Semiconductor device
By providing a titanium-containing layer in the gate insulating layer of the oxide semiconductor device and optimizing the insulating layer structure, an abnormal electrical characteristics and reliability problems caused by oxygen defects are solved, and a semiconductor device with high mobility and high reliability is realized.
Patent Information
- Application Number
- CN202380027827.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-30
- Filing Date
- 2023-03-14
- Publication Date
- 2024-11-01
AI Technical Summary
In a semiconductor device using an oxide semiconductor, there are problems with abnormal electrical characteristics and reliability caused by oxygen defects, and when the indium ratio in the oxide semiconductor layer is increased to enhance mobility, oxygen defects are easily formed, and it is difficult to maintain high reliability at the same time and high mobility.
The titanium-containing layer is provided in the gate insulating layer, and the thickness is controlled below 50% of the first region to suppress the formation of oxygen defects and repair the oxygen defects in the oxide semiconductor layer, while optimizing the thickness and structure of the insulating layer to ensure that High mobility and reliability.
The combination of high mobility and high reliability in an oxide semiconductor device is achieved, and the electrical characteristics change and in-plane deviation are suppressed, and the stability and performance of the semiconductor device are improved.
Smart Images

Figure CN118891736A_ABST
Abstract
Description
Technical Field
[0001] One embodiment of the present invention relates to a semiconductor device and a method for manufacturing the semiconductor device. In particular, one embodiment of the present invention relates to a semiconductor device using an oxide semiconductor as a channel and a method for manufacturing the semiconductor device. Background Art
[0002] In recent years, the development of semiconductor devices that use oxide semiconductors for channels instead of amorphous silicon, low-temperature polycrystalline silicon, and single-crystal silicon has been continuously developed (for example, Patent Documents 1 to 6). Semiconductor devices that use oxide semiconductors in channels can be formed with simple structures and low-temperature processes, just like semiconductor devices that use amorphous silicon in channels. It is known that semiconductor devices that use oxide semiconductors in channels have higher mobility than semiconductor devices that use amorphous silicon in channels.
[0003] In order to make a semiconductor device using an oxide semiconductor in a channel operate stably, it is important to supply oxygen to the oxide semiconductor layer in its manufacturing process to reduce oxygen vacancies formed in the oxide semiconductor layer. For example, as one method of supplying oxygen to the oxide semiconductor layer, a technique of forming an insulating layer covering the oxide semiconductor layer under the condition that the insulating layer contains more oxygen is disclosed.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Publication No. 2021-141338
[0007] Patent Document 2: Japanese Patent Application Publication No. 2014-099601
[0008] Patent Document 3: Japanese Patent Application Publication No. 2021-153196
[0009] Patent Document 4: Japanese Patent Application Publication No. 2018-006730
[0010] Patent Document 5: Japanese Patent Application Publication No. 2016-184771
[0011] Patent Document 6: Japanese Patent Application Publication No. 2021-108405 Summary of the invention
[0012] Problems to be solved by the invention
[0013] However, the insulating layer formed under the condition of containing more oxygen will contain many defects. Under its influence, it is believed that the characteristics of the semiconductor device are abnormal due to the capture of electrons in the defects or the characteristics of the reliability test are changed. On the other hand, if an insulating layer with fewer defects is used, it is impossible to increase the oxygen contained in the insulating layer. Therefore, it is impossible to fully supply oxygen from the insulating layer to the oxide semiconductor layer. In this way, it is required to realize a structure that can reduce the defects in the insulating layer that cause the characteristics of the semiconductor device to change and at the same time repair the oxygen deficiency formed in the oxide semiconductor layer.
[0014] In addition, by relatively increasing the ratio of indium contained in the oxide semiconductor layer, a semiconductor device with high mobility can be obtained. However, when the ratio of indium contained in the oxide semiconductor layer is high, oxygen vacancies are easily formed in the oxide semiconductor layer. Therefore, in order to achieve high mobility while maintaining high reliability, it is necessary to work on the structure of the insulating layer around the oxide semiconductor layer.
[0015] An object of one embodiment of the present invention is to realize a semiconductor device having high reliability and high mobility.
[0016] Means for solving problems
[0017] A semiconductor device involved in one embodiment of the present invention comprises: an oxide semiconductor layer arranged on an insulating surface; a gate insulating layer arranged on the oxide semiconductor layer; and a gate electrode arranged on the oxide semiconductor layer through the gate insulating layer, the gate electrode having a titanium-containing layer and a conductive layer in sequence from the gate insulating layer side, the gate insulating layer including a first region overlapping with the gate electrode and a second region not overlapping with the gate electrode, and the thickness of the titanium-containing layer is less than 50% of the thickness in the first region. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1A It is a cross-sectional view schematically showing a semiconductor device according to an embodiment of the present invention.
[0019] Figure 1B Yes Figure 1A An enlarged view of a portion of the semiconductor device shown is shown.
[0020] Figure 2 It is a plan view schematically showing a semiconductor device according to an embodiment of the present invention.
[0021] Figure 3 This is a timing chart showing a method for manufacturing a semiconductor device according to an embodiment of the present invention.
[0022] Figure 4 It is a cross-sectional view showing a method for manufacturing a semiconductor device according to an embodiment of the present invention.
[0023] Figure 5 It is a cross-sectional view showing a method for manufacturing a semiconductor device according to an embodiment of the present invention.
[0024] Figure 6 It is a cross-sectional view showing a method for manufacturing a semiconductor device according to an embodiment of the present invention.
[0025] Figure 7 It is a cross-sectional view showing a method for manufacturing a semiconductor device according to an embodiment of the present invention.
[0026] Figure 8 It is a cross-sectional view showing a method for manufacturing a semiconductor device according to an embodiment of the present invention.
[0027] Fig. 9 It is a cross-sectional view showing a method for manufacturing a semiconductor device according to an embodiment of the present invention.
[0028] Fig. 10A It is a cross-sectional view showing a method for manufacturing a semiconductor device according to an embodiment of the present invention.
[0029] Fig. 10B It is a cross-sectional view showing a method for manufacturing a semiconductor device according to an embodiment of the present invention.
[0030] Fig.11 It is a cross-sectional view showing a method for manufacturing a semiconductor device according to an embodiment of the present invention.
[0031] Fig.12 It is a cross-sectional view showing a method for manufacturing a semiconductor device according to an embodiment of the present invention.
[0032] Fig.13A It is a cross-sectional view schematically showing a semiconductor device according to an embodiment of the present invention.
[0033] Fig. 13B Yes Fig.13A An enlarged view of a portion of the semiconductor device shown is shown.
[0034] Fig.14 This is a timing chart showing a method for manufacturing a semiconductor device according to an embodiment of the present invention.
[0035] Fig.15 It is a cross-sectional view showing a method for manufacturing a semiconductor device according to an embodiment of the present invention.
[0036] Fig.16 It is a cross-sectional view showing a method for manufacturing a semiconductor device according to an embodiment of the present invention.
[0037] Fig.17 It is a cross-sectional view showing a method for manufacturing a semiconductor device according to an embodiment of the present invention.
[0038] Fig.18 It is a cross-sectional view showing a method for manufacturing a semiconductor device according to an embodiment of the present invention.
[0039] Fig.19 It is a cross-sectional view showing a method for manufacturing a semiconductor device according to an embodiment of the present invention.
[0040] Fig. 20 It is a cross-sectional view showing a method for manufacturing a semiconductor device according to an embodiment of the present invention.
[0041] Fig.21 It is a cross-sectional view showing a method for manufacturing a semiconductor device according to an embodiment of the present invention.
[0042] Fig. 22 It is a cross-sectional view showing a method for manufacturing a semiconductor device according to an embodiment of the present invention.
[0043] Fig.23 It is a cross-sectional view showing a method for manufacturing a semiconductor device according to a modification example of one embodiment of the present invention.
[0044] Fig.24 It is a cross-sectional view showing a method for manufacturing a semiconductor device according to an embodiment of the present invention.
[0045] Fig.25 It is a plan view schematically showing a display device according to one embodiment of the present invention.
[0046] Fig.26 This is a block diagram showing a circuit configuration of a display device according to an embodiment of the present invention.
[0047] Fig. 27 : is a circuit diagram showing a pixel circuit of a display device according to an embodiment of the present invention.
[0048] Fig.28 It is a cross-sectional view schematically showing a display device according to an embodiment of the present invention.
[0049] Fig.29 It is a plan view of a pixel electrode and a common electrode of a display device according to an embodiment of the present invention.
[0050] Fig.30 : is a circuit diagram showing a pixel circuit of a display device according to an embodiment of the present invention.
[0051] Fig.31 It is a cross-sectional view schematically showing a display device according to an embodiment of the present invention.
[0052] Fig.32 This is a diagram showing the electrical characteristics of a semiconductor device according to an embodiment of the present invention.
[0053] Fig.33 This is a diagram showing the electrical characteristics of a semiconductor device according to an embodiment of the present invention.
[0054] Fig.34 This is a diagram showing the electrical characteristics of a semiconductor device according to an embodiment of the present invention.
[0055] Fig.35 This is a diagram showing the electrical characteristics of a semiconductor device according to an embodiment of the present invention.
[0056] Fig.36 This is a diagram showing the electrical characteristics of a semiconductor device according to an embodiment of the present invention.
[0057] Fig.37 This is a diagram showing the electrical characteristics of a semiconductor device according to an embodiment of the present invention.
[0058] Fig.38 This is a diagram showing the in-plane variation of the threshold voltage of the semiconductor device according to one embodiment of the present invention.
[0059] Fig.39 This is a diagram showing the electrical characteristics of a semiconductor device according to an embodiment of the present invention.
[0060] Fig.40 This is a diagram showing the electrical characteristics of a semiconductor device according to an embodiment of the present invention.
[0061] Fig.41 This is a diagram showing the electrical characteristics of a semiconductor device according to an embodiment of the present invention.
[0062] Fig.42 This is a diagram showing the relationship between the thickness of the first region of the gate insulating layer and the threshold voltage of the semiconductor device according to one embodiment of the present invention. DETAILED DESCRIPTION
[0063] Hereinafter, various embodiments of the present invention will be described with reference to the accompanying drawings. The following disclosure is only an example. The configuration that can be easily conceived by those skilled in the art by appropriately changing the configuration of the embodiment while maintaining the gist of the invention is of course included in the scope of the present invention. With respect to the accompanying drawings, in order to make the description clearer, the width, thickness, shape, etc. of each part are sometimes schematically indicated compared to the actual method. However, the shape shown in the figure is only an example and does not limit the interpretation of the present invention. In this specification and each figure, the same figure mark is marked for the same configuration as that described in the accompanying drawings that have appeared, and the detailed description is sometimes appropriately omitted.
[0064] The so-called "semiconductor device" refers to all devices that can function by utilizing semiconductor characteristics. Transistors and semiconductor circuits are a form of semiconductor devices. The semiconductor device of the embodiment shown below can also be a transistor used in an integrated circuit (IC) such as a display device, a microprocessor (MPU), or a memory circuit.
[0065] The so-called "display device" refers to a structure that uses an electro-optical layer to display an image. For example, the term display device sometimes refers to a display panel including an electro-optical layer, or sometimes refers to a structure that is equipped with other optical components (such as polarization components, backlight sources, touch panels, etc.) relative to the display unit. As long as there is no technical contradiction, the "electro-optical layer" may include a liquid crystal layer, an electroluminescent (EL) layer, an electrochromic (EC) layer, and an electrophoretic layer. Therefore, with respect to the embodiments described later, a liquid crystal display device including a liquid crystal layer and an organic EL display device including an organic EL layer are exemplified as display devices for explanation, but the structure in this embodiment can be applied to a display device including the above-mentioned other electro-optical layers.
[0066] In each embodiment of the present invention, the direction from the substrate toward the oxide semiconductor layer is referred to as up or above. Conversely, the direction from the oxide semiconductor layer toward the substrate is referred to as down or below. Thus, for ease of explanation, the above or below phrases are used for explanation, but for example, the up-and-down relationship between the substrate and the oxide semiconductor layer may be configured in a different direction than that shown in the figure. In the following description, for example, the oxide semiconductor layer on the substrate is merely used to illustrate the up-and-down relationship between the substrate and the oxide semiconductor layer as described above, and other components may be configured between the substrate and the oxide semiconductor layer. Above or below refers to the stacking order in a structure having multiple layers stacked, and in the case of a pixel electrode described as above a transistor, it may also be a positional relationship in which the transistor and the pixel electrode do not overlap when viewed from above. On the other hand, in the case of a pixel electrode described as being vertically above a transistor, it refers to a positional relationship in which the transistor and the pixel electrode overlap when viewed from above.
[0067] In this specification, unless otherwise specified, expressions such as “α includes A, B, or C”, “α includes any one of A, B, and C”, and “α includes one selected from the group consisting of A, B, and C” do not exclude the case where α includes a plurality of combinations of A to C. In addition, the above expressions do not exclude the case where α includes other elements.
[0068] It should be noted that the following embodiments can be combined with each other as long as no technical contradiction occurs.
[0069] <First Embodiment>
[0070] use Figure 1A to Figure 12 A semiconductor device according to an embodiment of the present invention will be described.
[0071] [Configuration of Semiconductor Device 10]
[0072] use Figure 1A to Figure 2 A configuration of a semiconductor device 10 according to an embodiment of the present invention will be described. Figure 1A It is a cross-sectional view schematically showing a semiconductor device according to an embodiment of the present invention. Figure 1B Yes Figure 1A An enlarged view of a portion of the semiconductor device shown is shown. Figure 2 It is a plan view schematically showing a semiconductor device according to an embodiment of the present invention.
[0073] like Figure 1AAs shown, the semiconductor device 10 is provided on a substrate 100. The semiconductor device 10 includes a gate electrode 105, gate insulating layers 110 and 120, an oxide semiconductor layer 140, a gate insulating layer 150, a gate electrode 160, insulating layers 170 and 180, a source electrode 201, and a drain electrode 203. When the source electrode 201 and the drain electrode 203 are not particularly distinguished, they are sometimes collectively referred to as source / drain electrodes 200.
[0074] The gate electrode 105 is provided on the substrate 100. The gate insulating layer 110 and the gate insulating layer 120 are provided on the substrate 100 and the gate electrode 105. The oxide semiconductor layer 140 is provided on the gate insulating layer 120. The oxide semiconductor layer 140 is in contact with the gate insulating layer 120. The surface of the main surface of the oxide semiconductor layer 140 that is in contact with the gate insulating layer 120 is referred to as a lower surface 142.
[0075] The gate electrode 160 is opposite to the oxide semiconductor layer 140. The gate insulating layer 150 is provided between the oxide semiconductor layer 140 and the gate electrode 160. The gate insulating layer 150 is in contact with the oxide semiconductor layer 140. The surface in contact with the gate insulating layer 150 among the main surfaces of the oxide semiconductor layer 140 is referred to as an upper surface 141. The surface between the upper surface 141 and the lower surface 142 is referred to as a side surface 143. The insulating layers 170 and 180 are provided on the gate insulating layer 150 and the gate electrode 160. The insulating layers 170 and 180 are provided with openings 171 and 173 reaching the oxide semiconductor layer 140. The source electrode 201 is provided inside the opening 171. The source electrode 201 is in contact with the oxide semiconductor layer 140 at the bottom of the opening 171. The drain electrode 203 is provided inside the opening 173. The drain electrode 203 is in contact with the oxide semiconductor layer 140 at the bottom of the opening 173.
[0076] The gate electrode 105 has a function as a bottom gate of the semiconductor device 10 and a function as a light shielding film for the oxide semiconductor layer 140. The gate insulating layer 110 has a function as a barrier film for shielding impurities diffusing from the substrate 100 toward the oxide semiconductor layer 140. The gate insulating layers 110 and 120 have a function as gate insulating layers for the bottom gate.
[0077] The oxide semiconductor layer 140 is divided into a source region S, a drain region D, and a channel region CH. The channel region CH is a region vertically below the gate electrode 160 in the oxide semiconductor layer 140. The source region S is a region of the oxide semiconductor layer 140 that does not overlap with the gate electrode 160, and is a region closer to the source electrode 201 than the channel region CH. The drain region D is a region of the oxide semiconductor layer 140 that does not overlap with the gate electrode 160, and is a region closer to the drain electrode 203 than the channel region CH. The oxide semiconductor layer 140 in the channel region CH has physical properties as a semiconductor. The oxide semiconductor layer 140 in the source region S and the drain region D has physical properties as a conductor.
[0078] The gate electrode 160 has the function of serving as the top gate of the semiconductor device 10 and as a light shielding film for the oxide semiconductor layer 140. The gate insulating layer 150 has the function of serving as a gate insulating layer for the top gate and has the function of releasing oxygen through heat treatment in the manufacturing process. The insulating layers 170 and 180 have the function of insulating the gate electrode 160 from the source / drain electrode 200 to reduce the parasitic capacitance therebetween. The operation of the semiconductor device 10 is mainly controlled by the voltage supplied to the gate electrode 160. An auxiliary voltage is supplied to the gate electrode 105. However, in the case where the gate electrode 105 is used only as a light shielding film, it is also possible to place the gate electrode 105 in a floating state instead of supplying a specific voltage to the gate electrode 105. That is, the gate electrode 105 may also be simply referred to as a "light shielding film".
[0079] [Problems Newly Recognized in the Process of Implementing the Invention]
[0080] At present, in transistors using oxide semiconductors in the channel, molybdenum tungsten is used as the gate wiring (gate electrode), for example. In transistors using a molybdenum tungsten layer as the gate wiring, there is a problem of so-called normal conduction, in which the drain current Id begins to flow when the gate voltage Vg is lower than 0V. During the heat treatment in the manufacturing process of the transistor, the oxygen contained in the gate insulating layer moves to the molybdenum tungsten layer instead of being supplied to the oxide semiconductor layer. Therefore, the oxygen vacancies contained in the oxide semiconductor layer cannot be fully repaired, resulting in the electrical characteristics of the transistor becoming normally on.
[0081] In the gate wiring, a titanium layer is provided under the molybdenum-tungsten layer to form a stacked structure of a titanium layer and a molybdenum-tungsten layer, thereby preventing the transistor from being normally turned on. The titanium layer prevents the hydrogen and oxygen contained in the gate insulating layer 150 from moving through the titanium layer to the conductive layer 164 during the heat treatment in the manufacturing process of the transistor. On the other hand, the etching rate of the titanium layer is slower than the etching rate of the molybdenum-tungsten layer. Therefore, if the thickness of the titanium layer is thick, the processing time of the dry etching becomes longer, which causes the line width of the gate wiring to have an in-plane deviation. In addition, the gate insulating layer is removed due to over-etching, causing the thickness of the gate insulating layer to have an in-plane deviation. In particular, when a large-area substrate of the sixth generation or above is used as a substrate for manufacturing transistors, the influence of the in-plane deviation becomes greater. In addition, if the thickness of the titanium layer is thin, it cannot block the oxygen contained in the gate insulating layer 150 and causes it to react with the conductive layer 164. As a result, the electrical characteristics of the semiconductor device become normally turned on, and the deviation of the electrical characteristics becomes larger. For these reasons, the problem of deviation of the electrical characteristics of the transistor occurs within the substrate surface.
[0082] However, in a transistor using an oxide semiconductor in the channel, the source region and the drain region are formed by ion implantation using the gate wiring as a mask, thereby controlling the channel length, so that a short channel transistor can be formed. Typically, in the manufacturing process of a transistor using ion implantation and using low-temperature polysilicon for the channel, the thickness of the gate insulating layer is about 100nm. Therefore, most ion implantation devices have specifications for implantation under acceleration assuming that the thickness of the gate insulating layer is about 100nm. In order to use such an ion implantation device to form the source region and the drain region of a transistor using an oxide semiconductor in the channel, the thickness of the gate insulating layer needs to be set to about 100nm. However, in a transistor using an oxide semiconductor in the channel, when the thickness of the gate insulating layer is about 100nm, the oxygen vacancies contained in the oxide semiconductor layer cannot be fully repaired. This is because the amount of oxygen contained in the gate insulating layer is insufficient. As a result, the electrical characteristics of the transistor are prone to become normally conductive. The amount of oxygen needs to be ensured by the thickness of the gate insulating layer, so it is difficult to reduce the thickness of the gate insulating layer.
[0083] Therefore, in one embodiment of the present invention, a semiconductor device having normally-off electrical characteristics is provided. In addition, a semiconductor device having electrical characteristics with reduced variation within a substrate surface is provided.
[0084] In one embodiment of the present invention, Figure 1A and Figure 1BAs shown, the gate electrode 160 has a titanium-containing layer 162 and a conductive layer 164 in order from the gate insulating layer 150 side. In this specification, etc., the titanium-containing layer 162 is a layer containing titanium as a main component, for example, titanium, titanium nitride or titanium oxide. In addition, the titanium-containing layer 162 may also be a layer containing at least one of nitrogen or oxygen in the titanium layer. In addition, the titanium-containing layer 162 may also be a stacked structure of a titanium layer and a nitrogen-containing titanium layer in which nitrogen is added to the titanium layer. The titanium-containing layer 162 may also be a stacked structure of a titanium layer and an oxygen-containing titanium layer in which oxygen is added to the titanium layer. In addition, a structure including at least one of an oxidized region and a nitrided region in the titanium layer may also be used as the titanium-containing layer 162. As the conductive layer 164, molybdenum, tungsten or molybdenum-tungsten is used.
[0085] In addition, the gate insulating layer 150 includes a region overlapping with the gate electrode 160 (referred to as a first region 152) and a region not overlapping with the gate electrode 160 (referred to as a second region 154). In other words, the region overlapping with the gate electrode 160 is a region overlapping with the channel region CH of the oxide semiconductor layer 140. The region not overlapping with the gate electrode 160 includes a region overlapping with the source region S and the drain region D of the oxide semiconductor layer 140 and a region in contact with the gate insulating layer 120.
[0086] like Figure 1B As shown, in the gate insulating layer 150, the thickness T1 of the first region 152 is different from the thickness T2 of the second region 154. The thickness T1 of the first region 152 is the thickness when the gate insulating layer 150 is formed in the manufacturing process. The thickness T2 of the second region 154 is the thickness formed by dry etching when forming the gate electrode 160.
[0087] As described above, in the gate electrode 160, the thickness of the titanium-containing layer 162 affects the amount (thickness) of the gate insulating layer 150 removed. Therefore, the thickness T3 of the titanium-containing layer 162 is preferably less than 50% of the thickness T1 in the first region 152. Preferably, the thickness T3 is more than 20% and less than 30% of the thickness T1. For example, the thickness T3 of the titanium-containing layer 162 is preferably more than 25nm and less than 50nm. It should be noted that when the titanium-containing layer 162 is not provided (that is, when the thickness of the titanium-containing layer 162 is 0nm), the electrical characteristics of the transistor will become normally conductive.
[0088] If the thickness T3 of the titanium-containing layer 162 is less than 25 nm, hydrogen and oxygen contained in the gate insulating layer 150 will move to the conductive layer 164 through the titanium-containing layer during the heat treatment in the manufacturing process of the semiconductor device. As a result, there is a possibility that even the oxygen that should be supplied to the oxide semiconductor layer 140 will move to the conductive layer 164 and the oxygen deficiency in the oxide semiconductor layer 140 cannot be fully repaired. Therefore, if the thickness T3 of the titanium-containing layer 162 is at least 25 nm, it is possible to suppress the oxygen contained in the gate insulating layer 150 from moving to the conductive layer 164 through the titanium-containing layer during the heat treatment in the manufacturing process of the semiconductor device. As a result, during the heat treatment, the oxygen contained in the gate insulating layer 150 is supplied to the oxide semiconductor layer 140, thereby repairing the oxygen deficiency in the oxide semiconductor layer 140. Therefore, it is possible to suppress the transistor from being normally turned on.
[0089] In addition, if the thickness T3 of the titanium-containing layer 162 is greater than 50 nm, the dry etching processing time becomes longer when forming the gate electrode 160, thereby causing deviations in the line width of the gate wiring. In addition, the gate insulating layer is removed due to overetching, causing deviations in the thickness of the gate insulating layer. For these reasons, the electrical characteristics of the transistor within the substrate surface vary.
[0090] As described above, the thickness T3 of the titanium-containing layer 162 is set to be less than 50% of the thickness T1 of the first region of the gate insulating layer 150, preferably 20% to 30%. The thickness T3 of the titanium-containing layer 162 is set to be, for example, 25 nm to 50 nm. This can prevent the electrical characteristics of the transistor from becoming normally-on, and prevent the electrical characteristics of the transistor from deviating within the substrate surface.
[0091] In addition, the thickness of the first region T1 of the gate insulating layer 150 is preferably not less than 100 nm and not more than 125 nm. In addition, the thickness T3 of the titanium-containing layer 162 is preferably not less than 25% and less than 70% of the thickness T2 of the second region 154. For example, the thickness T2 of the second region 154 of the gate insulating layer 150 is preferably not less than 75 nm and not more than 100 nm. If the thickness of the first region T1 of the gate insulating layer 150 is less than 100 nm, the electrical characteristics of the semiconductor device become normally-on.
[0092] As described above, when the source region S and the drain region D are formed in the oxide semiconductor layer 140, an ion implantation device is used. If the thickness T2 of the second region 154 exceeds 100nm, there is a situation where the impurities do not reach the oxide semiconductor layer 140. In addition, if there is an in-plane deviation in the film thickness of the gate insulating layer 150, the impurities added to the source region S and the drain region D will be uneven, thereby causing uneven resistance. As a result, the electrical characteristics of the transistor have an in-plane deviation. In addition, the thickness T2 of the second region 154 of the gate insulating layer 150 is determined by the amount removed due to overetching when forming the gate electrode 160. Therefore, when the thickness of the first region 152 of the gate insulating layer 150 is less than 100nm, the thickness T2 of the second region sometimes becomes thinner than necessary. Therefore, the thickness T2 of the second region 154 of the gate insulating layer 150 is preferably set to be greater than 75nm and less than 100nm. In one embodiment of the present invention, even if the thickness of the gate insulating layer 150 is not less than 100 nm and not more than 125 nm, the electrical characteristics of the transistor can be suppressed from being normally-on, which will be described later.
[0093] In this embodiment, a dual-gate transistor in which gate electrodes are provided both above and below the oxide semiconductor layer is used as an example of the semiconductor device 10, but the present invention is not limited to this configuration. For example, a bottom-gate transistor in which the gate electrode is provided only below the oxide semiconductor layer or a top-gate transistor in which the gate electrode is provided only above the oxide semiconductor layer may be used as the semiconductor device 10. The above configuration is only one embodiment, and the present invention is not limited to the above configuration.
[0094] like Figure 2 As shown, in the D1 direction, the width of the gate electrode 105 is greater than the width of the gate electrode 160. The D1 direction is a direction connecting the source electrode 201 and the drain electrode 203, and is a direction indicating the channel length L of the semiconductor device 10. Specifically, the length in the D1 direction in the region (channel region CH) where the oxide semiconductor layer 140 and the gate electrode 160 overlap is the channel length L, and the width in the D2 direction of the channel region CH is the channel width W.
[0095] In this embodiment, a configuration in which the gate insulating layer 150 is formed on the entire surface and the openings 171 and 173 are provided in the gate insulating layer 150 is exemplified, but the present invention is not limited to this configuration. The gate insulating layer 150 may also be patterned. For example, the gate insulating layer 150 may be patterned in such a manner that the oxide semiconductor layer 140 in the source region S and the drain region D is exposed. That is, the gate insulating layer 150 in the source region S and the drain region D may be removed, and the oxide semiconductor layer 140 may be in contact with the insulating layer 170 in these regions.
[0096] exist Figure 2, the structure in which the source / drain electrode 200 does not overlap with the gate electrode 105 and the gate electrode 160 in a plan view is illustrated, but the present invention is not limited to this structure. For example, the source / drain electrode 200 may overlap with at least one of the gate electrode 105 and the gate electrode 160 in a plan view. The above structure is only one embodiment, and the present invention is not limited to the above structure.
[0097] [Material of Each Component of Semiconductor Device 10]
[0098] As the substrate 100, a glass substrate, a quartz substrate, a sapphire substrate, or other light-transmitting rigid substrate is used. When the substrate 100 needs to be flexible, a substrate containing resin such as a polyimide substrate, an acrylic substrate, a siloxane-based substrate, or a fluororesin substrate is used as the substrate 100. When a substrate containing resin is used as the substrate 100, impurities may be introduced into the above-mentioned resin in order to improve the heat resistance of the substrate 100. In particular, when the semiconductor device 10 is a top emission type display, since the substrate 100 does not need to be transparent, impurities that deteriorate the transparency of the substrate 100 may be used. When the semiconductor device 10 is used in an integrated circuit that is not a display device, as the substrate 100, a semiconductor substrate such as a silicon substrate, a silicon carbide substrate, or a compound semiconductor substrate, or a substrate that is not light-transmitting such as a conductive substrate such as a stainless steel substrate is used.
[0099] As the gate electrode 105 and the source / drain electrode 200, a common metal material is used. For example, as these materials, aluminum (Al), titanium (Ti), chromium (Cr), cobalt (Co), nickel (Ni), molybdenum (Mo), hafnium (Hf), tantalum (Ta), tungsten (W), bismuth (Bi), silver (Ag), copper (Cu), and alloys thereof or compounds thereof are used. As the gate electrode 105, the gate electrode 160, and the source / drain electrode 200, the above-mentioned materials may be used in a single layer form or in a stacked form.
[0100] In this embodiment, a stacked structure of a titanium-containing layer 162 and a conductive layer 164 is used as the gate electrode 160. The material used as the titanium-containing layer 162 and the material used as the conductive layer 164 are as described above.
[0101] A common insulating material is used as the gate insulating layers 110 and 120 and the insulating layers 170 and 180. For example, silicon oxide (SiO x ), silicon oxynitride (SiO x N y ), silicon nitride (SiN x ), silicon oxynitride (SiN x O y ), aluminum oxide (AlOx ), aluminum oxynitride (AlO x N y ), aluminum oxynitride (AlN x O y ), aluminum nitride (AlN x ) and other inorganic insulating layers.
[0102] As the gate insulating layer 150, an insulating layer containing oxygen among the above insulating layers is used. For example, as the gate insulating layer 150, silicon oxide (SiO x ), silicon oxynitride (SiO x N y ), aluminum oxide (AlO x ), aluminum oxynitride (AlO x N y ) and other inorganic insulating layers.
[0103] An insulating layer having a function of releasing oxygen by heat treatment is used as the gate insulating layer 120. For example, the temperature of the heat treatment for releasing oxygen from the gate insulating layer 120 is, for example, 600° C. or less, 500° C. or less, 450° C. or less, or 400° C. or less. That is, for example, when a glass substrate is used as the substrate 100, the gate insulating layer 120 releases oxygen at the heat treatment temperature performed in the manufacturing process of the semiconductor device 10.
[0104] As the gate insulating layer 150, an insulating layer with few defects is used. For example, when the composition ratio of oxygen in the gate insulating layer 150 is compared with the composition ratio of oxygen in an insulating layer having the same composition as the gate insulating layer 150 (hereinafter referred to as "another insulating layer"), the composition ratio of oxygen in the gate insulating layer 150 is closer to the stoichiometric ratio of the insulating layer than the composition ratio of oxygen in the other insulating layer. Specifically, silicon oxide (SiO x ), the oxygen composition ratio of silicon oxide used as the gate insulating layer 150 is closer to the stoichiometric ratio of silicon oxide than the oxygen composition ratio of silicon oxide used as the insulating layer 180. For example, as the gate insulating layer 150, a layer in which no defects are observed when evaluated by an electron spin resonance method (ESR) may be used.
[0105] The above SiO x N y and AlO x N y It is a silicon compound or aluminum compound containing nitrogen (N) at a ratio (x>y) less than oxygen (O). x O y and AlN x O yThese are silicon compounds and aluminum compounds containing oxygen at a ratio smaller than that of nitrogen (x>y).
[0106] As the metal oxide layer 190 (also referred to as metal oxide) used in the manufacturing process, a metal oxide containing aluminum as a main component is used, and the details will be described later. For example, aluminum oxide (AlO x ), aluminum oxynitride (AlO x N y ), aluminum oxynitride (AlN x O y ), aluminum nitride (AlN x ) and other inorganic insulating layers. The so-called "metal oxide layer with aluminum as the main component" means that the ratio of aluminum contained in the metal oxide layer 190 is greater than 1% of the entire metal oxide layer 190. The ratio of aluminum contained in the metal oxide layer 190 may also be greater than 5% and less than 70%, greater than 10% and less than 60%, or greater than 30% and less than 50% of the entire metal oxide layer 190. The above ratios may be mass ratios or weight ratios.
[0107] As the oxide semiconductor layer 140, an oxide metal having semiconductor characteristics is used. For example, as the oxide semiconductor layer 140, an oxide semiconductor containing two or more metals including indium (In) is used. The ratio of indium to the whole of the oxide semiconductor layer 140 is 50% or more. As the oxide semiconductor layer 140, in addition to indium, at least one of gallium (Ga), zinc (Zn), aluminum (Al), hafnium (Hf), yttrium (Y), zirconium oxide (Zr) or lanthanide elements can be used. As the oxide semiconductor layer 140, other elements other than the above can also be used.
[0108] The oxide semiconductor layer 140 may be amorphous or crystalline. The oxide semiconductor layer 140 may also be a mixed phase of amorphous and crystalline. As described below, in an oxide semiconductor layer 140 in which the ratio of indium is 50% or more, oxygen vacancies are easily formed. Crystalline oxide semiconductors are less likely to form oxygen vacancies than amorphous oxide semiconductors. Therefore, it is preferred that the oxide semiconductor layer 140 as described above is crystalline.
[0109] [Method of Manufacturing Semiconductor Device 10]
[0110] use Figure 3 to Figure 12 A method for manufacturing a semiconductor device according to an embodiment of the present invention will be described. Figure 3 This is a timing chart showing a method for manufacturing a semiconductor device according to an embodiment of the present invention. Figures 4 to 12 It is a cross-sectional view showing a method for manufacturing a semiconductor device according to an embodiment of the present invention.
[0111] like Figure 3 and Figure 4 As shown, a gate electrode 105 is formed on the substrate 100 as a bottom gate, and gate insulating layers 110 and 120 are formed on the gate electrode 105 ( Figure 3 The gate insulating layer 110 is formed of silicon nitride. The gate insulating layer 120 is formed of silicon oxide. The gate insulating layers 110 and 120 are formed by CVD (Chemical Vapor Deposition).
[0112] By using silicon nitride as the gate insulating layer 110, the gate insulating layer 110 can block, for example, impurities diffusing from the substrate 100 toward the oxide semiconductor layer 140. Silicon oxide used as the gate insulating layer 120 has a property of releasing oxygen by heat treatment.
[0113] like Figure 3 and Figure 5 As shown, an oxide semiconductor layer 140 ( Figure 3 In this process, an oxide semiconductor layer 140 may be formed on the substrate 100. The oxide semiconductor layer 140 is formed by sputtering or atomic layer deposition (ALD: Atomic Layer Deposition).
[0114] For example, the thickness of the oxide semiconductor layer 140 is greater than 10 nm and less than 100 nm, greater than 15 nm and less than 70 nm, or greater than 20 nm and less than 40 nm. In this embodiment, an oxide containing indium (In) and gallium (Ga) is used as the oxide semiconductor layer 140. The oxide semiconductor layer 140 before the heat treatment (OS annealing) described later is amorphous. In addition, as the oxide semiconductor layer 140, an oxide containing indium (In), gallium (Ga) and zinc (Zn), that is, so-called IGZO, may also be used.
[0115] When the oxide semiconductor layer 140 is crystallized by OS annealing described later, the oxide semiconductor layer 140 after film formation and before OS annealing is preferably in an amorphous state (a state in which the crystalline component of the oxide semiconductor is small). That is, the film formation conditions of the oxide semiconductor layer 140 are preferably conditions in which the oxide semiconductor layer 140 immediately after film formation is not crystallized as much as possible. For example, when the oxide semiconductor layer 140 is formed by sputtering, the oxide semiconductor layer 140 is formed under a state in which the temperature of the object to be formed (the substrate 100 and the structure formed thereon) is controlled.
[0116] When a film is formed on an object to be formed by sputtering, ions generated in the plasma and atoms recoiled from the sputtering target will collide with the object to be formed. Therefore, the temperature of the object to be formed will rise along with the film forming process. If the temperature of the object to be formed rises during the film forming process, the oxide semiconductor layer 140 contains microcrystals in the state just after the film is formed. Due to the microcrystals, the subsequent crystallization caused by OS annealing is hindered. In order to control the temperature of the object to be formed as described above, the film can also be formed while cooling the object to be formed. For example, the object to be formed can also be cooled from the surface opposite to the film forming surface in such a way that the temperature of the film forming surface of the object to be formed (hereinafter referred to as the "film forming temperature") is below 100°C, below 70°C, below 50°C or below 30°C. By forming the oxide semiconductor layer 140 while cooling the object to be formed as described above, an oxide semiconductor layer 140 with a small crystalline component in the state just after the film is formed can be formed.
[0117] like Figure 3 and Figure 6 As shown, the pattern of the oxide semiconductor layer 140 is formed ( Figure 3 Although not shown in the figure, a resist mask is formed on the oxide semiconductor layer 140, and the oxide semiconductor layer 140 is etched using the resist mask. The oxide semiconductor layer 140 can be etched by wet etching or dry etching. As wet etching, an acidic etchant can also be used for etching. For example, oxalic acid or hydrofluoric acid can be used as an etchant.
[0118] After the patterning of the oxide semiconductor layer 140, the oxide semiconductor layer 140 is subjected to a heat treatment (OS annealing) ( Figure 3 In this embodiment, the oxide semiconductor layer 140 is crystallized by the OS annealing.
[0119] like Figure 3 and Figure 7 As shown, a gate insulating layer 150 is formed on the oxide semiconductor layer 140 ( Figure 3"GI formation" of step S3005). For example, silicon oxide is formed as the gate insulating layer 150. The gate insulating layer 150 is formed by a CVD method. For example, in order to form an insulating layer with few defects as described above as the gate insulating layer 150, the gate insulating layer 150 may be formed at a film forming temperature of 350°C or higher. In this embodiment, the thickness of the gate insulating layer 150 is greater than 100 nm and less than 125 nm. The thickness of the gate insulating layer 150 is equivalent to the thickness T1 of the first region 152. As the gate insulating layer, for example, silicon oxide is used. After the gate insulating layer 150 is formed, a process of injecting oxygen into a portion of the gate insulating layer 150 may also be performed. The gate insulating layer 150 is sometimes referred to as a "first insulating layer". A metal oxide layer 190 ( Figure 3 The metal oxide layer 190 is formed by sputtering. Oxygen is injected into the gate insulating layer 150 by the formation of the metal oxide layer 190.
[0120] For example, the thickness of the metal oxide layer 190 is 5 nm to 100 nm, 5 nm to 50 nm, 5 nm to 30 nm, or 7 nm to 15 nm. In this embodiment, aluminum oxide is used as the metal oxide layer 190. Aluminum oxide has a high barrier property against gas. In this embodiment, aluminum oxide used as the metal oxide layer 190 is used to suppress the diffusion of oxygen injected into the gate insulating layer 150 to the outside when the metal oxide layer 190 is formed.
[0121] For example, when the metal oxide layer 190 is formed by sputtering, the process gas used for sputtering may remain in the film of the metal oxide layer 190. For example, when Ar is used as the process gas for sputtering, Ar may remain in the film of the metal oxide layer 190. The remaining Ar can be detected by SIMS (Secondary Ion Mass Spectrometry) analysis performed on the metal oxide layer 190.
[0122] In a state where the gate insulating layer 150 is formed on the oxide semiconductor layer 140 and the metal oxide layer 190 is formed on the gate insulating layer 150, a heat treatment (oxidation annealing) for supplying oxygen to the oxide semiconductor layer 140 is performed ( Figure 3In the process from forming the oxide semiconductor layer 140 to forming the gate insulating layer 150 on the oxide semiconductor layer 140, a large number of oxygen vacancies are generated on the upper surface 141 and the side surface 143 of the oxide semiconductor layer 140. The oxygen released from the gate insulating layers 120 and 150 by the above-mentioned oxidation annealing is supplied to the oxide semiconductor layer 140 to repair the oxygen vacancies.
[0123] In the above-mentioned oxidation annealing, oxygen injected into the gate insulating layer 150 is blocked by the oxidized metal layer 190. Therefore, the oxygen is suppressed from being released into the atmosphere. Therefore, the oxygen is efficiently supplied to the oxide semiconductor layer 140 by the oxidation annealing to repair oxygen vacancies.
[0124] like Figure 3 and Figure 8 As shown, after the oxidation annealing, the oxide metal layer 190 is etched (removed) ( Figure 3 As for etching of the metal oxide layer 190, wet etching or dry etching may be used. As wet etching, for example, diluted hydrofluoric acid (DHF) is used. The metal oxide layer 190 formed on the entire surface is removed by this etching. In other words, the removal of the metal oxide layer 190 is performed without using a mask. In other words, by this etching, at least all of the metal oxide layer 190 in the area overlapping with the oxide semiconductor layer 140 formed into a certain pattern when viewed from above is removed.
[0125] Next, a gate electrode 160 ( Figure 3 GE formation in step S3009). Fig. 9 As shown, the titanium-containing layer 162 and the conductive layer 164 are sequentially formed. In the gate electrode 160, the titanium-containing layer 162 and the conductive layer 164 are formed by sputtering or atomic layer deposition. In this embodiment, as described above, it is preferred that the gate electrode 160 uses a stacked structure of the titanium-containing layer 162 and the conductive layer 164. In this embodiment, the thickness of the titanium-containing layer 162 is greater than 25nm and less than 50nm. In addition, the thickness of the conductive layer 164 is greater than 100nm and less than 400nm.
[0126] In the case of a stacked structure of a titanium layer and a nitrogen-containing titanium layer formed by adding nitrogen to the titanium layer as the titanium-containing layer 162, nitrogen may be injected into the titanium layer using an ion implantation device. Alternatively, when the titanium layer is formed by sputtering, the nitrogen-containing titanium layer may be formed by using nitrogen gas. For example, the thickness of the titanium layer is within a range of 25 nm to 50 nm, and the area of several nm from the surface is the area where nitrogen is added.
[0127] like Fig. 10AAs shown, the titanium-containing layer 162 and the conductive layer 164 are patterned by a photolithography process. The titanium-containing layer 162 and the conductive layer 164 are processed by dry etching. The etching rate of the titanium-containing layer 162 is slower than the etching rate of the conductive layer 164. In the present embodiment, the thickness of the titanium-containing layer 162 is greater than 25 nm and less than 50 nm. Therefore, the in-plane deviation of the line width of the gate electrode 160 within the substrate surface can be suppressed. In addition, in the second region 154 of the gate insulating layer 150, the in-plane deviation of the amount removed can be suppressed. By dry etching, the thickness T2 of the second region 154 is made greater than 75 nm and less than 100 nm. In addition, if the relationship between the thickness T3 of the titanium-containing layer 162 and the thickness of the gate insulating layer 150 is considered, the thickness T3 of the titanium-containing layer 162 is preferably greater than 25% and less than 70% of the thickness T2 of the second region 154. As described above, the gate electrode 160 is formed so as to be in contact with the gate insulating layer 150 exposed by removing the oxidized metal layer 190 .
[0128] In a state where the gate electrode 160 is patterned, the resistance of the source region S and the drain region D of the oxide semiconductor layer 140 is reduced ( Figure 3 Specifically, impurities are injected into the oxide semiconductor layer 140 from the gate electrode 160 side through the gate insulating layer 150 by ion implantation. For example, argon (Ar), phosphorus (P), and boron (B) are injected into the oxide semiconductor layer 140 by ion implantation. Oxygen vacancies are formed in the oxide semiconductor layer 140 by ion implantation, thereby reducing the resistance of the oxide semiconductor layer 140. Since the gate electrode 160 is provided above the oxide semiconductor layer 140 that functions as the channel region CH of the semiconductor device 10, impurities are not injected into the oxide semiconductor layer 140 in the channel region CH.
[0129] In this embodiment, the thickness T2 of the second region 154 of the gate insulating layer 150 is formed to be greater than 75 nm and less than 100 nm. If it is within this range, the acceleration condition of the ion implantation device is satisfied, so impurities can be uniformly added in the substrate surface. In addition, when the thickness T2 of the second region 154 exceeds 100 nm, in the region where the oxide semiconductor layer 140 overlaps with the tapered portion of the gate electrode 105, it is equivalent to effectively increasing the thickness of the gate insulating layer 150.
[0130] Fig. 10B Yes Fig. 10A An enlarged view of a portion of the semiconductor device shown. Specifically, Fig. 10BIt is an enlarged view near the gate electrode 105. The gate electrode 105 includes an upper surface 105a and a tapered portion 105b. In the region where the oxide semiconductor layer 140 overlaps with the upper surface 105a of the gate electrode 105 and in the region where the gate electrode 105 is not provided, the thickness of the second region 154 becomes a thickness T2. However, the thickness of the region where the oxide semiconductor layer 140 overlaps with the tapered portion 105b becomes a thickness T4 thicker than the thickness T2. In such a state, when the impurity 145 is added by ion implantation, if the thickness T4 is less than 125nm, the impurity 145 can be uniformly added to the source region S and the drain region D of the oxide semiconductor layer 140. If the thickness T4 exceeds 125nm, there is a situation where the acceleration conditions of the ion implantation device are not met. In the region of the oxide semiconductor layer 140 overlapping with the tapered portion 105b, the addition of the impurity 145 is sometimes insufficient. As a result, the resistance of the source region S and the drain region D sometimes becomes uneven within the substrate surface. Furthermore, when dry etching of the gate electrode 160 occurs, if the amount of the gate insulating layer 150 removed varies within the plane, this tendency becomes more significant.
[0131] like Figure 3 and Fig.11 As shown, insulating layers 170 and 180 are formed on the gate insulating layer 150 and the gate electrode 160 as interlayer films ( Figure 3 The insulating layers 170 and 180 are formed by CVD. For example, silicon nitride is formed as the insulating layer 170, and silicon oxide is formed as the insulating layer 180. The materials used as the insulating layers 170 and 180 are not limited to the above. The thickness of the insulating layer 170 is not less than 50 nm and not more than 500 nm. The thickness of the insulating layer 180 is not less than 50 nm and not more than 500 nm.
[0132] like Figure 3 and Fig.12 As shown, openings 171 and 173 are formed in the gate insulating layer 150 and the insulating layers 170 and 180 ( Figure 3 The oxide semiconductor layer 140 in the source region S is exposed through the opening 171. The oxide semiconductor layer 140 in the drain region D is exposed through the opening 173. The source / drain electrodes 200 ( Figure 3 Step S3013 of "SD formation"), thereby completing Figure 1A A semiconductor device 10 is shown.
[0133] The semiconductor device 10 manufactured by the above manufacturing method can obtain a mobility of 30 [cm 2 / Vs] or more, 35[cm 2 / Vs] or more or 40[cm 2 / Vs] or above. The mobility in this embodiment refers to the field effect mobility in the saturation region of the semiconductor device 10. Specifically, the mobility refers to the maximum value of the field effect mobility in the region where the potential difference (Vd) between the source electrode and the drain electrode is greater than the value (Vg-Vth) obtained by subtracting the threshold voltage (Vth) of the semiconductor device 10 from the voltage (Vg) supplied to the gate electrode.
[0134] In this embodiment, after forming the gate insulating layer 150, the metal oxide layer 190 is formed and oxidative annealing is performed. Through this oxidative annealing, the oxygen can be efficiently supplied to the oxide semiconductor layer 140 to fully repair the oxygen deficiency. Therefore, even if the thickness T1 of the first region 152 of the gate insulating layer 150 is greater than 100 nm and less than 125 nm, and the thickness T2 of the second region 154 is greater than 75 nm and less than 100 nm, the electrical characteristics of the transistor can be suppressed from becoming normally-on.
[0135] <Second Embodiment>
[0136] use Figures 13A to 24 A semiconductor device according to an embodiment of the present invention will be described.
[0137] [Configuration of Semiconductor Device 10]
[0138] The configuration of the semiconductor device 10 according to this embodiment is similar to that of the semiconductor device 10 according to the first embodiment, but is different from the semiconductor device 10 according to the first embodiment in that an oxide metal layer 130 (also referred to as metal oxide) is provided between the gate insulating layer 120 and the oxide semiconductor layer 140. In the following description, description of the same configuration as that of the first embodiment is omitted, and the differences from the first embodiment are mainly described.
[0139] Fig.13A It is a cross-sectional view schematically showing a semiconductor device according to an embodiment of the present invention. Fig. 13B Yes Fig.13A An enlarged view of a portion of the semiconductor device shown. Fig.13AAs shown, the semiconductor device 10 includes a gate electrode 105 , gate insulating layers 110 , 120 , a metal oxide layer 130 , an oxide semiconductor layer 140 , a gate insulating layer 150 , a gate electrode 160 , insulating layers 170 , 180 , a source electrode 201 , and a drain electrode 203 .
[0140] The metal oxide layer 130 is provided on the gate insulating layer 120. The metal oxide layer 130 is in contact with the gate insulating layer 120. The oxide semiconductor layer 140 is provided on the metal oxide layer 130. The oxide semiconductor layer 140 is in contact with the metal oxide layer 130. The surface of the main surface of the oxide semiconductor layer 140 that is in contact with the metal oxide layer 130 is referred to as a lower surface 142. The end of the metal oxide layer 130 is substantially consistent with the end of the oxide semiconductor layer 140.
[0141] In this embodiment, no semiconductor layer or oxide semiconductor layer is provided between the metal oxide layer 130 and the substrate 100 .
[0142] In this embodiment, a metal oxide layer is provided below and in contact with the oxide semiconductor layer 140. Fig.13A and Fig. 13B In the embodiment, the structure in which the metal oxide layer 130 is in contact with the gate insulating layer 120 and the oxide semiconductor layer 140 is in contact with the metal oxide layer 130 is illustrated, but the present invention is not limited to this structure. Other layers may be provided between the gate insulating layer 120 and the metal oxide layer 130. Other layers may be provided between the metal oxide layer 130 and the oxide semiconductor layer 140.
[0143] exist Fig.13A In the embodiment, the side wall of the metal oxide layer 130 and the side wall of the oxide semiconductor layer 140 are arranged in a straight line, but the present invention is not limited to this configuration. The angle of the side wall of the metal oxide layer 130 relative to the main surface of the substrate 100 may be different from the angle of the side wall of the oxide semiconductor layer 140 relative to the main surface of the substrate 100. The cross-sectional shape of the side wall of at least one of the metal oxide layer 130 and the oxide semiconductor layer 140 may be curved.
[0144] The metal oxide layer 130 is a layer containing metal oxide having aluminum as a main component, similarly to the metal oxide layer 190, and has a function as a gas barrier film for shielding gases such as oxygen and hydrogen. The metal oxide layer 130 is made of the same material as the metal oxide layer 190. The material of the metal oxide layer 130 may be the same as or different from that of the metal oxide layer 190.
[0145] like Fig. 13BAs shown, in the gate insulating layer 150, the thickness T1 of the first region 152 is different from the thickness T2 of the second region 154. The thickness T1 of the first region 152 is the thickness when the gate insulating layer 150 is formed in the manufacturing process. The thickness T2 of the second region 154 is the thickness formed by dry etching when forming the gate electrode 160.
[0146] The planar shape of the semiconductor device 10 is Figure 2 Similarly, although illustration is omitted, the planar pattern of the metal oxide layer 130 is substantially the same as the planar pattern of the oxide semiconductor layer 140 when viewed from above. Fig.13A When the lower surface 142 of the oxide semiconductor layer 140 is covered by the metal oxide layer 130 , in particular, in the present embodiment, the lower surface 142 of the oxide semiconductor layer 140 is entirely covered by the metal oxide layer 130 .
[0147] In this embodiment, a configuration in which the entire lower surface 142 of the oxide semiconductor layer 140 is covered by the oxide metal layer 130 is exemplified, but the present invention is not limited to this configuration. For example, a portion of the lower surface 142 of the oxide semiconductor layer 140 may not be in contact with the oxide metal layer 130. For example, the entire lower surface 142 of the oxide semiconductor layer 140 in the channel region CH may be covered by the oxide metal layer 130, and the entire or a portion of the lower surface 142 of the oxide semiconductor layer 140 in the source region S and the drain region D may not be covered by the oxide metal layer 130. That is, the entire or a portion of the lower surface 142 of the oxide semiconductor layer 140 in the source region S and the drain region D may not be in contact with the oxide metal layer 130. However, in the above configuration, a portion of the lower surface 142 of the oxide semiconductor layer 140 in the channel region CH may not be covered by the oxide metal layer 130, and the other portion of the lower surface 142 may be in contact with the oxide metal layer 130.
[0148] The ratio of indium in the oxide semiconductor layer 140 is set to 50% or more, thereby realizing a semiconductor device 10 with high mobility. On the other hand, in such an oxide semiconductor layer 140 , oxygen contained in the oxide semiconductor layer 140 is easily reduced, so that oxygen vacancies are easily formed in the oxide semiconductor layer 140 .
[0149] In the semiconductor device 10, hydrogen is released from a layer (e.g., gate insulating layers 110 and 120) disposed closer to the substrate 100 than the oxide semiconductor layer 140 during a heat treatment process in the manufacturing process. As the hydrogen reaches the oxide semiconductor layer 140, oxygen vacancies are generated in the oxide semiconductor layer 140. The generation of the oxygen vacancies is more significant when the pattern size of the oxide semiconductor layer 140 is larger. In order to suppress the generation of such oxygen vacancies, it is necessary to suppress the hydrogen from reaching the lower surface 142 of the oxide semiconductor layer 140. The above content is the first subject.
[0150] In addition, the upper surface 141 of the oxide semiconductor layer 140 is affected by a process (e.g., a patterning process or an etching process) after forming the oxide semiconductor layer 140. On the other hand, the lower surface 142 of the oxide semiconductor layer 140 (the surface of the oxide semiconductor layer 140 on the substrate 100 side) is not affected in the above manner.
[0151] Therefore, the oxygen vacancies formed near the upper surface 141 of the oxide semiconductor layer 140 are more than the oxygen vacancies formed near the lower surface 142 of the oxide semiconductor layer 140. That is, the oxygen vacancies in the oxide semiconductor layer 140 are not uniformly present in the thickness direction of the oxide semiconductor layer 140, but are unevenly distributed in the thickness direction of the oxide semiconductor layer 140. Specifically, the oxygen vacancies in the oxide semiconductor layer 140 are less toward the lower surface 142 of the oxide semiconductor layer 140, and more toward the upper surface 141 of the oxide semiconductor layer 140.
[0152] In the case where the oxygen supply treatment is uniformly performed on the oxide semiconductor layer 140 having the above-described oxygen vacancy distribution, if the amount of oxygen required to repair the oxygen vacancy formed on the upper surface 141 side of the oxide semiconductor layer 140 is supplied, oxygen will be excessively supplied to the lower surface 142 side of the oxide semiconductor layer 140. As a result, on the lower surface 142 side, a defect energy level different from the oxygen vacancy is formed due to the excess oxygen. As a result, phenomena such as characteristic changes in reliability tests or a decrease in field effect mobility occur. Therefore, in order to suppress such a phenomenon, it is necessary to supply oxygen to the upper surface 141 side of the oxide semiconductor layer 140 while suppressing the oxygen supply to the lower surface 142 side of the oxide semiconductor layer 140.
[0153] The above-mentioned problems are newly recognized problems in the process of realizing the present invention, rather than problems that have been recognized in the past. In the previous structure and manufacturing method, even if the initial characteristics of the semiconductor device are improved by oxygen supply treatment to the oxide semiconductor layer, the characteristics change in the reliability test will occur, and there is a trade-off relationship between the initial characteristics and the reliability test. However, the structure involved in this embodiment can solve the above-mentioned problems and obtain good initial characteristics and reliability tests of the semiconductor device 10.
[0154] [Method of Manufacturing Semiconductor Device 10]
[0155] use Figure 14 to Figure 24 A method for manufacturing a semiconductor device according to an embodiment of the present invention will be described. Fig.14 This is a timing chart showing a method for manufacturing a semiconductor device according to an embodiment of the present invention. Figure 15 to Figure 24 1 is a cross-sectional view showing a method for manufacturing a semiconductor device according to an embodiment of the present invention. In the following description of the manufacturing method, a method for manufacturing the semiconductor device 10 using aluminum oxide as the metal oxide layers 130 and 190 will be described.
[0156] like Fig.14 and Fig.15 As shown, a gate electrode 105 is formed on the substrate 100 as a bottom gate, and gate insulating layers 110 and 120 are formed on the gate electrode 105 ( Fig.14 (“Bottom GI / GE formation” in step S2001). For example, silicon nitride is formed as the gate insulating layer 110. For example, silicon oxide is formed as the gate insulating layer 120. The gate insulating layers 110 and 120 are formed by a CVD (Chemical Vapor Deposition) method.
[0157] By using silicon nitride as the gate insulating layer 110, the gate insulating layer 110 can block, for example, impurities diffusing from the substrate 100 toward the oxide semiconductor layer 140. Silicon oxide used as the gate insulating layer 120 has a property of releasing oxygen by heat treatment.
[0158] like Fig.14 and Fig.16 As shown, a metal oxide layer 130 and an oxide semiconductor layer 140 are formed on the gate insulating layer 120 ( Fig.14 The metal oxide layer 130 and the oxide semiconductor layer 140 are formed by sputtering or atomic layer deposition (ALD: Atomic Layer Deposition).
[0159] The thickness of the metal oxide layer 130 is, for example, 1 nm to 100 nm, 1 nm to 50 nm, 1 nm to 30 nm or 1 nm to 10 nm. In this embodiment, aluminum oxide is used as the metal oxide layer 130. Aluminum oxide has a high barrier property against gas. In this embodiment, aluminum oxide used as the metal oxide layer 130 blocks hydrogen and oxygen released from the gate insulating layer 120, and inhibits the released hydrogen and oxygen from reaching the oxide semiconductor layer 140.
[0160] For example, the thickness of the oxide semiconductor layer 140 is 10 nm to 100 nm, 15 nm to 70 nm, or 20 nm to 40 nm. In this embodiment, an oxide containing indium (In) and gallium (Ga) is used as the oxide semiconductor layer 140. The oxide semiconductor layer 140 before OS annealing described below is amorphous.
[0161] When the oxide semiconductor layer 140 is crystallized by OS annealing described later, the oxide semiconductor layer 140 after film formation and before OS annealing is preferably in an amorphous state (a state in which the crystalline component of the oxide semiconductor is small). That is, the film formation conditions of the oxide semiconductor layer 140 are preferably conditions in which the oxide semiconductor layer 140 immediately after film formation is not crystallized as much as possible. For example, when the oxide semiconductor layer 140 is formed by sputtering, the oxide semiconductor layer 140 is formed under a state in which the temperature of the film formation object (the substrate 100 and the structure formed thereon) is controlled.
[0162] When a film is formed on an object to be formed by sputtering, ions generated in the plasma and atoms recoiled from the sputtering target will collide with the object to be formed. Therefore, the temperature of the object to be formed will rise along with the film forming process. If the temperature of the object to be formed rises during the film forming process, the oxide semiconductor layer 140 contains microcrystals in the state just after the film is formed. Due to the microcrystals, the subsequent crystallization caused by OS annealing is hindered. In order to control the temperature of the object to be formed as described above, the film can also be formed while cooling the object to be formed. For example, the object to be formed can also be cooled from the surface opposite to the film forming surface in such a way that the temperature of the film forming surface of the object to be formed is below 100°C, below 70°C, below 50°C, or below 30°C. By forming the oxide semiconductor layer 140 while cooling the object to be formed as described above, an oxide semiconductor layer 140 with a small amount of crystalline components in the state just after the film is formed can be formed.
[0163] like Fig.14 and Fig.17 As shown, the pattern of the oxide semiconductor layer 140 is formed ( Fig.14Although not shown in the figure, a resist mask is formed on the oxide semiconductor layer 140, and the oxide semiconductor layer 140 is etched using the resist mask. The oxide semiconductor layer 140 can be etched by wet etching or dry etching. As wet etching, an acidic etchant can also be used for etching. For example, oxalic acid or hydrofluoric acid can be used as an etchant.
[0164] After the patterning of the oxide semiconductor layer 140, the oxide semiconductor layer 140 is subjected to a heat treatment (OS annealing) ( Fig.14 In this embodiment, the oxide semiconductor layer 140 is crystallized by the OS annealing.
[0165] like Fig.14 and Fig.18 As shown, the pattern of the oxidized metal layer 130 is formed ( Fig.14 The metal oxide layer 130 is etched using the oxide semiconductor layer 140 patterned in the above process as a mask. The metal oxide layer 130 may be etched by wet etching or dry etching. For example, diluted hydrofluoric acid (DHF) is used as the wet etching. By etching the metal oxide layer 130 using the oxide semiconductor layer 140 as a mask as described above, the photolithography process can be omitted.
[0166] like Fig.14 and Fig.19 As shown, the gate insulating layer 150 ( Fig.14 GI formation in step S2006). For example, silicon oxide is formed as the gate insulating layer 150. The gate insulating layer 150 is formed by a CVD method. For example, as the gate insulating layer 150, in order to form an insulating layer with few defects as described above, the gate insulating layer 150 may be formed at a film forming temperature of 350°C or higher. The thickness of the gate insulating layer 150 is, for example, 50 nm to 300 nm, 60 nm to 200 nm, or 70 nm to 150 nm. After the gate insulating layer 150 is formed, a process of injecting oxygen into a portion of the gate insulating layer 150 may be performed. A metal oxide layer 190 ( Fig.14 The metal oxide layer 190 is formed by sputtering. Oxygen is injected into the gate insulating layer 150 by forming the metal oxide layer 190.
[0167] For example, the thickness of the metal oxide layer 190 is 5 nm to 100 nm, 5 nm to 50 nm, 5 nm to 30 nm, or 7 nm to 15 nm. In this embodiment, aluminum oxide is used as the metal oxide layer 190. Aluminum oxide has a high barrier property against gas. In this embodiment, aluminum oxide used as the metal oxide layer 190 is used to suppress the diffusion of oxygen injected into the gate insulating layer 150 to the outside when the metal oxide layer 190 is formed.
[0168] For example, when the metal oxide layer 190 is formed by sputtering, the process gas used for sputtering may remain in the film of the metal oxide layer 190. For example, when Ar is used as the process gas for sputtering, Ar may remain in the film of the metal oxide layer 190. The remaining Ar can be detected by SIMS (Secondary Ion Mass Spectrometry) analysis performed on the metal oxide layer 190.
[0169] In a state where the gate insulating layer 150 is formed on the oxide semiconductor layer 140 and the metal oxide layer 190 is formed on the gate insulating layer 150, a heat treatment (oxidation annealing) for supplying oxygen to the oxide semiconductor layer 140 is performed ( Fig.14 In the process from forming the oxide semiconductor layer 140 to forming the gate insulating layer 150 on the oxide semiconductor layer 140, a large number of oxygen vacancies are generated on the upper surface 141 and the side surface 143 of the oxide semiconductor layer 140. The oxygen released from the gate insulating layers 120 and 150 by the above-mentioned oxidation annealing is supplied to the oxide semiconductor layer 140 to repair the oxygen vacancies.
[0170] Oxygen released from the gate insulating layer 120 by the oxidation annealing is blocked by the oxidized metal layer 130. Therefore, it is difficult to supply oxygen to the lower surface 142 of the oxide semiconductor layer 140. Oxygen released from the gate insulating layer 120 diffuses from the region where the oxidized metal layer 130 is not formed to the gate insulating layer 150 provided on the gate insulating layer 120, and reaches the oxide semiconductor layer 140 via the gate insulating layer 150. As a result, oxygen released from the gate insulating layer 120 is not easily supplied to the lower surface 142 of the oxide semiconductor layer 140, and is mainly supplied to the side surface 143 and the upper surface 141 of the oxide semiconductor layer 140. In addition, oxygen released from the gate insulating layer 150 by the oxidation annealing is supplied to the upper surface 141 and the side surface 143 of the oxide semiconductor layer 140. Although hydrogen may be released from the gate insulating layers 110 and 120 due to the above-mentioned oxidation annealing, the hydrogen is blocked by the oxidized metal layer 130.
[0171] As described above, the oxidation annealing step can suppress supply of oxygen to the lower surface 142 of the oxide semiconductor layer 140 having a small amount of oxygen vacancies, while supplying oxygen to the upper surface 141 and the side surface 143 of the oxide semiconductor layer 140 having a large amount of oxygen vacancies.
[0172] Similarly, in the above-mentioned oxidation annealing, oxygen injected into the gate insulating layer 150 is blocked by the oxidized metal layer 190. Therefore, the oxygen is suppressed from being released into the atmosphere. Therefore, through the oxidation annealing, the oxygen is efficiently supplied to the oxide semiconductor layer 140 to repair oxygen vacancies.
[0173] like Fig.14 and Fig. 20 As shown, after the oxidation annealing, the oxide metal layer 190 is etched (removed) ( Fig.14 As for etching of the oxidized metal layer 190, wet etching or dry etching may be used. As for wet etching, for example, diluted hydrofluoric acid (DHF) is used.
[0174] Next, a gate electrode 160 ( Fig.14 GE formation in step S2010). Fig.21 As shown, the titanium-containing layer 162 and the conductive layer 164 are sequentially formed. The titanium-containing layer 162 and the conductive layer 164 in the gate electrode 160 are formed by sputtering or atomic layer deposition. In this embodiment, as described above, for the gate electrode 160, a stacked structure of the titanium-containing layer 162 and the conductive layer 164 is preferably used. In this embodiment, the thickness of the titanium-containing layer 162 is greater than or equal to 25 nm and less than or equal to 50 nm.
[0175] like Fig. 22 As shown, the titanium-containing layer 162 and the conductive layer 164 are patterned by a photolithography process. The titanium-containing layer 162 and the conductive layer 164 are processed by dry etching. The etching rate of the titanium-containing layer 162 is slower than the etching rate of the conductive layer 164. In the present embodiment, the thickness of the titanium-containing layer 162 is greater than 25 nm and less than 50 nm. Therefore, the in-plane deviation of the line width of the gate electrode 160 within the substrate surface can be suppressed. In addition, the in-plane deviation of the amount removed in the second region 154 of the gate insulating layer 150 can be suppressed. By dry etching, the thickness T2 of the second region 154 is made greater than 75 nm and less than 100 nm. As described above, the gate electrode 160 is formed in a manner that is in contact with the gate insulating layer 150 exposed by removing the oxide metal layer 190.
[0176] In a state where the gate electrode 160 is patterned, the resistance of the source region S and the drain region D of the oxide semiconductor layer 140 is reduced ( Fig.14Specifically, impurities are injected into the oxide semiconductor layer 140 from the gate electrode 160 side through the gate insulating layer 150 by ion implantation. For example, argon (Ar), phosphorus (P), and boron (B) are implanted into the oxide semiconductor layer 140 by ion implantation. Oxygen vacancies are formed in the oxide semiconductor layer 140 by ion implantation, thereby reducing the resistance of the oxide semiconductor layer 140. Since the gate electrode 160 is provided above the oxide semiconductor layer 140 that functions as the channel region CH of the semiconductor device 10, impurities are not injected into the oxide semiconductor layer 140 in the channel region CH.
[0177] like Fig.14 and Fig.23 As shown, insulating layers 170 and 180 are formed on the gate insulating layer 150 and the gate electrode 160 as interlayer films ( Fig.14 The insulating layers 170 and 180 are formed by CVD. For example, silicon nitride is formed as the insulating layer 170, and silicon oxide is formed as the insulating layer 180. The materials used as the insulating layers 170 and 180 are not limited to the above. The thickness of the insulating layer 170 is not less than 50 nm and not more than 500 nm. The thickness of the insulating layer 180 is not less than 50 nm and not more than 500 nm.
[0178] like Fig.14 and Fig.24 As shown, openings 171 and 173 are formed in the gate insulating layer 150 and the insulating layers 170 and 180 ( Fig.14 The oxide semiconductor layer 140 in the source region S is exposed through the opening 171. The oxide semiconductor layer 140 in the drain region D is exposed through the opening 173. The source / drain electrodes 200 ( Fig.14 Step S2014 of "SD formation"), thereby completing Fig.13A A semiconductor device 10 is shown.
[0179] The semiconductor device 10 manufactured by the above manufacturing method can obtain a mobility of 50 [cm 2 / Vs] or more, 55[cm 2 / Vs] or more or 60[cm 2 / Vs] or above. The mobility in this embodiment refers to the field effect mobility in the saturation region of the semiconductor device 10. Specifically, the mobility refers to the maximum value of the field effect mobility in the region where the potential difference (Vd) between the source electrode and the drain electrode is greater than the value (Vg-Vth) obtained by subtracting the threshold voltage (Vth) of the semiconductor device 10 from the voltage (Vg) supplied to the gate electrode.
[0180] <Third Embodiment>
[0181] use Figure 25 to Figure 29 A display device using a semiconductor device according to an embodiment of the present invention will be described. In the following embodiment, a circuit configuration in which the semiconductor device 10 described in the first and second embodiments is applied to a liquid crystal display device will be described.
[0182] [Overview of Display Device 20]
[0183] Fig.25 1 is a top view showing an overview of a display device according to an embodiment of the present invention. Fig.25 As shown, the display device 20 includes an array substrate 300, a sealing portion 310, an opposing substrate 320, a flexible printed circuit substrate 330 (FPC 330), and an IC chip 340. The array substrate 300 and the opposing substrate 320 are bonded together by the sealing portion 310. A plurality of pixel circuits 301 are arranged in a matrix in a liquid crystal region 22 surrounded by the sealing portion 310. The liquid crystal region 22 is a region that overlaps with a liquid crystal element 311 described later in a plan view.
[0184] The sealing region 24 provided with the sealing portion 310 is the region around the liquid crystal region 22. The FPC 330 is provided in the terminal region 26. The terminal region 26 is the region where the array substrate 300 is exposed from the counter substrate 320 and is provided outside the sealing region 24. The outside of the sealing region 24 refers to the region provided with the sealing portion 310 and the outside of the region surrounded by the sealing portion 310. The IC chip 340 is provided on the FPC 330. The IC chip 340 supplies a signal for driving each pixel circuit 301.
[0185] [Circuit Configuration of Display Device 20]
[0186] Fig.26 FIG. 1 is a block diagram showing a circuit configuration of a display device according to an embodiment of the present invention. Fig.26As shown, a source driving circuit 302 is provided at a position adjacent to the liquid crystal region 22 in the D1 direction (column direction) with respect to the pixel circuit 301, and a gate driving circuit 303 is provided at a position adjacent to the liquid crystal region 22 in the D2 direction (row direction). The source driving circuit 302 and the gate driving circuit 303 are provided in the above-mentioned sealing region 24. However, the region where the source driving circuit 302 and the gate driving circuit 303 are provided is not limited to the sealing region 24, and may be any region as long as it is outside the region where the pixel circuit 301 is provided.
[0187] The source wiring 304 extends from the source driver circuit 302 along the D1 direction and is connected to the plurality of pixel circuits 301 arranged in the D1 direction. The gate wiring 305 extends from the gate driver circuit 303 along the D2 direction and is connected to the plurality of pixel circuits 301 arranged in the D2 direction.
[0188] The terminal region 26 is provided with a terminal portion 306. The terminal portion 306 and the source driver circuit 302 are connected via a connection wiring 307. Similarly, the terminal portion 306 and the gate driver circuit 303 are connected via a connection wiring 307. By connecting the FPC 330 to the terminal portion 306, an external device connected to the FPC 330 is connected to the display device 20, and each pixel circuit 301 provided in the display device 20 is driven by a signal from the external device.
[0189] The semiconductor device 10 described in the first embodiment and the second embodiment is used as a transistor included in the pixel circuit 301 , the source driver circuit 302 , and the gate driver circuit 303 .
[0190] [Pixel Circuit 301 of Display Device 20]
[0191] Fig. 27 FIG. 1 is a circuit diagram showing a pixel circuit of a display device according to an embodiment of the present invention. Fig. 27 As shown, the pixel circuit 301 includes elements such as the semiconductor device 10, the holding capacitor 350, and the liquid crystal element 311. The semiconductor device 10 has a gate electrode 160, a source electrode 201, and a drain electrode 203. The gate electrode 160 is connected to the gate wiring 305. The source electrode 201 is connected to the source wiring 304. The drain electrode 203 is connected to the holding capacitor 350 and the liquid crystal element 311. In this embodiment, for the sake of convenience of description, the electrode represented by the figure mark "201" is called the source electrode, and the electrode represented by the figure mark "203" is called the drain electrode, but it is also possible that the electrode represented by the figure mark "201" functions as a drain electrode and the electrode represented by the figure mark "203" functions as a source electrode.
[0192] [Cross-sectional structure of display device 20]
[0193] Fig.28 FIG. 1 is a cross-sectional view of a display device according to an embodiment of the present invention. Fig.28 As shown in FIG. 1 , the display device 20 is a display device using the semiconductor device 10. In this embodiment, the semiconductor device 10 is used in the pixel circuit 301, but the semiconductor device 10 can also be used in peripheral circuits including the source driver circuit 302 and the gate driver circuit 303. In the following description, the semiconductor device 10 is used in the pixel circuit 301. Figure 1A The semiconductor device 10 shown is the same and therefore its description is omitted.
[0194] An insulating layer 360 is provided on the source electrode 201 and the drain electrode 203. A common electrode 370 provided in common to a plurality of pixels is provided on the insulating layer 360. An insulating layer 380 is provided on the common electrode 370. An opening 381 is provided on the insulating layers 360 and 380. A pixel electrode 390 is provided on the insulating layer 380 and inside the opening 381. The pixel electrode 390 is connected to the drain electrode 203.
[0195] Fig.29 FIG. 1 is a top view of a pixel electrode and a common electrode of a display device according to an embodiment of the present invention. Fig.29 As shown, the common electrode 370 has an overlapping region that overlaps with the pixel electrode 390 in a plan view and a non-overlapping region that does not overlap with the pixel electrode 390. When a voltage is supplied between the pixel electrode 390 and the common electrode 370, a transverse electric field is formed from the pixel electrode 390 in the overlapping region toward the common electrode 370 in the non-overlapping region. The liquid crystal molecules included in the liquid crystal element 311 are moved by the transverse electric field, thereby determining the grayscale of the pixel.
[0196] <Fourth Embodiment>
[0197] use Fig.30 and Fig.31 A display device using a semiconductor device according to an embodiment of the present invention will be described. In this embodiment, a circuit configuration in which the semiconductor device 10 described in the first and second embodiments is applied to an organic EL display device will be described. The overview and circuit configuration of the display device 20 are related to Fig.25 and Fig.26 The contents shown are the same, so the description is omitted.
[0198] [Pixel Circuit 301 of Display Device 20]
[0199] Fig.30 FIG. 1 is a circuit diagram showing a pixel circuit of a display device according to an embodiment of the present invention. Fig.30As shown, the pixel circuit 301 includes components such as a driving transistor 11, a selection transistor 12, a holding capacitor 210 and a light-emitting element DO. The driving transistor 11 and the selection transistor 12 have the same structure as the semiconductor device 10. The source electrode of the selection transistor 12 is connected to the signal line 211, and the gate electrode of the selection transistor 12 is connected to the gate line 212. The source electrode of the driving transistor 11 is connected to the anode power line 213, and the drain electrode of the driving transistor 11 is connected to one end of the light-emitting element DO. The other end of the light-emitting element DO is connected to the cathode power line 214. The gate electrode of the driving transistor 11 is connected to the drain electrode of the selection transistor 12. The holding capacitor 210 is connected to the gate electrode and the drain electrode of the driving transistor 11. A grayscale signal that determines the light intensity of the light-emitting element DO is supplied to the signal line 211. A signal for selecting a pixel row to which the above-mentioned grayscale signal is to be written is supplied to the gate line 212.
[0200] [Cross-sectional structure of display device 20]
[0201] Fig.31 It is a cross-sectional view of a display device according to one embodiment of the present invention. Fig.31 The display device 20 shown in FIG. Fig.28 The display device 20 shown is similar, but Fig.31 The structure above the insulating layer 360 in the display device 20 and Fig.28 The structure above the insulating layer 360 in the display device 20 is different. Fig.31 The display device 20 is configured as follows: Fig.28 The description of the same structure as the display device 20 is omitted, and the differences between the two are described.
[0202] like Fig.31 As shown, the display device 20 has a pixel electrode 390, a light-emitting layer 392 and a common electrode 394 (light-emitting element DO) above the insulating layer 360. The pixel electrode 390 is arranged on the insulating layer 360 and inside the opening 381. An insulating layer 362 is arranged on the pixel electrode 390. An opening 363 is arranged in the insulating layer 362. The opening 363 corresponds to the light-emitting area. That is, the insulating layer 362 divides the pixel. The light-emitting layer 392 and the common electrode 394 are arranged on the pixel electrode 390 exposed by the opening 363. The pixel electrode 390 and the light-emitting layer 392 are arranged separately with respect to each pixel. On the other hand, the common electrode 394 is arranged in common with multiple pixels. Different materials are used for the light-emitting layer 392 according to the display color of the pixel.
[0203] In the third and fourth embodiments, the semiconductor device described in the first and second embodiments is applied to a liquid crystal display device and an organic EL display device, but the semiconductor device can also be applied to display devices other than the above display devices (for example, a self-luminous display device or an electronic paper display device other than an organic EL display device). In addition, unless otherwise specified, the semiconductor device can be applied to display devices ranging from small and medium-sized to large display devices.
[0204] Example
[0205] First, the results of examining the dependency of the thickness T3 of the titanium-containing layer of the gate electrode 160 on the electrical characteristics of the semiconductor device 10 according to the above-described embodiment will be described.
[0206] [Electrical Characteristics 1 of Semiconductor Device 10]
[0207] use Figure 32 to Figure 37 The electrical characteristics of the semiconductor device 10 according to the above-described embodiment will be described. Figure 32 to Figure 37 This is a diagram showing the electrical characteristics of a semiconductor device according to an embodiment of the present invention. Figure 32 to Figure 37 The electrical characteristics of the semiconductor device shown are the electrical characteristics of the semiconductor device 10 shown in the first embodiment.
[0208] [Initial characteristics]
[0209] Figure 32 to Figure 37 The measurement conditions of the electrical characteristics shown are as follows.
[0210] ·Size of channel region CH: W / L=6.0μm / 3.0μm
[0211] Source-drain voltage: 0.1V (dashed line), 10V (solid line)
[0212] ·Gate voltage: -15V~+15V
[0213] ·Measurement environment: room temperature, dark room
[0214] Thickness of oxide semiconductor layer (IGZO): 30nm
[0215] ·Thickness of gate insulating layer (silicon oxide): 125nm
[0216] Thickness of titanium-containing layer (titanium): 0nm, 7nm, 25nm, 32nm, 50nm, 90nm
[0217] Thickness of Mo-Tungsten layer: 300nm
[0218] ·Measurement location: 20 locations within the substrate surface
[0219] exist Figure 32 to Figure 37 , there is shown an electrical characteristic (Id-Vg characteristic) of the semiconductor device 10. The horizontal axis represents the gate voltage Vg, and the vertical axis represents the drain current (Id). Figure 32 to Figure 37 These correspond to the cases where the thickness T3 of the titanium-containing layer is 0 nm, 7 nm, 25 nm, 32 nm, 50 nm, and 90 nm, respectively. Fig.38 It is a diagram showing the in-plane variation of the threshold voltage of the semiconductor device 10 .
[0220] like Fig.32 , Fig.33 , Fig.37 As shown, when the thickness T3 of the titanium-containing layer was 0 nm, 7 nm, and 90 nm, in-plane deviation was observed in the electrical characteristics of the transistor at 20 locations. It was confirmed that the electrical characteristics of the transistors all showed so-called normally-on characteristics in which the drain current Id began to flow when the gate voltage Vg was lower than 0 V.
[0221] In contrast, Figure 34 to Figure 36 As shown, when the thickness T3 of the titanium-containing layer was 25 nm, 32 nm, and 50 nm, no in-plane deviation was observed in the electrical characteristics of the transistor at 20 locations. In addition, it was confirmed that the electrical characteristics of the transistor showed a so-called normally-off characteristic in which the drain current Id began to flow when the gate voltage Vg was higher than 0 V.
[0222] exist Fig.38 The relationship between the thickness T3 of the titanium-containing layer of the gate insulating layer 150 and the threshold voltage of the semiconductor device is shown in FIG. It is confirmed that when the thickness T3 of the titanium-containing layer is 0 nm, 7 nm, and 90 nm, the electrical characteristics of the semiconductor device become normally on and the normally off characteristics cannot be obtained. In addition, the in-plane deviation of the threshold voltage of the semiconductor device is confirmed. Fig.38 As shown, it was confirmed that the normally-on characteristic was exhibited when the thickness T3 of the titanium-containing layer was 25 nm, 32 nm, and 50 nm. In addition, it was shown that the in-plane variation of the threshold voltage of the semiconductor device was suppressed.
[0223] It is shown that the thickness of the titanium-containing layer is preferably 50% or less of the thickness in the first region of the gate insulating layer.
[0224] Next, the results of examining the dependency of the electrical characteristics of the semiconductor device 10 according to the above-described embodiment on the thickness of the gate insulating layer 150 will be described.
[0225] [Electrical Characteristics 2 of Semiconductor Device 10]
[0226] use Figure 39 to Figure 42 The electrical characteristics of the semiconductor device 10 according to the above-described embodiment will be described. Figure 39 to Figure 41This is a diagram showing the electrical characteristics of a semiconductor device according to an embodiment of the present invention. Figure 39 to Figure 41 The electrical characteristics shown are the electrical characteristics of the semiconductor device 10 shown in the first embodiment.
[0227] Figure 39 to Figure 41 The measurement conditions of the electrical characteristics shown are as follows.
[0228] ·Size of channel region CH: W / L=6.0 μm / 2.0 μm
[0229] Source-drain voltage: 0.1V (dashed line), 10V (solid line)
[0230] ·Gate voltage: -15V~+15V
[0231] ·Measurement environment: room temperature, dark room
[0232] Thickness of oxide semiconductor layer (IGZO): 30nm
[0233] Thickness of titanium-containing layer (Ti): 25 nm
[0234] ·Thickness of gate insulating layer (silicon oxide): 100nm, 125nm, 150nm
[0235] Thickness of Mo-Tungsten layer: 300nm
[0236] ·Measurement location: 20 locations within the substrate surface
[0237] Here, the thicknesses of the gate insulating layer 100 nm, 125 nm, and 150 nm are all the thicknesses in the first region 152. By dry etching when forming the gate electrode, the thickness T2 of the second region 154 of the gate insulating layer 150 becomes 75 nm, 100 nm, and 125 nm, respectively.
[0238] exist Figure 39 to Figure 41 , the electrical characteristics (Id-Vg characteristics) of the semiconductor device 10 are shown. The horizontal axis is the gate voltage Vg, and the vertical axis is the drain current (Id). Fig.39 In the semiconductor device shown in FIG. 1 , the thickness of the first region of the oxide semiconductor layer 140 is 100 nm, and the thickness of the second region is 75 nm. Fig.40 In the semiconductor device shown in FIG. 1 , the thickness of the first region of the oxide semiconductor layer 140 is 125 nm, and the thickness of the second region is 100 nm. Fig.41 In the semiconductor device shown, the thickness of the first region of the oxide semiconductor layer 140 is 150 nm, and the thickness of the second region is 125 nm.
[0239] In addition, Fig.41 In the present invention, a deviation in the on-state current of the semiconductor device is confirmed within the substrate surface. Fig.41 The thickness T2 of the second region 154 of the gate insulating layer 150 of the semiconductor device in the embodiment of the present invention is 125 nm, which is more than 100 nm. Therefore, it is believed that during the ion implantation of the oxide semiconductor layer 140, impurities are not uniformly added to the oxide semiconductor layer 140 within the substrate surface, and the resistance of the source region S and the drain region D become non-uniform within the substrate surface. In particular, in the region where the oxide semiconductor layer 140 overlaps with the tapered portion of the gate electrode 105, the thickness of the gate insulating layer 150 is effectively increased. In other words, it is believed that in the region where the oxide semiconductor layer 140 overlaps with the tapered portion of the gate electrode 105, an area where the addition of impurities is not sufficiently performed is generated, resulting in the resistance of the source region S and the drain region D becoming non-uniform within the substrate surface. As a result, it is believed that the on-current of the semiconductor device within the substrate surface has a deviation.
[0240] exist Fig.42 The relationship between the thickness T1 of the first region 152 of the gate insulating layer 150 and the threshold voltage of the semiconductor device is shown in FIG. 1. When the thickness T1 of the first region 152 is less than 100 nm, the electrical characteristics of the semiconductor device become normally-on, and the normally-off characteristics cannot be obtained. Fig.42 As shown, when the thickness T1 of the first region 152 is 100 nm or more, it is confirmed that a so-called normally-on characteristic is exhibited in which the drain current Id starts to flow when the gate voltage Vg is lower than 0 V.
[0241] As described above, it can be seen that there is a correlation between the thickness of the titanium-containing layer 162 of the semiconductor device and the thickness of the gate insulating layer 150. If the relationship between the thickness of the titanium-containing layer 162 and the thickness of the gate insulating layer 150 is taken into account, the thickness of the titanium-containing layer is preferably less than 50% of the thickness of the gate insulating layer in the first region. In addition, the thickness of the titanium-containing layer is preferably more than 25% and less than 70% of the thickness of the gate insulating layer in the second region. A semiconductor device according to an embodiment of the present invention can have normally-off electrical characteristics and can suppress the deviation of electrical characteristics within the substrate surface. By using such a semiconductor device in a display device, a good display device with suppressed deviation can be provided.
[0242] The various embodiments described above as embodiments of the present invention can be implemented in appropriate combination as long as they do not contradict each other. In addition, solutions obtained by adding, deleting or changing the design of components or adding, omitting or changing the conditions of processes based on the semiconductor devices and display devices of the various embodiments by those skilled in the art are also included in the scope of the present invention as long as they have the gist of the present invention.
[0243] Even if there are other effects different from the effects brought about by the schemes of the above-mentioned embodiments, if they are clearly known from the description of this specification or can be easily predicted by those skilled in the art, they are of course understood to be the effects brought about by the present invention.
[0244] Description of Reference Numerals
[0245] 10: semiconductor device, 11: driving transistor, 12: selecting transistor, 20: display device, 22: liquid crystal region, 24: sealing region, 26: terminal region, 100: substrate, 105, 160: gate electrode, 110, 120, 150: gate insulating layer, 130, 190: metal oxide layer, 140: oxide semiconductor layer, 141: upper surface, 142: lower surface, 143: side surface, 170, 180: insulating layer, 171, 173: opening, 200: source / drain electrode, 201: source electrode, 203: drain electrode, 210: holding capacitor, 211: signal line, 212: gate line, 213: anode Power supply line, 214: cathode power supply line, 220: resist mask, 300: array substrate, 301: pixel circuit, 302: source driving circuit, 303: gate driving circuit, 304: source wiring, 305: gate wiring, 306: terminal portion, 307: connection wiring, 310: sealing portion, 311: liquid crystal element, 320: opposing substrate, 330: flexible printed circuit substrate (FPC), 340: IC chip, 350: holding capacitor, 360, 362: insulating layer, 363, 381: opening, 370: common electrode, 380: insulating layer, 390: pixel electrode, 392: light-emitting layer, 394: common electrode
Claims
1. A semiconductor device comprising: an oxide semiconductor layer disposed on the insulating surface; a gate insulating layer disposed on the oxide semiconductor layer; and a gate electrode provided on the oxide semiconductor layer via the gate insulating layer, The gate electrode includes a titanium-containing layer and a conductive layer in order from the gate insulating layer side, The gate insulating layer includes a first region overlapping with the gate electrode and a second region not overlapping with the gate electrode, The thickness of the titanium-containing layer is less than 50% of the thickness of the gate insulating layer in the first region.
2. The semiconductor device according to claim 1, wherein The thickness of the titanium-containing layer is greater than or equal to 25 nm and less than or equal to 50 nm.
3. The semiconductor device according to claim 1, wherein The thickness of the first region of the gate insulating layer is greater than or equal to 100 nm and less than or equal to 125 nm.
4. The semiconductor device according to claim 1, wherein The thickness of the titanium-containing layer is greater than or equal to 25% and less than 70% of the thickness of the gate insulating layer in the second region.
5. The semiconductor device according to claim 1, wherein The thickness of the second region of the gate insulating layer is greater than or equal to 75 nm and less than or equal to 100 nm.
6. The semiconductor device according to claim 1, wherein The titanium-containing layer is a titanium layer.
7. The semiconductor device according to claim 1, wherein The titanium-containing layer includes a titanium layer and a titanium nitride layer. 8 . The semiconductor device according to claim 1 , further comprising a metal oxide layer mainly composed of aluminum, wherein the metal oxide layer is provided on the insulating surface so as to be in contact with a lower portion of the oxide semiconductor layer.
9. The semiconductor device according to claim 1, wherein: The oxide semiconductor layer contains two metal elements including indium, In the oxide semiconductor layer, a ratio of indium is 50% or more.