Unidirectional composite material, spar cap and windmill blade

By controlling the fluctuation amplitude and spiral pitch of the carbon fiber fiber axis in a unidirectional composite material, and using the alternating arrangement of right-hand and left-hand spirals, the problem of fiber axis cracks in the windmill blades is solved. , achieving both high elastic modulus and high compression strength.

CN118891147APending Publication Date: 2024-11-01TORAY INDUSTRIES INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380028420.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-12-05
Filing Date
2023-02-07
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

During the process of large-scale windmill blades, existing carbon fiber drawing molded products are prone to fiber shaft cracks due to bolt hole openings or mold curvature. The high elastic modulus carbon fiber has low compression strength, making it difficult to take into account both high elastic modulus and high compression strength. .

Method used

By controlling the fiber axis fluctuation amplitude, spiral pitch and twisted state of carbon fibers in a one-way composite material, the resistance and elastic modulus of the fiber axis are ensured. The alternating arrangement of carbon fibers with right-hand and left-hand spirals is used to increase the number of interweaving between fibers. , enhance crack resistance.

Benefits of technology

It effectively improves the crack resistance and elastic modulus of the carbon fiber fiber shaft, avoids damage to fiber shaft cracks after the windmill blades are large, and meets the needs of high elastic modulus and high compression strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118891147A_ABST
    Figure CN118891147A_ABST
Patent Text Reader

Abstract

Provided is a draw-molded article having high resistance to cracks along the fiber axis of carbon fibers and having a high elastic modulus. The present invention is a unidirectional composite material containing carbon fibers and a matrix resin, wherein the fluctuation range of the fiber axis is 1.5 [mu] m or more when a single fiber of the carbon fibers is observed from the side surface within a linear distance of 1 mm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a unidirectional composite material which has high resistance to cracks along the fiber axis of the carbon fibers and a high elastic modulus and comprises carbon fibers arranged in a unidirectional manner. Background Art

[0002] In recent years, the scope of application of carbon fiber with low specific gravity and excellent mechanical properties has become increasingly wider, and with it, the requirements have become increasingly diversified and advanced. The form used to utilize carbon fiber varies depending on the application, and it is used in various forms from continuous fiber to discontinuous fiber. Unidirectional composite fibers, especially drawn molded products, are one of the representative forms of utilization. The carbon fibers are arranged in a unidirectional manner and impregnated and cured with resin, so they exhibit excellent mechanical properties in the orientation direction of the carbon fibers. For drawn molded products, it is preferred that the reinforcing fibers are highly uniaxially oriented. It is important to improve the homogeneity of the impregnated resin by improving the straightness of the reinforcing fibers. For example, Patent Document 1 proposes a method for improving the straightness of the reinforcing fibers by repeatedly opening and closing the fibers while applying tension for drawing molding.

[0003] In wind power generation, the enlargement of windmill blades is being promoted in order to improve power generation efficiency and increase power generation. Carbon fiber drawing molded products have a high elastic modulus and can obtain materials with the same shape in the length direction, so they are being used as spar caps for large-scale windmill blades. On the other hand, when the windmill blades are enlarged, the difficulty in transportation can be cited as a problem. In response to this problem, a windmill blade that can be divided, transported and assembled is proposed. For example, Patent Document 2 proposes a structure in which the inner and outer parts of the windmill blade can be bolted at a connection area set in the thick wall part.

[0004] In addition, when the wind turbine blade is enlarged, a wide drawn product is required for the spar cap portion, but the wider the width, the more difficult it is to conform to the curvature of the blade mold. In response to this problem, a technology has been proposed to design the shape of the drawn product so that it is easy to deform only in a certain direction. For example, Patent Document 3 proposes a method of using a drawn product with grooves in the span direction to give the drawn product lateral flexibility and make it possible to match the curvature of the wind turbine blade mold.

[0005] In the case of wind turbine blades being enlarged, the higher the elastic modulus of the drawn molded product used, the more preferred it is. However, the higher the elastic modulus of the carbon fiber, the lower the compressive strength, and the higher the risk of damage due to compression failure. In response to this issue, a method of using carbon fibers having both high elastic modulus and high compressive strength for drawn molded products is considered. For example, Patent Document 4 proposes a method of controlling the crystallization state of carbon fibers by twisting or the like in a carbonization process, thereby obtaining carbon fibers having both high elastic modulus and high compressive strength.

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent Application Publication No. 2018-001682

[0009] Patent Document 2: International Publication No. 2013 / 083451

[0010] Patent Document 3: U.S. Patent Application Publication No. 2019 / 0270261

[0011] Patent Document 4: International Publication No. 2019 / 203088 Summary of the invention

[0012] Problems to be solved by the invention

[0013] However, the conventional technology has the following problems.

[0014] Patent document 2 proposes a structure in which the inner and outer parts of a windmill blade can be fixed by bolts in a connection area provided in a thick wall portion, but when the same bolt hole is opened on a spar cap of a drawn product using carbon fiber, cracks are sometimes generated along the fiber axis of the carbon fiber. In addition, Patent document 3 proposes a method of matching the curvature of a windmill blade mold by giving the drawn product lateral flexibility by using a drawn product having grooves in the span direction, but when the curvature of the windmill blade mold is large, cracks are sometimes generated along the fiber axis of the carbon fiber. The inventors of the present application have found through research that the cause of these problems is that in conventional drawn products, since the carbon fibers are arranged in a highly uniaxial orientation, the resistance to cracks along the fiber axis of the carbon fibers is low.

[0015] Patent document 4 proposes a method for controlling the crystallization state of carbon fibers by twisting or the like in a carbonization process, thereby obtaining carbon fibers having both a high elastic modulus and a high compressive strength. However, the carbon fibers twisted in the carbonization process obviously have residual undulations in the fibers due to the influence of twisting, which sometimes results in a decrease in the straightness of the reinforcing fibers.

[0016] Therefore, an object of the present invention is to provide a unidirectional composite material that is easy to avoid damage in post-processing required to cope with the increase in the size of wind turbine blades, has high resistance to cracks along the fiber axis of carbon fibers, and has a high elastic modulus.

[0017] Means for solving problems

[0018] In order to achieve the above-mentioned object, the present invention is as follows.

[0019] [1] A unidirectional composite material comprising carbon fibers and a matrix resin, wherein a fluctuation amplitude of a fiber axis of a single fiber of the carbon fibers when observed from the side within a linear distance of 1 mm is 1.5 μm or more.

[0020] [2] The unidirectional composite material according to [1], wherein the average value of the helical pitch of the fiber axis of the carbon fibers is 5.50 cm or less.

[0021] [3] The unidirectional composite material according to [1] or [2], wherein when the average value of the distance between single fibers of the carbon fibers contained in the unidirectional composite material is set to R (μm) and the fluctuation amplitude of the fiber axis of the carbon fibers is set to D (μm), formula (1) is satisfied:

[0022] 2.0≤D÷R≤35.0···Formula (1).

[0023] [4] The unidirectional composite material according to any one of [1] to [3], wherein the volume content of the carbon fibers is 60% by volume or more.

[0024] [5] The unidirectional composite material according to any one of [1] to [4], wherein the carbon fiber bundle is contained in the matrix resin in a twisted state with a twist number of 10 turns / m or less.

[0025] [6] A unidirectional composite material according to any one of [1] to [5], wherein, in a cross section perpendicular to the fiber direction of the unidirectional composite material, when the cross-sectional area of ​​the carbon fiber bundle contained in the unidirectional composite material is set to X (mm 2 ), a resin-rich portion having an area of ​​3% or more of X does not substantially exist.

[0026] [7] The unidirectional composite material according to any one of [1] to [6], wherein the carbon fibers include both carbon fibers having a right-handed helix on the fiber axis of the single fiber and carbon fibers having a left-handed helix on the fiber axis of the single fiber.

[0027] [8] The unidirectional composite material according to [7], wherein when the number of carbon fiber bundles formed by carbon fibers having a right-handed helix in the fiber axis of a single fiber is set to N A (roots), the number of carbon fiber bundles formed by carbon fibers having a left-handed helix in the fiber axis of a single fiber is N B (root) time, than N A / (N A +N B ) is 0.4~0.6.

[0028] [9] A unidirectional composite material according to [7] or [8], wherein carbon fiber bundles formed by carbon fibers having a right-handed helix on the fiber axis of a single fiber and carbon fiber bundles formed by carbon fibers having a left-handed helix on the fiber axis of a single fiber are alternately arranged in the width direction of the unidirectional composite material.

[0029]

[10] The unidirectional composite material according to any one of [1] to [9], which has a tensile elastic modulus of 150 GPa or more.

[0030]

[11] The unidirectional composite material according to any one of [1] to

[10] , which is a draw-molded product.

[0031]

[12] The unidirectional composite material according to any one of [1] to

[11] , wherein the average value of the single fiber diameter of the carbon fibers is 6.0 μm or less, and the unidirectional composite material is a unidirectional prepreg molded product.

[0032]

[13] A spar cap comprising the unidirectional composite material according to any one of [1] to

[12] .

[0033]

[14] A windmill blade comprising the spar cap described in

[13] .

[0034] Effects of the Invention

[0035] The unidirectional composite material of the present invention is prepared by untwisting a twisted yarn with a large twist and using it to manufacture the unidirectional composite material, and effectively controlling the fluctuation amplitude of the fiber axis of the single fiber of the carbon fiber, thereby becoming a unidirectional composite material with high resistance to cracks along the fiber axis of the carbon fiber and a high elastic modulus. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] [ Figure 1 ] Figure 1 It is a schematic diagram showing the evaluation method of the fluctuation amplitude of the fiber axis.

[0037] [ Figure 2 ] Figure 2 This is a schematic diagram showing a method for evaluating the helical pitch of a single fiber.

[0038] [ Figure 3 ] Figure 3 This is a schematic diagram showing a method for obtaining the average value of the distance between single fibers of carbon fibers included in a unidirectional composite material.

[0039] [ Figure 4 ] Figure 4 This is a schematic diagram showing a method for calculating the area of ​​the resin-rich portion when there is no carbon fiber inside.

[0040] [ Figure 5 ] Figure 5This is a schematic diagram showing a method for calculating the area of ​​the resin-rich portion when carbon fibers are contained inside.

[0041] [ Figure 6 ] Figure 6 It is a schematic diagram showing a method for evaluating the crack resistance along the fiber axis of carbon fiber.

[0042] [ Figure 7 ] Figure 7 A schematic diagram showing the spiral direction of carbon fibers during drawing. DETAILED DESCRIPTION

[0043] In the present invention, the term "carbon fiber" is used in a broad sense including carbon fiber bundles and single fibers of carbon fiber. In addition, a carbon fiber bundle refers to a bundle of multiple single fibers of carbon fiber (for clarity, single fibers of carbon fiber are sometimes simply referred to as "single fibers") gathered together.

[0044] The unidirectional composite material of the present invention is a unidirectional composite material comprising carbon fibers and a matrix resin, wherein the fluctuation amplitude of the fiber axis when a single fiber of the carbon fibers is observed from the side within a linear distance of 1 mm is 1.5 μm or more. Whether the fluctuation amplitude is 1.5 μm or more can be easily confirmed by first taking out a single fiber from the sampled carbon fiber bundle and observing it by the method described below when the unidirectional composite material is manufactured using a carbon fiber bundle.

[0045] The measurement of the fluctuation amplitude of the present invention is evaluated by observing the single fiber of the carbon fiber from a direction orthogonal to the fiber axis in an environment where no stress other than gravity is applied. It should be noted that in the fiber having fluctuations in three dimensions, the fiber axis and the orthogonal direction are defined as follows. In the projection image of the single fiber of the carbon fiber placed on a horizontal plane, the straight line connecting two points 1,000 μm apart is used as the imaginary fiber axis at the observation position, and the vertical direction is used as the direction orthogonal to the fiber axis. That is, the so-called fluctuation amplitude refers to the value approximately measured in the projection image.

[0046] Regarding the above fluctuation range, Figure 1As shown, the center of the thickness direction of the observed single fiber 1 of the carbon fiber is arbitrarily selected as the contact point A, the center of the thickness direction of the single fiber 1 of the carbon fiber at a straight line distance of 1 mm (1,000 μm) is defined as the contact point B, point A is defined as the origin of the XY coordinate system, that is, the point of X = 0 μm, Y = 0 μm, and contact point B is defined as the point on the X axis, that is, X = 1,000 μm, Y = 0 μm, and the difference obtained by subtracting the minimum value Ymin (μm) from the maximum value Ymax (μm) among the values ​​of the Y coordinate through which the center of the thickness direction of the single fiber passes is defined as ΔY (μm). The measurement of the fluctuation range is performed on 50 randomly selected independent single fibers, and the average value is used.

[0047] The above fluctuation amplitude can be interpreted as a parameter indicating the twist strength of the carbon fiber used in the unidirectional composite material, and the larger the above fluctuation amplitude, the stronger the twist. As also explained in the background art, it is generally believed that unidirectional composite materials, especially drawn molded products, preferably have reinforcing fibers arranged in a highly uniaxial orientation, but the inventors of the present application have deliberately conducted research on using carbon fibers with a large fluctuation amplitude that intentionally make the uniaxial orientation microscopically disordered for unidirectional composite materials, and the results showed an unexpected effect of being able to improve the resistance to cracks along the fiber axis.

[0048] By making the above-mentioned fluctuation amplitude 1.5 μm or more, the number of times that the single fibers of adjacent carbon fibers are intertwined with each other can be increased, and the resistance to cracks along the fiber axis of the carbon fiber can be improved. The above-mentioned fluctuation amplitude is preferably 3.0 μm or more, more preferably 4.0 μm or more, and further preferably 4.5 μm or more. In addition, from the viewpoint of improving the resistance to cracks along the fiber axis of the carbon fiber, there is no particular upper limit to the above-mentioned fluctuation amplitude. In order to obtain carbon fiber with a large fluctuation amplitude, it is necessary to strengthen the twisting, which sometimes requires reducing the manufacturing speed. Therefore, from the viewpoint of productivity, it is preferably less than 30 μm.

[0049] On the other hand, in the case of a unidirectional composite material, whether the fluctuation width is 1.5 μm or more can be determined by the method described below using single fibers obtained by cutting out the unidirectional composite material and removing the matrix resin.

[0050] The unidirectional composite material of the present invention preferably has an average value of the helical pitch of the fiber axis of the above-mentioned carbon fiber of 5.50 cm or less. In the present invention, the helical pitch of the fiber axis of the single fiber is a morphological feature of the fiber axis related to the twisting strength of the twisted yarn. That is, in the case of twisted yarn, when manufacturing a carbon fiber bundle, it is obtained by processing it in a twisted state, but the carbon fiber bundle obtained in this way sometimes maintains the twisted form.

[0051] Here, the state in which the twisted form is maintained refers to a state in which the twist is not released from the carbon fiber bundle even if the carbon fiber bundle is cut to form a free end. In contrast, when a carbon fiber bundle that has not been twisted once is forcibly twisted in the manufacturing process and a free end is formed by cutting an arbitrary portion, since the fiber axis of the single fiber constituting the carbon fiber bundle is originally straight, the twist is naturally released from the free end in sequence due to the high rigidity of the carbon fiber. A carbon fiber bundle that maintains a twisted form is easy to obtain, especially when it has been twisted in the carbonization process.

[0052] When a single fiber is taken out from such a carbon fiber bundle that maintains the twisted shape and observed, the fiber axis of the single fiber describes a "helix". In the present invention, the helical pitch refers to the distance in the axial direction of the fiber that the helix advances during one revolution. The average value of the above helical pitch refers to the average value of the helical pitch obtained by taking out a plurality of single fibers of carbon fibers contained in a unidirectional composite material and evaluating them. The detailed evaluation method is described later.

[0053] The so-called average value of the helical pitch is 5.50 cm or less, which means that when manufacturing the carbon fiber bundle, the treatment is carried out in a state of giving a sufficiently strong twist, and the carbon fiber with the above-mentioned large fluctuation amplitude is easy to obtain, so the number of times the single fibers of adjacent carbon fibers are intertwined with each other can be increased, and the resistance to cracks along the fiber axis of the carbon fiber can be improved. The average value of the helical pitch is further preferably 4.50 cm or less, and particularly preferably 3.50 cm or less. In addition, from the viewpoint of improving the resistance to cracks along the fiber axis of the carbon fiber, the upper limit of the above-mentioned helical pitch is not particularly limited, but in order to obtain carbon fiber with a large helical pitch, it is necessary to give a strong twist, and sometimes it is necessary to reduce the manufacturing speed. Therefore, from the viewpoint of productivity, it is further preferably 1.00 cm or more.

[0054] In addition, the spiral direction of the fiber axis of a single fiber has two types, right-handed and left-handed, depending on the twisting direction applied to the carbon fiber bundle being processed in the manufacturing process. "Z twist" and "S twist" which are general technical terms indicating the twisting direction are equivalent to right-handed and left-handed as the spiral direction of a single fiber, respectively. That is, a Z-twisted twisted yarn is formed by a single fiber whose spiral direction of the fiber axis is right-handed, and an S-twisted twisted yarn is formed by a single fiber whose spiral direction of the fiber axis is left-handed.

[0055] According to the research of the inventors of the present application, in order to improve the resistance to cracks along the fiber axis of the carbon fiber, if the twist is too strong for the purpose of increasing the fluctuation amplitude, the unidirectional composite material sometimes warps. As a structure that not only improves the crack resistance but also suppresses the warping of the unidirectional composite material, the unidirectional composite material preferably includes both carbon fibers with a right-handed helix on the fiber axis of the single fiber and carbon fibers with a left-handed helix on the fiber axis of the single fiber as carbon fibers. According to the research of the inventors of the present application, by mixing and using carbon fibers with a right-handed helix on the fiber axis of the single fiber (hereinafter sometimes referred to as right-handed carbon fibers) and carbon fibers with a left-handed helix on the fiber axis of the single fiber (hereinafter sometimes referred to as left-handed carbon fibers), the number of times that the single fibers of adjacent carbon fibers are intertwined with each other can be increased, which can not only improve the crack resistance along the fiber axis of the carbon fiber, but also suppress the warping of the unidirectional composite material.

[0056] Whether both right-handed carbon fibers and left-handed carbon fibers are contained can be easily confirmed by observing the sampled carbon fiber bundle during the stage of directly manufacturing a unidirectional composite material from the carbon fiber bundle or during the stage of manufacturing an intermediate substrate for obtaining a unidirectional composite material.

[0057] Specifically, first, if the sampled carbon fiber bundle is cut to form a free end, the twist is gradually restored starting from the free end in the direction of the twist originally maintained by the carbon fiber bundle. Therefore, if the restored twist direction is the Z twist direction, the helical axis of the fiber axis is right-handed, and if it is the S twist direction, the helical direction of the fiber axis is left-handed. Therefore, the sampled carbon fiber bundle is arbitrarily confirmed within a range from a few to the total number. When a carbon fiber bundle with a right-handed helical direction of the fiber axis and a carbon fiber bundle with a left-handed helical direction of the fiber axis are observed, it can be judged that it is a unidirectional composite material containing right-handed carbon fibers and left-handed carbon fibers.

[0058] On the other hand, in the case of a unidirectional composite material, whether right-handed carbon fibers and left-handed carbon fibers are contained can be determined by the method described below using single fibers obtained by cutting out the unidirectional composite material and removing the matrix resin.

[0059] The unidirectional composite material of the present invention preferably includes both carbon fiber bundles formed by right-handed carbon fibers and carbon fiber bundles formed by left-handed carbon fibers. In this case, the number of carbon fiber bundles formed by right-handed carbon fibers is N. A (roots), the number of carbon fiber bundles formed by left-handed carbon fibers is N B (root), preferably N A / (N A +N B ) is 0.4 to 0.6. A / (N A +NB ) is in the range of 0.4 to 0.6, so that in the unidirectional composite material, the right-handed carbon fiber and the left-handed carbon fiber are easy to contact, which can increase the number of times the single fibers are intertwined with each other, thereby easily improving the crack resistance and also easily suppressing the warping of the unidirectional composite material.

[0060] In the present invention, for simplicity, this ratio is recorded as ratio f A The ratio f A The calculation is based on the number of carbon fiber bundles. A A value of 0.4 corresponds to composite formation at a ratio of 6 left-handed carbon fiber bundles to 4 right-handed carbon fiber bundles.

[0061] In the unidirectional composite material of the present invention, when the unidirectional composite material is equally divided into two parts in the width direction, it is preferred that any ratio N of the two divided pieces is A / (N A +N B ) are all 0.4 to 0.6. By making any ratio N A / (N A +N B ) are all in the range of 0.4 to 0.6, so that the right-handed carbon fiber and the left-handed carbon fiber in the unidirectional composite material are easy to contact, which can increase the number of times the single fibers are intertwined with each other, thereby easily improving the crack resistance and also easily suppressing the warping of the unidirectional composite material. In addition, it is further preferred that when the unidirectional composite material is equally divided into four parts in the width direction, any ratio N of the four fragments after the division is A / (N A +N B ) are mixed so that the ratio N of each of the four fragments after division becomes 0.4 to 0.6. A / (N A +N B ) are all in the range of 0.4 to 0.6, which makes it easier to improve the crack resistance and suppress the warping of the unidirectional composite material.

[0062] When the width of the unidirectional composite material is 50 mm or more, it is preferable to divide the unidirectional composite material into two equal parts in the width direction. n When the width of the unidirectional composite material after division is 10 mm or more and 20 mm or less, the unidirectional composite material after division is divided into two parts (n is a natural number). n Any ratio N of the fragments A / (N A +N B ) are all between 0.4 and 0.6. n Any ratio N of the fragments A / (N A +NB ) are all in the range of 0.4 to 0.6, which makes it easier to improve the crack resistance and suppress the warping of the unidirectional composite material.

[0063] It should be noted that the unidirectional composite material of the present invention is preferably in the form of a long strip, with the long side direction in the cross section perpendicular to the fiber direction being the width direction and the short side direction being the thickness direction. However, in the case of a square, i.e., a regular quadrangular prism-shaped unidirectional composite material at this stage, the direction of any side is the width direction.

[0064] In the case where the unidirectional composite material of the present invention includes both a carbon fiber bundle formed of right-handed carbon fibers and a carbon fiber bundle formed of left-handed carbon fibers, it is preferred that the right-handed carbon fiber bundles and the left-handed carbon fiber bundles are arranged alternately in the width direction of the unidirectional composite material. By arranging the right-handed carbon fiber bundles and the left-handed carbon fiber bundles alternately in the width direction, the right-handed carbon fibers and the left-handed carbon fibers in the unidirectional composite material are easily in contact with each other, and the number of times the single fibers are intertwined with each other can be increased, so that the crack resistance is easily improved and the warping of the unidirectional composite material is also easily suppressed.

[0065] The volume content of carbon fiber in the unidirectional composite material of the present invention is preferably 60% by volume or more. The greater the volume content of carbon fiber, the more the number of times the single fibers of adjacent carbon fibers are intertwined with each other can be increased, and the more the resistance to cracks along the fiber axis of the carbon fiber can be improved. The volume content of carbon fiber is more preferably 65% ​​by volume or more. If the volume content of carbon fiber is increased, lint is generated due to the increase in the drawing force during drawing and molding, and sometimes the process becomes difficult, so the volume content of carbon fiber is more preferably 80% by volume or less.

[0066] In the unidirectional composite material of the present invention, when the average value of the inter-fiber distance of the carbon fibers contained in the unidirectional composite material is R (μm) and the fluctuation width of the fiber axis of the carbon fibers is D (μm), the formula (1) is preferably satisfied.

[0067] 2.0≤D÷R≤35.0···Formula (1)

[0068] According to the research results of the inventors of the present application, by controlling to satisfy the above formula (1), it is possible to improve the resistance to cracks along the fiber axis of the carbon fiber without seriously compromising productivity. In formula (1), D÷R is an index indicating the ease of interweaving of single fibers of adjacent carbon fibers. The larger the value, the more crack resistance can be improved. D÷R is more preferably 3.5 or more. In addition, from the perspective of improving the resistance to cracks along the fiber axis of the carbon fiber, there is no particular upper limit on D÷R, but in order to increase D÷R, it is necessary to increase the fluctuation amplitude D and reduce the average value R of the distance between single fibers, or both. In order to increase the fluctuation amplitude D, it is necessary to give a stronger twist, and in order to reduce the average value R of the distance between single fibers, it is necessary to increase the volume content of carbon fiber. Since when D÷R is excessively increased, the productivity is sometimes greatly reduced, it is preferably 35.0 or less. D÷R is more preferably 15.0 or less, and particularly preferably 10.0 or less.

[0069] In the unidirectional composite material of the present invention, the carbon fiber bundle is preferably included in the matrix resin in a twisted state with 10 twists / m or less. If the twist of the carbon fiber bundle is 10 twists / m or less, the single fibers included in the adjacent carbon fiber bundles are easily intertwined with each other, which can improve the crack resistance. More preferably, it is 5 twists / m or less.

[0070] In the unidirectional composite material of the present invention, in a cross section perpendicular to the fiber direction of the unidirectional composite material, when the cross-sectional area of ​​the carbon fiber bundle contained in the unidirectional composite material is set to X (mm 2 ), it is preferred that a resin-rich portion having an area of ​​3% or more of X does not substantially exist. It should be noted that the resin-rich portion refers to a portion that does not contain carbon fibers and is composed only of resin. In addition, in the present invention, regarding the fact that a resin-rich portion having an area of ​​3% or more of the cross-sectional area X of the carbon fiber bundle does not substantially exist, it means that a process of cutting the unidirectional composite material perpendicular to the fiber direction and observing the cross-section is repeated 3 times for any cross-section, and in any observation, a resin-rich portion having an area of ​​3% or more of the cross-sectional area X of the carbon fiber bundle does not exist. By making the resin-rich portion having an area of ​​3% or more of the cross-sectional area X of the carbon fiber bundle substantially non-existent, the single fibers contained in adjacent carbon fiber bundles are easily intertwined with each other, thereby improving the crack resistance.

[0071] In the present invention, the tensile modulus of the unidirectional composite material is preferably 150 GPa or more. By making the tensile modulus of the unidirectional composite material be 150 GPa or more, the rigidity required for the unidirectional composite material for large windmill blades can be satisfied. The tensile modulus of the unidirectional composite material is more preferably 200 GPa or more, and particularly preferably 240 GPa or more. From the viewpoint of improving rigidity, there is no particular limit on the upper limit of the tensile modulus of the unidirectional composite material. If the tensile modulus of carbon fiber is increased in order to increase the tensile modulus of the unidirectional composite material, it sometimes causes a decrease in tensile strength and the generation of lint. Therefore, the tensile modulus of the unidirectional composite material is more preferably less than 500 GPa, and particularly preferably less than 400 GPa.

[0072] As the unidirectional composite material of the present invention, there can be cited drawn products, unidirectional prepreg blank products, filament winding products, etc., but preferably drawn products or unidirectional prepreg blank products in which the average single fiber diameter of the carbon fiber is 6.0 μm or less. From the aspect of efficiency when manufacturing large parts, the unidirectional composite material of the present invention is preferably able to efficiently manufacture drawn products of the same shape in the length direction. In addition, from the aspect of suitability when manufacturing parts of complex shapes, the unidirectional composite material of the present invention is a unidirectional prepreg blank product. In order to meet the dimensional stability often required for complex shapes, it is preferred that the average single fiber diameter of the carbon fiber is 6.0 μm or less.

[0073] It should be noted that when using the unidirectional composite material of the present invention to manufacture parts, the unidirectional composite materials can be bonded to each other to form an integrated structure, or non-woven fabrics or textiles can be laminated between the unidirectional composite materials and then impregnated with resin and cured to form an integrated structure. In addition, the unidirectional composite material of the present invention can be bonded to different isotropic composite materials, etc.

[0074] As the matrix resin used in the unidirectional composite material of the present invention, any of a thermosetting resin and a thermoplastic resin can be used. As the thermosetting resin, vinyl ester resin, epoxy resin, unsaturated polyester resin, acrylic resin, etc. can be used. In addition, as the thermoplastic resin, polyamide resin, polyester resin, polycarbonate resin, polyphenylene sulfide resin, polyether sulfone resin, polyether ether ketone resin, etc. can be used.

[0075] The spar cap of the present invention is preferably a spar cap comprising the unidirectional composite material of the present invention. By comprising the unidirectional composite material of the present invention, a spar cap having high resistance to cracks along the fiber axis of the carbon fiber and a high elastic modulus can be made. It should be noted that the spar cap is a reinforcing material constituting a spar for windmill blades, aircraft main wings, ship masts, etc., and is mostly used to improve the strength and elastic modulus of the structure. Therefore, a spar cap with high strength and elastic modulus is preferably used because the reinforcing effect becomes larger. In addition, since cracks sometimes occur in the spar cap and the reinforcing effect becomes weak, it is preferred to use a spar cap with high resistance to cracks. The spar cap of the present invention may contain only the unidirectional composite material of the present invention, or may contain the unidirectional composite material of the present invention and other unidirectional composite materials, or an isotropic composite material. The spar cap of the present invention may contain a material formed by bonding unidirectional composite materials to each other and integrating them, or may contain a material formed by laminating non-woven fabrics or fabrics between unidirectional composite materials and then impregnating resin and curing them to integrate them.

[0076] The windmill blade of the present invention is preferably a windmill blade including the spar cap of the present invention. The larger the windmill blade, the more the amount of electricity generated by wind power generation increases, so it is preferable to use a large-scale windmill blade, and damage may sometimes occur in the post-processing required to cope with the large-scale. On the other hand, by including the spar cap of the present invention, it is possible to make a windmill blade that is easy to avoid damage in the post-processing required to cope with the large-scale. The windmill blade of the present invention may include only the spar cap of the present invention, or may include the spar cap of the present invention and other spar caps. For example, the spar cap of the present invention may be used only in a portion that is prone to cracking or a portion that is prone to deformation.

[0077] The twisted yarn used in the unidirectional composite material of the present invention can be obtained by, for example, the method described in Japanese Patent Publication No. 2014-141761 and the method described in International Publication No. 19 / 203088. The twisted yarn can be passed through the carbonization process while applying high tension in a twisted state, thereby effectively improving the degree of crystal orientation, and the twisting tension can be suppressed to the minimum required to produce a high-quality carbon fiber bundle with less single fiber breakage. It is important that by adopting the structure of the unidirectional composite material of the present invention, a unidirectional composite material with high resistance to cracks along the fiber axis of the carbon fiber and a high elastic modulus can be effectively obtained.

[0078] Example

[0079] Hereinafter, the present invention will be described in detail based on Examples, but the present invention is not limited thereto.

[0080] The measuring methods of various physical property values ​​described in this specification are as follows.

[0081] <Tensile elastic modulus of carbon fiber>

[0082] The tensile modulus of carbon fiber is determined according to the resin impregnation bundle test method of JIS R7608:2004 in the following steps. Where the carbon fiber has twisting, the evaluation is performed after untwisting by imparting a twist with the same number of reverse rotations as the twist. As the resin formulation, "CELLOXIDE (registered trademark)" 2021P (manufactured by Daicel Corporation) / boron trifluoride monoethylamine (manufactured by Tokyo Chemical Industry Co., Ltd.) / acetone = 100 / 3 / 4 (parts by mass) is used, and as the curing conditions, normal pressure, temperature of 125°C, and time of 30 minutes are used. A bundle of 10 carbon fibers is measured, and the average value is taken as the tensile modulus. It should be noted that the strain range when calculating the tensile modulus is set to 0.1 to 0.6%.

[0083] <Twist of carbon fiber bundle>

[0084] For the twist of the carbon fiber bundle (twists / m), pull out 1m of the carbon fiber bundle to be measured, twist one end with the length direction of the fiber bundle as the rotation axis, and divide the number of twists by 1 until the twist is completely released. The number of twists is counted with 360 degrees as one cycle. When visually judging whether the twist has completely disappeared, if it is difficult to see with the eyes, insert a thin and straight needle such as a cultured handle needle into the carbon fiber bundle and go deep along the length direction of the carbon fiber bundle as needed to judge the tiny twist residue and make fine adjustments. Perform 3 measurements and use the average value as the twist of the carbon fiber bundle.

[0085] <Twist of carbon fiber bundles included in unidirectional composite materials>

[0086] First, cut out a 25 cm long cuboid from any position of the unidirectional composite material along the fiber orientation direction. Place the unidirectional composite material cut into a cuboid into an electric furnace set to a nitrogen atmosphere at a temperature of 450°C and burn out the matrix resin. Then take out the remaining carbon fiber bundle, twist one end with the length direction of the fiber bundle as the rotation axis, and divide the number of twists until the twist is completely released by 0.25 for calculation. The number of twists is counted with 360 degrees as 1 week. When visually judging whether the twist has completely disappeared, if it is difficult to see with the eyes, insert a thin and straight needle such as a cultured handle needle into the carbon fiber bundle and go deep along the length direction of the carbon fiber bundle as needed to judge the tiny twist residue and make fine adjustments. Perform 3 measurements and take the average value as the twist of the carbon fiber bundle.

[0087] <Range of Fluctuation of Fiber Axis of Carbon Fiber>

[0088] Randomly collect 50 single fibers from the carbon fiber bundle used in the unidirectional composite material. In the case where it is difficult to obtain a carbon fiber bundle that has been drawn and formed before manufacturing a unidirectional composite material, cut a 1 cm long rectangle from any position of the unidirectional composite material along the fiber orientation direction. If the width in the direction orthogonal to the fiber direction is 5 cm or more, cut a rectangle 1 cm long and 5 cm wide. The above-mentioned unidirectional composite material cut into rectangles is placed in an electric furnace set to a nitrogen atmosphere at a temperature of 450°C and the matrix resin is burned out. Then, the aggregate of the remaining carbon fiber bundles is placed in a 50 mL glass container with a lid and shaken up and down 50 times, so that the single fibers are fully mixed with each other, and then 50 single fibers of carbon fibers are randomly collected therefrom.

[0089] Next, make the single fiber of the carbon fiber to be evaluated into 1 to 5 mm long and place it on the copy paper. When the single fiber is attached to the copy paper due to the influence of static electricity, remove the static electricity by conventional methods. Use an optical microscope to observe from the vertical direction of the paper surface to obtain an image. The magnification of the objective lens of the optical microscope is set to 10 times. The image is saved in jpg format with 2592 pixels horizontally and 1944 pixels vertically.

[0090] The acquired image is read into the open source image processing software "ImageJ", and an arbitrary point on the fiber axis is set as point A, and a point on the fiber axis 1,000 μm away from point A is set as point B. Next, "Bilinear Interpolation" is selected as the interpolation algorithm during rotation, and the image is rotated so that points A and B are horizontal. After binarization, skeletonization is performed to extract the fiber axis in the form of a curve with a width of 1 pixel. At this time, if dust or the like is attached to the fiber surface, the fiber axis may sometimes be bifurcated, but the side chains outside the fiber axis are ignored.

[0091] Finally, the difference ΔY (μm) obtained by subtracting the minimum value Ymin from the maximum value Ymax from the Y coordinate of the fiber axis between point A and point B is read as the fluctuation amplitude of the evaluated single fiber. The average of the fluctuation amplitudes evaluated for 50 different single fibers is taken as the fluctuation amplitude of the present invention.

[0092] In addition, in this Example, the upright microscope "DM2700M" manufactured by Leica Microsystems Co., Ltd. was used as an optical microscope.

[0093] <Helical Pitch of Fiber Axis of Single Fiber>

[0094] Cut the single fiber of the carbon fiber to be measured into a length of 10±0.5cm and place it on a copy paper spread on a horizontal platform. When the single fiber adheres to the copy paper due to the influence of static electricity, remove the static electricity by conventional methods. If the single fiber adheres to the copy paper and does not separate when the copy paper carrying the single fiber is turned upside down, the static electricity removal is insufficient, so additional static electricity removal is performed. Visually observe from the normal direction of the single fiber and in the direction parallel to the paper surface, and measure the distance between the points where the single fiber contacts the copy paper. For example, when the spiral pitch is 3.0cm, if Figure 2 In the example shown, the contact with the copy paper is made at three contact points, namely, A, B, and C. Therefore, in this case, the distance AB and the distance BC are measured, and the average value (3.0 cm) thereof is defined as the helical pitch of the fiber axis of the single fiber.

[0095] Each value is read to the first decimal place, that is, 1 mm. When calculating the average value, if there are digits below the second decimal place, keep them at the second decimal place. For example, the average of 2.2 cm, 2.3 cm, and 2.2 cm is 2.23333···cm. The third decimal place is rounded off and the average value is 2.23 cm. The evaluation of the helical pitch of the fiber axis of a single fiber is performed once for the single fiber to be evaluated.

[0096] <Average value of the helical pitch of the fiber axis of carbon fiber>

[0097] Randomly collect 50 single fibers from the carbon fiber bundle used in the unidirectional composite material. In the case where it is difficult to obtain a carbon fiber bundle that has been drawn and formed before manufacturing a unidirectional composite material, cut a 13 cm long rectangle from any position of the unidirectional composite material along the fiber orientation direction. If the width in the direction orthogonal to the fiber direction is 5 cm or more, cut a rectangle 13 cm long and 5 cm wide. The unidirectional composite material cut into rectangles is placed in an electric furnace set to a nitrogen atmosphere at a temperature of 450°C and the matrix resin is burned out, and then 50 single fibers are randomly collected from the remaining carbon fiber bundle. For the obtained single fibers, the helical pitch of the fiber axis is evaluated by the above method, and the evaluation values ​​of the helical pitch are averaged to calculate the average value of the pitch of the fiber axis of the carbon fiber bundle. The average value of the helical pitch is rounded to the second decimal place.

[0098] <Helical Direction of Fiber Axis of Single Fiber>

[0099] In the above-mentioned method for measuring the helical pitch, the helical direction of the fiber axis of the single fiber is confirmed by visually observing from the fiber axis instead of the normal direction of the single fiber. Right-handedness refers to the direction of advancing toward the depth of the clockwise dial when rotating in the clockwise direction, and is also called Z-handedness. Left-handedness is the opposite, and is also called S-handedness.

[0100] <Determination of Carbon Fibers with Different Helical Directions of the Fiber Axes in Unidirectional Composite Materials>

[0101] First, a 13 cm long cuboid is cut out from any position of the unidirectional composite material along the fiber orientation direction. The unidirectional composite material cut into a cuboid is placed in an electric furnace set to a nitrogen atmosphere at a temperature of 450°C and the matrix resin is burned out, and then 50 single fibers are randomly collected from the remaining carbon fiber bundles. Next, the spiral direction of the fiber axis is evaluated by the above method. When it can be confirmed that there are more than 3 single fibers with right-handed spiral directions and 3 single fibers with left-handed spiral directions of the fiber axis, it is judged to be a unidirectional composite material containing carbon fibers with right-handed spiral directions and carbon fibers with left-handed spiral directions of the fiber axis of the single fiber.

[0102] <The existence ratio of carbon fiber bundles formed by single fibers with right-handed helical direction of the fiber axis f A >

[0103] First, a 13 cm long cuboid is cut from any position of the unidirectional composite material along the fiber orientation direction. The unidirectional composite material cut into a cuboid is placed in an electric furnace set to a nitrogen atmosphere at a temperature of 450°C and the matrix resin is burned out. Then, each carbon fiber bundle is identified by visually confirming the aggregate of the remaining carbon fiber bundles. Next, three single fibers are collected from each carbon fiber bundle, and the helical direction of the fiber axis is evaluated by the above method. For a certain carbon fiber bundle, the helical direction of the entire bundle of the carbon fiber bundle is determined by majority vote based on the evaluation results of the helical direction of the fiber axis of the three single fibers collected from the carbon fiber bundle.

[0104] For example, when the evaluation results of the spiral direction of the fiber axis of three single fibers collected from a carbon fiber bundle are right-handed, right-handed, and left-handed, it is judged that the carbon fiber bundle is formed by single fibers whose fiber axis has a right-handed spiral direction (that is, it is a carbon fiber bundle formed by single fibers whose fiber axis has a right-handed spiral direction).

[0105] Here, the number of carbon fiber bundles formed of single fibers having a right-handed helix in the fiber axis is N. A (roots), the number of carbon fiber bundles formed by single fibers having a left-handed helix on the fiber axis is N B (root), calculate the ratio N A / (N A +N B ), which is taken as the existence ratio f of the carbon fiber bundle formed by the single fiber whose helical direction of the fiber axis is right-handed A When a unidirectional composite material is equally divided into two parts in the width direction, the f of the two fragments after the division is A , when the image is equally divided into four parts in the width direction, the f of the four fragments after division Aand divide the unidirectional composite material equally into two in the width direction n The unidirectional composite material is divided into two parts (n is a natural number) until the width of the divided unidirectional composite material becomes 10 mm or more and 20 mm or less. n Fragment of A It can be obtained by the same method as above.

[0106] When the carbon fiber bundle is also cut during the division of the unidirectional composite material, the weight of the cut carbon fiber bundle is measured. When it is more than 70% of the weight of the uncut carbon fiber bundle, it is counted as 1 carbon fiber bundle; when it is more than 30% and less than 70% of the weight of the uncut carbon fiber bundle, it is counted as 0.5 carbon fiber bundle; when it is less than 30% of the weight of the uncut carbon fiber bundle, it is counted as 0 carbon fiber bundle.

[0107] <Determination of carbon fiber bundles with different helical directions of the fiber axes arranged alternately in the width direction of the unidirectional composite material>

[0108] First, a 13 cm long cuboid is cut out from any position of the unidirectional composite material along the fiber orientation direction. The unidirectional composite material cut into a cuboid is placed in an electric furnace set to a nitrogen atmosphere at a temperature of 450°C and the matrix resin is burned out. Then, each carbon fiber bundle is identified by visually confirming the aggregate of the remaining carbon fiber bundles. Next, three single fibers are collected from each carbon fiber bundle, and the spiral direction of the fiber axis is evaluated by the above method. For a certain carbon fiber bundle, the spiral direction of the bundle as a whole of the carbon fiber bundle is determined by majority vote based on the evaluation results of the spiral direction of the fiber axis of the three single fibers collected from the carbon fiber bundle. Then, by confirming the position of the right-handed carbon fiber bundle and the position of the left-handed carbon fiber bundle, it is determined whether the carbon fiber bundles with different spiral directions of the fiber axis are arranged alternately in the width direction of the unidirectional composite material.

[0109] <Volume Content of Carbon Fiber in Unidirectional Composite Material>

[0110] First, a 13 cm long rectangular parallelepiped is cut from any position of the unidirectional composite material along the fiber orientation direction. If the width in the direction perpendicular to the fiber direction is 5 cm or more, a rectangle of 13 cm long and 5 cm wide is cut. After measuring the mass of the unidirectional composite material cut into rectangles, the mass of the carbon fiber obtained by placing it in an electric furnace set to a nitrogen atmosphere at a temperature of 450°C and burning out the matrix resin is measured, thereby calculating the mass content W of the carbon fiber in the unidirectional composite material. f .

[0111] Next, the density ρ of the unidirectional composite material was determined by the test method for plastic density in JIS K7112:1999. cThen, the density of the carbon fiber obtained by burning out the matrix resin was determined according to the test method for carbon fiber density of JIS R7603:1999. f .

[0112] Finally, the volume content of carbon fiber V is calculated according to the following formula: f .

[0113] V f =W f ×(ρ c ÷ρ f )

[0114] <Average value of single fiber diameter of carbon fiber>

[0115] The single fiber of the carbon fiber was observed and evaluated by using a scanning electron microscope (SEM). 50 single fibers were evaluated, and the average value was taken as the average value of the single fiber diameter. It should be noted that in the examples and comparative examples of the present invention, observation was performed using a SEM "S-4800" manufactured by Hitachi High-Technologies.

[0116] <Average value of distance between single fibers of carbon fibers included in unidirectional composite materials>

[0117] Figure 3 Shows a cross section of a unidirectional composite material perpendicular to the fiber direction. Figure 3 As shown, the calculated value of the distance between single fibers 4 of the carbon fiber assuming that the single fibers 4 of the carbon fiber are uniformly dispersed in the unidirectional composite material is obtained as the average value R of the distance between single fibers of the carbon fiber contained in the unidirectional composite material by the following steps.

[0118] When the single fibers 4 of the carbon fiber are dispersed at equal distances from each other, as shown in FIG. Figure 3 As shown on the right side of , it is represented by a structure with a length L as a repeating unit obtained by connecting the centers of the single fibers 4 of each carbon fiber. At this time, the average value R of the distance between the single fibers of the carbon fiber can be expressed as R = L-2r using the distance L between the centers of the single fibers of the carbon fiber and the radius r of the single fiber of the carbon fiber.

[0119] In addition, the area of ​​the single fiber of the carbon fiber contained inside (π×r 2 ÷2) relative to the area of ​​the regular triangle of length L as the repeating unit (√3÷4×L 2 ) ratio and the volume content of carbon fiber V f The same can be obtained by (π×r 2 ÷2)÷(√3÷4×L 2 )=V f÷100. If this formula is transformed, it becomes L=r×{200×π÷(√3×V f )} 0.5 .

[0120] As mentioned above, since we can get R = r × [{200 × π ÷ (√3 × V f )} 0.5 -2], the radius r of the single fiber of the carbon fiber obtained by dividing the average value of the single fiber diameter of the carbon fiber obtained by the above method by 2 and the volume content V of the carbon fiber obtained by the above method are f The value of is used to calculate and determine the average value R of the distance between single fibers of the carbon fibers contained in the unidirectional composite material.

[0121] <Number of Single Fibers Included in Carbon Fiber Bundle>

[0122] First, a 13 cm long cuboid is cut from any position of the unidirectional composite material along the fiber orientation direction. The unidirectional composite material cut into a cuboid is placed in an electric furnace set to a nitrogen atmosphere at a temperature of 450°C and the matrix resin is burned out. Then, the remaining carbon fiber bundles are visually confirmed to identify each carbon fiber bundle, and the carbon fiber bundles are evaluated by observing them with a SEM. There are 3 carbon fiber bundles to be evaluated, and the average value is taken as the number of single fibers contained in the carbon fiber bundles. The number of single fibers is calculated in units of 1,000. It should be noted that in the embodiments and comparative examples of the present invention, observation was performed using a scanning electron microscope (SEM) "S-4800" manufactured by Hitachi High-Technologies.

[0123] <Cross-sectional area of ​​carbon fiber bundles included in unidirectional composite materials>

[0124] The cross-sectional area of ​​the single fiber when the single fiber of the carbon fiber is assumed to be a perfect circle is calculated using the average value of the single fiber diameter of the carbon fiber obtained by the above method. The cross-sectional area of ​​the carbon fiber bundle contained in the unidirectional composite material is calculated by multiplying the cross-sectional area of ​​the obtained single fiber by the number of single fibers contained in the carbon fiber bundle obtained by the above method.

[0125] <Evaluation of the substantial absence of a resin-rich portion having an area of ​​3% or more of the cross-sectional area X of the carbon fiber bundle in the unidirectional composite material>

[0126] First, the unidirectional composite material was cut perpendicularly to the fiber direction to obtain a cross section with a width of 20 mm and a thickness of 1 mm, and the cross section was observed using a laser microscope. Next, the cross-sectional area of ​​the carbon fiber bundle obtained by the above method was used to calculate the area that was 3% of the cross-sectional area of ​​the carbon fiber bundle, and then the presence or absence of a resin-rich portion with an area larger than the same was evaluated.

[0127] like Figure 4 As shown, the area of ​​the resin-enriched portion 7 is obtained by connecting the center points of the single fibers 6 of the carbon fibers surrounding the resin-enriched portion 7 and dividing it by the area of ​​the single fibers 6 of the carbon fibers contained in the same area after confirming the existence of the resin-enriched portion 7 consisting of substantially only resin by a laser microscope. It should be noted that the portion that is vacant at a distance greater than the average value of the single fiber diameter of the carbon fibers is regarded as a continuous resin-enriched portion, and the portion that stays at a distance less than the average value of the single fiber diameter of the carbon fibers is regarded as a discontinuous resin-enriched portion, thereby determining the single fibers 6 of the carbon fibers surrounding the area of ​​the resin-enriched portion 7.

[0128] In addition, after determining the single fiber 6 of the carbon fiber surrounding the resin-enriched portion 7 according to the above criteria, as shown in FIG. Figure 5 As shown, it is known that when the resin-enriched portion 7 contains single carbon fiber fibers 6, the area of ​​the resin-enriched portion 7 is calculated by subtracting the area surrounded by the internal single carbon fiber fibers 6 from the area of ​​the internal single carbon fiber fibers 6.

[0129] The above evaluation is performed on three cross sections, and if a resin-rich portion having an area of ​​3% or more of the cross-sectional area X of the carbon fiber bundle is not present in any of the observations, it is judged that a resin-rich portion having an area of ​​3% or more of the cross-sectional area X of the carbon fiber bundle is substantially absent. It should be noted that in the examples and comparative examples of the present invention, a laser microscope "VHX-7000" manufactured by KEYENCE was used.

[0130] <Tensile elastic modulus of unidirectional composite materials>

[0131] The tensile modulus of the unidirectional composite material is determined according to JIS K7164: 2005. Ten test pieces cut out from the unidirectional composite material are measured, and the average value is taken as the tensile modulus. The strain range for calculating the tensile modulus is 0.1 to 0.6%.

[0132] <Crack resistance along the fiber axis of carbon fibers of unidirectional composite materials>

[0133] First, if Figure 6 As shown on the left, the unidirectional composite material was cut into pieces with a length of 100 mm in the fiber axis direction, 20 mm in the direction perpendicular to the fiber axis, and 1 mm in the thickness direction to obtain the evaluation sample 8. Figure 6 As shown in the center, two 12 mm wide pliers are held in both hands, and the pliers are used to hold the evaluation sample 8 at two locations, namely, the pliers holding portion 9 (width: 12 mm, length: 5 mm). Figure 6As shown on the right, the evaluation sample 8 is bent in a direction perpendicular to the fiber axial direction D for 1 second so that the holding portions are at an angle of 90 degrees to each other, and a crack E is formed along the fiber axial direction D of the carbon fiber, and then restored to 0 degrees. Finally, using a tensile tester, the clamp holding portion 9 is held with a clamp, and stretched in a direction perpendicular to the fiber axial direction D at a crosshead speed of 2 mm / min, and the crack resistance is evaluated according to the following criteria. It should be noted that in the embodiments and comparative examples of the present invention, a tensile tester "5565 Universal Tester" manufactured by INSTRON Corporation is used.

[0134] S: In order to tear along the fiber axis D, a force of 5 kgf or more must be applied.

[0135] A: In order to tear along the fiber axis D, a force of 2 kgf or more and less than 5 kgf must be applied.

[0136] B: The sample cracks along the fiber axis D at the time when the crack is formed, or the sample cracks along the fiber axis D under a force less than 2 kgf.

[0137] In Examples 1 to 11 and Comparative Examples 1 to 2 described below, the conditions described in Tables 1 and 2 were used for the implementation methods described in the following flame resistant fiber production examples 1 to 3.

[0138] [Example 1 of producing flame resistant fiber]

[0139] A monomer composition composed of acrylonitrile and itaconic acid was polymerized by a solution polymerization method using dimethyl sulfoxide as a solvent to obtain a spinning solution containing a polyacrylonitrile copolymer. A coagulated sliver was obtained by a dry-wet spinning method in which the obtained spinning solution was filtered, temporarily discharged from the spinning spinneret into the air, and introduced into a coagulation bath containing an aqueous solution of dimethyl sulfoxide. In addition, the coagulated sliver was washed with water, stretched in warm water at 90°C at a bath stretch ratio of 3 times, and then a silicone oil agent was applied. It was dried using a roller heated to a temperature of 160°C, and stretched with pressurized water vapor at a stretch ratio of 4 times to obtain a carbon fiber precursor fiber bundle with a single fiber fineness of 1.1 dtex. Next, 8 obtained carbon fiber precursor fiber bundles were combined to make the number of single fibers 24,000, and heat-treated in an oven at 230-270°C in an air atmosphere at a stretch ratio of 1 to obtain a flame-resistant fiber bundle.

[0140] [Production Example 2 of Flame Resistant Fiber]

[0141] In Flame Resistant Fiber Production Example 1, a flame resistant fiber bundle was obtained in the same manner except that the single fiber fineness of the carbon fiber precursor fiber bundle was 0.8 dtex and four carbon fiber precursor fiber bundles were combined to form 12,000 single fibers.

[0142] [Production Example 3 of Flame Resistant Fiber]

[0143] In the flame resistant fiber production example 1, a flame resistant fiber bundle was obtained in the same manner except that the single fiber fineness of the carbon fiber precursor fiber bundle was changed to 0.8 dtex.

[0144] [Example of manufacturing drawn molded products]

[0145] First, as an uncured epoxy resin composition, a composition obtained by mixing a curing agent and a curing accelerator in an epoxy resin is used, and a carbon fiber bundle stretched in one direction is passed through a resin impregnation tank to allow the above-mentioned epoxy resin composition to adhere. After scraping off excess resin, it is cured by passing through a rectangular hole-shaped mold with a width of 20 mm and a thickness of 1 mm, the center of which is heated to 180°C in the molding direction, and is continuously drawn by a drawing device and cut into 8 m in length, thereby obtaining a drawn molded product.

[0146] [Example of manufacturing unidirectional prepreg molded product]

[0147] First, an uncured epoxy resin composition obtained by mixing a curing agent and a curing accelerator in an epoxy resin is applied to a release paper using a reverse roll coater to prepare a resin film. Next, a carbon fiber bundle aligned in one direction is sandwiched between the resin films from both sides, and the carbon fiber bundle is heated and pressurized to be impregnated with the resin, thereby obtaining a unidirectional prepreg.

[0148] The unidirectional prepreg blank was cut into squares with a cutting machine having a size of 13 cm in the fiber axis direction and 13 cm in the direction perpendicular to the fiber axis, and sandwiched between a SUS tool plate and an aluminum pressure plate forming a square of 13 cm square. After being bagged with a bag film and a sealant, the temperature was raised to 180°C in an autoclave to cure it, thereby obtaining a unidirectional prepreg blank molded product with a width of 13 cm, a length of 13 cm, and a thickness of 1 mm.

[0149] [Example 1]

[0150] The flame resistant fiber bundle obtained by flame resistant fiber manufacturing example 1 was twisted to produce a twisted flame resistant fiber bundle with a twist of 25 turns / m. The twisted flame resistant fiber bundle was pre-carbonized in a nitrogen atmosphere at a temperature of 300 to 800°C with a draw ratio of 0.97 to obtain a pre-carbonized fiber bundle. Next, the pre-carbonized fiber bundle was carbonized in a nitrogen atmosphere at a temperature of 1,000 to 1,800°C while appropriately adjusting the draw ratio to obtain a carbon fiber bundle. The evaluation results are summarized in Table 1.

[0151] After the carbon fiber bundle was untwisted to a state without residual twist, a drawn molded product was obtained according to the drawing molded product manufacturing example. The evaluation results of the carbon fiber volume content, tensile elastic modulus, and resistance to cracks along the fiber axis of the carbon fiber obtained by analyzing the drawn molded product are shown in Table 2.

[0152] [Example 2]

[0153] A carbon fiber bundle and a pultruded product were obtained in the same manner as in Example 1 except that the carbonization treatment was performed in a nitrogen atmosphere at a temperature of 1,000 to 2,100° C. The evaluation results of the carbon fibers and the pultruded product are shown in Tables 1 and 2.

[0154] [Example 3]

[0155] A carbon fiber bundle and a pultruded product were obtained in the same manner as in Example 1 except that the carbonization treatment was performed in a nitrogen atmosphere at a temperature of 1,000 to 1,400° C. The evaluation results of the carbon fibers and the pultruded product are shown in Tables 1 and 2.

[0156] [Example 4]

[0157] A carbon fiber bundle and a pultruded product were obtained in the same manner as in Example 1 except that the twist was set to 45 twists / m and the volume content of the carbon fibers was reduced. Tables 1 and 2 show the evaluation results of the carbon fibers and the pultruded product.

[0158] [Example 5]

[0159] A carbon fiber bundle and a pultruded product were obtained in the same manner as in Example 1 except that the volume content of the carbon fibers was reduced. Tables 1 and 2 show the evaluation results of the carbon fibers and the pultruded product.

[0160] [Example 6]

[0161] The flame resistant fiber bundle obtained by flame resistant fiber manufacturing example 2 was twisted to produce a twisted flame resistant fiber bundle with a twist of 45 turns / m. The twisted flame resistant fiber bundle was pre-carbonized in a nitrogen atmosphere at a temperature of 300 to 800°C with a draw ratio of 0.97 to obtain a pre-carbonized fiber bundle. Next, the pre-carbonized fiber bundle was carbonized in a nitrogen atmosphere at a temperature of 1,000 to 1,800°C while appropriately adjusting the draw ratio to obtain a carbon fiber bundle. The evaluation results are summarized in Table 1.

[0162] After the carbon fiber bundle was untwisted to a state without residual twist, a drawn molded product was obtained according to the drawing molded product manufacturing example. The evaluation results of the carbon fiber volume content, tensile elastic modulus, and resistance to cracks along the fiber axis of the carbon fiber obtained by analyzing the drawn molded product are shown in Table 2.

[0163] [Example 7]

[0164] The flame resistant fiber bundle obtained by flame resistant fiber manufacturing example 1 was twisted to produce a twisted flame resistant fiber bundle with a Z twist of 45 twists / m and a twisted flame resistant fiber bundle with an S twist of 45 twists / m. Each twisted flame resistant fiber bundle was pre-carbonized at a draw ratio of 0.97 in a nitrogen atmosphere at a temperature of 300 to 800°C to obtain a pre-carbonized fiber bundle with a Z twist and an S twist, respectively. Next, these pre-carbonized fiber bundles were carbonized in a nitrogen atmosphere at a temperature of 1,000 to 1,800°C while appropriately adjusting the draw ratio to obtain a Z twist and an S twist carbon fiber bundle.

[0165] After the carbon fiber bundles imparted with Z twist and the carbon fiber bundles imparted with S twist are untwisted to form a state without residual twist, a drawn molded product is obtained according to the drawing molded product manufacturing example. Figure 7 As shown in FIG. 1 , right-handed (Z-twisted) carbon fiber bundles 11 and left-handed (S-twisted) carbon fiber bundles 12 are arranged alternately in the width direction at a ratio of 7:6 in number of strands in a drawing die 10. The evaluation results of Vf, tensile elastic modulus, crack resistance, etc. obtained by analyzing the drawing molded product are shown in Table 2.

[0166] The properties of the carbon fiber, the elastic modulus and the crack resistance of the drawn molded product are the same as those of Example 4, but the warpage of the drawn molded product is much less than that of Example 4, and the drawn molded product has high dimensional stability.

[0167] [Example 8]

[0168] The flame resistant fiber bundle obtained by flame resistant fiber manufacturing example 3 was twisted to produce a twisted flame resistant fiber bundle with a Z twist of 15 twists / m. The twisted flame resistant fiber bundle was pre-carbonized in a nitrogen atmosphere at a temperature of 300 to 800°C with a draw ratio of 0.97 to obtain a pre-carbonized fiber bundle. Next, the pre-carbonized fiber bundle was carbonized in a nitrogen atmosphere at a temperature of 1,000 to 1,800°C while appropriately adjusting the draw ratio to obtain a carbon fiber bundle. The evaluation results are summarized in Table 1.

[0169] After the carbon fiber bundle was untwisted to a state without residual twist, a drawn molded product was obtained according to the drawing molded product manufacturing example. The evaluation results of the carbon fiber volume content, tensile elastic modulus, and resistance to cracks along the fiber axis of the carbon fiber obtained by analyzing the drawn molded product are shown in Table 2.

[0170] [Example 9]

[0171] The carbon fiber bundle was untwisted, the residual twist was reduced to 5 twists / m, and a pultruded product was obtained according to the pultruded product manufacturing example. A carbon fiber bundle and a pultruded product were obtained in the same manner as in Example 1. The evaluation results of the carbon fiber and the pultruded product are shown in Tables 1 and 2.

[0172] [Example 10]

[0173] The carbon fiber bundle was untwisted, the residual twist was reduced to 15 twists / m, and then a pultruded product was obtained according to the pultruded product manufacturing example. The carbon fiber bundle and the pultruded product were obtained in the same manner as in Example 1. The evaluation results of the carbon fiber and the pultruded product are shown in Tables 1 and 2. In the cross section of the pultruded product, a resin-rich portion having an area of ​​3% or more of the cross-sectional area X of the carbon fiber bundle existed, and the crack resistance itself was high but inferior to that of Example 1.

[0174] [Example 11]

[0175] The flame resistant fiber bundle obtained by flame resistant fiber manufacturing example 2 was twisted to produce a twisted flame resistant fiber bundle with a twist of 25 turns / m. The twisted flame resistant fiber bundle was pre-carbonized in a nitrogen atmosphere at a temperature of 300 to 800°C with a draw ratio of 0.97 to obtain a pre-carbonized fiber bundle. Next, the pre-carbonized fiber bundle was carbonized in a nitrogen atmosphere at a temperature of 1,000 to 1,800°C while appropriately adjusting the draw ratio to obtain a carbon fiber bundle. The evaluation results are summarized in Table 1.

[0176] After the carbon fiber bundle is untwisted to a state without residual twist, a unidirectional prepreg molded product is obtained according to the unidirectional prepreg molded product manufacturing example. The evaluation results of the volume content of carbon fiber, tensile elastic modulus, and resistance to cracks along the fiber axis of the carbon fiber obtained by analyzing the unidirectional prepreg molded product are shown in Table 2.

[0177] [Comparative Example 1]

[0178] The carbon fiber bundles shown in Table 1 were obtained in the same manner as in Example 1 except that the twist was set to 0 twists / m. The drawing ratio during the carbonization treatment was increased in order to increase the tensile elastic modulus of the carbon fiber bundle, resulting in a very large amount of fuzz. The attempt to obtain a drawn molded product according to the drawn molded product production example occurred, but the fuzz accumulated in the spinneret, making it difficult to obtain a drawn molded product.

[0179] [Comparative Example 2]

[0180] The carbon fiber bundles shown in Table 1 were obtained in the same manner as in Comparative Example 1 except that the drawing ratio during the carbonization treatment was suppressed to a low level. The tensile elastic modulus of the carbon fiber bundle was reduced, but a carbon fiber bundle with less fuzz was obtained. Next, a drawn molded product was obtained according to the example of producing a drawn molded product. The evaluation results of the carbon fibers and the drawn molded product are shown in Tables 1 and 2.

[0181] [Table 1]

[0182]

[0183] [Table 2]

[0184]

[0185] Industrial Applicability

[0186] According to the present invention, by untwisting a twisted yarn with a large twist number and using it to manufacture a unidirectional composite material, the fluctuation amplitude of the fiber axis of a single fiber of carbon fiber is effectively controlled, thereby obtaining a unidirectional composite material with high resistance to cracks along the fiber axis of the carbon fiber. In addition, a wind turbine blade obtained by using the unidirectional composite material for a spar cap can easily avoid damage during post-processing required for large-scale production.

[0187] Description of Reference Numerals

[0188] 1: Single fiber of carbon fiber

[0189] 2: Copy paper

[0190] A: Contact point A

[0191] B: Contact point B

[0192] C: Contact point C

[0193] 3: Cross-section of unidirectional composite material (when uniformly dispersed)

[0194] 4: Single fiber of carbon fiber

[0195] L: The distance between the centers of the single carbon fibers (when evenly dispersed)

[0196] R: The average distance between single fibers of carbon fibers contained in unidirectional composite materials

[0197] r: The radius of a single carbon fiber

[0198] 5: Cross section of unidirectional composite material

[0199] 6: Single fiber of carbon fiber

[0200] 7: Resin enrichment section

[0201] D: Fiber axis direction

[0202] E: Crack

[0203] 8: Evaluation samples

[0204] 9: Pliers holding part

[0205] 10: Drawing die (rectangular hole shape)

[0206] 11: Right-handed (Z-twisted) carbon fiber bundle

[0207] 12: Left-handed (S-twisted) carbon fiber bundle

Claims

1. A unidirectional composite material comprising carbon fibers and a matrix resin, wherein a fluctuation range of a fiber axis of a single fiber of the carbon fibers when observed from the side within a linear distance of 1 mm is 1.5 μm or more.

2. The unidirectional composite material according to claim 1, wherein: The average value of the helical pitch of the fiber axis of the carbon fibers is 5.50 cm or less.

3. The unidirectional composite material according to claim 1 or 2, wherein: When the average value of the distance between single fibers of the carbon fibers contained in the unidirectional composite material is set to R (μm) and the fluctuation amplitude of the fiber axis of the carbon fibers is set to D (μm), the formula (1) is satisfied: 2.0≤D÷R≤35.0···Formula (1).

4. The unidirectional composite material according to claim 1 or 2, wherein: The volume content of the carbon fibers is 60 volume % or more.

5. The unidirectional composite material according to claim 1 or 2, wherein: The carbon fiber bundle is contained in the matrix resin in a twisted state with 10 twists / m or less.

6. The unidirectional composite material according to claim 1 or 2, wherein: In the cross section perpendicular to the fiber direction of the unidirectional composite material, when the cross-sectional area of ​​the carbon fiber bundle contained in the unidirectional composite material is set to X (mm 2 ), a resin-rich portion having an area of ​​3% or more of X does not substantially exist.

7. The unidirectional composite material according to claim 1 or 2, wherein: The carbon fibers include both carbon fibers in which the fiber axis of a single fiber has a right-handed helix and carbon fibers in which the fiber axis of a single fiber has a left-handed helix.

8. The unidirectional composite material according to claim 7, wherein: When the number of carbon fiber bundles formed by carbon fibers having a right-handed helix in the fiber axis of a single fiber is N A (roots), the number of carbon fiber bundles formed by carbon fibers having a left-handed helix in the fiber axis of a single fiber is N B (root) time, than N A / (N A +N B ) is 0.4~0.

6.

9. The unidirectional composite material according to claim 7, wherein: Carbon fiber bundles formed of carbon fibers whose fiber axes have a right-handed helix in single fibers and carbon fiber bundles formed of carbon fibers whose fiber axes have a left-handed helix in single fibers are alternately arranged in the width direction of the unidirectional composite material.

10. The unidirectional composite material according to claim 1 or 2, which has a tensile elastic modulus of 150 GPa or more. The unidirectional composite material according to claim 1 or 2, which is a draw-molded product.

12. The unidirectional composite material according to claim 1 or 2, wherein: The average single fiber diameter of the carbon fiber is 6.0 μm or less, and the unidirectional composite material is a unidirectional prepreg molded product.

13. A spar cap comprising the unidirectional composite material according to claim 1 or 2.

14. A windmill blade comprising the spar cap according to claim 13.