Deposition of ceramic layers using liquid organometallic precursors
By using a mixture of non-halogenated liquid organometallic compounds and gaseous carbon, nitrogen or oxygen for chemical vapor deposition, the problem of difficult transportation of high-melting halides and toxic by-products is solved, and efficient and safe deposition of the ceramic layer is achieved.
Patent Information
- Application Number
- CN202380018052.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-01-21
- Filing Date
- 2023-01-20
- Publication Date
- 2024-11-01
AI Technical Summary
In the existing chemical vapor deposition technology, the use of metal halides as the precursor of the ceramic layer has problems of transporting difficulties and toxic by-products, especially high melting point solid halides are difficult to transport and produce halogen-containing gases.
Using non-halogenated liquid organometallic compounds as metal precursors, a conveyable mixture is formed by mixing gaseous carbon, nitrogen or oxygen with liquid organometallic precursors to deposit ceramic layers, using the low melting point and halogen-free properties of liquid organometallic compounds. Avoid the production of complex conveying systems and toxic gases.
It realizes efficient deposition of ceramic layers, reduces or eliminates toxic and corrosive by-products, improves the safety of the deposition process and the purity of the product, and is suitable for applications such as nuclear fuel.
Smart Images

Figure BDA0004954315560000051 
Figure BDA0004954315560000061 
Figure HDA0004954315570000011
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This nonprovisional application claims the benefit of U.S. Provisional Patent Application No. 63 / 301,656, filed on January 21, 2022. The entire disclosure of the prior application is incorporated herein by reference. Technical Field
[0003] Various exemplary embodiments disclosed herein generally relate to the deposition of ceramic materials using non-halogenated liquid organometallic compounds as metal precursors. In particular, embodiments disclosed herein relate to the deposition of ceramic layers on solid substrates by chemical vapor deposition using non-halogenated liquid organometallic compounds as metal precursors. In addition, embodiments disclosed herein relate to the infiltration of ceramic materials into porous or particulate substrates by chemical vapor infiltration using non-halogenated liquid organometallic compounds as metal precursors. Background Art
[0004] Chemical vapor deposition (CVD) of metal-containing ceramics for nuclear fuel particles is traditionally performed in fluidized bed reactors using metal halides. Some halogen-containing metal or metalloid compounds are liquids that can be easily delivered to the CVD deposition system. For example, silane such as Si(CH3) (4-n) Cl n It is a liquid that can be injected into the carrier gas line of the CVD deposition system. However, many metal halides are high melting point solids, that is, solids that melt at >200°C, and they are not easy to be transported into the CVD system. Metal halide deposition sources may also produce halogen-containing toxic gas byproducts.
[0005] Chemical vapor deposition is used to make nuclear fuel particles. For example, a tri-structural isotropic (TRISO) nuclear fuel particle includes two layers of carbon deposited on a nuclear fuel core, followed by a silicon carbide (SiC) layer and an outer layer of dense pyrolytic carbon (PyC). The SiC layer is typically deposited using methyltrichlorosilane (MTS) or another liquid chlorosilane introduced into a chemical vapor deposition reactor via a carrier gas. While this method works well for depositing silicon-based ceramic layers, chemical vapor deposition is inconvenient using chlorides of other metals such as zirconium, hafnium or tungsten because these chlorides are typically high melting point solids.
[0006] In view of the above, it is desirable to develop a technique for depositing a ceramic layer using a precursor gas containing a liquid or low melting point metal. In particular, it is desirable to develop a technique for depositing a ceramic layer using a precursor gas containing a non-halogenated metal. Summary of the invention
[0007] The present disclosure relates to novel CVD and chemical vapor infiltration (CVI) systems and methods that allow gaseous carbon, nitrogen or oxygen precursors to be mixed with liquid organometallic precursors. The resulting mixture can be transported to a CVD or CVI reactor and used to deposit a ceramic layer. The liquid organometallic precursor can be transported to an evaporation unit with a limited liquid flow rate through a liquid mass flow controller (e.g., a valve, such as a ball valve or a needle valve). When the liquid of the limited flow rate flows into the evaporator, the carrier gas is mixed into the liquid and heated in the evaporation unit at or above the boiling temperature of the liquid. The liquid is evaporated and transported to a CVD or CVI reaction chamber. The systems and methods disclosed herein can be used to deposit ceramic materials directly onto nuclear fuels. This also allows ceramic matrix materials to be infiltrated into porous fuel forms, or surface coatings of solid fuel forms, by chemical metal infiltration. Therefore, the systems and methods disclosed herein allow the production of structural metals or ceramic nuclear fuels.
[0008] New organometallic precursors, such as liquid organometallic compounds of zirconium, hafnium, niobium, tantalum, tungsten, titanium and vanadium, have been identified as useful CVD or CVI metal precursors for depositing ceramic materials using the systems and methods disclosed herein. These liquid organometallic compounds can be introduced into a CVD or CVI system or reactor without the need for a complex delivery system. A technique has been developed for delivering liquid organometallic precursors to a CVD or CVI system using a liquid evaporator that saturates the carrier gas delivered to the chemical reactor. This saturated gas mixture can be delivered directly to a reactor for depositing a metal layer, or mixed with other gases (e.g., a gaseous carbon source, a gaseous nitrogen source and / or a gaseous oxygen source) for producing various ceramic coatings, and / or for depositing ceramic matrix materials into porous materials by CVI.
[0009] In addition, due to the use of halogen-free liquid organometallic compounds as metal precursors for CVD or CVI deposited ceramic materials, the systems and methods disclosed herein significantly reduce and / or eliminate toxicity and corrosiveness during the deposition of ceramic layers on particulate substrates (including nuclear fuel cores). The systems and methods disclosed herein allow for the production of cermets directly on nuclear fuel, with increased safety and avoidance of the release of toxic halogen gases into the environment.
[0010] Various embodiments disclosed herein relate to a method for depositing a metal or ceramic layer by chemical vapor deposition by introducing particles into a fluidized bed reactor; heating the fluidized bed reactor to a desired operating temperature T1; and starting a carrier gas to flow through an evaporator. A non-halogenated liquid organometallic precursor is introduced into the evaporator and evaporated. A first mixture of the carrier gas and the evaporated non-halogenated liquid organometallic precursor is allowed to leave the evaporator and is optionally mixed with a gaseous carbon source, a gaseous nitrogen source, a gaseous oxygen source, or a mixture thereof to obtain a second mixture. If a gaseous carbon source, a gaseous nitrogen source, or a gaseous oxygen source is not used, the first mixture flows into a fluidized bed reactor at an operating temperature T1 to deposit the desired metal coating on the particles. Alternatively, a second mixture containing a carbon source, a nitrogen source, or an oxygen source flows into a fluidized bed reactor at an operating temperature T1 to deposit the desired ceramic coating on the particles.
[0011] In various embodiments disclosed herein, the step of introducing particles into a fluidized bed reactor includes introducing particles as nuclear fuel cores. The particles may be nuclear fuel cores, the nuclear fuel cores being selected from the group consisting of oxides, carbides, carbon oxides and nitrides of metals, the metals being selected from the group consisting of uranium, plutonium and thorium. The particles may be nuclear fuel cores, the nuclear fuel cores being selected from the group consisting of uranium oxide, uranium carbide, uranium nitride, uranium oxycarbide and mixtures thereof.
[0012] In various embodiments, each particle includes a nuclear fuel core and at least one carbon layer on the core. Each nuclear fuel core may have multiple carbon layers, including, for example, a porous carbon buffer layer on the core and a pyrolytic carbon dense layer on the buffer layer.
[0013] In various embodiments, each particle includes a nuclear fuel core and at least one ceramic layer on the core. Each nuclear fuel core may have multiple ceramic layers, such as metal oxide layers, metal carbide layers, metal nitride layers, metal oxycarbide layers, or alloy layers thereof.
[0014] In various embodiments of the method for depositing a metal or ceramic layer by chemical vapor deposition, a second mixture containing a carbon source, a nitrogen source or an oxygen source flows into a fluidized bed reactor operating at an operating temperature T1 to deposit a desired ceramic coating on the particles. The method may also include the following steps:
[0015] depositing an inner carbon layer on the nuclear fuel core prior to introducing the non-halogenated liquid organometallic precursor into the vaporizer; and
[0016] An outer carbon layer is deposited over the desired ceramic coating.
[0017] The non-halogenated liquid organometallic precursor may be a compound of a metal selected from the group consisting of Zr, Hf, Nb, Ta, W, V, Ti and mixtures thereof. The metal in the non-halogenated liquid organometallic precursor may be combined with an alkoxy group, an amino group, an imino group or a combination thereof.
[0018] In various embodiments, the non-halogenated liquid organometallic precursor has the formula M +n L n 、M +n L 1 (n-m) L 2 (m) or (L 3 =) p M +n L (n-2p) ,in:
[0019] M is Zr, Hf, Nb, Ta, W, V, Ti or a mixture thereof;
[0020] L and L 1 Independently selected from C1-C4 alkyl groups, C1-C4 alkoxy groups, bis(C1-C4 dialkyl)amide groups or combinations thereof;
[0021] L 2 It is a cyclopentadienyl anion;
[0022] L 3 is O= or RN=, wherein R is an alkyl group;
[0023] m is 1 or 2;
[0024] p is 1 or 2; and
[0025] The valence of metal M is n.
[0026] The non-halogenated liquid organometallic precursor can be:
[0027] a metal alkoxide selected from the group consisting of titanium (IV) isopropoxide, titanium (IV) isobutoxide, hafnium (IV) butoxide, niobium (V) tert-butoxide, niobium (III) tert-butoxide, and zirconium (IV) butoxide; or
[0028] A metal amine selected from the group consisting of:
[0029] (tert-Butylimino)tris(diethylamino)tantalum(V);
[0030] (tert-Butylimino)tris(diethylamino)niobium(V);
[0031] (tert-Butylimino)tris(methylethylamino)niobium(V);
[0032] Tris(diethylamino)niobium(III);
[0033] Tris(methylethylamino)niobium(III);
[0034] Tris(diethylamino)niobium(III);
[0035] Tris(dimethylamino)cyclopentadienylzirconium(IV);
[0036] Tetrakis(isopropylmethylamino)zirconium(IV);
[0037] Tetrakis(ethylmethylamino)zirconium(IV);
[0038] Tetrakis(diethylamino)zirconium(IV);
[0039] Tris(dimethylamino)cyclopentadienylhafnium(IV);
[0040] Bis(methylimino)bis(dimethylamino)tungsten(VI); and
[0041] Bis(tert-butylimino)bis(dimethylamino)tungsten(VI).
[0042] In various embodiments, the second mixture comprises a carbon source, a nitrogen source, or an oxygen source. The second mixture may comprise a gaseous carbon source; and the second mixture may flow into a fluidized bed reactor to deposit a desired metal carbide coating on the particles. The second mixture may comprise a gaseous nitrogen source; and the second mixture may flow into a fluidized bed reactor to deposit a desired metal nitride coating on the particles. The second mixture may comprise a gaseous oxygen source; and the second mixture may flow into a fluidized bed reactor to deposit a desired metal oxide coating on the particles.
[0043] Various embodiments disclosed herein relate to a method for providing a porous substance having a metal or ceramic matrix by chemical vapor infiltration. The method comprises the following steps:
[0044] introducing a porous substance into a chemical vapor infiltration reactor;
[0045] Heating the chemical vapor infiltration reactor to a desired operating temperature T1;
[0046] Start the flow of carrier gas through the evaporator;
[0047] injecting a non-halogenated liquid organometallic precursor into an evaporator, and evaporating the non-halogenated liquid organometallic precursor;
[0048] allowing a first mixture of a carrier gas and a vaporized non-halogenated liquid organometallic precursor to exit a vaporizer;
[0049] Optionally, mixing the first mixture with a gaseous carbon source, a gaseous nitrogen source, a gaseous oxygen source or a mixture thereof to obtain a second mixture; and allowing the first mixture to flow into a chemical vapor infiltration reactor operating at an operating temperature T1 and pass through a porous substance to deposit a desired metal matrix in the void space of the porous substance; or
[0050] The second mixture is flowed into a chemical vapor infiltration reactor operating at temperature T1 and passed through a porous mass to deposit a desired ceramic matrix within the void spaces of the porous mass.
[0051] In the chemical vapor infiltration method, the non-halogenated liquid organometallic precursor can be a compound of a metal selected from the group consisting of Zr, Hf, Nb, Ta, W, V, Ti and mixtures thereof. The metal in the non-halogenated liquid organometallic precursor can be combined with an alkoxy group, an amino group, an imino group or a combination thereof. The non-halogenated liquid organometallic precursor can have a formula M +n L n 、M +n L 1 (n-m) L 2 (m) or (L3=) p M +n L (n-2p) ,in:
[0052] M is Zr, Hf, Nb, Ta, W, V, Ti or a mixture thereof;
[0053] L and L 1 Independently selected from C1-C4 alkyl groups, C1-C4 alkoxy groups, bis(C1-C4 dialkyl)amide groups or combinations thereof;
[0054] L 2 It is a cyclopentadienyl anion;
[0055] L 3 is O= or RN=, wherein R is an alkyl group;
[0056] m is 1 or 2;
[0057] p is 1 or 2; and
[0058] n is the valence of the metal M.
[0059] Various embodiments disclosed herein relate to a method of coating a metal or ceramic layer on a solid material by chemical vapor deposition, comprising the steps of:
[0060] introducing a solid material into a chemical vapor deposition reactor;
[0061] heating the chemical vapor deposition reactor to a desired operating temperature T1;
[0062] Start the flow of carrier gas through the evaporator;
[0063] injecting a non-halogenated liquid organometallic precursor into an evaporator, and evaporating the non-halogenated liquid organometallic precursor;
[0064] allowing a first mixture of a carrier gas and a vaporized non-halogenated liquid organometallic precursor to exit a vaporizer;
[0065] Optionally, mixing the first mixture with a gaseous carbon source, a gaseous nitrogen source, a gaseous oxygen source, or a mixture thereof to obtain a second mixture; and
[0066] Allowing the first mixture to flow into a chemical vapor deposition reactor operating at temperature T1 to deposit a desired metal coating on a solid material; or
[0067] The second mixture is flowed into a chemical vapor deposition reactor operating at temperature T1 to deposit a desired ceramic coating on the solid material.
[0068] In the method of coating a metal or ceramic layer on a solid material by chemical vapor deposition, the non-halogenated liquid organometallic precursor may be a compound of a metal selected from the group consisting of Zr, Hf, Nb, Ta, W, V, Ti and mixtures thereof. The metal in the non-halogenated liquid organometallic precursor may be combined with an alkoxy group, an amino group, an imino group or a combination thereof. BRIEF DESCRIPTION OF THE DRAWINGS
[0069] For a better understanding of the various exemplary embodiments, reference is made to the accompanying drawings, in which:
[0070] Figure 1 A prior art fluidized bed CVD system is shown which uses solid metal halides as metal precursors for depositing ceramic layers.
[0071] 2A and 2B show the Figure 1 Particles with a ceramic layer deposited by the system.
[0072] Figure 3 Shown by Figure 1 Nuclear fuel particles with a ceramic layer deposited by the system.
[0073] Figure 4 and Figure 5 Shows Figure 1 A modification of the system allows the deposition of ceramic layers containing metal mixtures.
[0074] Figure 6 A fluidized bed CVD system for depositing ceramic layers using liquid organometallic compounds as metal precursors is shown.
[0075] Figure 7 A flow chart showing a fluidized bed CVD method for depositing a ceramic layer using a liquid organometallic compound as a metal precursor is shown.
[0076] Figure 8 and Fig. 9 A system for evaporating a liquid organometallic compound to produce a gaseous metal precursor for depositing a ceramic layer is shown.
[0077] Fig.10a Shows Figure 6 The first modification of the evaporator in the system allows the deposition of ceramic layers containing metal mixtures.
[0078] Fig.10b Shows Figure 6 A second modification of the evaporator in the system allows the deposition of ceramic layers containing metal mixtures.
[0079] Fig.11 A flow chart showing a fluidized bed CVD method for depositing a mixed metal containing ceramic layer using a mixture of liquid organometallic compounds as metal precursors is shown.
[0080] Fig.12a and 12b An isobaric chemical vapor infiltration (CVI) reactor is shown.
[0081] Fig.13 Products produced by chemical vapor infiltration (CVI) are shown.
[0082] Fig.14 Products produced by chemical vapor deposition (CVD) on bulk material are shown.
[0083] Fig.15 A forced flow chemical vapor infiltration (CVI) reactor is shown.
[0084] Fig.16 A tubular chemical vapor deposition (CVD) reactor is shown. DETAILED DESCRIPTION
[0085] Referring now to the drawings, wherein like numerals indicate like components or steps, broad aspects of various exemplary embodiments are disclosed.
[0086] As used herein, a TRISO particle comprises a uranium-based ceramic nuclear fuel core as a core, coated in sequence with:
[0087] inner porous carbon layer;
[0088] Internal dense pyrolytic carbon layer;
[0089] Ceramic layers, such as carbides, nitrides, oxides or oxycarbides of metals; and
[0090] External dense pyrolytic carbon layer.
[0091] As used herein, TRISO-like particles include a ceramic nuclear fuel core, such as an oxide, carbide, nitride or oxycarbide of uranium, plutonium, thorium or a mixture thereof as a core; coated with at least one carbon layer and at least one ceramic layer, such as a carbide, nitride, oxide or oxycarbide of a metal. The carbon layer and the ceramic layer can be deposited in any order.
[0092] Oxides, carbides, nitrides and borides of metals such as zirconium, hafnium, vanadium, niobium, tantalum and titanium are highly valued due to their chemical and mechanical properties. These properties include high melting points, density and hardness. This makes thin ceramic layers of zirconium, hafnium, niobium, tantalum or mixtures thereof highly valuable in nuclear applications for both terrestrial and space applications. However, the chlorides and other halides of these metals are high melting point solids, as shown in Table 1. While these compounds can be evaporated by sublimation, in many cases sublimation occurs at temperatures in excess of 300°C, as shown in Table 1.
[0093] Chemical vapor deposition (CVD) and chemical vapor infiltration (CVI) of oxides, carbides, borides, and nitrides of transition metals have historically been difficult due to the use of halide-based metal precursors, such as the metal halide salts of Table 1. Utilization of these halide-based precursors is difficult for two reasons:
[0094] The presence of halides, which can cause toxicity and corrosion problems, and
[0095] The chemistry of halides is not ideal.
[0096]
[0097]
[0098] Table 1. Thermal properties of metal halide CVD source compounds.
[0099] The halides in Table 1 are not ideal for CVD / CVI because they exist as solids at standard temperature and pressure (STP) and / or have low vapor pressures at STP. Due to these non-ideal chemical properties, delivery of the Table 1 precursors requires complex delivery systems, such as pneumatic delivery systems, metal chlorination systems, or salt sublimation furnaces. This makes CVD and CVI production of metal carbides very difficult and not feasible outside of laboratory scale operations.
[0100] Some metal halide precursors, such as vanadium(IV) chloride and titanium(IV) chloride, are liquids at STP. While this makes them appear to be useful CVD / CVI metal deposition source materials, they are not without problems. They contain halides that may generate halogen gas and / or hydrogen halide gas at deposition temperatures. For example, when vanadium(IV) chloride is heated, it may generate toxic fumes of vanadium oxide and chlorine-containing gases.
[0101] Figure 1 A prior art system for depositing a ceramic layer using solid metal halide MX4 as a metal source 11 is shown. A carrier gas enters the sublimation furnace 10 through a gas inlet 12. The carrier gas carries the evaporated metal halide MX4. 4(vap) The sublimation furnace 10 passes through the outlet 13. A valve or other mass flow controller 14 controls the speed of the carrier gas through the outlet 13. The valve 14 can be responsive to the MX 4(vap) The signal of the concentration sensor (not shown) is used to adjust the carrier gas flow rate. If the metal concentration in the carrier gas is lower than the desired value, the carrier gas flow rate can be increased using valve 14. If the metal concentration in the carrier gas is higher than the desired value, the carrier gas flow rate can be reduced using valve 14.
[0102] Figure 1 The system includes at least one of a gaseous oxygen source 16a, a gaseous nitrogen source 16b and a gaseous carbon source 16c. These oxygen sources, nitrogen sources and carbon sources flow through gas inlets 15a, 15b and 15c, respectively. Valves 17a, 17b and 17c can be used to control the flow rates of the oxygen source, nitrogen source and carbon source, respectively. For example, if carbide ceramics are required, valve 17c can be opened and valves 17a and 17b can be closed. For example, if nitride ceramics are required, valve 17b can be opened and valves 17a and 17c can be closed. If carbonitride ceramics are required, valves 17b and 17c can be opened and valve 17a can be closed. The oxygen source, nitrogen source and carbon source flow through the gas flow channel 15, which merges with the outlet 13 of the sublimation furnace 10. Then, the carrier gas in the outlet 13 carries the evaporated metal halide MX 4(vap) , and the oxygen source, nitrogen source and / or carbon source gas from the gas flow channel 15 enter the channel 18 and flow to the fluidized bed reactor 19. In the fluidized bed reactor 19, the evaporated metal halide MX 4(vap) Reacting with the oxygen, nitrogen and / or carbon source gases to produce a ceramic coating on the particles 21, the carrier gas leaves the reactor through passage 20. The fluidized bed reactor 19 is heated by a heat source 19a, which may be a resistive heat source 19a configured to flow electrical energy through the reactor 19.
[0103] Figure 2a Shows Figure 1 The core particle 1 with a ceramic coating 4 is produced by a system. The particle 1 can be a solid metal or a ceramic. Figure 1 The core particle 1 is not melted at the deposition temperature of the fluidized bed reactor 19. In various embodiments, the core particle 1 is a nuclear fuel core. As used herein, the "fuel core 1" is a core particle 1 made of a radioactive ceramic material.
[0104] Figure 2b Shows Figure 1 The particle 1 having a ceramic coating 4 produced by the system of the present invention, wherein the coating 4 can have different structures. The particle 1 can be a solid metal or a ceramic. The coating 4 can have an inner layer 4a, an intermediate layer 4b and an outer layer 4c, and can be formed by adjusting the flow rate of the deposition gas during deposition in the fluidized bed reactor 19. For example, in one embodiment, the layers 4a to 4c are metal carbide layers M n C (2-n) , where the ratio of metal to carbon is different. During the deposition of layer 4a, the metal halide MX with respect to the evaporated 4(vap) The carbon source gas is concentrated so that n<1, n<0.8 or n≤0.5, and the metal carbide layer 4a is rich in carbon. During the deposition of layer 4b, the concentration of the carbon source gas is relative to the evaporated metal halide MX 4(vap) can be reduced, so n = 1, the metal carbide layer 4b is MC. During the deposition of layer 4c, the concentration of the carbon source gas relative to the evaporated metal halide MX 4(vap) It can be further reduced, so that n>1, and the metal carbide layer 4c is carbon-poor.
[0105] Figure 1 The system can be used to produce Figure 3 A tri-structural isotropic (TRISO) nuclear fuel particle is shown. The TRISO particle comprises a core particle 1, wherein the particle 1 is a fuel core core having a center composed of a uranium ceramic material, such as uranium oxide (e.g., UO2 or U3O8), uranium carbide (UC), uranium nitride (e.g., UN2 or U2N3) or uranium oxycarbide (UCO), coated with three isotropic materials deposited by chemical vapor deposition in a fluidized bed reactor 19. The fuel core core 1 is coated with a porous buffer layer 2 made of carbon, followed by a dense inner layer 3 of pyrolytic carbon (PyC), followed by a ceramic layer 4 that improves the structural integrity of the TRISO particle, followed by a dense outer layer 5 of PyC.
[0106] In various embodiments, Figure 1 The system can be used to produce similar Figure 3 A TRISO-like nuclear fuel particle is shown. The TRISO-like particle contains a fuel core 1 in the center, which is composed of a radioactive ceramic material, such as an oxide, carbide, oxycarbide or nitride of plutonium or thorium. The fuel core is coated with an isotropic material deposited by chemical vapor deposition in a fluidized bed reactor 19. The fuel core 1 can be coated with at least one of the following:
[0107] a porous buffer layer 2 made of carbon deposited on the fuel core,
[0108] a dense inner layer 3 of pyrolytic carbon (PyC) deposited on the fuel core; and
[0109] Ceramic layer 4.
[0110] The fuel core 1 may be coated with a porous carbon buffer layer and a pyrolytic carbon inner layer, which are sequentially deposited on the fuel core 1. The carbon-coated fuel core may then be coated with a ceramic layer 4 to increase the structural integrity of the TRISO-like particle, optionally followed by a PyC dense outer layer 5. In various embodiments, the fuel core 1 may be coated with a ceramic layer without depositing an intermediate carbon layer on the fuel core 1.
[0111] In various embodiments, Figure 1 The system can be used to produce TRISO-like nuclear fuel particles, which contain a fuel core 1 consisting of a radioactive ceramic material (e.g., an oxide, carbide, oxycarbide or nitride of uranium, plutonium or thorium) in the center. The fuel core can then be directly coated with a ceramic layer 4 without an intermediate carbon layer. The ceramic-coated fuel core can then optionally be coated with a PyC outer layer 5.
[0112] exist Figure 1 One problem with using solid metal halides as metal sources in systems is that it limits the options for preparing ceramic layers containing mixed metals by CVD. Figure 4 Shows Figure 1 The system modification scheme uses the first solid metal halide 11a (M 1 X4 and the second solid metal halide 11b (M 2 X4). The carrier gas leaving through the outlet 13 carries the evaporated metal halide M from the sublimation furnace 10. 1 X 4(vap) and M 2 X 4(vap) However, in the sublimation furnace, both halides 11a and 11b must be solid at the sublimation temperature, and both must have a reasonable vapor pressure at the desired sublimation temperature. Referring to Table 1, ZrCl4 and HfCl4 have similar melting points and sublimation temperatures, and can be co-deposited by CVD from the sublimation furnace 10, such as Figure 4 However, in the sublimation furnace 10, the evaporated metal halide M 1 X 4(vap) and M 2 X 4(vap) exists in equilibrium, resulting in a sediment containing a fixed proportion of M 1 and M 2In the case of mixed metal ceramics, it is difficult to control the final product. In addition, it may be desirable to co-deposit a first metal from a metal halide with a high sublimation temperature (e.g., ZrCl4) and a second metal from a metal halide with a low sublimation temperature (e.g., TaCl5). This cannot be achieved with Figure 4 A single sublimation furnace 10 is shown as conveniently implemented.
[0113] These problems can be solved by using multiple sublimation furnaces, such as Figure 5 The sublimation furnace 10a receives a carrier gas through a gas inlet 12a and contains a gas having a first sublimation temperature. 1 The first metal deposition precursor 11a of X4. The carrier gas carries the evaporated metal halide M from the sublimation furnace 10a. 1 X 4(vap) The sublimation furnace 10b receives a carrier gas through the gas inlet 12b and contains a second sublimation temperature of formula M. 2 The second metal deposition precursor 11b of X4. The carrier gas carries the evaporated metal halide M from the sublimation furnace 10b. 2 X 4(vap) Through outlet 13b. Outlets 13a and 13b each have valves (14a and 14b, respectively) for controlling the gas flow rate to their respective sublimation furnaces 10a and 10b. Outlets 13a and 13b may be combined to form a common gas flow line 13 leading to a fluidized bed reactor, typically such as Figure 1 shown.
[0114] Figure 5 The system allows the co-deposition of a first metal from a first metal halide sublimation source 11a having a high sublimation temperature (e.g., ZrCl4) and a second metal from a second metal halide sublimation source 11b having a low sublimation temperature (e.g., TaCl5). This can be achieved by heating the sublimation furnace 10a to a temperature at which the metal halide sublimation source 11a sublimates (e.g., 331°C for ZrCl4) and heating the sublimation furnace 10b to a temperature at which the metal halide sublimation source 11b sublimates (e.g., about 200°C for TaCl4). In addition, Figure 5 The system allows for co-deposition of a first metal from a first metal halide sublimation source 11a and a second metal from a second metal halide sublimation source 11b, where 11a and 11b have similar sublimation temperatures, such as ZrCl4 and HfCl4. This can be achieved by heating the sublimation furnace 10a and the sublimation furnace 10b to the sublimation temperature. The relative flow rates of the metal-containing carrier gas from the sublimation furnace 10a and the metal-containing carrier gas from the sublimation furnace 10b can be adjusted by using valves 22a and 22b to control the M content of the final deposited product. 1 With M 2 However, when using Figure 5When using a system with two independent sublimation furnaces, the complexity of the system is increased. In addition, it cannot avoid the formation of toxic halogen and hydrogen halide gases.
[0115] Figure 6 shows the use of liquid non-halogenated metal compounds ML 4(l) Systems for depositing ceramic layers as metal sources. The use of liquid non-halogenated metal compounds eliminates the need for a sublimation furnace and avoids the formation of toxic halogen-containing byproducts during CVD / CVI. Figure 6 In the system, a carrier gas enters the evaporator 23 through the gas inlet 12, and the flow rate of the carrier gas is controlled by a valve 30. The liquid non-halogenated metal compound is injected into the evaporator 23 through the inlet 32. The metal compound is evaporated, and the carrier gas carries the evaporated metal compound ML from the evaporator 23. 4(vap) Through outlet 13. A valve or other mass flow controller 14 controls the rate at which the carrier gas passes through outlet 13. Figure 6 The system includes at least one of a gaseous oxygen source 16a, a gaseous nitrogen source 16b and a gaseous carbon source 16c. These oxygen sources, nitrogen sources and carbon sources are similar to Figure 1 The oxygen source, nitrogen source and carbon source flow into the gas flow channel 15 through valves 17a, 17b and 17c, respectively, and the gas flow channel 15 merges with the outlet 13 of the evaporator 23. Then, the carrier gas in the outlet 13 carries the evaporated metal compound, and the oxygen source, nitrogen source and / or carbon source gas from the gas flow channel 15, enters the channel 18, and flows into the fluidized bed reactor 19. The carrier gas flow rate from the outlet 13 to the reactor 19 through the channel 18 can be controlled by the valve 14. Figure 6 The control valve used in the system can be a needle valve that can restrict the flow of fluid or gas in an incremental manner, allowing the needle valve to regulate the flow rate of the carrier gas flowing into the reactor 19, the carrier gas carrying the evaporated metal precursor, and the carbon source, nitrogen source and / or oxygen source. Figure 6 The valve used in the system can be a ball valve; however, ball valves do not allow incremental adjustment of flow and are therefore not preferred. Other types of valves that can be used include diaphragm valves, stop valves, pinch valves, bellows seals, and butterfly or throttle valves. Weir-type diaphragm valves are particularly useful for controlling the flow rate through the valve by incrementally restricting the flow of a fluid or gas.
[0116] The fluidized bed reactor 19 is maintained at a desired temperature T1 suitable for depositing a coating on the particles 21 and a pressure suitable for deposition. The fluidized bed reactor 19 is heated by a heat source 19a, which can be a resistive heat source 19a configured to allow electrical energy to flow through the reactor 19. The deposition pressure can be high, for example, greater than atmospheric pressure; atmospheric pressure; or a partial vacuum, for example, below atmospheric pressure. In the fluidized bed reactor 19, the evaporated metal compound reacts with the oxygen source, nitrogen source and / or carbon source gas to produce a ceramic coating on the particles 21, and the carrier gas leaves the reactor through the channel 20. Since the metal compound precursor injected into the evaporator is not a halogenated compound, the ceramic coating is deposited on the particles 21 without generating halogen or hydrogen halide gas. In various embodiments, the deposition of the ceramic layer by chemical vapor deposition using an organic metal compound as a metal precursor can be carried out in a fluidized bed reactor at atmospheric pressure or a partial vacuum. Deposition in the reactor can be carried out at a pressure of 1 Torr to 760 Torr, 1 Torr to 20 Torr, 10 Torr to 200 Torr, 20 Torr to 400 Torr, 20 Torr to 300 Torr, 400 Torr to 760 Torr, 400 Torr to 550 Torr, 300 Torr to 600 Torr, or 200 Torr to 500 Torr.
[0117] exist Figure 6 In the system, the temperature measurement in the evaporator 23 and the chemical deposition reactor 19 is performed using a combination of thermocouples and pyrometers (not shown), which can measure the temperature of the evaporator, the shell of the reactor 19 and the particles 21. Temperatures as low as 10°C or as high as 3000°C can be accurately measured.
[0118] The non-halogenated liquid organometallic precursor may be a compound of a metal selected from the group consisting of Zr, Hf, Nb, Ta, W, V, Ti and mixtures thereof. The metal in the non-halogenated liquid organometallic precursor may be combined with an alkoxy group, an amino group, an imino group or a combination thereof.
[0119] The methods disclosed herein involve using formula M +n L n 、M +n L 1 (n-m) L 2 (m) or (L 3 =) p M +n L (n-2p) The non-halogenated liquid metal compound deposits metal nitrides, carbides and oxides. In these formulas,
[0120] M is Zr, Hf, Nb, Ta, W, V, Ti or a mixture thereof;
[0121] L and L 1independently selected from a C1-C4 alkyl group, a C1-C4 alkoxy group or a bis(C1-C4 dialkyl)amide group;
[0122] L 2 It is a cyclopentadienyl anion;
[0123] L 3 is a divalent free radical, such as O= or RN=, wherein R is an alkyl group;
[0124] m is 1 or 2;
[0125] p is 1 or 2; and
[0126] The valence of metal M is n.
[0127] The discussion here may refer to compound ML4 as an example of a liquid organometallic compound useful as a metal precursor. This should not be understood to exclude compounds of trivalent, pentavalent or hexavalent metals.
[0128] Liquid metal compounds that can be used as metal deposition sources for CVD include:
[0129] Metal alkoxides, for example metal C1-C4 alkoxides, such as titanium(IV)isopropoxide, titanium(IV)isobutoxide, hafnium(IV)butoxide, niobium(V)tert-butoxide, niobium(III)tert-butoxide, and zirconium(IV)butoxide; and
[0130] Metal amines, such as:
[0131] (tert-Butylimino)tris(diethylamino)tantalum(V) t BuN = Ta (NEt2) 3, TBTDET);
[0132] (tert-Butylimino)tris(diethylamino)niobium(V) ( t BuN = Nb(NEt2)3, TBTDEN);
[0133] (tert-Butylimino)tris(methylethylamino)niobium(V) ( t BuN = Nb(NMeEt)3);
[0134] Tris(diethylamino)niobium(III) (Nb(NEt2)3);
[0135] Tris(methylethylamino)niobium(III) (Nb(NMeEt)3);
[0136] Tris(diethylamino)niobium(III) (Nb(NEt2)3);
[0137] Tris(dimethylamino)cyclopentadienylzirconium(IV) (CpZr(NMe2), ZyALD);
[0138] Tetrakis(isopropylmethylamino)zirconium(IV) (Zr(NiPrMe)4, TMPAZ);
[0139] Tetrakis(ethylmethylamino)zirconium(IV) (Zr(NEtMe)4, TEMAZ);
[0140] Tetrakis(diethylamino)zirconium(IV) (Zr(NiPrMe)4, TDEAZ);
[0141] Tris(dimethylamino)cyclopentadienylhafnium(IV) (CpZr(NMe2));
[0142] Bis(methylimino)bis(dimethylamino)tungsten(VI) ((MeN=)2W(NMe2)2); and
[0143] Bis(tert-butylimino)bis(dimethylamino)tungsten(VI) ((tBuN=)2W(NMe2)2).
[0144] Suitable carrier gases include argon, hydrogen, helium, nitrogen, carbon dioxide, and other carrier gases known in the art. The metal deposition source can be combined with a gaseous carbon source to produce a metal carbide ceramic coating. Suitable carbon sources for CVD include gaseous hydrocarbons such as methane, ethane, ethylene, propylene, acetylene, and natural gas. Alternatively, the metal deposition source can be combined with a gaseous oxygen source to produce a metal oxide ceramic coating. Suitable oxygen sources for CVD include ozone, oxygen, nitric oxide, and nitrous oxide. The metal deposition source can be combined with a gaseous nitrogen source to produce a metal nitride ceramic coating. Suitable nitrogen sources for CVD include nitrogen and ammonia. In addition, if desired, the carrier gas containing the evaporated metal deposition source can flow from the evaporator 23 to the fluidized bed reactor 19 without the introduction of a carbon source, an oxygen source, or a nitrogen source, thereby allowing a metal coating to be deposited instead of a ceramic coating. Use Figure 6 In a system of , pure metal layers can be deposited by closing valves 17a, 17b and 17c during CVD / CVI, and optionally removing sources 16a, 16b and 16c from the system.
[0145] Figure 7 Shows the use of Figure 6 Flow chart of the system for depositing ceramic on particles 21. In step 100, particles 21 are added to the fluidized bed reactor 19 for coating. In step 110, the fluidized bed reactor 19 is heated to the desired operating temperature T1. In step 120, a carrier gas is turned on to flow through the evaporator 23. In step 130, a liquid metal precursor ML is added to the evaporator 23. 4(L) Injected into the evaporator 23. In step 140, the evaporated metal precursor ML 4(v)The carrier gas leaves the evaporator 23 through the outlet 13 and mixes with the gaseous carbon source, nitrogen source or oxygen source. In step 150, the mixed gas flows into the fluidized bed reactor 19 operating at the temperature T1, thereby allowing the desired ceramic coating to be deposited on the particles 21 in step 160.
[0146] Figure 8 A first embodiment of an apparatus for evaporating a liquid organometallic compound used as a metal deposition precursor is shown. A liquid precursor compound 26 is delivered to an evaporation unit 23 at a defined liquid flow rate. A liquid supply cylinder 25 is pressurized with an inert gas (e.g., argon, helium, hydrogen, or nitrogen) supplied through an inlet 24. To control the pressure in the cylinder 25, a regulator or mass flow controller (e.g., valve 28) is used to control the flow rate of the pressurized gas. The pressure in the cylinder 25 provides a motive force for the liquid precursor compound 26 to flow into a dip tube 27. The dip tube 27 carries the liquid precursor compound 26 to the evaporator 23. The rate at which the liquid precursor compound 26 enters the evaporator 23 can be controlled by a liquid mass flow controller (e.g., valve 29) that controls the flow through the dip tube 27. As the liquid precursor compound 26 flows into the evaporator 23, a carrier gas flows into the evaporator 23 through the inlet 12. The pressure of the carrier gas in the evaporator can be controlled by adjusting the carrier gas flow rate using a valve 30. In the evaporator 23, the liquid precursor compound 26 is subjected to temperature and pressure conditions that cause the compound 26 to evaporate, and the evaporated compound 26 is mixed with a carrier gas. The evaporated precursor compound 26 is carried by the carrier gas to the outlet 13, which leads to the fluidized bed reactor 19, such as Figure 6 shown.
[0147] If the liquid precursor compound 26 is low-boiling, the evaporator 23 can be maintained at atmospheric pressure and heated to a temperature higher than the normal boiling point (i.e., the boiling point of the liquid precursor compound 26 at 1 standard atmosphere) to evaporate the compound 26. Alternatively, for low-boiling precursor compounds 26, the evaporator 23 can be maintained at ambient temperature, such as 25°C ± 5°C, and the pressure in the evaporator 23 can be reduced until the liquid precursor compound 26 boils. If the liquid precursor compound 26 is high-boiling, the evaporator 23 can be maintained at reduced pressure to reduce the boiling point of the compound 26, and heated until the compound 26 evaporates. For high-boiling compounds 26, boiling under reduced pressure reduces the possibility of thermal degradation of the compound 26 in the evaporator 23.
[0148] In various embodiments, the liquid precursor compound 26 is a liquid organometallic compound of zirconium, hafnium, niobium, tantalum, tungsten, vanadium, or titanium. If the liquid precursor compound 26 is a liquid organometallic compound, a metal-containing ceramic layer can be deposited in the fluidized bed reactor 19. For example, if the liquid precursor compound 26 is ZyALD, a zirconium ceramic layer, such as ZrC, Zr3N4, or ZrO2, can be deposited in the fluidized bed reactor 19.
[0149] Various embodiments disclosed herein include a bubbling cylinder that saturates a carrier gas with vapor of a liquid precursor compound 26. The carrier gas flows into the liquid supply cylinder 25 through the inlet 12. The flow rate of the carrier gas entering the liquid supply cylinder 25 can be controlled using a mass flow controller (e.g., valve 30). The carrier gas from the inlet 12 flows into a bubbler 31, which is submerged below the surface of the liquid precursor compound 26 in the liquid supply cylinder 25. As the carrier gas flows out of the bubbler 31 and passes through the liquid precursor compound 26 in the liquid supply cylinder 25, the liquid precursor compound 26 is entrained into the carrier gas as a vapor. Figure 6 As shown, the carrier gas containing the vaporized precursor compound 26 leaves the liquid supply cylinder 25 through the outlet 13 which leads to the fluidized bed reactor 19 .
[0150] If the liquid precursor compound 26 has a high vapor pressure and / or a low boiling point, then Fig. 9 The system entrains vapor from the liquid precursor compound 26 into the carrier gas without heating the liquid precursor compound 26 in the liquid supply cylinder 25. However, if the liquid precursor compound 26 has a low vapor pressure and / or a high boiling point, it is necessary to heat the liquid supply cylinder 25 to use Fig. 9 The system successfully entrains vapor from a liquid precursor compound 26 into a carrier gas.
[0151] In various embodiments, Fig. 9 The liquid precursor compound 26 used in the system is a liquid organometallic compound of zirconium, hafnium, niobium, tantalum, tungsten, vanadium or titanium.
[0152] The technology disclosed herein can be used to produce ceramic alloys by co-depositing liquid organometallic precursors with each other and / or with other gases. This enables the production of unique alloy cermets for terrestrial and space nuclear applications.
[0153] Fig.10a Shown for Figure 6 The first modification scheme of the evaporator of the system. Fig.10a In the system, the carrier gas enters the evaporator 23 through the gas inlet 12, and the flow rate of the carrier gas is controlled by the valve 30. The first liquid non-halogenated metal compound M 1 L 4(L) The second liquid non-halogenated metal compound M is injected into the evaporator 23 through the inlet 32a. 2 L 4(L) The first liquid non-halogenated metal compound and the second liquid non-halogenated metal compound are injected into the evaporator 23 through the inlet 32b. The flow rates of the first liquid non-halogenated metal compound and the second liquid non-halogenated metal compound are controlled by valves 33a and 33b, respectively. The source of each liquid non-halogenated metal compound can be Figure 8 or Fig. 9 system.
[0154] In the evaporator 23, the metal compound M 1 L4 and M 2 L4 is evaporated, and the carrier gas carries the evaporated metal compound from the evaporator 23 through the outlet 13. A valve or other mass flow controller 14 controls the speed of the carrier gas through the outlet 13. The carrier gas in the outlet 13 then flows to the fluidized bed reactor 19 carrying the evaporated metal compound, such as Figure 6 In various embodiments, valves 33a and 33b can be adjusted to allow M 1 L4 and M 2 L4 flows into the evaporator 23 at a fixed mass ratio, thereby allowing a ceramic alloy of constant composition to be deposited in the reactor 19 .
[0155] Alternatively, valves 33a and 33b may be adjusted so that M 1 L4 and M 2 L4 flows into the evaporator 23 in a variable ratio, thereby allowing a ceramic alloy with a variable composition to be deposited in the reactor 19. For example, if valves 33a and 33b are initially set to allow M 1 L4 and M 2 L4 flows into the evaporator 23 at a molar ratio of 2:1, and the initial deposition is rich in M 1 If valves 33a and 33b are subsequently adjusted so that M 1 L4 and M 2 L4 flows into the evaporator 23 at a molar ratio of 1:2 while continuing to deposit, then the M-rich 2 If valves 33a and 33b are returned to their original positions, the deposition of M-rich 1 This can be carried out in a fluidized bed reactor 19 without terminating the deposition process, producing a plurality of alternating layers, wherein two layers of the first ceramic material are separated by a layer of the second ceramic material.
[0156] Alternatively, during a single deposition process, valves 33a and 33b may be:
[0157] Initial setting is M 1 L4 and M 2 L4 flows into the evaporator 23 at a molar ratio of 2:1, so that the M-rich 1 The first ceramic alloy layer and then
[0158] Adjust M 1 L4 and M 2 L4 flows into the evaporator 23 at a molar ratio of 1:1, so that a substantially equal amount of M is deposited on the first ceramic alloy layer. 1 and M 2The second ceramic alloy layer is then
[0159] Adjust M 1 L4 and M 2 L4 flows into the evaporator 23 at a molar ratio of 1:2, so that M-rich 2 The third ceramic alloy layer.
[0160] Thus, the techniques disclosed herein allow for the deposition of multiple ceramic layers where the composition of each layer is changed in a step-wise manner.
[0161] Fig.10b Shown for Figure 6 The second modification scheme of the evaporator system of the system. Fig.10b In the system, the carrier gas enters the first evaporator 23a through the gas inlet 12a, and the flow rate of the carrier gas is controlled by the valve 30a. 1 L4 (L) The carrier gas is injected into the first evaporator 23a through the inlet 32a. The carrier gas enters the second evaporator 23b through the gas inlet 12b, and the flow rate of the carrier gas is controlled by the valve 30b. 2 L 4(L) The first liquid non-halogenated metal compound and the second liquid non-halogenated metal compound are injected into the second evaporator 23b through the inlet 32b. The flow rates of the first liquid non-halogenated metal compound and the second liquid non-halogenated metal compound are controlled by valves 33a and 33b, respectively. The source of each liquid non-halogenated metal compound can be Figure 8 or Fig. 9 system.
[0162] In the evaporators 23a and 23b, the metal compound M 1 L4 and M 2 L4 is evaporated. The carrier gas carries the evaporated metal compound M from the evaporator 23a. 1 L4 passes through outlet 13a. A valve or other mass flow controller 14a controls the speed of the carrier gas through outlet 13a. Similarly, the carrier gas carries the evaporated metal compound M from evaporator 23b. 2 L4 passes through outlet 13b, where valve 14b controls the speed of the carrier gas passing through outlet 13b. Outlets 13a and 13b can merge into channel 13, and then the carrier gas carries the evaporated metal compound to flow into the fluidized bed reactor 19, generally as Figure 6 In various embodiments, valves 33a and 33b can be adjusted to allow M 1 L4 and M 2 L4 flows into evaporators 23a and 23b at a fixed mass ratio, respectively, thereby allowing a ceramic alloy of a constant composition to be deposited in reactor 19. Valves 33a and 33b can be adjusted to adjust M 1L4 and M 2 L4 flows into the evaporators 23 a and 23 b respectively at a variable mass ratio, thereby allowing a ceramic alloy of variable composition to be deposited in the reactor 19 .
[0163] Fig.11 Shows the use of Figure 6 A flowchart of a modification scheme for depositing a ceramic alloy on particles 21 of a system, wherein the evaporator 23 is as follows Fig.10a Steps 100 to 120 are substantially the same as Figure 7 The flowchart of steps 100 to 120 is the same as that of the embodiment of the present invention. In step 120, the carrier gas is turned on to flow through the evaporator 23. In step 131, the first liquid metal precursor M is 1 L 4(L) Injected into the evaporator 23. In step 132, the second liquid metal precursor M 2 L 4(L) Inject into evaporator 23. If necessary, use Fig.10a Valves 33a and 33b regulate the M entering the evaporator 23. 1 L 4(L) and M 2 L 4(L) The relative flow rate is as shown in step 133. In step 141, the carrier gas carries the evaporated metal precursor M 1 L 4(vap) and M 2 L 4(vap) The mixture leaves the evaporator 23 through the outlet 13 and mixes with a gaseous carbon source, nitrogen source or oxygen source. In step 151, the mixed gas flows into the fluidized bed reactor 19 at the operating temperature T1, thereby allowing the desired ceramic alloy coating, such as M, to be deposited on the particles 21 in step 161. 1 n M 2 (1-n) C.
[0164] Fig.12a and 12b shows metal deposition by chemical vapor infiltration of evaporated organometallic compounds into porous materials. Chemical vapor infiltration uses Figure 6 A similar system is used except that a different reactor 34 is used. The reactor 34 includes a gas inlet 38 which directs the vaporized metal organic deposition precursor ML 4(vap) , a carrier gas and optionally a carbon source, a nitrogen source or an oxygen source are carried to the reactor 34. The inlet 38 can receive the evaporated organic metal deposition precursor from the vaporizer 23, substantially as Figure 6 As shown, and can receive a carbon source, a nitrogen source or an oxygen source from sources 16a, 16b and 16c, substantially as Figure 6The fluidized bed reactor 34 is heated by a heat source 42, which may be a resistive heat source.
[0165] exist Fig.12a and 12b In the embodiment, the screen or grid 35 supports a porous material that serves as a chemical vapor permeation substrate. Fig.12a As shown, the porous mass includes particles 37 supported by a mold 36. Fig.12a As shown, an organometallic precursor gas, which may be mixed with a carbon source, a nitrogen source, or an oxygen source and / or a carrier gas, flows around a porous substance at a constant pressure around a sample. This system provides isobaric chemical vapor infiltration, allowing consistent and high-quality growth of metal or ceramic layers, but requires extended processing times and may not uniformly infiltrate the sample. In various embodiments, the porous substance can be a fibrous material, such as a carbon fiber or ceramic fiber felt or mat.
[0166] As shown in Figure 12, the carrier gas carries ML 4(vap) The carrier gas enters the reactor and passes upward through the porous mass of particles or fibers 37. The metal or ceramic is deposited in the spaces between the particles or fibers 37 to form a consolidated mass. The carrier gas leaves the reactor through exhaust 39. The product after separation from the mold 36 is as shown in FIG. Fig.13 The particles or fibers 37 are surrounded by a matrix of deposited metal or ceramic 38. The system of Figure 12 can also be used to deposit a metal or ceramic layer 40 on a solid material.
[0167] exist Figure 12b In the embodiment, the screen or grid 35 supports a porous material, which includes a self-supporting material 43 of particles or fibers 44. In various embodiments, the self-supporting material 43 may include a solid material of sintered particles 44 or a non-woven material of fibers 44. The sintered particles 44 may be ceramic particles. The non-woven material of fibers 44 may be a ceramic fiber or a carbon fiber material. Figure 12b As shown, the organometallic precursor gas flows around the sample at a constant pressure around the porous material. The system provides isobaric chemical vapor infiltration into the material 43, allowing consistent and high-quality growth of metal or ceramic layers. Since the material 43 is self-supporting, no mold is required.
[0168] Figure 6 The system can be used during deposition of a ceramic layer on TRISO core particles. Figure 6 The system can be used during the deposition of a ceramic layer onto an uncoated nuclear fuel material such as uranium oxide or uranium oxycarbide. Figure 12b The system can be used to deposit a metal or ceramic layer 40 directly onto a solid structural nuclear material or fuel element 41, such as Fig.14 shown. Fig.12aThe system can be used to infiltrate ceramic or metal materials into a porous core material, and after removing the mold 36, the fuel particles 37 are dispersed in the metal matrix or ceramic matrix 38, such as Fig.13 shown.
[0169] Fig.15 Metal deposition by chemical vapor infiltration of vaporized organometallic compounds into porous materials using a forced flow reactor is shown. Fig.15 In the reactor 34, a gas inlet 38 is provided to transfer the evaporated metal organic deposition precursor ML 4(vap) , a carrier gas and optionally a carbon source, a nitrogen source or an oxygen source are carried to the reactor 34. The inlet 34 can receive the evaporated organic metal deposition precursor from the vaporizer 23, substantially as Figure 6 As shown, and can receive a carbon source, a nitrogen source or an oxygen source from sources 16a, 16b and 16c, substantially as Figure 6 The fluidized bed reactor 34 is heated by a heat source 42, which may be a resistive heat source.
[0170] exist Fig.12a and 12b In the case of an isobaric reactor using a screen or grid 35 that allows gas to flow through the reactor 34 at a constant pressure, Fig.15 Reactor 34 is a forced flow reactor in which the sample is partially sealed relative to the volume into which the precursor gas is injected into the CVI system. Fig.15 As shown, a porous mass of particles or fibers 37, which may be supported by a mold 36, is supported on a gas permeable support 46. If the porous mass is a self-supporting mass, such as a solid mass of sintered particles or nonwoven material, mold 36 may not be required. Support 46 may be supported by an air-impermeable support 45. This creates a pressure gradient, wherein the pressure P1 below support 46 is greater than the pressure P2 above support 46. This results in a pressure gradient between the initial volume of the CVI system and the exhaust volume of the CVI system. The resulting pressure gradient "forces" the precursor to pass through the porous mass of particles or fibers. The advantages of this system are increased penetration into the void volume / pores of the sample, as well as increased growth rate of the metal or ceramic material. However, compared to Fig.12a Compared with an isobaric system, the use of a forced flow system may reduce the quality of the metal or ceramic material deposited in the porous mass. In various embodiments, P1 is greater than or equal to atmospheric pressure, for example, 1 atmosphere to 5 atmospheres, 1.1 atmospheres to 4 atmospheres, 1.2 atmospheres to 3 atmospheres, or 1.3 atmospheres to 2.5 atmospheres, or 1.35 atmospheres to 2 atmospheres. In various embodiments, P2 is less than or equal to P1.
[0171] Tube furnace chemical vapor deposition reactors can be used to deposit metal or ceramic coatings onto solid materials that may normally be non-porous. This can be used to produce metal or ceramic coatings on core materials. Fig.15 A tube furnace CVD reactor 48 is shown which can coat all surfaces of sample 47 that are not in contact with the walls of the reactor 48. Sample 47 can be a generally homogeneous material, such as a solid ceramic, metal, or graphite block. Sample 47 can be a heterogeneous material, such as solid particles or fibers dispersed or distributed within a ceramic, metal, or graphite matrix. Sample 47 can be a heterogeneous nuclear fuel element, such as a nuclear fuel element having TRISO particles distributed within a graphite matrix. This is advantageous for materials where only specific surfaces are desired to have a metal or ceramic coating. Reactor 48 includes a gas inlet 38 which introduces vaporized metal organic deposition precursor ML 4(vap) , a carrier gas and optionally a carbon source, a nitrogen source or an oxygen source are carried to the reactor 34. The inlet 34 can receive the evaporated organic metal deposition precursor from the vaporizer 23, substantially as Figure 6 As shown, and can receive a carbon source, a nitrogen source or an oxygen source from sources 16a, 16b and 16c, substantially as Figure 6 As shown. Reactor 48 is heated by heat source 42, which may be a resistive heat source. Within reactor 48, the exposed surface of sample 47 may be coated with a metal or ceramic layer, and the carrier gas may be recycled through exhaust 39. If it is desired to coat all surfaces of sample 47, reactor 48 may be rotated about its axis by methods known in the art. This causes sample 47 to tumble within reactor 48, exposing all surfaces to the metal or ceramic precursor gas.
[0172] Compared to conventional nuclear fuels, the deposition of cermet materials using organometallic precursors can increase power density, increase burnup, and improve high-temperature applications. Cermet materials produced using organometallic precursors are used in materials testing reactors, isotope production reactors, and reactors developed for space power generation and propulsion. Infiltration of refractory ceramics prepared from organometallic liquid precursors into ceramic nonwoven materials using chemical vapor infiltration can produce high-strength and high-temperature resistant composite materials.
[0173] Example 1. Preparation of TRISO particles.
[0174] like Figure 3 As shown, use Figure 6 The system prepares TRISO particles. TRISO particles are prepared using uranium dioxide cores as particles 21, which are placed in a fluidized bed reactor 19 heated to a deposition temperature using electrical resistance. Liquid ZyALD is used as a zirconium source. Argon is used as a carrier gas. Ethylene and propylene are used as carbon sources.
[0175] The fluidized bed reactor is heated to a preliminary deposition temperature of 1400° C. Argon is used as a carrier gas and mixed with ethylene, and the resulting gas mixture flows into the fluidized bed reactor 19 through the inlet 19. The porous carbon layer, i.e. Figure 3 Layer 2, deposited on the uranium dioxide core, i.e. Figure 3 On the core 1.
[0176] The temperature of the fluidized bed reactor is lowered to a deposition temperature of 1200° C. to 1350° C. Argon is used as a carrier gas and mixed with a mixture of ethylene and propylene as a carbon source, and the resulting gas mixture flows into the fluidized bed reactor 19 through the inlet 19. An inner pyrolytic carbon layer, i.e., Figure 3 Layer 3.
[0177] The temperature of the fluidized bed reactor was raised to a deposition temperature of 1400°C to 1500°C. Argon flow was used as a carrier gas and flowed into Figure 6 The liquid ZyALD is injected into the evaporator 23 as a zirconium source, and the mixture of argon and evaporated ZyALD leaves the evaporator through the outlet 13. The ZyALD / argon mixture is mixed with ethylene as a carbon source. The resulting gas mixture containing ZyALD and ethylene flows into the fluidized bed reactor 19 through the inlet 19. A ceramic zirconium carbide layer, i.e., Figure 3 Layer 4.
[0178] After the ceramic layer is deposited, the temperature of the fluidized bed reactor is lowered to a deposition temperature of 1200° C. to 1350° C. The flow of ZyALD to the reactor 19 is stopped. Argon gas as a carrier gas is mixed with a mixture of ethylene and propylene as a carbon source, and the resulting gas mixture flows into the fluidized bed reactor 19 through the inlet 19. An outer pyrolytic carbon layer, i.e., Figure 3 Layer 5 completes the formation of the desired TRISO particles.
[0179] Example 2. Preparation of TRISO particles with ceramic multilayers.
[0180] like Figure 3 As shown, use Figure 6 The system prepares TRISO particles. TRISO particles are prepared using uranium dioxide cores as particles 21, which are placed in a fluidized bed reactor 19 that is resistively heated to a deposition temperature. Liquid ZyALD is used as a zirconium source. Argon is used as a carrier gas. Ethylene and propylene are used as carbon sources.
[0181] The fluidized bed reactor is heated to a preliminary deposition temperature of 1400° C. Argon is used as a carrier gas and mixed with ethylene, and the resulting gas mixture flows into the fluidized bed reactor 19 through the inlet 19. In the uranium dioxide core, i.e. Figure 3 A porous carbon layer is deposited on the core 1, that is, Figure 3Layer 2.
[0182] The temperature of the fluidized bed reactor is lowered to a deposition temperature of 1200° C. to 1350° C. Argon is used as a carrier gas and mixed with a mixture of ethylene and propylene as a carbon source, and the resulting gas mixture flows into the fluidized bed reactor 19 through the inlet 19. An inner pyrolytic carbon layer, i.e., Figure 3 Layer 3.
[0183] The temperature of the fluidized bed reactor was raised to a deposition temperature of 1400°C to 1500°C. Argon flow was used as a carrier gas and flowed into Figure 6 The liquid ZyALD is injected into the evaporator 23 as a zirconium source, and the mixture of argon and evaporated ZyALD leaves the evaporator through the outlet 13. The ZyALD / argon mixture is mixed with ethylene as a carbon source. The resulting gas mixture containing ZyALD and ethylene flows into the fluidized bed reactor 19 through the inlet 19. A ceramic zirconium carbide layer, i.e., Figure 3 Layer 4. Use Figure 6 The valves 17c and 14 adjust the molar ratio of ZyALD to ethylene. The initial molar ratio of ZyALD to ethylene is 1:2. It is then increased to a molar ratio of 1:1 and then to 2:1. The resulting ceramic zirconium carbide layer 4 is a triple layer with a carbon-rich inner layer and a zirconium-rich outer layer.
[0184] After the ceramic three layers are deposited, the temperature of the fluidized bed reactor is reduced to a deposition temperature of 1200° C. to 1350° C. The flow of ZyALD to the reactor 19 is stopped. Argon gas as a carrier gas is mixed with a mixture of ethylene and propylene as a carbon source, and the resulting gas mixture flows into the fluidized bed reactor 19 through the inlet 19. An outer pyrolytic carbon layer, i.e., Figure 3 Layer 5 completes the formation of the desired TRISO particles.
[0185] Example 3. Preparation of TRISO particles with ceramic multilayers.
[0186] like Figure 3 As shown, use Figure 6 The system is modified to include: Fig.10a The TRISO particles were prepared by using a uranium dioxide core as a particle 21, and the uranium dioxide core was placed in a fluidized bed reactor 19 which was resistively heated to the deposition temperature. Liquid ZyALD was used as a zirconium source. Bis(methylimino)-bis(dimethylamino)tungsten(VI) was used as a tungsten source. Argon was used as a carrier gas. Ethylene and propylene were used as carbon sources.
[0187] The fluidized bed reactor is heated to a preliminary deposition temperature of 1400° C. Argon is used as a carrier gas and mixed with ethylene, and the resulting gas mixture flows into the fluidized bed reactor 19 through the inlet 19. In the uranium dioxide core, i.e. Figure 3 A porous carbon layer is deposited on the core 1, that is, Figure 3 Layer 2.
[0188] The temperature of the fluidized bed reactor is lowered to a deposition temperature of 1200° C. to 1350° C. Argon is used as a carrier gas and mixed with a mixture of ethylene and propylene as a carbon source, and the resulting gas mixture flows into the fluidized bed reactor 19 through the inlet 19. An inner pyrolytic carbon layer, i.e., Figure 3 Layer 3.
[0189] The temperature of the fluidized bed reactor was raised to a deposition temperature of 1400°C to 1500°C. Argon flow was used as a carrier gas and flowed into Figure 6 The evaporator 23 is provided with a liquid ZyALD as a zirconium source through inlet 32a, and the liquid bis(methylimino)bis(dimethylamino)tungsten(VI) as a tungsten source is injected into the evaporator 23 through inlet 32b. The mixture of argon, evaporated ZyALD and evaporated tungsten source leaves the evaporator through outlet 13. The ZyALD / tungsten source / argon mixture is mixed with ethylene as a carbon source. The resulting gas mixture flows into the fluidized bed reactor 19 through inlet 19. A ceramic zirconium tungsten carbide layer, i.e., is deposited on the inner pyrolytic carbon layer 3. Figure 3 Layer 4.
[0190] At the beginning of the deposition of layer 4, the relative flow rates of ZyALD and bis(methylimino)bis(dimethylamino)tungsten(VI) are adjusted using valves 33a and 33b so that they enter the evaporator at a molar ratio of 2:1. A zirconium-rich zirconium tungsten carbide layer is deposited on the pyrolytic carbon layer 3. Subsequently, the relative flow rates of ZyALD and bis(methylimino)bis(dimethylamino)tungsten(VI) are adjusted using valves 33a and 33b so that they enter the evaporator at a molar ratio of 1:2 to deposit a tungsten-rich zirconium tungsten carbide layer to form a ceramic bilayer.
[0191] After the ceramic layer is deposited, the temperature of the fluidized bed reactor is lowered to a deposition temperature of 1200° C. to 1350° C. The flow of ZyALD to the reactor 19 is stopped. Argon gas as a carrier gas is mixed with a mixture of ethylene and propylene as a carbon source, and the resulting gas mixture flows into the fluidized bed reactor 19 through the inlet 19. An outer pyrolytic carbon layer, i.e., Figure 3 Layer 5 completes the formation of the desired TRISO particles.
[0192] Example 4. Preparation of a composite material containing carbon fibers in a zirconium carbide matrix.
[0193] Can be used Fig.12aA system for preparing a composite material containing carbon fibers in a zirconium carbide matrix, the system comprising Figure 6 The evaporator described. The carbon fiber felt containing fibers 37 can be placed on a screen 35 in a chemical vapor infiltration reactor 34, which is heated to the deposition temperature using resistance. Liquid ZyALD can be used as a zirconium source. Argon can be used as a carrier gas. Ethylene and propylene can be used as carbon sources.
[0194] The temperature of the chemical vapor infiltration reactor 34 is increased to a deposition temperature of 1400° C. to 1500° C. An argon flow is used as a carrier gas and flows into Figure 6 The ZyALD is injected into the evaporator 23 as a zirconium source through the inlet 32. The mixture of argon and evaporated ZyALD leaves the evaporator through the outlet 13. The ZyALD / argon mixture is mixed with ethylene as a carbon source. The resulting gas mixture flows into the chemical vapor infiltration reactor 34 through the inlet 38. The ceramic zirconium carbide is deposited in the spaces between the fibers 38 of the carbon fiber felt, forming a layer around the fibers 37. Fig.13 of matrix38.
[0195] Example 5. Deposition of zirconium carbide on a graphite substrate.
[0196] Can be used Fig.16 A system for preparing a coated graphite block, the system comprising Figure 6 The evaporator described above. A graphite ingot 47 with a size of 100 mm×50 mm×25 mm and a purity of 99.9% can be placed in a chemical vapor deposition reactor 48 heated to the deposition temperature using resistance. The reactor 48 can be rotated about its axis to cause the sample 47 to tumble inside the reactor 48. Liquid ZyALD can be used as a zirconium source. Argon can be used as a carrier gas. Ethylene and propylene can be used as carbon sources.
[0197] The temperature of the chemical vapor deposition reactor 48 is increased to a deposition temperature of 1400° C. to 1500° C. An argon gas stream is used as a carrier gas and flows into Figure 6 evaporator 23. Liquid ZyALD is injected into evaporator 23 as a zirconium source through inlet 32. A mixture of argon and evaporated ZyALD leaves the evaporator through outlet 13. The ZyALD / argon mixture is mixed with ethylene as a carbon source. The resulting gas mixture flows into chemical vapor deposition reactor 48 through inlet 38. A ceramic zirconium carbide layer is deposited on the outer surface of graphite ingot 47, forming a zirconium carbide layer on ingot 47.
[0198] Example 6. Deposition of zirconium carbide on nuclear fuel elements.
[0199] Can be used Fig.16 A system for preparing coated nuclear fuel elements, the system comprising Figure 6The evaporator described above. A nuclear fuel element 47 containing TRISO particles in a graphite matrix can be placed in a chemical vapor deposition reactor 48 that is heated to a deposition temperature using resistance. The reactor 48 can be rotated about its axis to cause the nuclear fuel element 47 to tumble within the reactor 48. Liquid ZyALD can be used as a zirconium source. Argon can be used as a carrier gas. Ethylene and propylene can be used as carbon sources.
[0200] The temperature of the chemical vapor deposition reactor 48 is increased to a deposition temperature of 1400° C. to 1500° C. Argon is used as a carrier gas and flows into Figure 6 The evaporator 23 is provided with liquid ZyALD as a zirconium source through inlet 32. A mixture of argon and evaporated ZyALD leaves the evaporator through outlet 13. The ZyALD / argon mixture is mixed with ethylene as a carbon source. The resulting gas mixture flows into a chemical vapor deposition reactor 48 through inlet 38. A ceramic zirconium carbide layer is deposited on the outer surface of the nuclear fuel element 47, forming a zirconium carbide layer on the nuclear fuel element 47. The resulting nuclear fuel element has a thickness corresponding to approximately Fig.14 A structure in which a zirconium carbide layer 40 has been deposited on a solid bulk material 41. In this example, the solid bulk material 41 includes a graphite matrix and TRISO particles dispersed in the solid graphite matrix.
[0201] in conclusion
[0202] Although various exemplary embodiments have been described in detail with particular reference to certain exemplary aspects, it will be understood that the invention has other embodiments and that the details thereof are capable of modification in various obvious respects. As will be apparent to those skilled in the art, such changes and modifications may be effected while remaining within the spirit and scope of the invention. Therefore, the foregoing disclosure, description and drawings are for illustrative purposes only and do not in any way limit the invention, which is limited only by the claims.
Claims
1. A method for depositing a metal or ceramic layer by chemical vapor deposition, comprising: a) introducing particles into a fluidized bed reactor; b) heating the fluidized bed reactor to a desired operating temperature T1; c) starting the carrier gas to flow through the evaporator; d) injecting a non-halogenated liquid organometallic precursor into the evaporator to evaporate the non-halogenated liquid organometallic precursor; e) allowing a first mixture of the carrier gas and the evaporated non-halogenated liquid organometallic precursor to exit the vaporizer; f) optionally mixing the first mixture with a gaseous carbon source, a gaseous nitrogen source, a gaseous oxygen source or a mixture thereof to obtain a second mixture; and g) Allowing the first mixture to flow into the fluidized bed reactor operating at temperature T1 to deposit a desired metal coating on the particles; or The second mixture is flowed into the fluidized bed reactor operating at temperature T1 to deposit a desired ceramic coating on the particles.
2. The method of claim 1, wherein the particles are nuclear fuel cores.
3. The method of claim 2, wherein the particles are nuclear fuel cores selected from the group consisting of oxides, carbides, oxycarbides and nitrides of metals selected from the group consisting of uranium, plutonium and thorium and mixtures thereof.
4. The method of claim 2, wherein the particles are nuclear fuel cores selected from the group consisting of uranium oxide, uranium carbide, uranium nitride, uranium oxycarbide, and mixtures thereof.
5. The method according to claim 2, wherein the nuclear fuel core comprises: Cores of ceramic uranium material, ceramic plutonium material, ceramic thorium material or mixtures thereof; and At least one coating of porous or non-porous pyrolytic carbon.
6. The method of claim 1, wherein each particle comprises a nuclear fuel core, a porous carbon buffer layer on the core, and a pyrolytic carbon dense layer on the buffer layer.
7. The method according to claim 2, wherein: Step (g) is a step of allowing the second mixture to flow into the fluidized bed reactor; and The method further comprises: a step of depositing an inner carbon layer on the nuclear fuel core prior to step (d); and The step of depositing an outer carbon layer over said desired ceramic coating.
8. The method of claim 1, wherein the non-halogenated liquid organometallic precursor is a compound of a metal selected from the group consisting of Zr, Hf, Nb, Ta, W, V, Ti, and mixtures thereof.
9. The method of claim 1, wherein the non-halogenated liquid organometallic precursor has a formula M +n L n 、M + n L 1 (n-m) L 2 (m) or (L 3 =) p M +n L (n-2p) ,in: M is Zr, Hf, Nb, Ta, W, V, Ti or a mixture thereof; L and L 1 Independently selected from C1-C4 alkyl groups, C1-C4 alkoxy groups, bis(C1-C4 dialkyl)amide groups or combinations thereof; L 2 It is a cyclopentadienyl anion; L 3 is O= or RN=, wherein R is an alkyl group; m is 1 or 2; p is 1 or 2; and n is the valence of the metal M.
10. The method of claim 1, wherein the non-halogenated liquid organometallic precursor is: a metal alkoxide selected from the group consisting of titanium (IV) isopropoxide, titanium (IV) isobutoxide, hafnium (IV) butoxide, niobium (V) tert-butoxide, niobium (III) tert-butoxide, and zirconium (IV) butoxide; or A metal amine selected from the group consisting of: (tert-Butylimino)tris(diethylamino)tantalum(V); (tert-Butylimino)tris(diethylamino)niobium(V); (tert-Butylimino)tris(methylethylamino)niobium(V); Tris(diethylamino)niobium(III); Tris(methylethylamino)niobium(III); Tris(diethylamino)niobium(III); Tris(dimethylamino)cyclopentadienylzirconium(IV); Tetrakis(isopropylmethylamino)zirconium(IV); Tetrakis(ethylmethylamino)zirconium(IV); Tetrakis(diethylamino)zirconium(IV); Tris(dimethylamino)cyclopentadienylhafnium(IV); Bis(methylimino)bis(dimethylamino)tungsten(VI); and Bis(tert-butylimino)bis(dimethylamino)tungsten(VI).
11. The method according to claim 1, wherein: Step (f) comprises mixing the first mixture with the gaseous carbon source to obtain the second mixture; and Step (g) comprises flowing the second mixture into the fluidized bed reactor operating at temperature T1 to deposit a desired metal carbide coating on the particles.
12. The method according to claim 11, wherein the gaseous carbon source is methane, ethane, ethylene, propylene, acetylene, natural gas or a mixture thereof.
13. The method of claim 1, wherein: Step (f) comprises mixing the first mixture with the gaseous nitrogen source to obtain the second mixture; and Step (g) comprises flowing the second mixture into the fluidized bed reactor operating at temperature T1 to deposit a desired metal nitride coating on the particles.
14. The method of claim 13, wherein the gaseous nitrogen source is nitrogen, ammonia or a mixture thereof.
15. The method of claim 1, wherein: Step (f) comprises mixing the first mixture with the gaseous oxygen source to obtain the second mixture; and Step (g) comprises flowing the second mixture into the fluidized bed reactor operating at temperature T1 to deposit a desired metal oxide coating on the particles.
16. The method of claim 15, wherein the gaseous oxygen source is ozone, oxygen, nitric oxide, nitrous oxide, or a mixture thereof.
17. A method of providing a porous substance having a metal or ceramic matrix by chemical vapor infiltration, comprising: a) introducing the porous material into a chemical vapor infiltration reactor; b) heating the chemical vapor infiltration reactor to a desired operating temperature T1; c) starting the carrier gas to flow through the evaporator; d) injecting a non-halogenated liquid organometallic precursor into the evaporator, and evaporating the non-halogenated liquid organometallic precursor; e) allowing a first mixture of the carrier gas and the evaporated non-halogenated liquid organometallic precursor to exit the vaporizer; f) optionally mixing the first mixture with a gaseous carbon source, a gaseous nitrogen source, a gaseous oxygen source or a mixture thereof to obtain a second mixture; and g) Allowing the first mixture to flow into the fluidized bed reactor operating at temperature T1 and pass through the porous substance to deposit a desired metal matrix within the void spaces of the porous substance; or The second mixture is flowed into the fluidized bed reactor operating at temperature T1 and passed through the porous mass to deposit a desired ceramic matrix within the void spaces of the porous mass.
18. The method of claim 17, wherein the non-halogenated liquid organometallic precursor is a compound of a metal selected from the group consisting of Zr, Hf, Nb, Ta, W, V, Ti, and mixtures thereof.
19. A method of coating a solid material with a metal or ceramic layer by chemical vapor deposition, comprising: a) introducing the solid material into a chemical vapor deposition reactor; b) heating the chemical vapor deposition reactor to a desired operating temperature T1; c) starting the carrier gas to flow through the evaporator; d) injecting a non-halogenated liquid organometallic precursor into the evaporator, and evaporating the non-halogenated liquid organometallic precursor; e) allowing a first mixture of the carrier gas and the evaporated non-halogenated liquid organometallic precursor to exit the vaporizer; f) optionally mixing the first mixture with a gaseous carbon source, a gaseous nitrogen source, a gaseous oxygen source or a mixture thereof to obtain a second mixture; and g) Allowing the first mixture to flow into the chemical vapor deposition reactor operating at temperature T1 to deposit a desired metal coating on the solid material; or The second mixture is flowed into the chemical vapor deposition reactor operating at temperature T1 to deposit a desired ceramic coating on the solid material.
20. The method of claim 19, wherein the non-halogenated liquid organometallic precursor is a compound of a metal selected from the group consisting of Zr, Hf, Nb, Ta, W, V, Ti, and mixtures thereof.
Citation Information
Cited By
Method for preparing ultra-high-temperature ceramic coating through ultra-high-temperature metal gas source based on molten salt medium
CN121272373A