Plated steel material and method for producing plated steel material
By optimizing the chemical composition and microstructure of the plating layer in the Zn-Al-Mg alloy layer of the plated steel, the Zn/Al/MgZn2 ternary eutectic is formed, and the problems of poor peelability and low corrosion resistance of the plating are solved, and the water is achieved Excellent workability and corrosion resistance of coated steel in the environment.
Patent Information
- Application Number
- CN202280093510.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-18
- Filing Date
- 2022-12-16
- Publication Date
- 2024-11-01
AI Technical Summary
The coated steel with high Mg concentration in the plating layer has poor peeling properties during processing and has poor corrosion resistance in an environment where water is prone to accumulation.
采用Zn-Al-Mg合金层的镀覆钢材,其镀层化学组成为Zn:超过65.00%、Al:超过5.00%且低于25.00%、Mg:超过3.00%且低于12.50%,并在镀层表面研磨至层厚的1/2后存在Zn/Al/MgZn2三元共晶,累计周长的平均值为100~300mm/mm2,且基体钢材与镀层界面粗糙度为0.3~2.0μm,通过热浸镀法形成镀层,并在特定冷却速度下控制镀层的微结构。
It improves the processability of the plated steel and maintains excellent corrosion resistance in an environment where water is prone to accumulation, reduces the local corrosion of Zn/Al/MgZn2 ternary eutectic, and the coating is not easy to peel off, ensuring the protection of the matrix metal.
Smart Images

Figure BDA0005038216580000221 
Figure BDA0005038216580000231 
Figure BDA0005038216580000241
Abstract
Description
Technical Field
[0001] The present disclosure relates to a plated steel material and a method for manufacturing the plated steel material. Background Art
[0002] For example, in the field of building materials, a variety of plated steels are used. Most of them are Zn-plated steels. Due to the demand for longer life of building materials, research on the high corrosion resistance of Zn-plated steels has been carried out, and various plated steels have been developed. The first high corrosion-resistant plated steel for building materials was Zn-5% Al-plated steel (Galfan-plated steel) with improved corrosion resistance by adding Al to the Zn-based coating. It is a well-known fact that adding Al to the coating improves corrosion resistance. By adding 5% Al, Al crystals are formed in the coating (specifically, Zn phase), and the corrosion resistance is improved. Zn-55% Al-1.6% Si plated steel (Galvalume steel) is also a plated steel with improved corrosion resistance based on basically the same reason.
[0003] Among them, the charm of Zn-based plated steel is the replacement corrosion protection effect for the base steel. That is, at the cut end surface of the plated steel, the cracked part of the plating during processing, and the exposed part of the base steel due to the peeling of the plating, the plating around the base steel is dissolved before the corrosion of the base steel, and the plating dissolved components form a protective film. This can prevent red rust from the base steel to a certain extent.
[0004] Generally speaking, when the Al concentration is low and the Zn concentration is high, this effect is easy to show, which is preferred. Therefore, highly corrosion-resistant plated steel materials such as those that suppress the Al concentration to a relatively low concentration of about 5% to 25% have been put into practical use in recent years. In particular, plated steel materials that suppress the Al concentration to a relatively low level and contain about 1 to 3% of Mg have excellent corrosion resistance compared to Galfan plated steel materials. Therefore, it has become the mainstream of the market as a plated steel material and is currently widely known in the market.
[0005] As the plated steel material containing a certain amount of Al and Mg, for example, a plated steel material disclosed in Patent Document 1 has been developed.
[0006] Specifically, Patent Document 1 discloses: "A hot-dip Zn-Al-Mg-Si steel material having a plated steel material surface on the surface of the steel material having a plating layer containing Al: 5 to 18 mass %, Mg: 1 to 10 mass %, Si: 0.01 to 2 mass %, and the remainder being Zn and unavoidable impurities, and the surface of the plated steel material has a thickness of 1 mm 2 There are more than 200 Al phases.
[0007] In addition, Patent Document 2 discloses: "A plated steel material comprising a steel material and a plated layer including a Zn-Al-Mg alloy layer disposed on the surface of the steel material, wherein the plated layer has the following chemical composition: containing Zn: more than 65.0%, Al: more than 5.0% and less than 25.0%, Mg: more than 3.0% and less than 12.5%, and Sn: 0.1% to 20.0%, wherein after the surface of the Zn-Al-Mg alloy layer is polished to 1 / 2 of the layer thickness, in a reflected electron image of the Zn-Al-Mg alloy layer obtained when observed with a scanning electron microscope at a magnification of 100 times, Al crystals are present, and the average value of the cumulative circumference of the Al crystals is 88 to 195 mm / mm 2 ”.
[0008] Prior art literature
[0009] Patent Literature
[0010] Patent Document 1: Japanese Patent Application Laid-Open No. 2001-355053
[0011] Patent Document 2: WO2019 / 221193 Summary of the invention
[0012] Problems to be solved by the invention
[0013] However, for plated steel materials with high Mg concentration in the coating, if the plated steel materials are processed, the coating will peel off and the processability will be poor. In addition, for example, in an environment where water is easily accumulated, such as when the plated steel sheet is set in a direction parallel to the ground for use, the corrosion resistance will be poor.
[0014] Therefore, an object of the present disclosure is to provide a plated steel material having excellent workability and excellent corrosion resistance even when used in an environment where water easily accumulates, and a method for producing the same.
[0015] Means for solving problems
[0016] The above-mentioned problems are solved by the following means.
[0017] <1> A plated steel material comprising: a base steel material; and a plating layer including a Zn-Al-Mg alloy layer disposed on a surface of the base steel material.
[0018] The above-mentioned coating has the following chemical composition: in terms of mass % it contains:
[0019] Zn: more than 65.00%,
[0020] Al: more than 5.00% and less than 25.00%,
[0021] Mg: more than 3.00% and less than 12.50%,
[0022] Sn: 0% to 3.00%,
[0023] Bi: 0% or more and less than 5.00%,
[0024] In: 0% or more and less than 2.00%,
[0025] Ca: 0% to 3.00%,
[0026] Y: 0% to 0.50%,
[0027] La: 0% or more and less than 0.50%,
[0028] Ce: 0% or more and less than 0.50%,
[0029] Si: 0% or more and less than 2.50%,
[0030] Cr: 0% or more and less than 0.25%,
[0031] Ti: 0% or more and less than 0.25%,
[0032] Zr: 0% or more and less than 0.25%,
[0033] Mo: 0% or more and less than 0.25%,
[0034] W: 0% or more and less than 0.25%,
[0035] Ag: 0% or more and less than 0.25%,
[0036] P: 0% or more and less than 0.25%,
[0037] Ni: 0% or more and less than 0.25%,
[0038] Co: 0% or more and less than 0.25%,
[0039] V: 0% or more and less than 0.25%,
[0040] Nb: 0% or more and less than 0.25%,
[0041] Cu: 0% or more and less than 0.25%,
[0042] Mn: 0% or more and less than 0.25%,
[0043] Li: 0% or more and less than 0.25%,
[0044] Na: 0% or more and less than 0.25%,
[0045] K: 0% or more and less than 0.25%,
[0046] Fe: 0% to 5.00%,
[0047] Sr: 0% or more and less than 0.5%,
[0048] Sb: 0% or more and less than 0.5%,
[0049] Pb: 0% or more and less than 0.5%,
[0050] B: 0% or more and less than 0.5%, and
[0051] Impurities,
[0052] In the reflected electron image of the Zn-Al-Mg alloy layer obtained by observing the surface of the plated layer at a magnification of 100 times using a scanning electron microscope after grinding the surface of the plated layer to 1 / 2 of the layer thickness, there is a Zn / Al / MgZn2 ternary eutectic, and the average value of the cumulative circumference of the Zn / Al / MgZn2 ternary eutectic is 100 to 300 mm / mm 2 .
[0053] <2> according to <1> The plated steel material, wherein the plated layer includes an Al-Fe alloy layer between the base steel material and the Zn-Al-Mg alloy layer.
[0054] <3> according to <1> or <2> The plated steel material, wherein the interface roughness Ra between the base steel material and the plated layer is 0.3-2.0 μm.
[0055] <4> according to <1> ~ <3> The method for manufacturing a plated steel material as described in any one of the preceding claims, wherein a base steel material having a surface roughness Ra of 0.3 to 2.0 μm on the plated surface is immersed in a plating bath, and after being scooped out from the above-mentioned plating bath, is cooled in a temperature range of 450 to 395°C at an average cooling rate of 5 to 20°C / s, in a temperature range of 395 to 340°C at an average cooling rate of 3°C / s or less, and in a temperature range of 340 to 280°C at an average cooling rate of 10 to 20°C / s.
[0056] Effects of the Invention
[0057] According to the present disclosure, it is possible to provide a plated steel material having excellent workability and excellent corrosion resistance even when used in an environment where water easily accumulates, and a method for producing the same. BRIEF DESCRIPTION OF THE DRAWINGS
[0058] FIG1(A) is a reflected electron image of a Zn-Al-Mg alloy layer obtained when the surface of the plated layer in the Zn-Al-Mg plated steel material of the present disclosure is polished to 1 / 2 of the layer thickness and then observed using a scanning electron microscope at a magnification of 100 times.
[0059] FIG1(B) is an image obtained by binarizing a reflected electron image of a Zn—Al—Mg alloy layer. DETAILED DESCRIPTION
[0060] Hereinafter, an example of the present disclosure will be described.
[0061] In addition, in this disclosure, "%" indicating the content of each element in the chemical composition means "mass %".
[0062] The numerical range expressed using "to" means a range including the numerical values described before and after "to" as the lower limit and the upper limit.
[0063] When “more than” or “less than” is indicated about the numerical values described before and after “to”, the numerical range means a range not including these numerical values as the lower limit or the upper limit.
[0064] The content of elements in a chemical composition may be described as element concentration (for example, Zn concentration, Mg concentration, etc.).
[0065] The plated steel material of the present disclosure includes: a base steel material; and a plating layer including a Zn—Al—Mg alloy layer disposed on the surface of the base steel material.
[0066] The plated steel material of the present invention has a coating layer having a predetermined chemical composition, and a Zn / Al / MgZn2 ternary eutectic is present in a reflected electron image of a Zn-Al-Mg alloy layer obtained by observing the coating layer with a magnification of 100 times using a scanning electron microscope after the coating layer surface is polished to 1 / 2 of the layer thickness, and the average value of the cumulative perimeter of the Zn / Al / MgZn2 ternary eutectic is 100 to 300 mm / mm 2 .
[0067] The plated steel material of the present disclosure has excellent workability due to the above-mentioned configuration, and has excellent corrosion resistance even when used in an environment where water easily accumulates. The plated steel material of the present disclosure has been found based on the following findings.
[0068] In the case of a plated steel material having a high Mg concentration in the plating layer, a hard intermetallic compound phase is formed in the plating layer. Therefore, when the plated steel material is processed, the intermetallic compound phase is cracked and the plating layer becomes easy to peel off.
[0069] In addition, when used in an environment where water easily accumulates, the Zn / Al / MgZn2 ternary eutectic in the plating layer corrodes locally, and the corrosion reaches the base metal early.
[0070] Therefore, the Zn / Al / MgZn2 ternary eutectic, which is the cause of local corrosion, is uniformly dispersed in the coating layer. That is, the average value of the cumulative perimeter of the Zn / Al / MgZn2 ternary eutectic is set within a predetermined range.
[0071] This can reduce local corrosion of the Zn / Al / MgZn2 ternary eutectic. In addition, since the soft Zn / Al / MgZn2 ternary eutectic functions as a buffer during processing, it can reduce cracking of the surrounding intermetallic compound phase.
[0072] From the above findings, it was found that the plated steel material of the present disclosure has excellent workability due to the above-mentioned configuration and has excellent corrosion resistance even when used in an environment where water easily accumulates.
[0073] Hereinafter, the plated steel material of the present disclosure will be described in detail.
[0074] (Base steel)
[0075] There is no particular restriction on the shape of the base steel material. In addition to steel plates, base steel materials include steel pipes, civil engineering materials (gates, corrugated pipes, drainage ditch covers, flying sand prevention plates, bolts, wire mesh, guardrails, waterproof walls, etc.), home appliance components (air conditioner outdoor unit casings, etc.), automobile parts (travel components, etc.), etc., which have been processed by forming. Forming can be performed by various plastic processing methods such as pressing, roll forming, and bending.
[0076] There is no particular limitation on the material of the base steel material, and various base steel materials such as general steel, pre-plated steel, Al-killed steel, ultra-low carbon steel, high carbon steel, various high-tensile steels, and some high-alloy steels (steel containing strengthening elements such as Ni and Cr) can be used.
[0077] Regarding the base steel material, there are no particular restrictions on conditions such as the method for producing the base steel material and the method for producing the base steel sheet (hot rolling method, pickling method, cold rolling method, etc.).
[0078] In addition, as a base steel material, the hot-rolled steel sheet, hot-rolled steel strip, cold-rolled steel sheet, and cold-rolled steel strip described in JIS G 3302 (2010) can also be applied.
[0079] The interface roughness Ra between the base steel material and the plating layer is preferably 0.3 to 2.0 μm.
[0080] By setting the surface roughness Ra of the base steel material to 0.3 μm or more, the average value of the cumulative perimeter of the Zn / Al / MgZn2 ternary eutectic can be controlled to be within the above range.
[0081] By setting the surface roughness Ra of the base steel material to 2.0 μm or less, non-plating can be suppressed.
[0082] It should be noted that the method for measuring the interface roughness Ra between the base steel material and the coating layer is as follows.
[0083] The base steel material may also be a pre-plated steel material. The pre-plated steel material is obtained, for example, by an electrolytic treatment method or a displacement plating method. In the electrolytic treatment method, the base steel material is immersed in a sulfuric acid bath or a chloride bath containing metal ions of various pre-plating components for electrolytic treatment, thereby obtaining the pre-plated steel material. In the displacement plating method, the base steel material is immersed in an aqueous solution containing metal ions of various pre-plating components and the pH of which is adjusted with sulfuric acid, so that the metal is precipitated by displacement, thereby obtaining the pre-plated steel material.
[0084] As the pre-plated steel material, a Ni pre-plated steel material can be cited as a representative example.
[0085] (Plating)
[0086] The plating layer includes a Zn-Al-Mg alloy layer. In addition to the Zn-Al-Mg alloy layer, the plating layer may also include an Al-Fe alloy layer. The Al-Fe alloy layer is disposed between the base steel material and the Zn-Al-Mg alloy layer.
[0087] That is, the plating layer may be a single layer structure of a Zn-Al-Mg alloy layer, or a laminated structure including a Zn-Al-Mg alloy layer and an Al-Fe alloy layer. In the case of a laminated structure, it is preferable that the Zn-Al-Mg alloy layer is set as a layer constituting the surface of the plating layer.
[0088] However, an oxide film of the plating constituent element may be formed on the surface of the plating layer with a thickness of about 50 nm, but it is considered to be thin relative to the thickness of the entire plating layer (about 8 to 60 μm) and does not constitute the main body of the plating layer.
[0089] The coating weight is preferably 40 to 300 g / m2 per side. 2 .
[0090] If the coating weight is set to 40g / m 2 If the coating weight is set to 300 g / m 2 If the amount is less than 10%, it is possible to suppress the appearance defects such as sagging patterns of the plating layer.
[0091] Next, the chemical composition of the plating layer will be described.
[0092] The chemical composition of the plating layer is set to the following chemical composition: containing by mass %:
[0093] Zn: more than 65.00%,
[0094] Al: more than 5.00% and less than 25.00%,
[0095] Mg: more than 3.00% and less than 12.50%,
[0096] Sn: 0% to 3.00%,
[0097] Bi: 0% or more and less than 5.00%,
[0098] In: 0% or more and less than 2.00%,
[0099] Ca: 0% to 3.00%,
[0100] Y: 0% to 0.50%,
[0101] La: 0% or more and less than 0.50%,
[0102] Ce: 0% or more and less than 0.50%,
[0103] Si: 0% or more and less than 2.50%,
[0104] Cr: 0% or more and less than 0.25%,
[0105] Ti: 0% or more and less than 0.25%,
[0106] Zr: 0% or more and less than 0.25%,
[0107] Mo: 0% or more and less than 0.25%,
[0108] W: 0% or more and less than 0.25%,
[0109] Ag: 0% or more and less than 0.25%,
[0110] P: 0% or more and less than 0.25%,
[0111] Ni: 0% or more and less than 0.25%,
[0112] Co: 0% or more and less than 0.25%,
[0113] V: 0% or more and less than 0.25%,
[0114] Nb: 0% or more and less than 0.25%,
[0115] Cu: 0% or more and less than 0.25%,
[0116] Mn: 0% or more and less than 0.25%,
[0117] Li: 0% or more and less than 0.25%,
[0118] Na: 0% or more and less than 0.25%,
[0119] K: 0% or more and less than 0.25%,
[0120] Fe: 0% to 5.00%,
[0121] Sr: 0% or more and less than 0.50%,
[0122] Sb: 0% or more and less than 0.50%,
[0123] Pb: 0% or more and less than 0.50%,
[0124] B: 0% or more and less than 0.50%, and
[0125] Impurities.
[0126] In the chemical composition of the plating layer, Sn, Bi, In, Ca, Y, La, Ce, Si, Cr, Ti, Zr, Mo, W, Ag, P, Ni, Co, V, Nb, Cu, Mn, Li, Na, K, Fe, Sr, Sb, Pb and B are optional components. That is, these elements may not be included in the plating layer. When these optional components are included, the content of each optional element is preferably in the range described below.
[0127] Among them, the chemical composition of the coating is the average chemical composition of the entire coating (when the coating is a single-layer structure of a Zn-Al-Mg alloy layer, it is the average chemical composition of the Zn-Al-Mg alloy layer; when the coating is a stacked structure of an Al-Fe alloy layer and a Zn-Al-Mg alloy layer, it is the average chemical composition of the Al-Fe alloy layer and the Zn-Al-Mg alloy layer combined).
[0128] Hereinafter, each element of the plating layer will be described.
[0129] Zn: more than 65.00%
[0130] Zn is an element necessary for obtaining corrosion resistance. When the concentration of Zn is considered in terms of atomic composition ratio, since the Zn layer is formed together with low specific gravity elements such as Al and Mg, it is necessary to set the Zn concentration as the main component in terms of atomic composition ratio.
[0131] Therefore, the Zn concentration is set to be more than 65.00%. The Zn concentration is preferably 70.00% or more. It should be noted that the upper limit of the Zn concentration is the concentration of the remainder excluding elements other than Zn and impurities.
[0132] Al: more than 5.00% and less than 25.00%
[0133] Al is an element necessary for forming Al crystals and ensuring corrosion resistance. Furthermore, Al is an element necessary for improving the adhesion of the plating layer and ensuring workability. Therefore, the lower limit of the Al concentration is set to more than 5.00% (preferably 10.00% or more).
[0134] On the other hand, if the Al concentration increases excessively, the corrosion resistance tends to deteriorate. Therefore, the upper limit of the Al concentration is set to less than 25.00% (preferably 23.00% or less).
[0135] Mg: more than 3.00% and less than 12.50%
[0136] Mg is an element necessary for ensuring corrosion resistance. Therefore, the lower limit of the Mg concentration is set to be more than 3.0% (preferably more than 4.00%).
[0137] On the other hand, if the Mg concentration increases excessively, workability tends to deteriorate. Therefore, the upper limit of the Mg concentration is set to less than 12.50% (preferably 10.00% or less).
[0138] Sn: 0~3.00%
[0139] Sn is an element that contributes to corrosion resistance and initial discoloration resistance. Therefore, the lower limit of the Sn concentration is preferably more than 0.00% (preferably 0.05% or more, more preferably 0.10% or more).
[0140] On the other hand, if the Sn concentration increases excessively, the corrosion resistance and the initial discoloration resistance tend to deteriorate. Therefore, the upper limit of the Sn concentration is set to 3.00% or less.
[0141] Bi: 0% or more and less than 5.00%
[0142] Bi is an element that contributes to corrosion resistance. Therefore, the lower limit of the Bi concentration is preferably more than 0.00% (preferably 0.10% or more, more preferably 3.00% or more).
[0143] On the other hand, if the Bi concentration increases excessively, the corrosion resistance tends to deteriorate. Therefore, the upper limit of the Bi concentration is set to less than 5.00% (preferably 4.80% or less).
[0144] In: 0% or more and less than 2.00%
[0145] In is an element that contributes to corrosion resistance. Therefore, the lower limit of the In concentration is preferably more than 0.00% (preferably 0.10% or more, more preferably 1.00% or more).
[0146] On the other hand, if the In concentration increases excessively, the corrosion resistance tends to deteriorate. Therefore, the upper limit of the In concentration is set to less than 2.00% (preferably 1.80% or less).
[0147] Ca: 0%~3.00%
[0148] Ca is an element that can adjust the optimal Mg dissolution amount for imparting corrosion resistance. Therefore, the lower limit of the Ca concentration is preferably more than 0.00% (preferably 0.05% or more).
[0149] On the other hand, if the Ca concentration increases excessively, the corrosion resistance and workability tend to deteriorate. Therefore, the upper limit of the Ca concentration is set to 3.00% or less (preferably 1.00% or less).
[0150] Y: 0%~0.50%
[0151] Y is an element that contributes to corrosion resistance. Therefore, the lower limit of the Y concentration is preferably more than 0.00% (preferably 0.10% or more).
[0152] On the other hand, if the Y concentration increases excessively, the corrosion resistance tends to deteriorate. Therefore, the upper limit of the Y concentration is set to 0.50% or less (preferably 0.30% or less).
[0153] La and Ce: 0% or more and less than 0.50%
[0154] La and Ce are elements that contribute to corrosion resistance. Therefore, the lower limits of the La concentration and the Ce concentration are preferably more than 0.00% (preferably 0.10% or more), respectively.
[0155] On the other hand, if the La concentration and the Ce concentration increase excessively, the corrosion resistance tends to deteriorate. Therefore, the upper limits of the La concentration and the Ce concentration are each set to less than 0.50% (preferably 0.40% or less).
[0156] Si: 0% or more and less than 2.50%
[0157] Si is an element that suppresses the growth of the Al-Fe alloy layer and thus contributes to improving corrosion resistance. Therefore, the Si concentration is preferably more than 0.00% (preferably 0.05% or more, more preferably 0.10% or more). In particular, in the case where Sn is not contained (i.e., when the Sn concentration is 0%), from the perspective of ensuring corrosion resistance, the Si concentration is preferably 0.10% or more (preferably 0.20% or more).
[0158] On the other hand, if the Si concentration increases excessively, the corrosion resistance and workability tend to deteriorate. Therefore, the upper limit of the Si concentration is set to less than 2.50%. In particular, from the viewpoint of corrosion resistance, the Si concentration is preferably 2.40% or less, more preferably 1.80% or less, and further preferably 1.20% or less.
[0159] Cr, Ti, Zr, Mo, W, Ag, P, Ni, Co, V, Nb, Cu, Mn, Li, Na and K: 0% or more and less than 0.25%
[0160] Cr, Ti, Zr, Mo, W, Ag, P, Ni, Co, V, Nb, Cu, Mn, Li, Na, and K are elements that contribute to corrosion resistance. Therefore, the lower limits of the concentrations of Cr, Ti, Zr, Mo, W, Ag, P, Ni, Co, V, Nb, Cu, Mn, Li, Na, and K are each preferably more than 0.00% (preferably 0.05% or more, more preferably 0.10% or more).
[0161] On the other hand, if the concentration of Cr, Ti, Zr, Mo, W, Ag, P, Ni, Co, V, Nb, Cu, Mn, Li, Na, and K increases excessively, the corrosion resistance tends to deteriorate. Therefore, the upper limit of the concentration of Cr, Ti, Zr, Mo, W, Ag, P, Ni, Co, V, Nb, Cu, Mn, Li, Na, and K is set to less than 0.25%. The upper limit of the concentration of Cr, Ti, Zr, Mo, W, Ag, P, Ni, Co, V, Nb, Cu, Mn, Li, Na, and K is preferably 0.22% or less.
[0162] Fe: 0%~5.00%
[0163] When the plating layer is formed by hot-dip plating, a certain Fe concentration is contained in the Zn—Al—Mg alloy layer and the Al—Fe alloy layer.
[0164] It has been confirmed that when the Fe concentration is 5.00% or less, even if it is contained in the plating layer (especially the Zn-Al-Mg alloy layer), it has no adverse effect on the performance. Since most of Fe is contained in the Al-Fe alloy layer, if the thickness of this layer is large, the Fe concentration generally increases.
[0165] Sr, Sb, Pb and B: 0% or more and less than 0.50%
[0166] Sr, Sb, Pb, and B are elements that contribute to corrosion resistance. Therefore, the lower limits of the concentrations of Sr, Sb, Pb, and B are each preferably greater than 0.00% (preferably 0.05% or more, more preferably 0.10% or more).
[0167] On the other hand, if the concentrations of Sr, Sb, Pb, and B are excessively increased, the corrosion resistance tends to deteriorate. Therefore, the upper limit values of the concentrations of Sr, Sb, Pb, and B are each set to less than 0.50%.
[0168] Impurities
[0169] Impurities are components contained in raw materials or components mixed in during the manufacturing process, and are components not intentionally contained. For example, in the plating layer, components other than Fe may be mixed in small amounts as impurities due to mutual atomic diffusion between the base steel material and the plating bath.
[0170] The chemical composition of the coating was determined by the following method.
[0171] First, the coating is stripped and dissolved with an acid containing an inhibitor that inhibits corrosion of the base steel material to obtain an acid solution. Next, the obtained acid solution is measured by ICP analysis to obtain the chemical composition of the coating (when the coating is a single-layer structure of a Zn-Al-Mg alloy layer, it is the chemical composition of the Zn-Al-Mg alloy layer; when the coating is a laminated structure of an Al-Fe alloy layer and a Zn-Al-Mg alloy layer, it is the combined chemical composition of the Al-Fe alloy layer and the Zn-Al-Mg alloy layer). There is no particular limitation on the acid species as long as it can dissolve the coating. It should be noted that the chemical composition is measured as an average chemical composition. It should be noted that in ICP analysis, the Zn concentration is calculated using the "formula: Zn concentration = 100% - other element concentrations (%)".
[0172] Here, in the case where a pre-plated steel material is used as the base steel material, the components of the pre-plating layer thereof are also detected.
[0173] For example, in the case of using a pre-Ni plated steel material, in the ICP analysis, not only Ni in the plated layer but also Ni in the pre-Ni plated layer is detected. 2 ~3g / m 2 When a pre-plated steel material (thickness of about 0.1 to 0.3 μm) is used as the base steel material, even if the Ni concentration contained in the plating layer is 0%, the Ni concentration is detected to be 0.1 to 15% when measured by ICP analysis.
[0174] Here, the method of determining whether the base steel material is a Ni-pre-plated steel material is as follows.
[0175] From the target steel material, a sample is collected, whose cross section is cut along the thickness direction of the coating layer and serves as a measurement surface.
[0176] For the measurement surface of the sample, the Ni concentration is measured by line analysis near the interface between the coating and the base steel in the steel by an electron beam microanalyzer (Electron Probe MicroAnalyser: FE-EPMA). The measurement conditions are: acceleration voltage of 15kV, beam diameter of about 100nm, irradiation time of each point of 1000ms, and measurement interval of 60nm. It should be noted that the measurement distance is a distance that can confirm whether the Ni concentration is concentrated at the interface between the coating and the base steel in the steel.
[0177] Furthermore, if the Ni concentration is concentrated at the interface between the plating layer in the steel material and the base steel material, the base steel material is determined to be a Ni-pre-plated steel material.
[0178] In addition, when using a Ni-pre-plated steel material as a base steel material, the Ni concentration of the plating layer is defined as a value measured as follows.
[0179] First, the luminescence intensity of Ni was measured for three or more standard samples with different Ni concentrations (BAS Zn alloy standard samples IMN ZH1, ZH2, and ZH4) using a high-frequency glow discharge luminescence surface analyzer (GDS: manufactured by Horiba, Ltd., model: GD-Profiler2). A calibration curve was prepared based on the relationship between the obtained Ni luminescence intensity and the Ni concentration of the standard sample.
[0180] Next, the luminescence intensity of Ni at the 1 / 2 position of the film thickness of the plated steel material to be measured was measured using a high-frequency glow discharge luminescence surface analyzer (GDS: manufactured by Horiba, Ltd., model: GD-Profiler2). The Ni concentration at the 1 / 2 position of the plated layer was determined from the obtained Ni luminescence intensity and the prepared standard curve. The obtained Ni concentration at the 1 / 2 position of the plated layer was defined as the Ni concentration of the plated layer.
[0181] When a Ni-pre-plated steel material is used as the base steel material, the Zn concentration of the plating layer is defined as the Zn concentration calculated by the following formula.
[0182] Formula: Zn concentration = 100 - (concentration of elements other than Zn and Ni obtained by ICP analysis + Ni concentration obtained by GDS)
[0183] It should be noted that the measurement conditions of the high-frequency glow discharge light emission surface analysis device were set as follows.
[0184] HV: 630V
[0185] Anode diameter: φ4mm
[0186] Gas: Ar
[0187] Gas pressure: 600Pa
[0188] Output power: 35W
[0189] Next, the Al—Fe alloy layer will be described.
[0190] The Al-Fe alloy layer is a layer that may be formed on the surface of the base steel material (specifically, between the base steel material and the Zn-Al-Mg alloy layer) and in which the Al5Fe phase is the main phase in terms of the structure. The Al-Fe alloy layer is formed by mutual atomic diffusion of the base steel material and the plating bath. Since the steel material disclosed in the present invention forms the plating layer by hot dip plating, it is easy to form an Al-Fe alloy layer in the plating layer containing the Al element. Since the plating bath contains Al above a certain concentration, the Al5Fe phase is formed most. However, atomic diffusion takes time, and there are also parts where the Fe concentration becomes high in the part close to the base steel material. Therefore, the Al-Fe alloy layer may also partially contain a small amount of AlFe phase, Al3Fe phase, Al5Fe2 phase, etc. In addition, since a certain concentration of Zn is also contained in the plating bath, a small amount of Zn is also contained in the Al-Fe alloy layer.
[0191] There is no significant difference in corrosion resistance between the Al5Fe phase, Al3Fe phase, AlFe phase, and Al5Fe2 phase. The corrosion resistance here refers to the corrosion resistance of the portion not affected by welding.
[0192] Here, when Si is contained in the plating layer, Si is particularly easy to be taken into the Al-Fe alloy layer, and it is possible to form an Al-Fe-Si intermetallic compound phase. As the intermetallic compound phase to be identified, there is an AlFeSi phase, and as isomers, there are α, β, q1, q2-AlFeSi phases. Therefore, it is possible to detect these AlFeSi phases in the Al-Fe alloy layer. The Al-Fe alloy layer containing these AlFeSi phases is also called an Al-Fe-Si alloy layer.
[0193] Note that the Al—Fe—Si alloy layer is also thinner than the Zn—Al—Mg alloy layer, and therefore has little influence on the corrosion resistance of the entire plating layer.
[0194] In addition, when various pre-plated steel materials are used for the base steel material, the structure of the Al-Fe alloy layer may change depending on the amount of pre-plating. Specifically, there are the following situations: a pure metal layer used for pre-plating remains around the Al-Fe alloy layer; an intermetallic compound phase (such as Al3Ni phase) formed by combining the constituent components of the Zn-Al-Mg alloy layer with the pre-plating components forms an alloy layer; a part of Al atoms and Fe atoms are replaced to form an Al-Fe alloy layer; or a part of Al atoms, Fe atoms and Si atoms are replaced to form an Al-Fe-Si alloy layer, etc.
[0195] That is, the Al—Fe alloy layer refers to a layer including alloy layers of various forms described above in addition to the alloy layer mainly composed of the Al 5 Fe phase.
[0196] In addition, when a plating layer is formed on a Ni-plated steel material among various pre-plated steel materials, an Al-Ni-Fe alloy layer is formed as an Al-Fe alloy layer.
[0197] The thickness of the Al—Fe alloy layer is, for example, 0 μm to 7 μm.
[0198] From the viewpoint of improving the adhesion of the plating layer (specifically, the Zn—Al—Mg alloy layer) and ensuring corrosion resistance and workability, the thickness of the Al—Fe alloy layer is preferably 0.05 μm to 5 μm.
[0199] Generally, since the thickness of the Zn-Al-Mg alloy layer is thicker than that of the Al-Fe alloy layer, the Al-Fe alloy layer contributes less to the corrosion resistance of the plated steel material than the Zn-Al-Mg alloy layer. However, the Al-Fe alloy layer contains Al and Zn, which are corrosion-resistant elements, at a certain concentration or more, as inferred from the component analysis results. Therefore, the Al-Fe alloy layer has a certain degree of corrosion resistance to the base steel material.
[0200] Furthermore, when a plating layer having a chemical composition specified in the present disclosure is formed by hot-dip plating, an Al—Fe alloy layer having a thickness of 100 nm or more is often formed between the base steel material and the Zn—Al—Mg alloy layer.
[0201] From the viewpoint of corrosion resistance, the thicker the Al-Fe alloy layer, the better. Therefore, the thickness of the Al-Fe alloy layer is preferably 0.05 μm or more. However, since a thick Al-Fe alloy layer will cause a significant deterioration in processability, the thickness of the Al-Fe alloy layer is preferably 7 μm or less. If the thickness of the Al-Fe alloy layer is 7 μm or less, the amount of cracks and powdering generated starting from the Al-Fe alloy layer is reduced, and processability is improved. The thickness of the Al-Fe alloy layer is further preferably 5 μm or less, and further preferably 2 μm or less.
[0202] The thickness of the Al—Fe alloy layer is measured as follows.
[0203] After the sample was embedded in resin, it was polished, and the thickness of any five locations of the identified Al-Fe alloy layer was measured in the reflected electron image of the SEM of the coating cross section (the cut surface along the thickness direction of the coating) (wherein the magnification was 10,000 times, the size of the field of view: 50 μm in length × 200 μm in width, and the field of view was set to be able to visually confirm the Al-Fe alloy layer). Then, the arithmetic average of the five locations was taken as the thickness of the Al-Fe alloy layer.
[0204] It should be noted that the thickness of the coating was measured at any five locations in the reflected electron image of the cross-sectional SEM (where the magnification was 500 times, the size of the field of view was 198 μm in length × 244 μm in width, and the field of view was set to allow visual confirmation of the entire coating). Then, the arithmetic average of the five locations was taken as the thickness of the coating.
[0205] (Characteristics of plated steel)
[0206] -The average value of the cumulative perimeter of the Zn / Al / MgZn2 ternary eutectic-
[0207] In the reflected electron image of the Zn-Al-Mg alloy layer obtained by observing the surface of the plated layer at a magnification of 100 times using a scanning electron microscope after grinding the surface of the plated layer to 1 / 2 of the layer thickness, there is a Zn / Al / MgZn2 ternary eutectic, and the average value of the cumulative circumference of the Zn / Al / MgZn2 ternary eutectic is 100 to 300 mm / mm 2 .
[0208] If the average value of the cumulative perimeter of the Zn / Al / MgZn2 ternary eutectic is less than 100 mm / mm 2, the Zn / Al / MgZn2 ternary eutectic, which is the cause of local corrosion, coarsens, and the corrosion resistance deteriorates. In particular, if used in an environment where water easily accumulates, the Zn / Al / MgZn2 ternary eutectic in the coating corrodes locally, and the corrosion reaches the base metal early. In addition, when the plated steel is processed, the Zn / Al / MgZn2 ternary eutectic does not function as a buffer material, the intermetallic compound phase cracks, the coating becomes easy to peel off, and the processability becomes poor.
[0209] If the average value of the cumulative perimeter of the Zn / Al / MgZn2 ternary eutectic exceeds 300 mm / mm 2 , the Zn / Al / MgZn2 ternary eutectic is excessively refined, so when the plated steel is processed, the Zn / Al / MgZn2 ternary eutectic does not function as a buffer material, the intermetallic compound phase cracks, the coating becomes easy to peel off, and the processability becomes poor.
[0210] Therefore, the average value of the cumulative perimeter of the Zn / Al / MgZn2 ternary eutectic is set to 100-300 mm / mm 2 The average value of the cumulative perimeter of the Zn / Al / MgZn2 ternary eutectic is preferably 105 to 290 mm / mm 2 , more preferably 110 to 280 mm / mm 2 .
[0211] In the reflected electron image of the Zn-Al-Mg alloy layer, the area fraction of the Zn / Al / MgZn2 ternary eutectic is not particularly limited, but is preferably 10 to 50%, more preferably 13 to 45%, from the viewpoint of workability and corrosion resistance.
[0212] As the remaining structure other than the Zn / Al / MgZn2 ternary eutectic, Al crystals, MgZn2 phases, etc. can be listed.
[0213] Here, the method for measuring the average value of the cumulative perimeter of the Zn / Al / MgZn2 ternary eutectic and the area fraction of the Zn / Al / MgZn2 ternary eutectic is described.
[0214] The average value of the cumulative perimeter of the Zn / Al / MgZn2 ternary eutectic and the area fraction of the Zn / Al / MgZn2 ternary eutectic were measured using a reflected electron image of the Zn-Al-Mg alloy layer obtained by observing the surface of the plated layer at a magnification of 100 times using a scanning electron microscope after grinding the surface to 1 / 2 of the layer thickness. Specifically, it is as follows.
[0215] First, a sample was collected from the plated steel material to be measured. The sample was collected from a location other than the vicinity of the punched end surface of the plated steel material (2 mm from the end surface) where there was no defective portion of the plating layer.
[0216] Next, the surface of the plating layer (substantially a Zn—Al—Mg alloy layer) of the sample was polished in the thickness direction of the plating layer (hereinafter also referred to as “Z-axis direction”).
[0217] Specifically, the surface of the plated layer was dry-polished with a #1200 grit grinding sheet, and then finish-polished with a finishing liquid containing aluminum oxide with an average particle size of 3 μm, a finishing liquid containing aluminum oxide with an average particle size of 1 μm, and a finishing liquid containing colloidal silica.
[0218] It should be noted that before and after grinding, the Zn intensity of the surface of the coating is measured by XRF (fluorescent X-ray analysis), and the Zn intensity after grinding becomes 1 / 2 of the Zn intensity before grinding, which is set to 1 / 2 of the thickness of the coating. Since the Zn-Al-Mg alloy layer accounts for more than 1 / 2 of the thickness of the coating, the grinding surface obtained by grinding the surface of the coating to 1 / 2 of the thickness becomes the grinding surface of the Zn-Al-Mg alloy layer. Therefore, by analyzing the grinding surface, the metal structure contained in the Zn-Al-Mg alloy layer can be grasped.
[0219] Next, the polished surface was observed with a scanning electron microscope (SEM) at a magnification of 100 times to obtain a reflected electron image (hereinafter also referred to as "SEM reflected electron image"). The SEM observation conditions were set as follows: acceleration voltage: 15 kV, irradiation current: 10 nA, and field size: 1000 μm×800 μm.
[0220] Using the binary processing function based on two thresholds of WinROOF2015 (image analysis software) manufactured by Mitani Shoji, the Zn / Al / MgZn2 ternary eutectic was identified in the reflected electron image of the SEM (gray scale image saved in 8 bits, 256 colors). It should be noted that in the gray scale image saved in 8 bits, a luminance of 0 indicates black, and a maximum value of 255 indicates white. Generally, there is the following tendency: the phase with a smaller atomic number, the more Al and Mg content, the more black it appears, and the phase with a higher Zn content, the more white it appears. Moreover, the whitest structure in the coating structure is the Zn / Al / MgZn2 ternary eutectic (refer to Figure 1 (A))).
[0221] The identification results using FE-SEM or TEM show that, in the case of the reflected electron image of the SEM, if 160 and 215 are set as the threshold values of the light intensity, the Zn / Al / MgZn2 ternary eutectic can be identified with good accuracy. Therefore, the image is processed so that the color changes in the light intensity range of 160 to 215 occur, and the Zn / Al / MgZn2 ternary eutectic is identified (see FIG. 1(B)).
[0222] Next, the automatic shape feature measurement function of WinROOF2015 (image analysis software) manufactured by Mitani Shoji was used to accumulate the perimeter of the Zn / Al / MgZn2 ternary eutectic identified by the above image processing to obtain the cumulative perimeter of the Zn / Al / MgZn2 ternary eutectic. Then, the cumulative perimeter of the Zn / Al / MgZn2 ternary eutectic was divided by the area of the field of view to calculate the area per unit area (mm 2 )’s cumulative circumference of the Zn / Al / MgZn2 ternary eutectic.
[0223] This operation was performed in three fields of view, and the 2 ) is taken as the “average value of the cumulative perimeter of the Zn / Al / MgZn2 ternary eutectic”.
[0224] In addition, the area fraction of the Zn / Al / MgZn2 ternary eutectic can also be obtained using the automatic shape feature measurement function of WinROOF2015 (image analysis software) manufactured by Mitani Shoji. Specifically, in the reflected electron image of the Zn-Al-Mg alloy layer, this function is used to calculate the area fraction (area fraction relative to the field of view area) of the Zn / Al / MgZn2 ternary eutectic identified by binary conversion. Then, this operation is performed in three fields of view, and the arithmetic average thereof is taken as the area fraction of the "Zn / Al / MgZn2 ternary eutectic".
[0225] (Method for producing plated steel material)
[0226] Hereinafter, an example of the method for producing the plated steel material of the present disclosure will be described.
[0227] The plated steel material of the present disclosure is obtained by forming a plating layer having the above-specified chemical composition and metal structure on the surface (ie, one side or both sides) of a base steel material (base steel plate, etc.) by hot-dip plating.
[0228] Specifically, as an example, hot-dip plating is performed under the following conditions.
[0229] For example, a base steel material having a surface roughness Ra of 0.3 to 2.0 μm on the plated surface is immersed in a plating bath, taken out of the plating bath, and then cooled in a temperature range of 450 to 395° C. at an average cooling rate of 5 to 20° C. / s.
[0230] Next, cooling is performed in a temperature range of 395 to 340° C. at an average cooling rate of 3° C. / s or less.
[0231] Next, cooling is performed in a temperature range of 340 to 280° C. at an average cooling rate of 10 to 20° C. / s.
[0232] The plating is performed by a continuous hot-dip metal plating method such as the Mori strip nitriding galvanizing method, for example.
[0233] By setting the surface roughness Ra of the plated surface of the base steel material to 0.3 μm or more, it becomes easy to form solidification nuclei of the structure of the plated layer, so that Al primary crystals etc. are densely crystallized. As a result, the Zn / Al / MgZn2 ternary eutectic is finely dispersed, and the average value of the cumulative perimeter of the Zn / Al / MgZn2 ternary eutectic can be controlled within the above range.
[0234] However, if the surface roughness Ra of the plated surface of the base steel material exceeds 2.0 μm, the wettability of the plating is poor and the surface is likely to be left unplated.
[0235] The surface roughness Ra of the plated surface of the base steel material is measured as follows according to JIS B 0633:2001. For the plated surface of the base steel material before plating, the average surface roughness in a length of 10 mm is measured three times in two arbitrary directions at 90 degrees using a contact surface roughness meter. The arithmetic mean of the measured values of the average surface roughness obtained (a total of 6 measured values of 2 directions × 3 times) is calculated. The arithmetic mean is taken as the surface roughness Ra of the plated surface of the base steel material.
[0236] When measuring the interface roughness Ra between the base steel material and the plated layer, first, the plated layer is removed from the plated steel material by dissolving it with hydrochloric acid to which an inhibitor has been added. Then, the surface of the base steel material on the side where the plated layer has been removed is measured and the average value is calculated by the same method as above. This is taken as the interface roughness Ra between the base steel material and the plated layer.
[0237] In the present disclosure, the interface roughness Ra between the base steel material and the plating layer in the plated steel material (i.e. after plating) is roughly the same as the surface roughness Ra of the plated surface of the base steel material before plating. That is, by using a base steel material having a surface roughness Ra of 0.3 to 2.0 μm on the plated surface, the interface roughness Ra between the base steel material and the plating layer in the obtained plated steel material can be set to 0.3 to 2.0 μm.
[0238] The coating solidifies in the order of Al primary crystal, Al / MgZn2 phase, MgZn2 peritectic crystallized around the Al primary crystal, and Zn / Al / MgZn2 ternary eutectic.
[0239] Therefore, by cooling at an average cooling rate of 5°C / s or more in a temperature range of 450 to 395°C, the primary Al crystal and the Al / MgZn2 phase are finely dispersed. Then, by cooling at an average cooling rate of 3°C / s or less in a temperature range of 395 to 340°C, MgZn2 peritectic is reliably crystallized around the primary Al crystal. Thus, the Zn / Al / MgZn2 ternary eutectic can be refined.
[0240] However, if the average cooling rate in the temperature range of 450 to 395°C exceeds 20°C / s, the Al primary crystal and the Al / MgZn2 phase are excessively finely crystallized, and the Zn / Al / MgZn2 ternary eutectic is also excessively finely refined. In this case, the average value of the cumulative perimeter of the Zn / Al / MgZn2 ternary eutectic exceeds the above range.
[0241] Next, the Zn / Al / MgZn2 ternary eutectic is refined by cooling at an average cooling rate of 10 to 20°C / s in a temperature range of 340 to 280°C. Thus, the average value of the cumulative perimeter of the Zn / Al / MgZn2 ternary eutectic is controlled to be within the above range.
[0242] Hereinafter, post-treatment of the plated steel material applicable to the present disclosure will be described.
[0243] The plated steel material disclosed in the present invention may also form a film on the plated layer. The film may be formed into one layer or two or more layers. As the type of the film directly above the plated layer, for example, a chromate film, a phosphate film, and a chromate-free film may be listed. The chromate treatment, phosphate treatment, and chromate-free treatment for forming these films may be performed by known methods.
[0244] There are the following types of chromate treatment: electrolytic chromate treatment in which a chromate film is formed by electrolysis; reactive chromate treatment in which a film is formed by reaction with a raw material and then excess treatment liquid is washed away; and coating chromate treatment in which a treatment liquid is applied to the object to be coated and dried without washing to form a film. Any of these treatments may be used.
[0245] Examples of the electrolytic chromate treatment include electrolytic chromate treatment using chromic acid, silica sol, resin (acrylic resin, vinyl ester resin, vinyl acetate acrylic emulsion, carboxylated styrene butadiene latex, diisopropanolamine-modified epoxy resin, etc.), and hard silica.
[0246] Examples of the phosphate treatment include zinc phosphate treatment, calcium zinc phosphate treatment, and manganese phosphate treatment.
[0247] Chromate-free treatment is particularly suitable because it has no load on the environment. There are the following types of chromate-free treatment: electrolytic type chromate-free treatment that forms a chromate-free film by electrolysis; reactive type chromate-free treatment that forms a film by reaction with the raw material and then rinses away the excess treatment liquid; and coating type chromate-free treatment that forms a film by applying the treatment liquid to the object and drying it without washing with water. Any of these treatments can be used.
[0248] Furthermore, on the film just above the plating layer, there may also be one or more layers of organic resin films. The organic resin is not limited to a specific type, and examples thereof include polyester resins, polyurethane resins, epoxy resins, acrylic resins, polyolefin resins, or modified forms of these resins. The so-called modified form here refers to a resin obtained by reacting the reactive functional groups contained in the structures of these resins with other compounds (monomers, crosslinking agents, etc.) containing functional groups that can react with the functional groups in the structures.
[0249] As such an organic resin, one or more organic resins (unmodified resins) may be mixed and used, or one or more organic resins obtained by modifying at least one other organic resin in the presence of at least one organic resin may be mixed and used. In addition, any coloring pigment or rust-proof pigment may be included in the organic resin film. A water-based resin may also be used by dissolving or dispersing in water.
[0250] (Example)
[0251] A plating bath was prepared in the atmosphere using a predetermined amount of pure metal ingots so as to obtain a plating layer having a chemical composition shown in Tables 1 and 2. A hot dip plating simulator was used to prepare the plated steel sheets.
[0252] As the base steel material, a general hot-rolled steel sheet (C concentration < 0.1%) with a thickness of 2.3 mm was used, brush-polished, and degreased and pickled immediately before the plating process. The surface roughness Ra of the plated surface of the base steel material (recorded as "surface roughness Ra" in the table) is as shown in Tables 1 and 2.
[0253] In some examples, a pre-Ni plated steel material was used as the base steel material. The Ni deposition amount was set to 1 g / m 2 ~3g / m 2 In addition, the example using the Ni pre-plated steel material as the base steel material is described as "Ni pre-plated" in the column of "base steel material" in the table.
[0254] A contact type K thermocouple is installed on the back side of the plated surface of the base steel material in order to monitor the temperature of the steel material during the process of manufacturing the plated steel sheet.
[0255] In all samples, the base steel was subjected to the same reduction treatment method before immersion in the plating bath. That is, the base steel was heated from room temperature to 800°C by electric heating in a N2-H2 (5%) environment (dew point below -40°C, oxygen concentration below 25ppm), maintained for 60 seconds, cooled to the plating bath temperature + 10°C by N2 gas blowing, and immediately immersed in the plating bath.
[0256] It should be noted that for any plated steel sheet, the plating bath temperature is 500°C as a basic temperature, and in some levels, the plating bath temperature is further set to a higher temperature. The immersion time in the plating bath is set to the time in the table (2 seconds). The N2 gas wiping pressure is adjusted so that the plating thickness becomes 30μm (±1μm).
[0257] Then, after the base steel material is taken out from the coating bath, a coating layer is obtained by a cooling process in which the average cooling rates in the first to third stages shown in Tables 1 and 2 are set to the conditions shown in Tables 1 and 2.
[0258] · Average cooling rate in the first stage: Average cooling rate in the temperature range of 450 to 395°C
[0259] Average cooling rate in the second stage: Average cooling rate in the temperature range of 395 to 340°C
[0260] Average cooling rate in the third stage: Average cooling rate in the temperature range of 340 to 280°C
[0261] It should be noted that in the cooling process, the steel material is cooled by blowing N2 gas onto the plated steel material. At this time, the cooling is performed while adjusting the blowing amount of N2 gas so as to achieve a predetermined cooling rate in the above-mentioned temperature range.
[0262] - Various measurements -
[0263] A sample was cut out from the obtained plated steel sheet, and the following items were measured according to the above-mentioned method.
[0264] Average value of the cumulative perimeter of the Zn / Al / MgZn2 ternary eutectic (recorded as "perimeter of the ternary eutectic" in the table)
[0265] Area fraction of Zn / Al / MgZn2 ternary eutectic (recorded as “area fraction of ternary eutectic” in the table)
[0266] ·Thickness of the Al-Fe alloy layer (In the example where a Ni-pre-plated steel sheet is used as the base steel material, the thickness of the Al-Ni-Fe alloy layer is indicated.)
[0267] -Processability-
[0268] A sample was cut out from the obtained plated steel sheet. Then, the sample was subjected to 1T bending, and the processed portion was tape-peeled to evaluate the area ratio of the plated layer attached to the tape. The area ratio of the attached plated layer was evaluated as "A" when it was 5% or less, and "NG" when it exceeded 5%.
[0269] -Corrosion resistance-
[0270] A sample was cut out from the obtained plated steel sheet. Then, the sample was laid flat and subjected to 21 cycles of a combined cycle corrosion test (CCT) according to the corrosion acceleration test (JASO M609-91). After the corrosion test, the corrosion loss was 35 g / m 2 The following situations are rated as "A" and will exceed 35g / m 2 Rated as "NG".
[0271] The Examples are listed in Tables 1 and 2.
[0272] [Table 1-1]
[0273]
[0274] [Table 1-2]
[0275]
[0276] [Table 1-3]
[0277]
[0278] [Table 1-4]
[0279]
[0280] [Table 2-1]
[0281]
[0282] [Table 2-2]
[0283]
[0284] [Table 2-3]
[0285]
[0286] [Table 2-4]
[0287]
[0288] From the above results, it is understood that the examples of the plated steel materials according to the present disclosure are superior in workability compared to the comparative examples, and are superior in corrosion resistance even when used in an environment where water easily accumulates.
[0289] In Test No. 95, since a large amount of non-plating occurred and the appearance was highly uneven, the perimeter and area fraction of the ternary eutectic were not measured.
[0290] The preferred embodiments and examples of the present disclosure are described in detail above with reference to the attached drawings, but the present disclosure is not limited to the examples. Anyone with ordinary knowledge in the technical field to which the present disclosure belongs can obviously think of various variations or modifications within the scope of the technical ideas recorded in the claims, and these are of course understood to belong to the technical scope of the present disclosure.
[0291] It should be noted that the entire disclosure of Japanese Patent Application No. 2022-044295 is incorporated into this specification by reference.
[0292] All documents, patent applications, and technical standards described in this specification are incorporated into this specification by reference to the same extent as if each document, patent application, and technical standard was specifically and individually described as being incorporated by reference.
Claims
1. A plated steel material comprising: a base steel material; and a plating layer including a Zn-Al-Mg alloy layer disposed on a surface of the base steel material, The coating has the following chemical composition: in mass % it contains: Zn: more than 65.00%, Al: more than 5.00% and less than 25.00%, Mg: more than 3.00% and less than 12.50%, Sn: 0% to 3.00%, Bi: 0% or more and less than 5.00%, In: 0% or more and less than 2.00%, Ca: 0% to 3.00%, Y:0%~0.50%、 La: 0% or more and less than 0.50%, Ce: 0% or more and less than 0.50%, Si: 0% or more and less than 2.50%, Cr: 0% or more and less than 0.25%, Ti: 0% or more and less than 0.25%, Zr: 0% or more and less than 0.25%, Mo: 0% or more and less than 0.25%, W: 0% or more and less than 0.25%, Ag: 0% or more and less than 0.25%, P: 0% or more and less than 0.25%, Ni: 0% or more and less than 0.25%, Co: 0% or more and less than 0.25%, V: 0% or more and less than 0.25%, Nb: 0% or more and less than 0.25%, Cu: 0% or more and less than 0.25%, Mn: 0% or more and less than 0.25%, Li: 0% or more and less than 0.25%, Na: 0% or more and less than 0.25%, K: 0% or more and less than 0.25%, Fe: 0% to 5.00%, Sr: 0% or more and less than 0.50%, Sb: 0% or more and less than 0.50%, Pb: 0% or more and less than 0.50%, B: 0% or more and less than 0.50%, and Impurities, In the reflected electron image of the Zn-Al-Mg alloy layer obtained by observing the surface of the plated layer at a magnification of 100 times using a scanning electron microscope after grinding the surface of the plated layer to 1 / 2 of the layer thickness, there is a Zn / Al / MgZn2 ternary eutectic, and the average value of the cumulative circumference of the Zn / Al / MgZn2 ternary eutectic is 100 to 300 mm / mm 2 .
2. The plated steel material according to claim 1, wherein: The plating layer includes an Al—Fe alloy layer between the base steel material and the Zn—Al—Mg alloy layer.
3. The plated steel material according to claim 1 or claim 2, wherein: The interface roughness Ra between the base steel material and the coating is 0.3-2.0 μm.
4. The method for producing a plated steel material according to claim 1 or claim 2, wherein: A base steel material having a surface roughness Ra of 0.3 to 2.0 μm on the plated surface is immersed in a plating bath, and after being scooped out of the plating bath, is cooled in a temperature range of 450 to 395°C at an average cooling rate of 5 to 20°C / s, in a temperature range of 395 to 340°C at an average cooling rate of less than 3°C / s, and in a temperature range of 340 to 280°C at an average cooling rate of 10 to 20°C / s.
Citation Information
Patent Citations
Zinc alloy plated steel material having excellent weldability and processed-part corrosion resistance and method of manufacturing same
CN107223166A
High corrosion-resistant hot-dip galvanized steel sheet excellent in appearance uniformity
JP2013014794A
Plated steel
WO2018139619A1
Plated steel material
WO2021095442A1