agent and 2% LiTFSI are added, and the slurry is fully stirred again, and the slurry is coated on one surface of the polypropylene base film 1 by a double-sided roller of a gravure coating machine, and baked at 80°C to form a coating 2 diaphragm, and the thickness of the coating 2 is 2μm. It is then used to assemble lithium batteries, the battery structure is NCM│Li metal, and the coating 2 on the diaphragm faces the positive electrode side of the battery.
[0140] Comparative Example 6
[0141] The difference between this comparative example and comparative example 1 is that the coating 2 is arranged on the side of the base film 1 facing the negative electrode of the battery, and the thickness of the coating 2 is 2 μm.
[0142] According to the preparation method of modified lithium aluminum titanium phosphate, 700 nm Li 1.3 Al 0.3 Ti 1.7 (PO4)3 particles, take 30% Li by mass percentage 1.3 Al 0.3 Ti 1.7 (PO4)3 particles, 7% thickener containing lithium carboxymethyl cellulose, 1% dispersant and 55% deionized water are fully stirred and sanded, and then 4.2% adhesive containing lithium polymethacrylate, 0.8% wetting agent and 2% LiTFSI are added, and the slurry is fully stirred again, and the slurry is coated on one surface of the polypropylene base film 1 by a double-sided roller of a gravure coating machine, and baked at 80°C to form a coating 2 diaphragm, and the thickness of the coating 2 is 2μm. It is then used to assemble a lithium battery, the battery structure is NCM│Li metal, and the coating 2 on the diaphragm faces the negative electrode side of the battery.
[0143] Comparative Example 7
[0144] The difference between this comparative example and comparative example 1 is that the solid electrolyte is Li7La3Zr2O 12 .
[0145] According to the mass percentage, 30% solid electrolyte, 7% thickener containing lithium carboxymethyl cellulose, 1% dispersant and 55% deionized water were fully stirred and sanded, and then 4.2% adhesive containing lithium polymethacrylate, 0.8% wetting agent and 2% LiTFSI were added, and the slurry was fully stirred again, and the slurry was coated on both surfaces of the polypropylene base film 1 by a double-sided roller of a gravure coating machine, and baked at 80°C to form a solid electrolyte coating 2 diaphragm, the thickness of the first coating 21 and the second coating 22 were 1μm each, and the total thickness of the coating 2 was 2μm. It was then used to assemble lithium batteries, and the battery structure was NCM│Li metal.
[0146] Comparative Example 8
[0147] The difference between this comparative example and comparative example 1 is that the solid electrolyte is Li 1.3 Al x Ge 1.7 (PO4)3.
[0148] According to the mass percentage, 30% solid electrolyte, 7% thickener containing lithium carboxymethyl cellulose, 1% dispersant and 55% deionized water were fully stirred and sanded, and then 4.2% adhesive containing lithium polymethacrylate, 0.8% wetting agent and 2% LiTFSI were added, and the slurry was fully stirred again, and the slurry was coated on both surfaces of the polypropylene base film 1 by a double-sided roller of a gravure coating machine, and baked at 80°C to form a solid electrolyte coating 2 diaphragm, the thickness of the first coating 21 and the second coating 22 were 1μm each, and the total thickness of the coating 2 was 2μm. It was then used to assemble lithium batteries, and the battery structure was NCM│Li metal.
[0149] Comparative Example 9
[0150] The difference between this comparative example and comparative example 1 is that aluminum oxide is used to replace the solid electrolyte as the coating 2 coated on both surfaces of the polypropylene base film 1, and the thickness of the two coatings 2 is 1 μm, and the total thickness of the coating 2 is 2 μm. It is then used to assemble a lithium battery, and the battery structure is NCM│Li metal.
[0151] The different solid electrolytes in Examples 1 to 18 were prepared according to the raw material ratios in Table 1 below.
[0152] Table 1
[0153]
[0154] The physical and chemical properties of the separators in Examples 1 to 18 and Comparative Examples 1 to 9 and the electrochemical properties of the assembled batteries were tested. The specific test methods are as follows:
[0155] The coating thickness of the diaphragm is measured by using a Mahr thickness gauge, and the unit is μm. The test is based on GB / T6672-2001 "Mechanical measurement method for thickness of plastic films and sheets".
[0156] The permeability of the membrane is measured using an EG01-55-1MR permeability meter and is expressed as the time taken for 100 mL of gas to pass through a membrane of a fixed area.
[0157] The thermal shrinkage of the diaphragm is tested by baking in an oven. The specific test method is: cut the sample into 100mm×100mm strips, measure the length A1 of the strips, set the oven temperature to 150℃, keep the temperature for 1h after reaching the temperature, use a stopwatch or directly use the timer of the oven, take out the strips after 1h, cool for 10min, and measure the length A2 of the strips. The longitudinal thermal shrinkage = (A1-A2) / A1×100%. In this example, the average value of 5 parallel test samples is taken as the thermal shrinkage value of the sample (referred to as "thermal shrinkage value").
[0158] The test method for the ionic conductivity of the diaphragm is: symmetrical batteries are assembled using inert stainless steel electrodes, diaphragm samples, aluminum-plastic membrane shells and standard electrolyte (1.0 mol / L LiPF6 / EC+EMC+DMC (volume ratio 1:1:1)); under 23-cell assembly, the electrochemical workstation is used to test the EIS. As the number of diaphragm layers increases, the resistance of the symmetrical battery also increases accordingly, and there is a linear relationship - the slope of the symmetrical battery resistance to the number of diaphragm layers is the diaphragm resistance R S .
[0159] The calculation formula of membrane ion conductivity is: S =d / (R S *A);
[0160] Among them, σ S is the ion conductivity of the diaphragm, unit: mS / cm; d is the thickness of the diaphragm, unit: μm; A is the effective area of the diaphragm in the symmetrical battery, unit: cm 2 .
[0161] The test method for battery energy density is: assemble the battery in a glove box with a closed argon atmosphere. The oxygen and water content in the glove box are generally controlled below 0.01ppm during operation. During the assembly process, place the NCM positive electrode sheet in the center of the positive electrode shell and then put in the diaphragm. Add 2-3 drops of electrolyte to make it completely wet. Put in the lithium electrode sheet and buckle the negative electrode shell. Press it with a tablet press and the assembly is completed. The discharge capacity can be obtained by constant current charge and discharge test of the battery.
[0162] Battery energy density (Wh / kg) = battery capacity (mAh) × discharge platform voltage (V) / battery mass (kg); battery capacity is the discharge capacity; discharge platform voltage: as the discharge progresses, the battery voltage changes very little, and this section accounts for the vast majority of the entire discharge time, which is the discharge platform voltage; battery mass is the overall mass of the assembled battery.
[0163] The test method for the number of cycles at room temperature is as follows: first, at 23±2℃, discharge at a constant current of 1C until the termination voltage reaches 2.7V, then switch to constant current charging until the charging voltage rises to 4.4V, and stop charging; then the battery is discharged at a constant current of 1C until the discharge termination voltage is reached, stop discharging, and record the discharge capacity; thus completing one cycle; the battery repeats charge and discharge until the discharge capacity is lower than 80% of the discharge capacity in the first week, and record the total number of cycles of the battery at this time.
[0164] The specific test results are shown in Table 2 below.
[0165]
[0166]
[0167]
[0168] As can be seen from the above table, the diaphragm contains solid electrolyte Li 1.3+x Al 0.3 Ti 1.7 (PO4)3(SiO4) x The coating 2 can inhibit the reduction of titanium and improve the battery cycle performance. At the same time, the high-porosity base membrane 1 can also improve the wettability of the composite diaphragm and the electrolyte, accelerate the transmission of lithium ions, improve the ion conductivity, and thus improve the energy density of the lithium battery.
[0169] In Examples 1 to 7, the solid electrolyte Li 1.3+x Al 0.3 Ti 1.7 (PO4)3(SiO4) x The lithium content in the membrane is different. From the test results in the table, it can be seen that with the increase of lithium content, the ionic conductivity of the membrane increases, and at the same time, the energy density of the battery prepared therefrom increases, and the number of room temperature cycles increases.
[0170] The particle size of the solid electrolyte in Example 5 is different from that in Example 8, Example 9 and Example 10. It can be seen from the data in the table that as the particle size of the solid electrolyte increases, the ionic conductivity of the diaphragm decreases. As the particle size increases, the battery energy density and the number of room temperature cycles are improved. When the solid electrolyte particle size reaches 700nm, the battery energy density and the number of room temperature cycles are the largest and the performance is the best. When the electrolyte particle size continues to increase to 900nm, the value decreases compared to 700nm. The solid electrolyte particle size affects the performance of the diaphragm, and a better particle range should be selected when preparing the diaphragm.
[0171] The coating position and quantity of the coating 2 in Example 5 are different from those in Examples 11 and 12. Example 5 is double-sided coating, Example 11 is coating the coating 2 on the side facing the positive electrode, and Example 12 is coating the coating 2 on the side facing the negative electrode. It can be seen from the test results in the table that when the coating 2 is coated on both sides in Example 5, the ionic conductivity value increases, and the battery energy density and room temperature cycle performance are also better than those in Examples 11 and 12, indicating that the battery performance is better when the coating 2 is coated on both sides.
[0172] The total thickness of the coating 2 in Example 5 is different from that in Example 13 to Example 15. It can be seen from the test results in the table that with the increase of the thickness of the coating 2, the air permeability value of the diaphragm increases, the air permeability decreases, the heat shrinkage decreases, the ionic conductivity decreases, and the energy density and room temperature cycle number of the battery both decrease, indicating that the thickness of the coating 2 affects the performance of the diaphragm and the battery, and with the increase of the thickness, the various properties of the diaphragm are all reduced. When the total thickness of the coating 2 is in the range of 2μm-9μm, the performance of the diaphragm and the battery is better.
[0173] The adhesives in Example 5 and Example 16 are different. It can be seen from the test results in the table that when an adhesive containing lithium polymethacrylate is selected, it can not only achieve the lithium supplement effect, but also because it contains a large number of carboxyl functional groups, it can complex and decomplex with lithium ions to transport lithium ions, thereby helping to improve the ionic conductivity of the diaphragm.
[0174] The thickeners in Example 5 and Example 17 are different. From the test results in the table, it can be seen that when a thickener containing lithium carboxymethyl cellulose is selected, the lithium supplementation effect can be achieved, which is beneficial to improving the ionic conductivity of the separator.
[0175] Compared with Example 5 and Example 18, Example 18 does not use lithium salt additives. It can be seen from the test results in the table that the addition of lithium salt additives is beneficial to improving the ion conductivity, energy density and room temperature cycle performance of the battery.
[0176] The solid electrolytes in Comparative Examples 1 to 6 do not contain SiO2, that is, lithium aluminum titanium phosphate (LATP) is directly used as the raw material of the solid electrolyte. From the test results in the table, it can be seen that the doping of silicon (Si) is beneficial to improving the battery ion conductivity, energy density and room temperature cycle performance.
[0177] Compared with Comparative Examples 7 and 8, Example 1 also obtains aqueous solid electrolyte membranes prepared in Comparative Examples 7 and 8. From the test results in the table, it can be seen that the battery ion conductivity, energy density and room temperature cycle performance in Comparative Examples 7 and 8 are also good, but they have the problems of high cost, complex synthesis process, and instability in aqueous slurry system.
[0178] Compared with Example 9, the test results in the table show that the solid electrolyte Li 1.3+ x Al 0.3 Ti 1.7 (PO4)3(SiO4) x The ultra-thin aqueous solid electrolyte membrane prepared by coating 2 is beneficial to improving the ionic conductivity, energy density and room temperature cycle performance of the battery.
[0179] The above specific examples are used to illustrate the present application, which is only used to help understand the present application and is not intended to limit the present application. For technicians in the technical field to which the present application belongs, they can also make some simple deductions, deformations or substitutions based on the ideas of the present application.
Claims
1. An ultra-thin aqueous solid electrolyte membrane, characterized in that: The invention comprises a base film and a coating disposed on at least one surface of the base film, wherein the coating comprises a solid electrolyte; the solid electrolyte comprises Li 1.3+x Al 0.3 Ti 1.7 (PO4)3(SiO4) x ; Among them, 0≤X≤0.
7.
2. The ultra-thin aqueous solid electrolyte membrane according to claim 1, characterized in that: The solid electrolyte includes Li 1.4 Al 0.3 Ti 1.7 (PO4)3(SiO4) 0.1 , Li 1.5 Al 0.3 Ti 1.7 (PO4)3(SiO4) 0.2 , Li 1.6 Al 0.3 Ti 1.7 (PO4)3(SiO4) 0.3 , Li 1.7 Al 0.3 Ti 1.7 (PO4)3(SiO4) 0.4 , Li 1.8 Al 0.3 Ti 1.7 (PO4)3(SiO4) 0.5 , Li 1.9 Al 0.3 Ti 1.7 (PO4)3(SiO4) 0.6 、Li2Al 0.3 Ti 1.7 (PO4)3(SiO4) 0.7 One of them.
3. The ultra-thin aqueous solid electrolyte membrane according to claim 1, characterized in that: The base film satisfies at least one of the conditions (1)-(2): (1) The porosity of the base film is 30%-60%; (2) The base film is a polypropylene porous film.
4. The ultra-thin aqueous solid electrolyte membrane according to claim 1, characterized in that: The solid electrolyte satisfies at least one of the conditions (1)-(2): (1) The particle size of the solid electrolyte is 300nm-900nm; (2) In the slurry for preparing the coating, the mass percentage of the solid electrolyte is 20%-40%.
5. The ultra-thin aqueous solid electrolyte membrane according to claim 1, characterized in that: The coating satisfies at least one of the conditions (1)-(2): (1) The coating further comprises a thickener, a dispersant, an adhesive and a wetting agent; Optionally, the thickener includes at least one of sodium carboxymethyl cellulose, lithium carboxymethyl cellulose, carboxyethyl cellulose, sodium alginate or polyacrylamide; Optionally, in the slurry for preparing the coating, the mass percentage of the thickener is 1%-10%; Optionally, the dispersant includes at least one of sodium polyacrylate, ammonium polyacrylate copolymer or polyvinyl alcohol; Optionally, in the slurry for preparing the coating, the mass percentage of the dispersant is 0.1%-2%; Optionally, the adhesive includes at least one of the copolymers formed by one or more monomers selected from the group consisting of lithium polymethacrylate, sodium polymethacrylate, polymethacrylate, styrene acrylic emulsion, polyvinyl alcohol, ethylene vinyl acetate copolymer, polyvinyl acetate, polyurethane, methyl methacrylate, methacrylic acid, ethacrylic acid, ethyl acrylate, ethyl methacrylate, propyl methacrylate or butyl methacrylate; Optionally, in the slurry for preparing the coating, the mass percentage of the adhesive is 1%-10%; Optionally, the wetting agent includes at least one of sodium dodecylbenzene sulfonate, polyoxyethylene alkylamine or sodium perfluorooctanoate; Optionally, in the slurry for preparing the coating, the mass percentage of the wetting agent is 0.1%-2%; (2) The total thickness of the coating is 1 μm-9 μm.
6. The ultra-thin aqueous solid electrolyte membrane according to claim 5, characterized in that: The coating also includes a lithium salt additive; Optionally, the lithium salt additive includes one or more of LiTFSI, LiPF6 and LiFSI; Optionally, in the slurry for preparing the coating, the mass percentage of the lithium salt additive is 1%-10%.
7. A method for preparing an ultra-thin aqueous solid electrolyte membrane, characterized in that: For preparing a solid electrolyte membrane as claimed in any one of claims 1 to 6, the steps include: Preparing a coating slurry raw material for a solid electrolyte separator according to a ratio, wherein the coating slurry raw material includes a solid electrolyte, a solvent, a thickener, a dispersant, an adhesive and a wetting agent; The solid electrolyte, the solvent, the thickener and the dispersant are stirred and mixed uniformly to obtain a premixed solution; Sand-grinding the premixed solution, adding the adhesive and the wetting agent, and stirring well to obtain a coating slurry; The coating slurry is applied on at least one surface of a base film to form a coating layer, and the solid electrolyte separator is formed after baking.
8. The method for preparing the ultra-thin aqueous solid electrolyte membrane according to claim 7, characterized in that: The mass percentage of the solvent in the coating slurry is 30%-80%.
9. The method for preparing an ultra-thin aqueous solid electrolyte membrane according to claim 7, characterized in that:The coating slurry raw material also includes a lithium salt additive. The premixed solution is sand-milled, and then the adhesive, the wetting agent and the lithium salt additive are added, and the coating slurry is obtained after fully stirring.
10. A lithium ion battery, characterized in that: It comprises the solid electrolyte membrane as described in any one of claims 1 to 6; or the solid electrolyte membrane prepared by the preparation method as described in any one of claims 7 to 9.
Citation Information
Patent Citations
Inorganic composite material with core-shell structure as well as preparation and application thereof
CN111129582A
A coating slurry and preparation method thereof as well as composite diaphragm and lithium ion battery
CN114188668B
Cited By
Oxide solid electrolyte, preparation method thereof and all-solid-state battery
CN119812449A
Preparation method of solid anode strip with high stability and low interface impedance
CN121076080A
A method for preparing a solid-state anode sheet with high stability and low interfacial impedance
CN121076080B
Oxide solid-state electrolyte and preparation method therefor, all-solid-state battery and electric device
WO2026143897A1