Aluminum alloy foil and method for producing same

By adding an appropriate amount of Ca and Fe to the aluminum alloy foil and controlling the crystal particle size, the problem of insufficient etching accuracy and strength of the aluminum foil is solved, and a high-strength and difficult-to-break printed wiring substrate is realized, which is suitable for complex wiring patterns. etching.

CN118891384APending Publication Date: 2024-11-01TOYO ALUMINIUM KK
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202380026941.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-18
Filing Date
2023-03-09
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The etching accuracy and strength of the existing aluminum foil on the printed wiring substrate are insufficient, resulting in easy disconnection of wires after the wiring is refined, and the prior art has failed to effectively realize fine-wire etching without circuit breakage.

Method used

Aluminum alloy foil containing Ca and Fe was prepared by casting and cold rolling process, the Ca content was controlled at 1.0-4.5% and the Fe content was 0.02-1.3%, and other trace elements were added to the aluminum alloy, and the average crystal was measured using EBSD. The particle size is less than 12μm, which improves yield and tensile strength, and realizes a high-strength and not easy to break the wire.

Benefits of technology

Excellent fine wire etching of circuit wiring is achieved, reducing the risk of wire breakage, and maintaining high strength and ductility under heat treatment above 200°C, thereby improving the mechanical properties of printed wiring substrates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005038053210000081
    Figure BDA0005038053210000081
  • Figure BDA0005038053210000091
    Figure BDA0005038053210000091
  • Figure HDA0005038053220000011
    Figure HDA0005038053220000011
Patent Text Reader

Abstract

The purpose of the present invention is to provide an aluminum alloy foil for a printed wiring board, which is excellent in fine line etching of circuit wiring and is not susceptible to line breakage and has high strength. An aluminum alloy foil having a Ca content of 1.0% by mass or more but less than 4.5% by mass, an Fe content of 0.02% by mass or more but less than 1.3% by mass, and a remainder comprising Al and other trace elements is used as the aluminum alloy foil, and the surface of the aluminum alloy foil is used as an observation surface. The average crystal grain size measured by electron beam backscatter diffraction at a grain boundary orientation difference of 15 DEG or more may be 12 [mu] m or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an aluminum alloy foil and a method for producing the same. Background Art

[0002] Printed wiring boards have long been used in electrical and electronic equipment. Generally, aluminum foil or copper foil is used as the wiring material of printed wiring boards. For example, IC tags are installed in the wiring part to function as antenna circuits. The wiring pattern is becoming more complicated year by year, and it is necessary to make the wiring thinner.

[0003] However, the precision of etching wiring with aluminum foil is much lower than that with copper foil. The etched surface of aluminum foil tends to become uneven, and if the wiring is made thinner, it is easy to break during etching.

[0004] Most aluminum foils are made of pure aluminum 1000 series materials and aluminum-iron 8000 series materials. These materials are also used as wiring materials. In addition, aluminum foil for printed wiring boards can be easily bonded to the substrate by removing rolling oil by annealing after cold rolling. Annealing at a temperature of at least 200°C is required to remove the rolling oil, and the mechanical properties of the aluminum foil vary greatly due to the annealing.

[0005] Patent Document 1 discloses an aluminum foil that contains one or two of Ni (nickel), Zn (zinc), and Ga (gallium) and increases the potential difference between an intermetallic compound and a parent phase to have high chemical solubility and enable sharp etching.

[0006] Patent Document 2 discloses that an aluminum foil containing 1.0 to 1.8 wt % of Fe (iron) and 0.4 to 0.6 wt % of Mn (manganese) has a line edge surface having appropriate strength and excellent sharpness during etching.

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent Document 1: Japanese Patent Application Publication No. 2012-149289

[0010] Patent Document 2: Japanese Patent Application Publication No. 2001-152270 Summary of the invention

[0011] However, in recent years, it has become increasingly difficult to achieve the required wiring pattern of a printed wiring board with the conventional etching accuracy of aluminum foil. In addition, the strength of the annealed aluminum foil is low, and when the wiring is further thinned, there is a risk of disconnection due to external forces in subsequent processes or during use.

[0012] In addition, although Patent Documents 1 and 2 disclose that etching sharpness is improved, there is actually no description that etching can be used to thin the line without circuit disconnection. In addition, in Patent Document 2, although higher strength is obtained by adding Mn and fine precipitates, it is still necessary to further improve the strength in order to achieve thinning.

[0013] Therefore, an object of the present invention is to provide a high-strength aluminum alloy foil for a printed wiring board which is excellent in etching of fine lines of circuit wiring and is less likely to break.

[0014] That is, in order to solve the above-mentioned problems, the aluminum alloy foil of the invention has the following features [1] to [6].

[0015] [1] An aluminum alloy foil having a Ca (calcium) content of 1.0 mass % or more and less than 4.5 mass %, a Fe (iron) content of 0.02 mass % or more and less than 1.3 mass %, and the remainder comprising Al (aluminum) and other trace elements.

[0016] [2] The aluminum alloy foil according to [1], wherein the average crystal grain size measured by an EBSD (electron beam backscatter diffraction) method with a grain boundary orientation difference of 15° or more is 12 μm or less, with the aluminum alloy foil surface as the observation surface.

[0017] [3] The aluminum alloy foil according to [1], wherein the yield strength of the aluminum alloy foil is 70 N / mm 2 above.

[0018] [4] The aluminum alloy foil according to [3], wherein the aluminum alloy foil has a tensile strength of 110 N / mm 2 above.

[0019] [5] The aluminum alloy foil according to any one of [1] to [4], wherein the thickness of the aluminum alloy foil is 6 μm to 80 μm.

[0020] [6] A method for producing an aluminum alloy foil, comprising:

[0021] A step of obtaining an ingot of an aluminum alloy by casting a molten aluminum alloy having a Ca (calcium) content of 1.0 mass % or more and less than 4.5 mass %, a Fe (iron) content of 0.02 mass % or more and less than 1.3 mass %, and the remainder containing Al (aluminum) and other trace elements; and

[0022] A step of cold-rolling the ingot to obtain a cold-rolled aluminum alloy foil.

[0023] The aluminum alloy foil obtained in the present invention can provide a high-strength printed wiring board that is excellent in fine line etching of circuit wiring and is less likely to break. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 A diagram showing the shape of wiring used in the wiring etching test of the embodiment.

[0025] Figure 2 yes Figure 1 SEM images of examples of wiring shapes DETAILED DESCRIPTION

[0026] Hereinafter, embodiments of the present invention will be described in detail.

[0027] The aluminum alloy foil of the present invention is a foil containing predetermined amounts of Ca (calcium) and Fe (iron), and the remainder includes Al (aluminum) and other trace elements.

[0028] [Ca (Calcium)]

[0029] The Ca contained in the aluminum alloy foil of the present invention has the effect of making the crystal grains after cold rolling extremely fine, and can maintain the fine crystal grains even after heat treatment at 200° C. or higher. The dispersion of the Al—Ca intermetallic compound can also improve the strength, and obtain an aluminum alloy foil with high strength and high ductility.

[0030] The content of Ca may be 1.0% by mass or more relative to the total amount of the aluminum alloy foil of the present invention, but may be less than 4.5% by mass. If the content of Ca is less than 1.0% by mass, the effect of grain refinement is small, while if it is 4.5% by mass or more, flexibility is lost and foil rolling becomes difficult. For the same reason, the content of Ca is preferably 1.5% by mass or more and less than 3.0% by mass.

[0031] [Fe(Iron)]

[0032] The Fe contained in the aluminum alloy foil of the present invention is an element that improves strength and elongation, and is usually added to the aluminum foil. The content of Fe can be 0.02% by mass or more, and can be less than 1.3% by mass, relative to the total amount of the aluminum alloy foil of the present invention. If the content of Fe is less than 0.02% by mass, it is difficult to obtain strength, and high-purity billets need to be used during production, so it will also cause a burden on cost. When the content is more than 1.3% by mass, the crystallization product tends to become coarse, and there is concern about elongation degradation and pinholes during rolling. For the same reason, the content of Fe is preferably 0.15% by mass or more and less than 0.8% by mass.

[0033] [Other trace elements]

[0034] The aluminum alloy foil of the present invention contains other trace elements including inevitable impurities as components other than Ca and Fe. Examples of the trace elements include Si (silicon), Mn (manganese), Cu (copper), V (vanadium), Ti (titanium), Zr (zirconium), Cr (chromium), Ni (nickel), Mg (magnesium), Zn (zinc), B (boron), Ga (gallium), and Bi (bismuth).

[0035] The content of each of these elements in the aluminum alloy foil is preferably 0.1 mass % or less.

[0036] [Determination of composition]

[0037] The composition of the aluminum alloy foil of the present invention is measured by inductively coupled plasma emission spectrometry. Examples of the measuring apparatus include iCAP6500DUO manufactured by Thermo Fisher Scientific and ICPS-8100 manufactured by Shimadzu Corporation.

[0038] [foil thickness]

[0039] The thickness of the aluminum alloy foil of the present invention is preferably 6 μm to 80 μm. If it is less than 6 μm, the workability in the manufacturing process of the printed wiring board deteriorates, and if it is thicker than 80 μm, the target fine line etching becomes difficult. For the same reason, it is preferably 10 μm to 40 μm.

[0040] [Average crystal particle size]

[0041] The average crystal grain size of the aluminum alloy foil in the present invention refers to the average value of the equivalent circle diameter of the crystal grains measured by the EBSD (electron beam backscatter diffraction) method with a grain boundary orientation difference of 15° or more with the aluminum alloy foil surface as the observation surface. It represents the average size of the crystal grains divided by the so-called high-angle grain boundaries. The smaller the average crystal grain size, the denser the dissolution pits during wiring etching, and the thinner the wire can be.

[0042] The average crystal grain size of the aluminum alloy foil of the present invention is preferably 12 μm or less because thinner wiring can be obtained compared to conventional pure aluminum and aluminum-iron materials. For the same reason, it is more preferably 8 μm or less.

[0043] [Tensile strength, yield strength]

[0044] The aluminum alloy foil of the present invention preferably has a tensile strength in the rolling direction of 110 N / mm 2 Above, the yield strength (0.2% yield strength) is 70N / mm 2 If it is within the above range, the risk of wire breakage can be reduced even when the wiring of the printed wiring substrate is made thinner. For the same reason, the preferred tensile strength is 130 N / mm2 Above, yield strength is 85N / mm 2 above.

[0045] [Manufacturing method]

[0046] Next, the method for producing the aluminum alloy foil of the present invention will be described.

[0047] In the method for producing an aluminum alloy foil of the present invention, first, an aluminum billet, various added metal elements, or an aluminum mother alloy containing them is prepared so as to have the above-mentioned composition range, and heated to form an aluminum alloy melt. Next, the melt is cast to produce an ingot.

[0048] Next, the obtained ingot is cold rolled to form a foil of a predetermined thickness. After the cold rolling, final annealing (FA) is performed as required for tempering and removal of rolling oil. The aluminum alloy foil of the present invention can be manufactured by these methods.

[0049] [Casting]

[0050] As described above, an aluminum billet, various added metal elements, or an aluminum mother alloy containing them is prepared so as to have the above-mentioned composition range, and heated at 680 to 1000° C., thereby obtaining an aluminum alloy melt.

[0051] The obtained aluminum alloy melt is cast to make an ingot. The casting method is not limited to a specific casting method as long as it is a method that can make an ingot or a cast plate, and a known method can be used. As examples of the casting method, DC casting (Direct Chill) and CC casting (Continuous Casting) can be used. However, in order to contain more Ca and Fe, which are the main elements of the present invention, it is preferred to select a casting method with a high casting cooling rate. From this point of view, it is particularly preferred to use CC casting that produces a high casting cooling rate, and twin-roll continuous casting is more preferred in the CC casting.

[0052] [Cold Rolling]

[0053] The obtained ingot or cast plate is cold rolled to form a cold rolled foil of a specified thickness. In addition, homogenization heat treatment and hot rolling can be performed before the cold rolling as required, and intermediate annealing (IA) can be performed on the way of the cold rolling process as required.

[0054] [Homogenization heat treatment, hot rolling]

[0055] In the method for manufacturing the aluminum alloy foil of the present invention, the homogenization heat treatment step and hot rolling are optional, but in the case of considering segregation in the casting structure, they can also be carried out within a range that does not affect the characteristics of the aluminum alloy foil, specifically at 450°C to 600°C. It should be noted that if the temperature of the homogenization heat treatment and hot rolling is higher than 600°C, the intermetallic compounds will coarsen, which will have an adverse effect on the strength, elongation, and grain structure of the aluminum alloy foil. The heat treatment time of the homogenization heat treatment step is preferably less than 20 hours in terms of production efficiency.

[0056] [Intermediate annealing (IA)]

[0057] In the method for manufacturing the aluminum alloy foil of the present invention, the intermediate annealing (IA) step is optional, but for the purpose of improving the rollability, it can also be performed within a range that does not affect the characteristics of the aluminum alloy foil, that is, below 450°C. It should be noted that if the intermediate annealing temperature is higher than 450°C, the intermetallic compounds will coarsen, which will have an adverse effect on the strength, elongation, and grain structure of the aluminum alloy foil. The heat treatment time is preferably less than 20 hours in terms of production efficiency.

[0058] [Final annealing (FA)]

[0059] In the method for manufacturing the aluminum alloy foil of the present invention, the final annealing (FA) step is optional, but in order to improve the bonding strength between the aluminum alloy foil and the substrate in the manufacture of the printed wiring substrate, it is preferably heat treated at 200°C to 400°C. It should be noted that if the final annealing temperature is lower than 200°C, the rolling oil attached to the aluminum alloy foil cannot be completely removed, and it is difficult to obtain the bonding strength with the substrate. When the final annealing temperature is greater than 400°C, it is difficult for the present invention to obtain the target strength and grain structure, and when heat-treated in the form of a coil, excessive adhesion of the aluminum foils occurs. The heat treatment time is preferably less than 80 hours in terms of production efficiency.

[0060] [Aluminum laminate]

[0061] The aluminum alloy foil of the present invention can be formed into an aluminum laminate by laminating at least one layer of an adherend on at least one surface thereof.

[0062] The adherend may or may not be flexible, and for example, a resin film such as polyethylene, polypropylene, polyester, polycarbonate, polyimide, polyamide, or a paper phenolic resin plate, a glass epoxy plate, or the like can be preferably used.

[0063] The method for laminating the aluminum alloy foil and the adherend is not limited, and examples thereof include lamination using an adhesive.

[0064] Furthermore, the surface of the aluminum alloy foil may be roughened, cleaned, coated, or the like before lamination.

[0065] [Printed wiring board]

[0066] The surface of the aluminum foil of the above-mentioned stack is printed with a resist ink in a pattern in a manner to form a desired wiring shape, and then immersed in an etching solution to dissolve the portion not printed with the resist ink. The resist is then peeled off as needed, thereby obtaining a printed wiring substrate in which the aluminum foil is formed into a wiring pattern.

[0067] As the printing method, a known method such as gravure printing and screen printing can be used.

[0068] As the resist ink, a known resist ink can be used, and an organic or inorganic resist or the like can be appropriately adopted depending on the etching solution, coating properties on the aluminum surface, and the like.

[0069] The etching liquid may be a known etching liquid, and may be acidic or alkaline as appropriate, and examples thereof include aqueous sodium hydroxide (caustic soda) solution, hydrochloric acid, ferrous chloride solution, cupric chloride solution, hydrogen peroxide, or mixed solutions thereof.

[0070] Example

[0071] The following examples and comparative examples are given to further clarify the content of the present invention. First, the test methods used in the examples are shown below.

[0072] (Test method)

[0073] [Tensile test, yield strength (0.2% yield strength)]

[0074] A short strip test piece of 15 mm in width and 200 mm in length was cut out in a manner that the tensile direction was parallel to the rolling direction. The tensile tester used was a Strograph VES5D manufactured by Toyo Seiki Seisaku-sho, Ltd. The test was conducted at a tensile speed of 10 mm / min and a chuck distance of 100 mm as the mark distance to obtain data on tensile strength and yield strength (0.2% yield strength). The test was conducted three times and the average value was calculated.

[0075] [Average crystal particle size]

[0076] Using a field emission scanning electron microscope (JSM-7200F manufactured by JEOL Ltd.) equipped with an EBSD analysis device (TSLSolutions Velocity), EBSD measurement was performed on the surface of the aluminum alloy foil at a magnification of 500 times in a field of view of 200μm×200μm with a step size (StepSize) of 0.4μm. The measurement results were analyzed using the analysis software OIM Analysis 8 (TSLSolutions) with Grain Tolerance Angle = 15°. The value calculated from the Average (average value): Area (area) in the Summary Statistics in the distribution of Grain Size (diameter) was used as the average crystal grain size. In addition, EBSD measurements were performed randomly in 3 fields of view, and the average value was found. As a pretreatment before the measurement, the surface of the aluminum alloy foil was mirror-finished by electrolytic polishing.

[0077] [Wiring etching test]

[0078] A 25 μm dry film resist is attached to the aluminum alloy foil, and the dry film resist is exposed to UV light through a photomask. The dry film resist can be cured only at a predetermined position through a photomask. Then, the resist at the uncured position is removed, and the resist film is formed into a target wiring shape. The aluminum alloy foil at the position where the resist film is not formed is etched and dissolved in a ferrous chloride aqueous solution, and finally the resist film is peeled off with caustic soda, thereby completing wiring etching.

[0079] The target wiring shape is as follows Figure 1 As shown in FIG. 1 , wiring (aluminum portion) and spacer (dissolved portion) are repeatedly arranged, and their widths are the same. The length of the wiring is 50 mm, and the number of wires is 10. The SEM image of the example of the wiring shape is shown in FIG. Figure 2 .

[0080] The test was conducted at five levels of line width: 50 μm, 75 μm, 100 μm, 125 μm, and 150 μm. The maximum fineness of wiring etching that can be achieved without breaking the line is shown in Table 2 by observation under an optical microscope.

[0081] (Examples 1 to 15, Comparative Examples 1 to 5)

[0082] Aluminum alloys of compositions A to K shown in Table 1 were melted and the molten metal was poured into a fixed mold to produce a small cast plate with a thickness of 6 mm, a width of 60 mm, and a length of 65 mm. The surface of the small cast plate was milled with a milling machine, and then aluminum alloy foil was produced under the conditions shown in Table 2. Table 2 also shows the tensile test results, average crystal grain size, and wiring etching test results.

[0083] In addition, the conditions for homogenization heat treatment, intermediate annealing, and final annealing are as follows.

[0084] Homogenization heat treatment

[0085] After the surface was milled from a thickness of 6 mm, the temperature was raised to the temperature shown in Table 2 over 2 hours in an air atmosphere, maintained for 10 hours, and then cooled in the furnace.

[0086] Intermediate annealing (IA)

[0087] After rolling to a thickness of 1 mm, the temperature was raised to the temperature shown in Table 2 over 2 hours in an air atmosphere, maintained for 5 hours, and then cooled in the furnace.

[0088] Final annealing (FA)

[0089] After the cold rolling was completed, the temperature was raised to the temperature shown in Table 2 over 2 hours in an air atmosphere, maintained for 5 hours, and then cooled in the furnace.

[0090] It should be noted that in Comparative Examples 4 and 5, the same test was conducted using the aluminum foil of the conventional composition 1N30 (manufactured by Toyo Aluminum Co., Ltd.) and the aluminum foil of the composition 8021 (manufactured by Toyo Aluminum Co., Ltd.). In the tests of Comparative Examples 4 and 5, slabs were produced by DC casting, and then subjected to homogenization heat treatment and hot rolling to produce plates having a thickness of 6 mm.

[0091] [Table 1]

[0092]

[0093] [Table 2]

[0094]

Claims

1. An aluminum alloy foil, wherein a calcium (Ca) content is 1.0 mass % or more and less than 4.5 mass %, an iron (Fe) content is 0.02 mass % or more and less than 1.3 mass %, and the remainder comprises aluminum (Al) and other trace elements.

2. The aluminum alloy foil according to claim 1, wherein The average crystal grain size measured by the electron beam backscatter diffraction method (EBSD) with the surface of the aluminum alloy foil as the observation surface and the grain boundary orientation difference of 15° or more was 12 μm or less.

3. The aluminum alloy foil according to claim 1, wherein The yield strength of aluminum alloy foil is 70N / mm 2 above.

4. The aluminum alloy foil according to claim 3, wherein The tensile strength of aluminum alloy foil is 110N / mm 2 above.

5. The aluminum alloy foil according to any one of claims 1 to 4, wherein The thickness of the aluminum alloy foil is 6 μm to 80 μm.

6. A method for producing an aluminum alloy foil, comprising: A step of obtaining an aluminum alloy ingot by casting a molten aluminum alloy having a calcium (Ca) content of 1.0 mass % or more and less than 4.5 mass %, an iron (Fe) content of 0.02 mass % or more and less than 1.3 mass %, and the remainder containing aluminum Al and other trace elements; and A step of cold-rolling the ingot to obtain a cold-rolled foil of an aluminum alloy foil.

Citation Information

Patent Citations

  • Aluminum alloy foil for printed circuit

    JP2001152270A

  • Aluminum foil for printed circuit

    JP2012149289A