Polycarbonate resin composition and antenna member

By mixing polystyrene-based resins and elastomers in polycarbonate resins, the melt viscosity ratio and copolymer types are optimized, and the thermal resistance and rigidity of polycarbonate resins in high-frequency band communication equipment in the prior art is solved. The problem is that a low-cost, low-distance tangent resin composition is realized, and is suitable for components for high-frequency band antennas.

CN118891323APending Publication Date: 2024-11-01MITSUBISHI ENG PLASTICS CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380028203.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-22
Filing Date
2023-03-03
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

When the existing polycarbonate resin improves the dielectric loss tangent and impact resistance, it is difficult to maintain sufficient heat resistance and rigidity, and the cost is high, making it difficult to meet the needs of high-frequency band communication equipment.

Method used

By mixing the polystyrene-based resin and elastomer into the polycarbonate resin, the melt viscosity ratio is controlled within the range of 4.5 to 12.5, and a specific copolymer such as butadiene/methyl (meth)acrylate copolymer is added. Optimize the ratio of polystyrene-based resin to elastomer, reduce the dielectric loss tangent and improve impact resistance.

Benefits of technology

A polycarbonate resin composition with low cost and low dielectric loss tangent has excellent heat resistance, impact resistance and rigidity, and is suitable for use in electronic and electrical equipment components in high frequency bands, especially antenna substrates and antennas. cover.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005046510580000081
    Figure BDA0005046510580000081
  • Figure BDA0005046510580000211
    Figure BDA0005046510580000211
  • Figure BDA0005046510580000241
    Figure BDA0005046510580000241
Patent Text Reader

Abstract

Provided are: a polycarbonate resin composition having a low relative dielectric constant and a low dielectric loss tangent, and excellent heat resistance, impact resistance, toughness, and rigidity; and an antenna member. The polycarbonate resin composition contains 30-120 parts by mass of a polystyrene resin (B) and 3-50 parts by mass of an elastomer (C) per 100 parts by mass of a polycarbonate resin (A), and is characterized in that the melt viscosity ratio ([eta] A / [eta] B) of the polycarbonate resin (A) and the polystyrene resin (B) at 260 DEG C and 1216 sec <-1 > is in the range of 4.5-12.5.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a polycarbonate resin composition, and more particularly to a polycarbonate resin composition having a low relative dielectric constant and a low dielectric loss tangent and excellent in heat resistance, impact resistance, toughness and rigidity, and an antenna member. Background Art

[0002] Improvements in the speed and capacity of signals used in mobile communication devices, their base station devices, network infrastructure devices such as servers and routers, and electronic devices such as large computers are ongoing. In addition, in addition to the above-mentioned electronic devices, efforts are being made to practically apply systems that process high-frequency radio signals to automobile or traffic system-related fields or indoor near-field communication fields.

[0003] In addition, in the field of information communications using GHz-level high-frequency signals, significant increases in speed have been achieved, and in Japan, commercial services of the fifth-generation mobile communication system (5G) started in March 2020, and research is being conducted on the use of higher frequency bands in the sixth-generation mobile communication system (6G), which will be the next-generation system.

[0004] In order to cope with such increases in capacity and speed, materials having a low relative dielectric constant and a low dielectric loss tangent are required for components of communication devices or radar devices used.

[0005] In Patent Document 1, the present applicant proposes that a resin composition containing a thermoplastic resin and aluminum oxide (B) provides a millimeter wave radar cover having a low relative dielectric constant, a low dielectric loss tangent, and excellent millimeter wave transmittance. However, aluminum oxide is a material having a high absolute value of a dielectric constant, and the document shows that in Example 2 containing the polycarbonate resin of Patent Document 1, the relative dielectric constant is 3.7 and the dielectric loss tangent is 0.0093.

[0006] In order to reduce the transmission loss of electromagnetic waves, it is necessary to have a material with not only a low relative dielectric constant but also a low dielectric loss tangent, because the magnitude of the dielectric loss occurring in the material is proportional to the product of the square root of the relative dielectric constant of the material and the dielectric loss tangent. However, it is difficult to say that the relative dielectric constant and dielectric loss tangent of the above materials are low enough to cope with the increase in capacity and speed.

[0007] In addition, in Patent Document 2, the present applicant discovered that a polycarbonate resin having a specific bisphenol unit has a low dielectric loss tangent, and proposed a millimeter wave radar cover made of a polycarbonate resin material having both a low relative dielectric constant and a low dielectric loss tangent by blending the polycarbonate resin into a general-purpose polycarbonate resin. This polycarbonate resin material is an effective material, but has a problem that its use is limited due to its high price.

[0008] As a material having good dielectric properties, polystyrene may be compounded, but polystyrene has disadvantages of poor compatibility with general-purpose polycarbonate resins, poor heat resistance, and poor impact resistance.

[0009] In addition, the base material or cover used for the antenna needs to have high rigidity or excellent impact resistance so as not only to sufficiently maintain rigidity but also to sufficiently withstand wind pressure when installed outdoors, and also needs to have excellent heat resistance to prevent functional impairment at high temperatures.

[0010] Prior art literature

[0011] Patent Literature

[0012] Patent Document 1: JP 2013-102512 A

[0013] Patent Document 2: JP 2019-195137 A Summary of the invention

[0014] Problem that the invention aims to solve

[0015] In view of the above circumstances, an object (problem) of the present invention is to provide a polycarbonate resin composition having a low relative dielectric constant and a low dielectric loss tangent and excellent in heat resistance, rigidity and impact resistance, and an antenna member made of such a resin composition at low cost.

[0016] When polystyrene resin is compounded into general-purpose polycarbonate resin, dielectric loss tangent becomes low, but impact resistance deteriorates significantly. Therefore, elastomer is added thereto to improve impact resistance, but there is a problem that excessive addition thereof leads to deterioration in strength, rigidity and heat resistance.

[0017] Solutions for solving problems

[0018] The present inventors have conducted intensive studies to solve the above problems and have found that a specific polycarbonate resin composition obtained by blending a polystyrene resin (B) and an elastomer (C) with a polycarbonate resin (A) can solve the above problems, thereby completing the present invention.

[0019] The present invention relates to the following polycarbonate resin composition and antenna member.

[0020] 1. A polycarbonate resin composition comprising 30 to 150 parts by mass of a polystyrene resin (B) and 3 to 60 parts by mass of an elastomer (C) relative to 100 parts by mass of a polycarbonate resin (A),

[0021] The polycarbonate resin (A) and the polystyrene resin (B) are heated at 260°C and 1216 sec. -1 The melt viscosity ratio (ηA / ηB) is in the range of 4.5 to 12.5.

[0022] 2. The polycarbonate resin composition according to 1, wherein the elastomer (C) is one or more selected from butadiene / methyl (meth)acrylate copolymers, butadiene / methyl (meth)acrylate / styrene copolymers and styrene / ethylene / butylene / styrene copolymers.

[0023] 3. The polycarbonate resin composition according to 1 or 2, wherein the dielectric loss tangent at a frequency of 5.8 GHz is 0.0040 or less.

[0024] 4. The polycarbonate resin composition according to any one of 1 to 3, wherein the content ratio of the polystyrene resin (B) to the elastomer (C) [(B) / (C)] is 9 or less.

[0025] 5. The polycarbonate resin composition according to any one of 1 to 4, which does not contain an acrylonitrile-butadiene-styrene copolymer, or when containing an acrylonitrile-butadiene-styrene copolymer, the content of the acrylonitrile-butadiene-styrene copolymer is 10 parts by mass or less relative to 100 parts by mass of the polycarbonate resin (A).

[0026] 6. A molded article of the polycarbonate resin composition according to any one of 1 to 5.

[0027] 7. An antenna component which uses electromagnetic waves with a frequency of 1 GHz or more, and is made of a polycarbonate resin composition having a dielectric loss tangent of 0.0040 or less at a frequency of 5.8 GHz and containing 30 to 150 parts by mass of a polystyrene resin (B) and 3 to 60 parts by mass of an elastomer (C) per 100 parts by mass of a polycarbonate resin (A).

[0028] 8. The antenna member according to 7, wherein the elastomer (C) is one or more selected from butadiene / methyl (meth)acrylate copolymers, butadiene / methyl (meth)acrylate / styrene copolymers, and styrene / ethylene / butylene / styrene copolymers.

[0029] 9. The antenna member according to 7 or 8, wherein the polycarbonate resin composition has a content ratio [(B) / (C)] of the polystyrene-based resin (B) to the elastomer (C) of 9 or less.

[0030] 10. The antenna member according to any one of 7 to 9, wherein the acrylonitrile-butadiene-styrene copolymer is not contained, or when the acrylonitrile-butadiene-styrene copolymer is contained, the content of the acrylonitrile-butadiene-styrene copolymer is 10 parts by mass or less based on 100 parts by mass of the polycarbonate resin (A).

[0031] Effects of the Invention

[0032] The polycarbonate resin composition of the present invention is low in cost, excellent in impact resistance, toughness, rigidity and heat resistance, has both low relative permittivity and low dielectric loss tangent, and has small transmission attenuation of electromagnetic waves. Therefore, the polycarbonate resin composition is suitable as an electronic and electrical equipment component that can even cope with high-frequency bands such as 5G or 6G, especially an antenna substrate or a radome, and can be particularly suitable for use as an antenna component using electromagnetic waves with a frequency of 1 GHz or more, and enables the reliability of electromagnetic waves to be fully ensured. DETAILED DESCRIPTION

[0033] Hereinafter, the present invention will be described in detail by showing embodiments or examples.

[0034] In the present specification, unless otherwise particularly described, “to” is used to mean that the numerical values ​​described before and after it are included as the lower limit value and the upper limit value.

[0035] [1] A polycarbonate resin composition comprising 30 to 150 parts by mass of a polystyrene resin (B) and 3 to 60 parts by mass of an elastomer (C) relative to 100 parts by mass of a polycarbonate resin (A);

[0036] The polycarbonate resin (A) and the polystyrene resin (B) are heated at 260°C and 1216 sec. -1 The melt viscosity ratio (ηA / ηB) is in the range of 4.5 to 12.5.

[0037] Hereinafter, each component and the like used in and constituting the polycarbonate resin composition of the present invention will be described in detail.

[0038] [Polycarbonate resin (A)]

[0039] The specific type of polycarbonate resin is not particularly limited, and examples thereof include polycarbonate polymers obtained by reacting dihydroxy compounds with carbonate precursors. At this time, in addition to dihydroxy compounds and carbonate precursors, polyhydroxy compounds and the like can also be reacted. In addition, a method in which carbon dioxide is used as a carbonate precursor and reacted with a cyclic ether can also be used. In addition, the polycarbonate polymer can be linear or branched. In addition, the polycarbonate polymer can be a homopolymer consisting of a repeating unit or a copolymer having two or more repeating units. At this time, as a copolymer, various copolymerization forms such as random copolymers and block copolymers can be selected. Usually, such polycarbonate polymers become thermoplastic resins.

[0040] In addition, polycarbonate resins can be classified into aromatic polycarbonate resins in which the carbons directly bonded to the carbonic acid bonds are each aromatic carbons and aliphatic polycarbonate resins in which the carbons are aliphatic carbons, and any polycarbonate resins can also be used. Among them, aromatic polycarbonate resins are preferred from the viewpoints of heat resistance, mechanical properties, electrical properties, etc.

[0041] Among monomers used as a raw material for the aromatic polycarbonate resin, examples of the aromatic dihydroxy compound include:

[0042] Dihydroxybenzenes, such as 1,2-dihydroxybenzene, 1,3-dihydroxybenzene (i.e., resorcinol), and 1,4-dihydroxybenzene;

[0043] Dihydroxybiphenyls, such as 2,5-dihydroxybiphenyl, 2,2'-dihydroxybiphenyl and 4,4'-dihydroxybiphenyl;

[0044] dihydroxynaphthalenes, such as 2,2'-dihydroxy-1,1'-binaphthyl, 1,2-dihydroxynaphthalene, 1,3-dihydroxynaphthalene, 2,3-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 2,6-dihydroxynaphthalene, 1,7-dihydroxynaphthalene and 2,7-dihydroxynaphthalene;

[0045] Dihydroxydiaryl ethers, such as 2,2'-dihydroxydiphenyl ether, 3,3'-dihydroxydiphenyl ether, 4,4'-dihydroxydiphenyl ether, 4,4'-dihydroxy-3,3'-dimethyldiphenyl ether, 1,4-bis(3-hydroxyphenoxy)benzene and 1,3-bis(4-hydroxyphenoxy)benzene;

[0046] Bis(hydroxyaryl)alkanes, such as 2,2-bis(4-hydroxyphenyl)propane (i.e. bisphenol A),

[0047] 1,1-bis(4-hydroxyphenyl)propane,

[0048] α,α'-bis(4-hydroxyphenyl)-1,4-diisopropylbenzene,

[0049] 1,3-Bis[2-(4-hydroxyphenyl)-2-propyl]benzene,

[0050] Bis(4-hydroxyphenyl)methane,

[0051] Bis(4-hydroxyphenyl)cyclohexylmethane,

[0052] Bis(4-hydroxyphenyl)phenylmethane,

[0053] Bis(4-hydroxyphenyl)(4-propenylphenyl)methane,

[0054] Bis(4-hydroxyphenyl)diphenylmethane,

[0055] Bis(4-hydroxyphenyl)naphthalene methane,

[0056] 1,1-Bis(4-hydroxyphenyl)ethane,

[0057] 1,1-bis(4-hydroxyphenyl)-1-phenylethane (i.e. bisphenol AP),

[0058] 1,1-Bis(4-hydroxyphenyl)-1-naphthaleneethane,

[0059] 1,1-bis(4-hydroxyphenyl)butane,

[0060] 2,2-bis(4-hydroxyphenyl)butane,

[0061] 2,2-Bis(4-hydroxyphenyl)pentane,

[0062] 1,1-bis(4-hydroxyphenyl)hexane,

[0063] 2,2-Bis(4-hydroxyphenyl)hexane,

[0064] 1,1-Bis(4-hydroxyphenyl)octane,

[0065] 2,2-Bis(4-hydroxyphenyl)octane,

[0066] 4,4-bis(4-hydroxyphenyl)heptane,

[0067] 2,2-Bis(4-hydroxyphenyl)nonane,

[0068] 1,1-Bis(4-hydroxyphenyl)decane and

[0069] 1,1-Bis(4-hydroxyphenyl)dodecane;

[0070] Bisphenols containing cardo structure, such as 9,9-bis(4-hydroxyphenyl)fluorene and 9,9-bis(4-hydroxy-3-methylphenyl)fluorene;

[0071] Dihydroxy diaryl sulfides, such as 4,4'-dihydroxy diphenyl sulfide and 4,4'-dihydroxy-3,3'-dimethyl diphenyl sulfide;

[0072] Dihydroxydiaryl sulfoxides, such as 4,4'-dihydroxydiphenyl sulfoxide and 4,4'-dihydroxy-3,3'-dimethyldiphenyl sulfoxide; and

[0073] Dihydroxydiaryl sulfones, such as 4,4'-dihydroxydiphenyl sulfone and 4,4'-dihydroxy-3,3'-dimethyldiphenyl sulfone; etc.

[0074] Among them, from the viewpoint of impact resistance and heat resistance, bis(hydroxyaryl)alkanes are preferred, bis(4-hydroxyphenyl)alkanes are more preferred, and 2,2-bis(4-hydroxyphenyl)propane (ie, bisphenol A) is particularly preferred.

[0075] The aromatic dihydroxy compound may be used alone, or two or more thereof may be used in any combination and in any ratio.

[0076] Among monomers used as a raw material of the aromatic polycarbonate resin, as examples of carbonate precursors, carbonyl halides and carbonates are used. The carbonate precursors may be used alone, or two or more thereof may be used in any combination and in any ratio.

[0077] Specific examples of the carbonyl halide include phosgene, and halogenated formats such as bischloroformate of a dihydroxy compound and monochloroformate of a dihydroxy compound.

[0078] Specific examples of carbonates include diaryl carbonates such as diphenyl carbonate and ditolyl carbonate; dialkyl carbonates such as dimethyl carbonate and diethyl carbonate; dicarbonates of dihydroxy compounds, monocarbonates of dihydroxy compounds, carbonates of dihydroxy compounds (such as cyclic carbonates), and the like.

[0079] The method for producing the polycarbonate resin is not particularly limited, and any method may be employed. Examples thereof include interfacial polymerization, melt transesterification, pyridine method, ring-opening polymerization of cyclic carbonate compounds, and solid phase transesterification of prepolymers.

[0080] The molecular weight of the polycarbonate resin can be arbitrarily selected and determined, and the viscosity average molecular weight Mv is usually 10000 or more, preferably 14000 or more, more preferably 16000 or more, and usually 40000 or less, preferably 30000 or less. When the viscosity average molecular weight is made to be above the lower limit of the above range, the mechanical strength of the resin composition can be further improved. On the other hand, when the viscosity average molecular weight is made to be below the upper limit of the above range, the reduction of the fluidity of the resin composition can be suppressed and improved, and the resin composition can be easily formed by improving the forming processability.

[0081] Two or more polycarbonate resins having different viscosity average molecular weights may be mixed for use. In such a case, a polycarbonate resin having a viscosity average molecular weight outside the above-described suitable range may also be mixed.

[0082] The polycarbonate resin also preferably includes a high molecular weight polycarbonate resin, for example, a polycarbonate resin having a viscosity average molecular weight Mv of 50000 to 95000. The viscosity average molecular weight of the high molecular weight polycarbonate resin is more preferably 55000 or more, still more preferably 60000 or more, especially 61000 or more, and particularly 62000 or more, and is more preferably 90000 or less, still more preferably 85000 or less, still more preferably 80000 or less, particularly preferably 75000 or less, and particularly preferably 70000 or less.

[0083] When a high molecular weight polycarbonate resin is contained, the content of the high molecular weight polycarbonate resin in the polycarbonate resin is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 15% by mass or more. The upper limit is preferably 40% by mass or less, and more preferably 30% by mass or less.

[0084] In the present invention, the viscosity average molecular weight Mv of the polycarbonate resin means the viscosity formula of Schnell after obtaining the intrinsic viscosity [η] (unit: dl / g) at 25° C. using dichloromethane as a solvent and an Ubbelohde viscometer, that is, η=1.23×10 -4 Mv 0.83 Calculated value.

[0085] In addition, the intrinsic viscosity [η] refers to the specific viscosity [η] when measuring the concentration [C] (g / dl) of each solution. sp ] and then calculate the value using the following formula.

[0086]

[0087] The terminal hydroxyl concentration of polycarbonate resin is arbitrary, can be appropriately selected and determined, and is generally below 2000ppm, preferably below 1500ppm, more preferably below 1000ppm. This makes it possible to further improve the retention thermal stability and color tone of the resin combination of the present invention. In addition, particularly in the polycarbonate resin manufactured by the melt transesterification method, the lower limit is generally more than 10ppm, preferably more than 30ppm, more preferably more than 40ppm. This makes it possible to suppress the reduction of molecular weight, and further improve the mechanical properties of the resin combination of the present invention.

[0088] The unit of the terminal hydroxyl concentration is the unit of the terminal hydroxyl mass relative to the mass of the polycarbonate resin, and is expressed in ppm. The measurement method is a colorimetric quantitative method using the titanium tetrachloride / acetic acid method (the method described in Macromol. Chem. 88 215 (1965)).

[0089] In addition, the polycarbonate resin may contain a polycarbonate oligomer to improve the appearance or fluidity of the molded article. The viscosity average molecular weight Mv of the polycarbonate oligomer is generally 1500 or more, preferably 2000 or more, and generally 9500 or less, preferably 9000 or less. In addition, the content of the polycarbonate oligomer is preferably set to less than 30% by mass of the polycarbonate resin (containing the polycarbonate oligomer).

[0090] In addition to virgin resin, the polycarbonate resin may be a polycarbonate resin regenerated from a used product (so-called material-recycled polycarbonate resin) or a polycarbonate resin manufactured from a polycarbonate resin that has been chemically decomposed and restored to a raw material (so-called chemically recycled polycarbonate resin), preferably containing both virgin resin and recycled resin, and may be composed of recycled polycarbonate resin. In the case of containing recycled polycarbonate resin, the proportion of recycled polycarbonate resin in the polycarbonate resin is preferably 40% or more, 50% or more, 60% or more, or 80% or more, and the proportion of recycled polycarbonate resin is also preferably 100%.

[0091] Polycarbonate resin (A) at 260°C and 1216 cm -1 The melt viscosity (ηA) under 100 to 2000 Pa·s is preferably within the range of 100 to 2000 Pa·s. By making the viscosity difference between the polycarbonate resin (A) and the polystyrene resin (B) closer, the melt viscosity ratio (ηA / ηB) of the polycarbonate resin (A) to the polystyrene resin (B) is within the range of 4.5 to 12.5, and in order to maintain toughness, the melt viscosity is more preferably 400 Pa·s or more, more preferably 500 Pa·s or more, and particularly preferably 600 Pa·s or more. In addition, the melt viscosity is more preferably 1500 Pa·s or less, more preferably 1250 Pa·s or less, and particularly preferably 1000 Pa·s or less.

[0092] [Polystyrene resin (B)]

[0093] The polycarbonate resin composition of the present invention contains 30 to 150 parts by mass of the polystyrene resin (B) based on 100 parts by mass of the polycarbonate resin (A).

[0094] The polystyrene resin is preferably a styrene homopolymer, but may be a resin obtained by copolymerizing other aromatic vinyl monomers such as α-methylstyrene, p-methylstyrene, vinyltoluene or vinylxylene to, for example, less than 50% by mass.

[0095] In addition, the polystyrene resin may be a rubber-reinforced polystyrene resin. The rubber-reinforced polystyrene resin is preferably a polystyrene resin in which a butadiene rubber component is copolymerized or compounded, and the amount of the butadiene rubber component is generally 1% by mass or more and less than 50% by mass, preferably 3 to 40% by mass, more preferably 5 to 30% by mass, and even more preferably 5 to 20% by mass. The rubber-reinforced polystyrene resin is particularly preferably a high-impact polystyrene (HIPS).

[0096] The polystyrene-based resin is particularly preferably a styrene homopolymer, a high-impact polystyrene or a mixture thereof.

[0097] The content of the polystyrene resin (B) is 30 to 150 parts by mass, preferably 40 parts by mass or more, more preferably 50 parts by mass or more, even more preferably 60 parts by mass or more, particularly preferably 70 parts by mass or more, and is preferably 140 parts by mass or less, more preferably 130 parts by mass or less, even more preferably 120 parts by mass or less, especially 110 parts by mass or less, 100 parts by mass or less, or 95 parts by mass or less, particularly preferably 90 parts by mass or less, relative to 100 parts by mass of the polycarbonate resin (A).

[0098] However, copolymers containing acrylonitrile such as acrylonitrile-butadiene-styrene copolymer (ABS resin) tend to increase dielectric loss tangent, and therefore are preferably not contained. Even in the case of containing a copolymer containing acrylonitrile, the amount thereof is preferably 10 parts by mass or less, more preferably 7 parts by mass or less, and even more preferably 5 parts by mass or less, 3 parts by mass or less, 2 parts by mass or less, or 1 part by mass or less relative to 100 parts by mass of the polycarbonate resin (A).

[0099] Polystyrene resin (B) at 260℃ and 1216cm -1 The melt viscosity (ηB) is preferably in the range of 30 to 300 Pa·s, more preferably 40 Pa·s or more, even more preferably 50 Pa·s or more, and particularly preferably 60 Pa·s or more. In addition, the melt viscosity (ηB) is more preferably 250 Pa·s or less, even more preferably 200 Pa·s or less, and particularly preferably 150 Pa·s or less.

[0100] In the present invention, at 260°C and 1216sec -1Under the above conditions, the melt viscosity ratio (ηA / ηB) of the melt viscosity ηA of the polycarbonate resin (A) to the melt viscosity ηB of the polystyrene resin (B) is in the range of 4.5 to 12.5. When the melt viscosity ratio is within such a range by reducing the melt viscosity difference between the polycarbonate resin (A) and the polystyrene resin (B), the compatibility of the two is improved, and the impact resistance can be improved.

[0101] ηA / ηB is preferably 6.0 or more, more preferably 7.0 or more, still more preferably 8.0 or more, particularly preferably 9.0 or more, and is preferably 12.0 or less, more preferably 11.5 or less, still more preferably 11.0 or less, particularly preferably 10.5 or less.

[0102] Polycarbonate resin (A) and polystyrene resin (B) at 260°C and 1216 sec -1 The melt viscosity below is a value measured using a capillary rheometer according to ISO 11443. Specifically, the melt viscosity can be calculated from the stress generated when a piston is pressed into a furnace having an inner diameter of 9.55 mm heated to 260° C. at a speed of 100 mm / min using an orifice having a capillary diameter of 1 mm and a capillary length of 10 mm.

[0103] [Elastomer (C)]

[0104] As the elastomer, a copolymer obtained by graft copolymerization of a rubber component and a monomer component copolymerizable with the rubber component is preferred. The production method of such a graft copolymer may be any of production methods such as bulk polymerization, solution polymerization, suspension polymerization and emulsion polymerization, and the copolymerization method may be single-stage grafting or multi-stage grafting.

[0105] For the rubber component, the glass transition temperature is usually 0°C or less, in particular, preferably -20°C or less, and more preferably -30°C or less. Specific examples of the rubber component include polybutadiene rubber, polyisoprene rubber or its hydride, butadiene-acrylic composite rubber, styrene-butadiene rubber, ethylene-α-olefin rubber such as ethylene-propylene rubber, ethylene-butene rubber, ethylene-octene rubber and ethylene-acrylic rubber, etc. These can be used alone, or two or more thereof can be mixed and used. Among them, polybutadiene rubber, polyisoprene rubber and its hydride, styrene-butadiene rubber are preferred.

[0106] The rubber component is preferably not a polyalkyl acrylate rubber such as polybutyl acrylate, poly(2-ethylhexyl acrylate) or a butyl acrylate / 2-ethylhexyl acrylate copolymer, or a silicone-based rubber such as an organopolysiloxane rubber, because dielectric loss tangent may increase.

[0107] Specific examples of the monomer components that can be graft-copolymerized with the rubber component include epoxy-containing (meth)acrylate compounds, such as aromatic vinyl compounds, vinyl cyanide compounds, (meth)acrylate compounds, (meth)acrylic acid compounds, and glycidyl (meth)acrylate; maleimide compounds, such as maleimide, N-methylmaleimide, and N-phenylmaleimide; and α,β-unsaturated carboxylic acid compounds such as maleic acid, phthalic acid, and itaconic acid, and their anhydrides (e.g., maleic anhydride, etc.). These monomer components can be used alone, or two or more thereof can be used in combination. Among them, aromatic vinyl compounds and (meth)acrylate compounds are preferred, and styrene, methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, cyclohexyl (meth)acrylate, and octyl (meth)acrylate, etc., can be preferably exemplified.

[0108] The elastomer is preferably a core / shell graft copolymer type elastomer. In particular, a core / shell graft copolymer consisting of a core layer containing at least one rubber component selected from a rubber containing polybutadiene, an ethylene / butene rubber and a rubber containing polybutyl acrylate and a shell layer formed by copolymerizing (meth) acrylate around the core layer is preferred, and a core / shell elastomer containing a butadiene-based rubber in the core is particularly preferred. In the core-shell graft copolymer, it is preferred to contain a rubber component of 40% by mass or more, and more preferably a rubber component of 60% by mass or more. In addition, it is preferred to contain a (meth) acrylic acid component of 10% by mass or more.

[0109] Preferred specific examples of these core / shell type graft copolymers preferably include butadiene / methyl (meth)acrylate copolymers (MB), butadiene / methyl (meth)acrylate / styrene copolymers (MBS), and styrene / ethylene / butylene / styrene copolymers (SEBS), and the like, and butadiene / methyl (meth)acrylate copolymers (MB), butadiene / methyl (meth)acrylate / styrene copolymers (MBS) and styrene / ethylene / butylene / styrene copolymers (SEBS) are more preferred.

[0110] The content of the elastomer (C) is 3 to 60 parts by mass relative to 100 parts by mass of the polycarbonate resin (A). When such an amount of elastomer is contained, the impact resistance, rigidity and heat resistance of the polycarbonate resin composition, as well as the relative dielectric constant and dielectric loss tangent can be well balanced. The content of the elastomer (C) is preferably 5 parts by mass or more, more preferably 7.5 parts by mass or more, even more preferably 10 parts by mass or more, particularly preferably 15 parts by mass or more, and preferably 55 parts by mass or less, more preferably 50 parts by mass or less, even more preferably 45 parts by mass or less, 40 parts by mass or less, 35 parts by mass or less or 30 parts by mass or less, particularly preferably 25 parts by mass or less.

[0111] The ratio of the content of the polystyrene resin (B) to the content of the elastomer (C) in the polycarbonate resin composition [content of the polystyrene resin (B) / content of the elastomer (C)] is preferably 9 or less because the notched Charpy impact strength value becomes higher.

[0112] [Stabilizer]

[0113] The polycarbonate resin composition of the present invention preferably contains a stabilizer, and the stabilizer is preferably a phosphorus stabilizer (heat stabilizer) or a phenol stabilizer (antioxidant).

[0114] As the phosphorus stabilizer, any known stabilizer can be used. Specific examples thereof include phosphorus oxygen acids such as phosphoric acid, phosphonic acid, phosphorous acid, phosphinic acid and polyphosphoric acid; acid pyrophosphate metal salts such as sodium acid pyrophosphate, potassium acid pyrophosphate and calcium acid pyrophosphate; phosphates of Group 1 or Group 2B metals such as potassium phosphate, sodium phosphate, cesium phosphate and zinc phosphate; organic phosphate compounds, organic phosphite compounds, and organic phosphite compounds, etc., and organic phosphite compounds are particularly preferred.

[0115] Examples of the organic phosphite compounds include triphenyl phosphite, tris(mononylphenyl) phosphite, tris(mononyl / dinonylphenyl) phosphite, tris(2,4-di-tert-butylphenyl) phosphite, monooctyl diphenyl phosphite, dioctyl monophenyl phosphite, monodecyl diphenyl phosphite, didecyl monophenyl phosphite, tridecyl phosphite, trilauryl phosphite, tristearyl phosphite, and 2,2-methylenebis(4,6-di-tert-butylphenyl)octyl phosphite, and the like.

[0116] Specific examples of these organic phosphite compounds include "ADK STAB 1178", "ADK STAB 2112" and "ADK STAB HP-10" manufactured by Adeka Corporation, "JP-351", "JP-360" and "JP-3CP" manufactured by Johoku Chemical Co., Ltd., and "IRGAFOS 168" manufactured by BASF.

[0117] One type of phosphorus-based stabilizer may be contained, or two or more types of phosphorus-based stabilizers may be contained in any combination and ratio.

[0118] The content of the phosphorus stabilizer is preferably 0.01 parts by mass or more, more preferably 0.03 parts by mass or more, and is usually 1 part by mass or less, preferably 0.7 parts by mass or less, and more preferably 0.5 parts by mass or less, relative to 100 parts by mass of the polycarbonate resin (A). In the case where the content of the phosphorus stabilizer is less than the lower limit of the above range, there is a possibility that the thermal stabilization effect may become insufficient, and in the case where the content of the phosphorus stabilizer is greater than the upper limit of the above range, there is a possibility that the effect may reach the upper limit and the inclusion of the phosphorus stabilizer may become uneconomical.

[0119] Examples of phenolic stabilizers include hindered phenolic antioxidants. Specific examples thereof include pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, thiodiethylenebis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], N,N'-hexane-1,6-diylbis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionamide], 2,4-dimethyl-6-(1-methylpentadecyl)phenol, diethyl[[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl]methyl]phosphonate, 3,3',3",5,5',5"-hexa-tert-butyl-a,a',a"-(mesitylene-2, 4,6-tolyl) tri-p-cresol, 4,6-bis(octylthiomethyl)-o-cresol, ethylenebis(oxyethylene)bis[3-(5-tert-butyl-4-hydroxy-m-tolyl)propionate], hexamethylenebis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, 2,6-di-tert-butyl-4-(4,6-bis(octylthio)-1,3,5-triazine-2-ylamino)phenol, and 2-[1-(2-hydroxy-3,5-di-tert-pentylphenyl)ethyl]-4,6-di-tert-pentylphenyl acrylate, etc.

[0120] Among them, pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] and octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate are preferred. Specific examples of these phenolic antioxidants include "IRGANOX 1010" and "IRGANOX 1076" manufactured by BASF, and "ADK STAB AO-50" and "ADK STAB AO-60" manufactured by Adeka Corporation.

[0121] One phenolic stabilizer may be contained, or two or more phenolic stabilizers may be contained in any combination and ratio.

[0122] The content of the phenolic stabilizer is preferably 0.01 parts by mass or more, and is usually 1 part by mass or less, preferably 0.5 parts by mass or less relative to 100 parts by mass of the polycarbonate resin (A). When the content of the phenolic stabilizer is made to be above the lower limit of the above range, the effect of the phenolic stabilizer can be fully obtained. In addition, when the content of the phenolic stabilizer exceeds the upper limit of the above range, the effect reaches the upper limit, and containing the phenolic stabilizer becomes uneconomical.

[0123] [Release agent]

[0124] The polycarbonate resin composition of the present invention preferably contains a mold release agent. Examples of the mold release agent include aliphatic carboxylic acids, esters of aliphatic carboxylic acids and alcohols, aliphatic hydrocarbon compounds having a number average molecular weight of 200 to 15,000, and polysiloxane-based silicone oils.

[0125] The example of aliphatic carboxylic acid includes saturated or unsaturated aliphatic monocarboxylic acid, dicarboxylic acid or tricarboxylic acid. Here, aliphatic carboxylic acid also includes alicyclic carboxylic acid. Wherein, preferred aliphatic carboxylic acid is monocarboxylic acid or dicarboxylic acid with carbon number 6 to 36, and aliphatic saturated monocarboxylic acid with carbon number 6 to 36 is more preferred. The specific example of such aliphatic carboxylic acid includes palmitic acid, stearic acid, caproic acid, capric acid, lauric acid, arachidic acid, behenic acid, lignoceric acid, cerotic acid, melissic acid, tritriacontanoic acid, montanic acid, adipic acid and azelaic acid etc.

[0126] As the aliphatic carboxylic acid in the ester of aliphatic carboxylic acid and alcohol, for example, the same carboxylic acid as the above-mentioned aliphatic carboxylic acid can be used. On the other hand, examples of alcohols include saturated or unsaturated monohydric alcohols or polyhydric alcohols. These alcohols may have substituents such as fluorine atoms or aromatic groups. Among them, monohydric saturated alcohols or polyhydric saturated alcohols having a carbon number of 30 or less are preferred, and aliphatic saturated monohydric alcohols or aliphatic saturated polyhydric alcohols having a carbon number of 30 or less are more preferred. Here, aliphatic is used as a term that also includes alicyclic compounds.

[0127] Specific examples of such alcohols include octanol, decanol, dodecanol, stearyl alcohol, behenyl alcohol, ethylene glycol, diethylene glycol, glycerin, pentaerythritol, 2,2-dihydroxyperfluoropropanol, neopentyl glycol, di(trimethylol)propane, dipentaerythritol, and the like.

[0128] The ester may contain aliphatic carboxylic acid and / or alcohol as impurities. In addition, the ester may be a pure substance or a mixture of multiple compounds. In addition, the aliphatic carboxylic acid and alcohol that are bonded to each other and constitute an ester may be used alone, or two or more thereof may be used in any combination and ratio.

[0129] Specific examples of the esters of aliphatic carboxylic acids and alcohols include beeswax (a mixture containing myricyl palmitate as a main component), stearyl stearate, behenyl behenate, stearyl behenate, glyceryl monopalmitate, glyceryl monostearate, glyceryl distearate, glyceryl tristearate, pentaerythritol monopalmitate, pentaerythritol monostearate, pentaerythritol distearate, pentaerythritol tristearate, pentaerythritol tetrastearate and the like.

[0130] Examples of aliphatic hydrocarbons having a number average molecular weight of 200 to 15000 include liquid paraffin, paraffin, microcrystalline wax, polyethylene wax, Fischer-Tropsch wax, and α-olefin oligomers having 3 to 12 carbon atoms, etc. Here, aliphatic hydrocarbons also include alicyclic hydrocarbons. In addition, these hydrocarbons may be partially oxidized.

[0131] Among them, paraffin wax, polyethylene wax or a partial oxide of polyethylene wax is preferred, and paraffin wax and polyethylene wax are more preferred.

[0132] In addition, the number average molecular weight of the aliphatic hydrocarbon is preferably 5,000 or less.

[0133] The aliphatic hydrocarbon may be a single substance, and may be used even when the aliphatic hydrocarbon is a mixture of substances having various constituent components or molecular weights, as long as the main component is within the above range.

[0134] Examples of the polysiloxane-based silicone oil include dimethyl silicone oil, methylphenyl silicone oil, diphenyl silicone oil, fluorinated alkyl silicone oil, and the like.

[0135] The above-mentioned release agents may be contained alone, or two or more thereof may be contained in any combination and ratio.

[0136] The content of the release agent is usually 0.001 parts by mass or more, preferably 0.01 parts by mass or more, and usually 2 parts by mass or less, preferably 1 part by mass or less, relative to 100 parts by mass of the polycarbonate resin (A). When the content of the release agent is lower than the lower limit of the above range, there is a case where the demolding effect is insufficient. When the content of the release agent exceeds the upper limit of the above range, there is a possibility that the degradation of hydrolysis resistance or mold contamination during injection molding may be caused.

[0137] [Additives, etc.]

[0138] The polycarbonate resin composition may contain other additives in addition to the above components, for example, additives such as ultraviolet absorbers, fillers, reinforcing materials (carbon fibers or glass fibers), pigments, dyes, flame retardants, antistatic agents, plasticizers or compatibilizers, or other resins in addition to the polycarbonate resin (A) and the polystyrene resin (B). One or more of these additives or other resins may be compounded.

[0139] When other resins other than the polycarbonate resin (A) and the polystyrene resin (B) are contained, the content thereof is preferably set to 40 parts by mass or less, more preferably set to 30 parts by mass or less, still more preferably set to 20 parts by mass or less or 10 parts by mass or less, and particularly preferably set to 5 parts by mass or less, relative to 100 parts by mass of the polycarbonate resin (A).

[0140] [Method for producing polycarbonate resin composition]

[0141] The method for producing the polycarbonate resin composition is not limited, and a known method for producing the polycarbonate resin composition can be widely adopted, and the following method is exemplified, in which each essential component and other components compounded as needed are pre-mixed using various mixers such as a tumbler or a Henschel mixer, and then melt-kneaded using a mixer such as a Banbury mixer, a roll, a Brabender, a single-screw extruder, a twin-screw extruder or a kneader. The temperature of the melt-kneading is not particularly limited, but is generally in the range of 240° C. to 320° C.

[0142] The pellets obtained by granulating the polycarbonate resin composition are shaped by various molding methods to produce a molded product. Alternatively, the resin melt-kneaded using an extruder may be directly shaped without producing pellets to produce a molded product.

[0143] As a method for manufacturing a molded product, any molding method commonly used for a polycarbonate resin composition can be used. Examples thereof include injection molding, ultra-high-speed injection molding, injection compression molding, two-color molding, hollow molding such as gas-assisted molding, molding using an insulating mold, molding using a rapid heating mold, foam molding (including supercritical fluid), insert molding, IMC (in-mold coating molding), extrusion molding, sheet molding, thermoforming, rotational molding, lamination molding, press molding, and blow molding. In addition, a molding method using a hot runner method can also be used.

[0144] Among them, injection molding methods such as injection molding method, ultra-high speed injection molding method and injection compression molding method are preferable.

[0145] In addition, a hard coating layer may be provided on the surface of the molded product. As a hard coating agent for forming the hard coating layer, a known material may be appropriately used, and various hard coating agents may be used, such as a silicone hard coating agent, an acrylic hard coating agent, a silazane hard coating agent, and a polyurethane hard coating agent. The hard coating agent may be a double coating type hard coating agent, in which a primer layer is provided before applying the hard coating agent to improve adhesion or weather resistance. The coating method of the hard coating agent is not particularly limited, and may also be applied by any coating method such as spray coating, dip coating, flow coating, spin coating, rod coating, curtain coating, die coating, gravure coating, roller coating, blade coating, or air knife coating.

[0146] The thickness of the hard coat layer is preferably 1 to 50 μm, more preferably 5 to 30 μm.

[0147] The polycarbonate resin composition of the present invention has a small dielectric loss tangent, and the dielectric loss tangent at a frequency of 5.8 GHz is preferably 0.0040 or less, more preferably 0.0038 or less, still more preferably 0.0036 or less, particularly preferably 0.0034 or less.

[0148] In addition, the polycarbonate resin composition of the present invention also has a small relative dielectric constant, and the relative dielectric constant is preferably 2.8 or less, more preferably 2.7 or less, and still more preferably 2.6 or less.

[0149] Details of specific methods for measuring dielectric loss tangent and relative permittivity are described in the Examples.

[0150] The polycarbonate resin composition of the present invention has excellent heat resistance, and the load deflection temperature used as an indicator thereof is preferably higher than 86° C., more preferably higher than 90° C., and still more preferably higher than 92° C. The load deflection temperature is measured according to ISO 75-2, and the details of its specific measurement method are as described in the Examples.

[0151] The polycarbonate resin composition of the present invention has excellent impact resistance, and the Charpy impact strength is preferably NB (no break) in the case of no notch or 10 kJ / m in the case of notch. 2 The Charpy impact strength is measured according to ISO 179-1 and 2, and the details of the specific measurement method thereof are as described in the Examples.

[0152] The polycarbonate resin composition of the present invention has excellent rigidity, and preferably has a flexural modulus of 2000 MPa or more and a flexural strength of 67 MPa or more. The flexural modulus and flexural strength are measured according to ISO 178, and the details of the specific measurement method thereof are as described in the Examples.

[0153] In addition, the polycarbonate resin composition of the present invention has excellent toughness, and the tensile break nominal strain is preferably 20% or more. The tensile break nominal strain is measured according to ISO 527, and the details of its specific measurement method are described in the Examples.

[0154] The polycarbonate resin composition of the present invention is particularly preferably suitable for use in electronic and electrical equipment components using electromagnetic waves with a frequency of 1 GHz or more. The electronic and electrical equipment components composed of the polycarbonate resin composition of the present invention can be used in a wide range of frequency bands with a frequency of 1 GHz or more. Electronic and electrical equipment components can be applied to frequency bands up to 52.6 GHz as the 5G radio communication standard "NR", frequency bands up to about 90 GHz being studied for future 5G evolution, or sub-terahertz waves of 90G to 300 GHz for 6G. Of course, electronic and electrical equipment components are also applicable to existing low-frequency bands or frequency bands of 10 to 20 GHz as 6G low-frequency bands / mid-frequency bands.

[0155] Examples of electronic and electrical equipment parts to which the molded articles of the polycarbonate resin composition of the present invention can be used include parts for electronic and electrical equipment frames, circuit boards, semiconductor interlayer insulating films, antenna parts (substrates, radomes, and radomes), insulating materials for high-frequency coaxial cables, resistors, basic parts such as switches, capacitors, and photoelectric sensors, IC sockets and connectors, transportation equipment such as automobiles, bicycles, motorcycles, trucks, railway vehicles, helicopters, and airplanes, construction machinery such as bulldozers, hydraulic excavators, and cranes, ships such as merchant ships, special-purpose ships, fishing boats, and naval vessels, agricultural machinery such as tractors and harvesters, smartphones, tablet computers, wearable devices, computers, television receivers, VR glasses, cameras, speakers, drones, robots, sensors, medical equipment, and analytical equipment, and the electronic and electrical equipment parts are particularly suitable as antenna substrates, radomes, and radomes.

[0156] The radome and radar cover are a housing or radome (radome) that accommodates or protects an antenna module that transmits or receives electromagnetic waves, and also include components that are arranged on the path of electromagnetic waves transmitted or received from the radar module.

[0157] [2] The antenna component of the second invention of the present application is an antenna component that uses electromagnetic waves with a frequency of 1 GHz or more, and is made of a polycarbonate resin composition having a dielectric loss tangent of 0.0040 or less at a frequency of 5.8 GHz and containing 30 to 150 parts by mass of a polystyrene resin (B) and 3 to 60 parts by mass of an elastomer (C) relative to 100 parts by mass of a polycarbonate resin (A).

[0158] Each component and the like constituting the polycarbonate resin composition used for the antenna member of the second invention will be described in detail below.

[0159] The polycarbonate resin (A) used in the resin composition of the antenna member of the second invention is the same as the polycarbonate resin (A) used in the resin composition of the first invention, and the preferred range including the content is also the same.

[0160] The polystyrene resin (B) used in the resin composition of the antenna member of the second invention is the same as the polystyrene resin (B) used in the resin composition of the first invention, and the preferred range including the content is also the same.

[0161] The elastomer (C) used in the resin composition of the antenna member of the second invention is the same as the elastomer (C) used in the resin composition of the first invention, and the preferred range including the content is also the same.

[0162] The resin composition for the antenna member of the second invention preferably contains a stabilizer. The stabilizer is the same as the stabilizer described in the resin composition of the first invention, and the preferred range including the content is also the same.

[0163] The resin composition for the antenna member of the second invention preferably contains a release agent. The release agent is the same as the release agent described in the resin composition of the first invention, and the preferred range including the content is also the same.

[0164] Other additives and resins that may be contained in the resin composition for the antenna member of the second invention are the same as those described for the resin composition of the first invention, and the preferred ranges including the content are also the same.

[0165] The method for producing the resin composition of the antenna member of the second invention is the same as the method for producing the resin composition of the first invention. In addition, the method for producing the molded product is the same as the method for producing the molded product of the first invention.

[0166] Furthermore, the same hard coating layer as described in the molded product of the first invention may be provided on the surface of the molded product.

[0167] The polycarbonate resin composition used in the second invention has a small dielectric loss tangent, and the dielectric loss tangent at a frequency of 5.8 GHz is preferably 0.0040 or less, more preferably 0.0038 or less, still more preferably 0.0036 or less, and particularly preferably 0.0034 or less. The relative dielectric constant of the polycarbonate resin composition used in the second invention is also small, and the relative dielectric constant is preferably 2.8 or less, more preferably 2.7 or less, and still more preferably 2.6 or less. The specific method for measuring the dielectric loss tangent and the relative dielectric constant is as described in the examples.

[0168] The polycarbonate resin composition used in the second invention has excellent heat resistance, and the load deflection temperature used as an indicator thereof is preferably higher than 86° C., more preferably higher than 90° C., and still more preferably higher than 92° C. The load deflection temperature is measured in accordance with ISO75-2, and the details of its specific measurement method are as described in the Examples.

[0169] The polycarbonate resin composition used in the second invention has excellent impact resistance, and the Charpy impact strength is preferably NB (no break) in the case of no notch or 10 kJ / m in the case of notch. 2 The Charpy impact strength is measured according to ISO 179-1 and 2, and the details of the specific measuring method thereof are as described in the Examples.

[0170] The polycarbonate resin composition used in the second invention has excellent rigidity, and preferably has a flexural modulus of 2000 MPa or more and a flexural strength of 67 MPa or more. The flexural modulus and flexural strength are measured according to ISO 178, and the details of the specific measurement methods are as described in the Examples.

[0171] Furthermore, the polycarbonate resin composition used in the second invention has excellent toughness, and the tensile nominal strain at break is preferably 20% or more. The tensile nominal strain at break is measured according to ISO 527, and the details of the specific measurement method thereof are as described in the Examples.

[0172] The molded article composed of the polycarbonate resin composition used in the second invention is used in an antenna component that uses electromagnetic waves with a frequency of 1 GHz or more. The antenna component of the present invention can be used in a wide range of frequency bands with a frequency of 1 GHz or more. The molded article can be applied to a frequency band of up to 52.6 GHz as the 5G radio communication standard "NR", a frequency band of up to about 90 GHz that is being studied for future 5G evolution, or a sub-terahertz wave of 90G to 300 GHz for 6G. Of course, the antenna component is also applicable to existing low-frequency bands or frequency bands of 10 to 20 GHz as 6G low-frequency bands / medium-frequency bands.

[0173] The antenna component of the second invention can be used as a component for sending or receiving electromagnetic waves with a frequency of more than 1 GHz, in particular, an antenna substrate, an antenna cover or a radar cover, and can be suitable for a shell or antenna cover (radar antenna cover) for accommodating or protecting an antenna module, as well as a component arranged on the path of electromagnetic waves sent or received from a radar module.

[0174] Furthermore, the same hard coating layer as described above may be provided on the surface of the antenna member of the present invention.

[0175] Example

[0176] Hereinafter, the first invention and the second invention (hereinafter, collectively referred to as "the present invention" in some cases) will be described more specifically using examples. However, these inventions should not be construed as being limited to the following examples.

[0177] The raw materials used in the following examples and comparative examples are shown in Table 1.

[0178] [Table 1]

[0179]

[0180] (Examples 1 to 19 of the first invention and comparative examples 1 to 4)

[0181] [Production of polycarbonate resin composition pellets]

[0182] The components shown in Table 1 were blended in the ratios (parts by mass) shown in Tables 2 to 4 below, mixed with a drum for 20 minutes, and then melt-kneaded at a drum temperature of 260° C. using a twin-screw extruder (manufactured by Shibaura Machine Co., Ltd., TEM26SX), and pellets of a polycarbonate resin composition were obtained by strand cutting.

[0183] <Relative dielectric constant and dielectric loss tangent>

[0184] The pellets obtained by the above method were dried at 100° C. for 5 hours, and a molded product of 100 mm×150 mm×about 2 mm thickness was obtained using an injection molding machine (ROBOSHOT S-2000i 150B manufactured by Fanuc Corporation). A 100 mm×1 mm×2 mm flat plate test piece was obtained by cutting from the flat plate test piece obtained by the above method, and the relative dielectric constant and dielectric loss tangent at a frequency of 5.8 GHz were measured by a perturbation method using a network analyzer manufactured by Keysight Technologies and a cavity resonator manufactured by Kanto Electronics Application and Development Co., Ltd.

[0185] <Flexural modulus and flexural strength>

[0186] The pellets obtained by the above method were dried at 100° C. for 5 hours, and then injection molded using a NEX80 III injection molding machine manufactured by Nissei Plastic Industrial Co., Ltd. under the conditions of a cylinder temperature of 260° C., a mold temperature of 80° C., and a molding cycle of 50 seconds to form an ISO multi-purpose test piece (4 mm thick). Using the obtained test piece, a bending test was performed at room temperature (23° C.) based on ISO-178 standard, and the bending modulus (unit: MPa) and the bending strength (unit: MPa) were measured.

[0187] <Charpy impact strength>

[0188] The pellets obtained by the above method were dried at 100° C. for 5 hours, and then injection molded using a NEX80 III injection molding machine manufactured by Nissei Plastic Industrial Co., Ltd. under the conditions of a barrel temperature of 260° C., a mold temperature of 80° C., and a molding cycle of 50 seconds, thereby preparing a 3 mm thick impact resistance test piece based on ISO 179-1 and 2. Using the obtained test piece, the Charpy impact strength (unit: kJ / m 2 ).

[0189] <Deflection Temperature under Load>

[0190] The pellets obtained by the above method were dried at 100° C. for 5 hours and then injection molded using a NEX80 III injection molding machine manufactured by Nissei Plastic Industrial Co., Ltd. under the conditions of a cylinder temperature of 260° C., a mold temperature of 80° C., and a molding cycle of 50 seconds to form an ISO multi-purpose test piece (4 mm thick). Using the obtained test piece and a 6A-2 HDT measuring instrument manufactured by Toyo Seiki Seisaku-Sho, Ltd., the load deflection temperature (unit: ° C.) was measured under high load (1.80 MPa) based on ISO 75-2.

[0191] <Tensile break nominal strain (unit: %)>

[0192] The pellets obtained by the above method were dried at 100° C. for 5 hours, and then injection molded using a NEX80 III injection molding machine manufactured by Nissei Plastic Industrial Co., Ltd. under the conditions of a cylinder temperature of 260° C., a mold temperature of 80° C., and a molding cycle of 50 seconds to form an ISO multi-purpose test piece (4 mm thick).

[0193] Using the obtained test piece, the tensile break nominal strain (unit: %) was measured in accordance with ISO 527 standard.

[0194] The above evaluation results are shown in Tables 2 to 4 below.

[0195] [Table 2]

[0196]

[0197] [Table 3]

[0198]

[0199] [Table 4]

[0200]

[0201] As can be clearly seen from the above results, the polycarbonate resin composition of the first invention has excellent mechanical properties (impact resistance, toughness, rigidity, heat resistance, etc.) and also has excellent electrical properties (relative dielectric constant and dielectric loss tangent). In contrast, in the case of the comparative example, results satisfying both mechanical properties and electrical properties were not obtained.

[0202] (Examples 20 to 33 of the second invention and comparative examples 5 to 9)

[0203] [Production of polycarbonate resin composition pellets]

[0204] The components shown in Table 1 were blended in the proportions (parts by mass) shown in Tables 5 to 7 below, mixed with a drum for 20 minutes, and then melt-kneaded at a drum temperature of 260° C. using a twin-screw extruder (manufactured by Shibaura Machine Co., Ltd., TEM26SX), and pellets of a polycarbonate resin composition were obtained by strand cutting.

[0205] The relative permittivity, dielectric loss tangent, flexural modulus, flexural strength, Charpy impact strength, and deflection temperature under load were measured in the same manner as described above.

[0206] The results are shown in Tables 5 to 7 below.

[0207] [Table 5]

[0208]

[0209] [Table 6]

[0210]

[0211] [Table 7]

[0212]

[0213] The antenna member of the present invention has excellent mechanical properties (impact resistance, rigidity, heat resistance, etc.) and also has excellent electrical properties (relative permittivity and dielectric loss tangent).

[0214] In contrast, in the case of the comparative example, it was not possible to obtain results satisfying both mechanical properties and electrical characteristics.

[0215] Industrial Applicability

[0216] The polycarbonate resin composition of the present invention has a low relative dielectric constant and a low dielectric loss tangent, has a reduced transmission attenuation, and is excellent in heat resistance, impact resistance, and rigidity, and can therefore be widely and appropriately used in various electronic and electrical equipment parts using electromagnetic waves. In addition, the antenna member of the present invention has both a low relative dielectric constant and a low dielectric loss tangent, has a reduced transmission attenuation, and is excellent in heat resistance, impact resistance, and rigidity, and can therefore be widely and appropriately used as various antenna members using electromagnetic waves with a frequency of 1 GHz or more.

Claims

1. A polycarbonate resin composition comprising 30 to 150 parts by mass of a polystyrene resin (B) and 3 to 60 parts by mass of an elastomer (C) relative to 100 parts by mass of a polycarbonate resin (A), wherein the polycarbonate resin (A) and the polystyrene resin (B) are heated at 260°C and 1216 sec. -1 The melt viscosity ratio (ηA / ηB) is in the range of 4.5 to 12.

5.

2. The polycarbonate resin composition according to claim 1, The elastomer (C) is one or more selected from butadiene / methyl (meth)acrylate copolymer, butadiene / methyl (meth)acrylate / styrene copolymer and styrene / ethylene / butylene / styrene copolymer.

3. The polycarbonate resin composition according to claim 1 or 2, The dielectric loss tangent at a frequency of 5.8 GHz is less than 0.0040.

4. The polycarbonate resin composition according to claim 1 or 2, The content ratio of the polystyrene resin (B) to the elastomer (C) [(B) / (C)] is 9 or less.

5. The polycarbonate resin composition according to claim 1 or 2, The acrylonitrile-butadiene-styrene copolymer is not contained, or when the acrylonitrile-butadiene-styrene copolymer is contained, the content of the acrylonitrile-butadiene-styrene copolymer is 10 parts by mass or less based on 100 parts by mass of the polycarbonate resin (A). 6 . A molded article of the polycarbonate resin composition according to claim 1 .

7. An antenna component, which uses electromagnetic waves with a frequency of 1 GHz or more, and is made of a polycarbonate resin composition having a dielectric loss tangent of 0.0040 or less at a frequency of 5.8 GHz and containing 30 to 150 parts by mass of a polystyrene resin (B) and 3 to 60 parts by mass of an elastomer (C) relative to 100 parts by mass of a polycarbonate resin (A).

8. The antenna member according to claim 7, The elastomer (C) is one or more selected from butadiene / methyl (meth)acrylate copolymer, butadiene / methyl (meth)acrylate / styrene copolymer and styrene / ethylene / butylene / styrene copolymer.

9. The antenna member according to claim 7 or 8, The polycarbonate resin composition has a content ratio [(B) / (C)] of the polystyrene resin (B) to the elastomer (C) of 9 or less.

10. The antenna member according to claim 7 or 8, The acrylonitrile-butadiene-styrene copolymer is not contained, or when the acrylonitrile-butadiene-styrene copolymer is contained, the content of the acrylonitrile-butadiene-styrene copolymer is 10 parts by mass or less based on 100 parts by mass of the polycarbonate resin (A).