Two-stage sand consolidation method based on soybean urease induced calcium carbonate deposition (EICP)

The two-stage sand-fixing method of induced calcium carbonate deposition in soybean urease solves the problems of microbial induction technology complexity and pollution of traditional grouting methods, and achieves efficient and environmentally friendly sand-soil curing, improving the strength and anti-seepage effect of sand-soil .

CN118894680APending Publication Date: 2024-11-05XIJING UNIV
View PDF 0 Cites 6 Cited by

Patent Information

Application Number
CN202410942092.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

In the prior art, the microbial-induced calcium carbonate deposition technology has a complex bacterial culture process, resulting in high costs and long maintenance cycles, making it difficult to quickly respond to the demand for repairing soils, and the introduction of microorganisms is accompanied by the risk of biological invasion; traditional grouting and reinforcement methods have high cost, Complex operation and environmental pollution problems; the second-stage infusion method has unevenness in the amount of calcium carbonate production and distribution, which affects the curing effect.

Method used

The second-stage sand-fixing method of soy urease-induced calcium carbonate deposition (EICP) is used to cure the standard sand through soy urease solution and cementitious solution, and then pour the soy urease solution and chlorination. Calcium solution and urea solution improve the curing strength and distribution uniformity of sand and soil.

Benefits of technology

It significantly improves the curing strength and anti-seepage sealing effect of sand soil, avoids the complexity of microbial induction technology and biosafety risks, achieves more environmentally friendly and economical soil reinforcement, and avoids environmental pollution from traditional grouting methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118894680A_ABST
    Figure CN118894680A_ABST
Patent Text Reader

Abstract

A two-stage sand consolidation method based on soybean urease induced calcium carbonate deposition (EICP) comprises the steps that traditional EICP consolidation is conducted on standard sand through soybean urease liquid and cementing liquid, a sandy soil sample is obtained after compaction and dehairing treatment, then the soybean urease liquid, a calcium chloride solution and a urea solution are sequentially poured to conduct two-stage sand consolidation on the sandy soil sample, and the two-stage sand consolidation result is obtained. Therefore, the solidification strength of the sandy soil is greatly improved; a permeation test and an unconfined compression test are respectively carried out on the solidified sandy soil solidified test block, and the test result shows that the method has an extremely remarkable solidification effect, so that the cementing fluid can be more uniformly distributed in rock and soil, the solidification accuracy and effectiveness are improved, the conversion efficiency is relatively high, and the application prospect is wide. Good application prospects are realized in the aspects of improving the sand strength, preventing seepage and plugging, repairing the surface and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of geotechnical engineering, and in particular to a two-stage sand consolidation method based on soybean urease-induced calcium carbonate deposition (EICP). Background Art

[0002] Earth-rock dam, as an important part of water conservancy construction, is a general term for earth dam, rockfill dam and earth-rock mixed dam. Its construction history is long and it is widely used all over the world. The reason why earth-rock dam is so common is mainly due to its many advantages. First, the construction cost of earth-rock dam is relatively low, which helps to save investment costs; second, it allows materials to be directly obtained at the construction site without long-distance transportation, further reducing construction costs; third, the structure of earth-rock dam is relatively simple and easy to construct; finally, earth-rock dam has a strong adaptive foundation deformation function and can withstand the challenges brought by various geological conditions.

[0003] The traditional grouting reinforcement method is a foundation treatment and reinforcement technology, which injects a gelling slurry (such as cement slurry, polymer, etc.) into the pores, cracks and voids of soil, rock formations or underground buildings through drilling. After injection, the grouting material will penetrate, fill, compact or split the soil or rock formation to form a whole, thereby improving the stability, bearing capacity and waterproofness of the foundation or rock formation. However, it has problems such as high cost, complex operation and environmental pollution. In order to solve the environmental pollution in construction projects, more and more green, environmentally friendly, and low-energy consumption building materials and process technologies have been developed and applied to actual production.

[0004] Microbial induced calcium carbonate deposition (MICP) technology is an emerging soil reinforcement technology. Urea is decomposed by urease produced by specific bacteria to generate carbonate ions. These ions combine with metal cations such as calcium ions in loess to form calcium carbonate precipitation, thereby filling the pores in the loess, increasing its density and strength, and effectively improving the geological properties of loess. However, the effect of MICP on soil solidification is affected by many factors such as bacterial species, concentration, reaction time, etc. There are still certain defects and challenges in terms of technical maturity, construction conditions, reinforcement effect, long-term stability, and environmental adaptability.

[0005] In the past few years, EICP has been considered as a technology to replace microbial induced calcium carbonate deposition. Since no organisms are directly involved in the process, EICP is considered a biomimetic technology. EICP technology provides new ideas and scientific basis for the rapid development of the field of biogeotechnical engineering. EICP is to mix urea, calcium chloride and urease in the soil. Urea is hydrolyzed under the catalysis of enzymes to generate ammonium ions and carbonate ions. Ammonium ions provide an alkaline environment in the solution, and carbonate ions and calcium ions combine to form calcium carbonate precipitation, thereby strengthening the soil.

[0006] At present, the EICP technology is used to solidify sandy soil. There are mainly two methods: mixed injection and step-by-step injection. Different injection methods will affect the amount and distribution of calcium carbonate, thereby changing the physical properties and mechanical strength of the soil. Compared with the mixed injection and step-by-step injection methods, the two-stage injection method will generate more calcium carbonate precipitation, thereby further improving the mechanical properties of the solidified sandy soil.

[0007] Mixed injection method: After the urease solution and the cementing liquid are mixed, they are added to the sand sample as soon as possible. After a period of chemical reaction, the mixed liquid is added at the same speed and the process is repeated. Since the urease solution and the cementing liquid will react chemically immediately, calcium carbonate crystals will be produced before the sand is injected, which is easy to clog at the injection end, resulting in uneven distribution of calcium carbonate in the sample after cementation and poor integrity.

[0008] Step-by-step infusion method: First, the urease solution is infused into the sample, and then the cementing liquid is added. After the infusion is completed, it needs to be left to stand for a period of time so that the urease can diffuse and penetrate into the sample, so that it can be directly adsorbed on the surface of the sand particles; continue to infuse the urease solution so that it is evenly distributed inside the sample, and finally the cementing liquid is infused to achieve the best effect. The step-by-step infusion method can produce calcium carbonate crystals within a certain period of time, and its distribution is more uniform than the single-phase infusion method. However, the subsequent infusion of the cementing liquid will cause the urease in the previous soil to be lost, which greatly reduces the amount of calcium carbonate produced and the conversion efficiency.

[0009] The patent application document with publication number CN117800759A discloses a method for curing concrete using microbial induced calcium carbonate deposition (MICP) technology. After the concrete is poured, MICP mineralizing liquid is sprayed on its surface. The mineralizing liquid is made by mixing bacterial solution and cementing solution. A dense calcium carbonate protective layer can be formed on its surface. While preventing the loss of water inside the concrete, the concrete's impermeability, cracking resistance and chloride ion corrosion resistance are greatly improved. However, the microbial induced calcium carbonate deposition technology has a complex bacterial culture process that leads to a long curing cycle and high cost, making it difficult to quickly respond to the needs of soil repair; at the same time, the introduction of microorganisms is also accompanied by a certain risk of biological invasion.

[0010] Liu Yang et al. (Liu Yang, Gao Yufeng, He Jia, et al. Experimental study on windbreak and sand fixation of soybean urease-induced calcium carbonate deposition technology [J]. Henan Science, 2019, 37(11): 1784-1789.) proposed an experimental study on windbreak and sand fixation of soybean urease-induced calcium carbonate deposition technology. The effect and mechanism of EICP were studied through indoor experiments. Urease was extracted from soybeans, mixed with equal amounts of calcium chloride and urea solution, and then sprayed on the surface of the sample to form a thin layer of hard crust on the surface of the sample. The windbreak and sand fixation effect of the technology was tested by testing the surface strength, wind erosion rate, water retention, permeability and calcium carbonate generation of the sample. When the EICP technology was used above, a simple spraying reinforcement method was adopted. Its effect was limited to the solidification of surface aeolian sand, and it mainly played a preliminary role in windbreak and sand fixation. It could not penetrate deeply into the sandy soil. The reinforcement effect and anti-seepage ability were both insufficient, and it was difficult to achieve the purpose of comprehensive strengthening. Summary of the invention

[0011] In order to overcome the defects of the above-mentioned prior art, the purpose of the present invention is to provide a two-stage sand consolidation method based on soybean urease induced calcium carbonate deposition (EICP), wherein the standard sand is subjected to traditional EICP solidification by soybean urease solution and a binder, and a sand sample is obtained after compaction and scraping, and then the sand sample is successively injected with soybean urease solution, calcium chloride solution and urea solution to carry out two-stage sand consolidation, thereby greatly improving the solidification strength of the sand; permeability tests and unconfined compression tests are carried out on the solidified sand test blocks, and the test results show that the present invention has a very significant solidification effect, so that the binder can be more evenly distributed in the rock and soil, improves the accuracy and effectiveness of solidification, and shows a higher conversion efficiency, and has a good application prospect in improving sand strength, anti-seepage sealing, surface repair and other aspects.

[0012] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0013] A two-stage sand consolidation method based on soybean urease-induced calcium carbonate deposition (EICP) specifically comprises the following steps:

[0014] Step 1: According to the dry density of 1.55g / cm 3 -1.65g / cm 3 Weigh a certain mass of standard sand, fully mix the standard sand with 0.5%-1% of soybean urease solution by mass of the standard sand, then add 0.5%-1% of cementing liquid by mass of the standard sand, and mix evenly to obtain a solidified sand block;

[0015] Step 2: compact the solidified sand blocks obtained in step 1 in 4-6 layers, scrape the layers between each other, and place them at 18-26°C for solidification to obtain a sand sample;

[0016] Step 3: The sand sample obtained in step 2 is infused with 1%-3% soybean urease solution by mass ratio of standard sand; after standing for 5-10 minutes, calcium chloride solution by mass ratio of standard sand is infused; after standing for 5-10 minutes, urea solution by mass ratio of standard sand is infused at last, and the mixture is infused at 1%-3% by mass ratio of standard sand, and the mixture is infused at 18-26°C for solidification to obtain a solidified sand test block.

[0017] The soybean urease solution in step 1 is:

[0018] The soybeans on the market are selected and dried in an oven at 40-60°C. The soybean particles are crushed by a grinder to obtain soybean powder. The soybean powder is sieved through a 0.1-0.3 mm sieve to filter out large particles and retain the soybean powder. The soybean powder is mixed with deionized water and stirred for 15-40 minutes to prepare a soybean solution with a concentration of 100-200 g / L. The soybean solution is centrifuged at a speed of 3000-6000 r / min for 15-30 minutes to extract the upper light yellow clear liquid, which is the soybean urease solution. The extracted soybean urease solution is stored at 4-6°C for later use.

[0019] The binder in step 1 is:

[0020] The urea solution of equal concentration and volume is uniformly mixed with the anhydrous calcium chloride solution to obtain a cementing liquid with a concentration of 0.5-1.5 mol / L.

[0021] In step 3, the calcium chloride solution is 80-100 g / L.

[0022] In step 3, the urea solution is 80-100 g / L.

[0023] The beneficial effects of the present invention are:

[0024] (1) Compared with the traditional grouting reinforcement method, the present invention utilizes EICP technology, which is more environmentally friendly, economical, and durable, and has a significant improvement in anti-seepage and strength.

[0025] (2) Compared with the mixed injection method, the mixed injection method is to mix the urease solution and the cementing liquid evenly and then inject the soil at one time under the EICP technology. Since the urease solution and the cementing liquid will immediately react chemically, calcium carbonate crystals will be produced before injecting the sand, which is easy to clog at the injection end, resulting in uneven distribution of calcium carbonate in the sample after cementation and poor integrity. The present invention solidifies the soil under the EICP technology, which can make the cementing liquid more evenly distributed in the sample, improve the accuracy and effectiveness of solidification, and show a higher conversion efficiency.

[0026] (3) Compared with the step-by-step perfusion method, the step-by-step perfusion method is to perfuse the soil with urease solution and cementing solution (a solution obtained by mixing urea solution and calcium chloride solution) step by step under the EICP technology, first perfusing the cementing solution and then perfusing the urease solution. Compared with the mixed perfusion method, the conversion efficiency of this method is further improved, and it has better mechanical properties than the mixed perfusion method. The present invention solidifies the soil under the EICP technology by sequentially perfusing the soil with urease solution, urea solution and calcium chloride solution, which can further improve the accuracy and effectiveness of solidification compared with the step-by-step perfusion method, and at the same time has higher strength and lower permeability than the step-by-step perfusion method.

[0027] (4) Compared with the MICP method of soil solidification, the two-stage sand consolidation method based on soybean urease-induced calcium carbonate deposition (EICP) of the present invention has a simpler operation process. Plant urease is directly extracted from soybeans and can directly induce the precipitation of calcium carbonate without going through a complex bacterial culture process. Since there is no direct participation of microorganisms in the precipitation process, the EICP technology is not limited by microbial growth and metabolism, so it can be applied to a wider range of soil types and particle size ranges, and avoids microbial ecological safety issues in practical applications.

[0028] In summary, based on the traditional EICP solidification, the present invention carries out two-stage sand consolidation on the sand sample, so that the binder is more evenly distributed in the rock and soil, the accuracy and effectiveness of the solidification are improved, and a higher conversion efficiency is shown, which greatly improves the solidification strength of the sand. It has good application prospects in improving the strength of loess, anti-seepage sealing, surface repair, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 It is a process flow chart of the present invention;

[0030] Figure 2 This is a flow chart of preparing sand sample of the present invention;

[0031] Figure 3 This is a flow chart of the preparation of soybean urease solution and cementing liquid according to the present invention;

[0032] Figure 4 It is a relationship diagram between the permeability coefficient and the pouring method under different dry density, cementation times and standing time of the present invention;

[0033] Figure 5 It is a relationship diagram between the unconfined compressive strength and the pouring method under different dry density, cementation times and standing time of the present invention;

[0034] Figure 6 The permeability coefficient of the present invention under different dry density, cementation times and standing time and CaCO 3 Generate quantity relationship diagram;

[0035] Figure 7 The unconfined compressive strength and CaCO3 of the present invention under different dry density, cementation times and standing time are 3 Generate quantity relationship diagram. DETAILED DESCRIPTION

[0036] The following will be combined with the accompanying drawings in the present invention and accompanied by text descriptions to clearly and completely explain the methods, processes and effects in the embodiments of the present invention.

[0037] Example 1

[0038] A two-stage sand consolidation method based on soybean urease-induced calcium carbonate deposition (EICP) specifically comprises the following steps:

[0039] Step 1: According to the dry density of 1.55g / cm 3 Weigh a certain mass of standard sand, mix the standard sand with 0.5% soybean urease solution by mass of the standard sand, then add 0.5% cementing liquid by mass of the standard sand, mix evenly to obtain a solidified sand block;

[0040] In the step 1, the soybean urease solution is:

[0041] Select soybeans from the market, dry them in an oven at 40°C, use a grinder to grind soybean particles to obtain soybean powder, pass the soybean powder through a 0.1 mm sieve, filter out large particles, and retain soybean powder; mix the soybean powder with deionized water and stir for 15 minutes to prepare a soybean solution with a concentration of 100 g / L, centrifuge the soybean solution at a speed of 3000 r / min for 15 minutes, extract the upper light yellow clear liquid, which is the soybean urease solution; store the extracted soybean urease solution at 4°C for later use;

[0042] The binder in step 1 is:

[0043] The urea solution of equal concentration and volume was uniformly mixed with the anhydrous calcium chloride solution to obtain a cementing solution with a concentration of 0.5 mol / L;

[0044] Step 2: Fill the solidified sand blocks obtained in step 1 into a mold with three layers of filter paper at the bottom in 4 layers. After filling, lay another layer of filter paper on the upper end of the mold. The lower ends of the mold are sealed with rubber plugs with holes, and the reserved holes are connected to the liquid outlet to ensure the uniform distribution of the cementing liquid inside the sample. Then, compact each layer of solidified sand blocks in the mold, scrape the layers, and let it stand at 18°C ​​for solidification to obtain a sand sample.

[0045] Step 3: The sand sample obtained in step 2 is infused with a soybean urease solution accounting for 1% of the mass ratio of the standard sand; after standing for 5 minutes, a calcium chloride solution accounting for 1% of the mass ratio of the standard sand is infused; after standing for 5 minutes, a urea solution accounting for 1% of the mass ratio of the standard sand is finally infused, and the sand is infused at 18°C ​​for curing to obtain a sand solidification test block;

[0046] In step 3, the calcium chloride solution is 80 g / L;

[0047] In step 3, the urea solution is 80 g / L.

[0048] Example 2

[0049] A two-stage sand consolidation method based on soybean urease-induced calcium carbonate deposition (EICP) specifically comprises the following steps:

[0050] Step 1: According to the dry density of 1.60g / cm 3 Weigh a certain mass of standard sand, mix the standard sand with soybean urease solution accounting for 0.75% of the mass of the standard sand, then add a cementing liquid accounting for 0.75% of the mass of the standard sand, and mix evenly to obtain a solidified sand block;

[0051] In the step 1, the soybean urease solution is:

[0052] Select soybeans from the market, dry them in an oven at 50°C, use a grinder to grind soybean particles to obtain soybean powder, pass the soybean powder through a 0.2 mm sieve, filter out large particles, and retain soybean powder; mix the soybean powder with deionized water and stir for 30 minutes to prepare a soybean solution with a concentration of 150 g / L, centrifuge the soybean solution at a speed of 4500 r / min for 25 minutes, extract the upper light yellow clear liquid, which is the soybean urease solution; store the extracted soybean urease solution at 5°C for later use;

[0053] The binder in step 1 is:

[0054] The urea solution of equal concentration and volume and the anhydrous calcium chloride solution were uniformly mixed to obtain a cementing solution with a concentration of 1.0 mol / L;

[0055] Step 2: Fill the solidified sand blocks obtained in step 1 into a mold with three layers of filter paper at the bottom in 5 layers. After filling, lay another layer of filter paper on the upper end of the mold. The lower ends of the mold are sealed with rubber plugs with holes, and the reserved holes are connected to the liquid outlet to ensure the uniform distribution of the cementing liquid inside the sample. Then, compact each layer of solidified sand blocks in the mold, scrape the layers, and let it stand at 22°C for solidification to obtain a sand sample.

[0056] Step 3: The sand sample obtained in step 2 is infused with soybean urease solution accounting for 2% of the mass ratio of the standard sand; after standing for 7 minutes, a calcium chloride solution accounting for 2% of the mass ratio of the standard sand is infused; after standing for 7 minutes, a urea solution accounting for 2% of the mass ratio of the standard sand is finally infused, and the sand is infused at 22° C. to obtain a sand solidification test block;

[0057] In step 3, the calcium chloride solution is 90 g / L;

[0058] The urea solution in step 3 is 90 g / L.

[0059] Example 3

[0060] A two-stage sand consolidation method based on soybean urease induced calcium carbonate deposition (EICP), characterized in that it specifically comprises the following steps:

[0061] Step 1: According to the dry density of 1.65g / cm 3 Weigh a certain mass of standard sand, fully mix the standard sand with 1% soybean urease solution by mass of the standard sand, then add 1% cementing liquid by mass of the standard sand, mix evenly to obtain a solidified sand block;

[0062] In the step 1, the soybean urease solution is:

[0063] Select soybeans from the market, dry them in an oven at 60°C, use a grinder to grind soybean particles to obtain soybean powder, pass the soybean powder through a 0.3 mm sieve, filter out large particles, and retain soybean powder; mix the soybean powder with deionized water and stir for 40 minutes to prepare a soybean solution with a concentration of 200 g / L, centrifuge the soybean solution at a speed of 6000 r / min for 30 minutes, extract the upper light yellow clear liquid, which is the soybean urease solution; store the extracted soybean urease solution at 6°C for later use;

[0064] The binder in step 1 is:

[0065] The urea solution of equal concentration and volume was uniformly mixed with the anhydrous calcium chloride solution to obtain a cementing solution with a concentration of 1.5 mol / L;

[0066] Step 2: Fill the solidified sand blocks obtained in step 1 into a mold with three layers of filter paper at the bottom in 6 layers. After filling, lay another layer of filter paper on the upper end of the mold. The lower ends of the mold are sealed with rubber plugs with holes, and the reserved holes are connected to the liquid outlet to ensure the uniform distribution of the cementing liquid inside the sample. Then, compact each layer of solidified sand blocks in the mold, scrape the layers, and let it stand at 26°C for solidification to obtain a sand sample.

[0067] Step 3: The sand sample obtained in step 2 is infused with a soybean urease solution accounting for 3% of the mass ratio of the standard sand; after standing for 10 minutes, a calcium chloride solution accounting for 3% of the mass ratio of the standard sand is infused; after standing for 10 minutes, a urea solution accounting for 3% of the mass ratio of the standard sand is finally infused, and the sand is allowed to stand and solidify at 26°C to obtain a sand solidification test block;

[0068] In step 3, the calcium chloride solution is 100 g / L;

[0069] In step 3, the urea solution is 100 g / L.

[0070] Example 4

[0071] A two-stage sand consolidation method based on soybean urease-induced calcium carbonate deposition (EICP) specifically comprises the following steps:

[0072] Step 1: According to the dry density of 1.65g / cm 3 Weigh a certain mass of standard sand, mix the standard sand with 1% of soybean urease solution by mass of the standard sand, then add 0.75% of cementing liquid by mass of the standard sand, mix evenly to obtain a solidified sand block;

[0073] In the step 1, the soybean urease solution is:

[0074] Select soybeans from the market, dry them in an oven at 50°C, use a grinder to grind soybean particles to obtain soybean powder, pass the soybean powder through a 0.2mm sieve, filter out large particles, and retain soybean powder; mix the soybean powder with deionized water and stir for 40 minutes to prepare a soybean solution with a concentration of 200g / L, centrifuge the soybean solution at a speed of 6000r / min for 30 minutes, extract the upper light yellow clear liquid, which is the soybean urease solution; store the extracted soybean urease solution at 5°C for later use;

[0075] The binder in step 1 is:

[0076] The urea solution of equal concentration and volume was uniformly mixed with the anhydrous calcium chloride solution to obtain a cementing solution with a concentration of 1.5 mol / L;

[0077] Step 2: Fill the solidified sand blocks obtained in step 1 into a mold with three layers of filter paper at the bottom in 6 layers. After filling, lay another layer of filter paper on the upper end of the mold. The lower ends of the mold are sealed with rubber plugs with holes, and the reserved holes are connected to the liquid outlet to ensure the uniform distribution of the cementing liquid inside the sample. Then, compact each layer of solidified sand blocks in the mold, scrape the layers, and let it stand at 25°C to solidify, so as to obtain a sand sample.

[0078] Step 3: The sand sample obtained in step 2 is infused with a soybean urease solution accounting for 3% of the mass ratio of the standard sand; after standing for 10 minutes, a calcium chloride solution accounting for 2% of the mass ratio of the standard sand is infused; after standing for 10 minutes, a urea solution accounting for 2% of the mass ratio of the standard sand is finally infused, and the sand is infused at 25°C for curing to obtain a sand solidification test block;

[0079] In step 3, the calcium chloride solution is 90 g / L;

[0080] The urea solution in step 3 is 90 g / L.

[0081] Test verification

[0082] The mixed injection method is adopted for the sand sample obtained in the above step 2. The specific solidification steps are: 10-20mL urease solution, 10-20mL calcium chloride and 10-20mL urea solution are mixed evenly and then directly injected into the sand sample. After standing for 10-20 minutes, the sand solidification specimen is inverted to obtain a solidified specimen.

[0083] The sand sample obtained in the above step 2 is injected in a step-by-step manner. The specific solidification steps are as follows: first inject 10-20 mL of urease solution, slowly inject until it is completely injected, let it stand for 10-20 minutes, then inject the binder (a mixture of 20-40 mL of calcium chloride solution and urea solution), also slowly inject until it is completely injected, let it stand for 10-20 minutes, and then invert the sample to obtain the sand solidification test block 2.

[0084] The variable head permeability test was performed on the sand solidification test block 1 obtained by the mixed injection method, the sand solidification test block 2 obtained by the step injection method, and the sand solidification test block obtained by the two-stage injection method of the present invention. According to the geotechnical test method standard (GBT50123-2019), each group of tests was set up with repeated tests. The test scheme is shown in Table 1 below.

[0085] Table 1 Penetration test scheme

[0086]

[0087] The above-mentioned cured samples were subjected to unconfined compressive strength tests. After the samples were cured, they were placed in an oven at 80°C for 24 hours, and then taken out and subjected to unconfined compressive strength tests using a soil static triaxial apparatus. According to the geotechnical test method standard (GB / T 50123-2019), the strain control method with a strain rate of 1.0% / min was used for loading. The test was stopped when the deviator stress peak appeared or the axial strain reached 15%. Each group of tests was set up for repeated tests. The test plan is shown in Table 2 below.

[0088] Table 2 Unconfined compressive strength test plan

[0089]

[0090]

[0091] Then the penetration test was carried out by Figure 4 As shown in the figure, the relationship curve between the permeability coefficient of solidified sand and the injection method when the cementation times are 2, 4, and 6 times is listed. It can be seen from the figure that when the initial dry density and the standing time are constant, the permeability coefficient of the mixed injection method is the highest, while the permeability coefficient of the two-stage injection method is the lowest. When the initial dry density is 1.65g / cm 3 When the cementation times were 6 and the standing time was 5 days, the permeability coefficients of the solidified sand in mixed injection, step injection and two-stage injection were 0.0010cm / s, 0.00078cm / s and 0.00062cm / s respectively. The main reason for the above phenomenon is that the urease solution and the cementing solution are mixed evenly and injected into the sample at one time during the mixed injection, which quickly generates CaCO 3 Crystals are formed, which hinders subsequent pouring and results in poor cementation of the sample. In the step-by-step pouring, the urease solution is first poured into the soil, and then allowed to diffuse and adhere freely between the soil particles. The subsequent pouring of the cementing fluid not only reduces the precipitation on the surface of the sample, but also alleviates the problems of blockage and uneven deposition. The two-stage pouring is carried out at intervals in multiple stages. First, the urease solution is poured into the soil, followed by the calcium chloride solution, and finally the urea solution, to maximize the reaction between urease and calcium ions, thereby promoting more CaCO 3 Crystal formation fills the soil pores and reduces soil permeability. The test results show that the two-stage pouring method has the best curing effect, the step-by-step pouring method has the second best curing effect, and the mixed pouring method has the worst curing effect.

[0092] Then the unconfined compressive strength test was carried out. Figure 5 As shown in the figure, the UCS of the solidified sand varies with the injection method when the number of cementation is 2, 4, and 6. As shown in the figure, when the number of cementation is constant, the UCS strength of the sand solidified by the two-stage injection method is relatively high, while the UCS strength of the sample using the mixed injection method is relatively low. When the number of cementation is low, the difference in UCS strength is not obvious, but as the number of injections increases, the difference in UCS strength is significant. When the initial dry density is 1.65g / cm 3 When the cementation times are 6 and the standing time is 5 days, the UCS of the solidified sand soil during mixed pouring, step pouring and two-stage pouring are 618.02kPa, 1403.61kPa and 1646.94kPa respectively. The test results show that the two-stage pouring method has the best curing effect, followed by the step pouring method, and the mixed pouring method is the worst. The unconfined compressive strength test results confirm the permeability test results well.

[0093] Figure 6 The relationship between the permeability coefficient and CaCO of the stabilized sand under different injection methods is summarized. 3 The relationship curve of the amount of CaCO 3 As the amount of generated material increases, the permeability coefficient of the sample decreases, and the two are negatively correlated. The determination coefficients of the distributed perfusion method and the two-stage perfusion method are relatively high, reaching 0.919 and 0.918 respectively, indicating that the permeability coefficient is closely related to CaCO 3 The main reason for the above phenomenon is that the CaCO generated by EICP mineralization 3 The crystals play the role of filling and cementing sand particles, thereby blocking the seepage channel of the soil, causing the seepage path to increase, and ultimately leading to a decrease in its permeability coefficient. 3 The amount of generated soil is negatively correlated with the permeability coefficient of sand.

[0094] Figure 7 The relationship curves between the unconfined compressive strength of sand and the amount of CaCO3 generated under different injection methods are summarized. 3 The unconfined compressive strength (UCS) of the sample increases with the increase of the generated amount, and the two are positively correlated. The determination coefficient of the two-stage infusion method reached 0.918, indicating that UCS is related to CaCO 3 The main reason for the above phenomenon is that the CaCO generated by EICP 3 Crystals fill and cement sand particles, increasing the bonding and friction between sand particles, making the originally loose sand particles cemented into a whole to jointly bear the external load, thereby improving the overall compressive strength, thus leading to CaCO 3 The generation amount was significantly positively correlated with the UCS of the sample.

[0095] When the two-stage infusion method is used, the initial dry density is 1.65g / cm 3 When the cementation times are 6 and the standing time is 5 days, the permeability coefficient of the solidified sand is 6.25×10 -4 cm / s, and the unconfined compressive strength reached 1646.94 kPa, which is the optimal condition for EICP solidification of standard sand.

[0096] The present invention and its embodiments are described above, which is not restrictive. The drawings are only one of the embodiments of the present invention. In short, if ordinary technicians in the field are inspired by it and design structural methods and embodiments similar to the technical solution without creativity without departing from the purpose of the invention, they should all fall within the protection scope of the present invention.

[0097] It can be seen from the above embodiments that compared with the prior art:

[0098] Compared with the traditional grouting reinforcement method, the present invention utilizes EICP technology, which is more environmentally friendly, economical, and durable, and at the same time has a significant improvement in anti-seepage and strength.

[0099] Compared with the mixed injection method, the mixed injection method is to mix the urease solution and the cementing liquid evenly and then inject the soil at one time under the EICP technology. Since the urease solution and the cementing liquid will immediately react chemically, calcium carbonate crystals will be produced before injecting the sand, which is easy to be blocked at the injection end, so that the calcium carbonate of the sample after the cementation is unevenly distributed and the integrity is poor. The present invention solidifies the soil under the EICP technology, which can make the cementing liquid more evenly distributed in the sample, improve the accuracy and effectiveness of the solidification, and show a higher conversion efficiency.

[0100] Compared with the step-by-step perfusion method, the step-by-step perfusion method is to perfuse the soil with urease solution and cementing solution (a solution obtained by mixing urea solution and calcium chloride solution) step by step under the EICP technology, first perfusing the cementing solution, and then perfusing the urease solution. Compared with the mixed perfusion method, the conversion efficiency of this method is further improved, and it has better mechanical properties than the mixed perfusion method. The present invention solidifies the soil under the EICP technology by sequentially perfusing the soil with urease solution, urea solution and calcium chloride solution, which can further improve the accuracy and effectiveness of solidification compared with the step-by-step perfusion method, and at the same time has higher strength and lower permeability than the step-by-step perfusion method.

[0101] Compared with the MICP method of soil solidification, the two-stage sand consolidation method based on soybean urease-induced calcium carbonate deposition (EICP) of the present invention has a simpler operation process. Plant urease is directly extracted from soybeans and can directly induce the precipitation of calcium carbonate without going through a complex bacterial culture process. Since there is no direct participation of microorganisms in the precipitation process, the EICP technology is not limited by microbial growth and metabolism, so it can be applied to a wider range of soil types and particle size ranges, and avoids microbial ecological safety issues in practical applications.

[0102] In summary, based on the traditional EICP solidification, the present invention carries out two-stage sand consolidation on the sand sample, so that the binder is more evenly distributed in the rock and soil, the accuracy and effectiveness of the solidification are improved, and a higher conversion efficiency is shown, which greatly improves the solidification strength of the sand. It has good application prospects in improving the strength of loess, anti-seepage sealing, surface repair, etc.

[0103] The present invention and its embodiments are described above, which is not restrictive. The drawings are only one of the embodiments of the present invention. In short, if ordinary technicians in the field are inspired by it and design structural methods and embodiments similar to the technical solution without creativity without departing from the purpose of the invention, they should all fall within the protection scope of the present invention.

Claims

1. A two-stage sand consolidation method based on soybean urease-induced calcium carbonate deposition (EICP), characterized in that: The specific steps include: Step 1: According to the dry density of 1.55g / cm 3 -1.65g / cm 3 Weigh a certain mass of standard sand, fully mix the standard sand with 0.5%-1% of soybean urease solution by mass of the standard sand, then add 0.5%-1% of cementing liquid by mass of the standard sand, and mix evenly to obtain a solidified sand block; Step 2: compact the solidified sand blocks obtained in step 1 in 4-6 layers, scrape the layers between each other, and place them at 18-26°C for solidification to obtain a sand sample; Step 3: The sand sample obtained in step 2 is infused with 1%-3% soybean urease solution by mass ratio of standard sand; after standing for 5-10 minutes, calcium chloride solution by mass ratio of standard sand is infused; after standing for 5-10 minutes, urea solution by mass ratio of standard sand is infused at last, and the mixture is infused at 1%-3% by mass ratio of standard sand, and the mixture is infused at 18-26°C for solidification to obtain a solidified sand test block.

2. A two-stage sand consolidation method based on soybean urease induced calcium carbonate deposition (EICP) according to claim 1, characterized in that: The soybean urease solution in step 1 is: Select soybeans from the market, dry them in an oven at 40-60°C, use a grinder to grind soybean particles to obtain soybean powder, pass the soybean powder through a 0.1-0.3 mm sieve, filter out large particles, and retain soybean powder; mix the soybean powder with deionized water and stir for 15-40 minutes to prepare a soybean solution with a concentration of 100-200 g / L, centrifuge the soybean solution at a speed of 3000-6000 r / min for 15-30 minutes, and extract the upper light yellow clear liquid, which is the soybean urease solution; The extracted soybean urease solution was stored at 4-6°C for later use.

3. A two-stage sand consolidation method based on soybean urease induced calcium carbonate deposition (EICP) according to claim 1, characterized in that: The binder in step 1 is: The urea solution of equal concentration and volume is uniformly mixed with the anhydrous calcium chloride solution to obtain a cementing liquid with a concentration of 0.5-1.5 mol / L.

4. A two-stage sand consolidation method based on soybean urease induced calcium carbonate deposition (EICP) according to claim 1, characterized in that: In step 3, the calcium chloride solution is 80-100 g / L.

5. A two-stage sand consolidation method based on soybean urease induced calcium carbonate deposition (EICP) according to claim 1, characterized in that: In step 3, the urea solution is 80-100 g / L.

6. A two-stage sand consolidation method based on soybean urease-induced calcium carbonate deposition (EICP), characterized in that: The specific steps include: Step 1: According to the dry density of 1.55g / cm 3 Weigh a certain mass of standard sand, mix the standard sand with 0.5% soybean urease solution by mass of the standard sand, then add 0.5% cementing liquid by mass of the standard sand, mix evenly to obtain a solidified sand block; In the step 1, the soybean urease solution is: Select soybeans from the market, dry them in an oven at 40°C, use a grinder to grind soybean particles to obtain soybean powder, pass the soybean powder through a 0.1 mm sieve, filter out large particles, and retain soybean powder; mix the soybean powder with deionized water and stir for 15 minutes to prepare a soybean solution with a concentration of 100 g / L, centrifuge the soybean solution at a speed of 3000 r / min for 15 minutes, extract the upper light yellow clear liquid, which is the soybean urease solution; store the extracted soybean urease solution at 4°C for later use; The binder in step 1 is: The urea solution of equal concentration and volume was uniformly mixed with the anhydrous calcium chloride solution to obtain a cementing solution with a concentration of 0.5 mol / L; Step 2: compact the solidified sand blocks obtained in step 1 in 4 layers, scrape the layers between them, and place them at 18°C ​​for solidification to obtain sand samples; Step 3: The sand sample obtained in step 2 is infused with a soybean urease solution accounting for 1% of the mass ratio of the standard sand; after standing for 5 minutes, a calcium chloride solution accounting for 1% of the mass ratio of the standard sand is infused; after standing for 5 minutes, a urea solution accounting for 1% of the mass ratio of the standard sand is finally infused, and the sand is infused at 18°C ​​for curing to obtain a sand solidification test block; In step 3, the calcium chloride solution is 80 g / L; In step 3, the urea solution is 80 g / L.

7. A two-stage sand consolidation method based on soybean urease induced calcium carbonate deposition (EICP), characterized in that: The specific steps include: Step 1: According to the dry density of 1.60g / cm 3 Weigh a certain mass of standard sand, mix the standard sand with soybean urease solution accounting for 0.75% of the mass of the standard sand, then add a cementing liquid accounting for 0.75% of the mass of the standard sand, and mix evenly to obtain a solidified sand block; In the step 1, the soybean urease solution is: Select soybeans from the market, dry them in an oven at 50°C, use a grinder to grind soybean particles to obtain soybean powder, pass the soybean powder through a 0.2 mm sieve, filter out large particles, and retain soybean powder; mix the soybean powder with deionized water and stir for 30 minutes to prepare a soybean solution with a concentration of 150 g / L, centrifuge the soybean solution at a speed of 4500 r / min for 25 minutes, extract the upper light yellow clear liquid, which is the soybean urease solution; store the extracted soybean urease solution at 5°C for later use; The binder in step 1 is: The urea solution of equal concentration and volume was uniformly mixed with the anhydrous calcium chloride solution to obtain a cementing solution with a concentration of 1.0 mol / L; Step 2: compact the solidified sand blocks obtained in step 1 in 5 layers, scrape the layers between them, and solidify them at 22°C to obtain sand samples; Step 3: The sand sample obtained in step 2 is infused with soybean urease solution accounting for 2% of the mass ratio of the standard sand; after standing for 7 minutes, a calcium chloride solution accounting for 2% of the mass ratio of the standard sand is infused; after standing for 7 minutes, a urea solution accounting for 2% of the mass ratio of the standard sand is finally infused, and the sand is infused at 22° C. to obtain a sand solidification test block; In step 3, the calcium chloride solution is 90 g / L; The urea solution in step 3 is 90 g / L.

8. A two-stage sand consolidation method based on soybean urease induced calcium carbonate deposition (EICP), characterized in that: The specific steps include: Step 1: According to the dry density of 1.65g / cm 3 Weigh a certain mass of standard sand, fully mix the standard sand with 1% soybean urease solution by mass of the standard sand, then add 1% cementing liquid by mass of the standard sand, mix evenly to obtain a solidified sand block; In the step 1, the soybean urease solution is: Select soybeans from the market, dry them in an oven at 60°C, use a grinder to grind soybean particles to obtain soybean powder, pass the soybean powder through a 0.3 mm sieve, filter out large particles, and retain soybean powder; mix the soybean powder with deionized water and stir for 40 minutes to prepare a soybean solution with a concentration of 200 g / L, centrifuge the soybean solution at a speed of 6000 r / min for 30 minutes, extract the upper light yellow clear liquid, which is the soybean urease solution; store the extracted soybean urease solution at 6°C for later use; The binder in step 1 is: The urea solution of equal concentration and volume was uniformly mixed with the anhydrous calcium chloride solution to obtain a cementing solution with a concentration of 1.5 mol / L; Step 2: compact the solidified sand blocks obtained in step 1 in 6 layers, scrape the layers between them, and solidify them at 26°C to obtain sand samples; Step 3: The sand sample obtained in step 2 is infused with a soybean urease solution accounting for 3% of the mass ratio of the standard sand; after standing for 10 minutes, a calcium chloride solution accounting for 3% of the mass ratio of the standard sand is infused; after standing for 10 minutes, a urea solution accounting for 3% of the mass ratio of the standard sand is finally infused, and the sand is allowed to stand and solidify at 26°C to obtain a sand solidification test block; In step 3, the calcium chloride solution is 100 g / L; In step 3, the urea solution is 100 g / L.

9. A two-stage sand consolidation method based on soybean urease induced calcium carbonate deposition (EICP), characterized in that: The specific steps include: Step 1: According to the dry density of 1.65g / cm 3 Weigh a certain mass of standard sand, mix the standard sand with 1% of soybean urease solution by mass of the standard sand, then add 0.75% of cementing liquid by mass of the standard sand, mix evenly to obtain a solidified sand block; In the step 1, the soybean urease solution is: Select soybeans from the market, dry them in an oven at 50°C, use a grinder to grind soybean particles to obtain soybean powder, pass the soybean powder through a 0.2 mm sieve, filter out large particles, and retain the soybean powder; mix the soybean powder with deionized water and stir for 40 minutes to prepare a soybean solution with a concentration of 200 g / L, centrifuge the soybean solution at a speed of 6000 r / min for 30 minutes, and extract the upper light yellow clear liquid, which is the soybean urease solution; The extracted soybean urease solution was stored at 5°C for later use; The binder in step 1 is: The urea solution of equal concentration and volume was uniformly mixed with the anhydrous calcium chloride solution to obtain a cementing solution with a concentration of 1.5 mol / L; Step 2: compact the solidified sand blocks obtained in step 1 in 6 layers, scrape the layers between them, and solidify them at 25°C to obtain sand samples; Step 3: The sand sample obtained in step 2 is infused with a soybean urease solution accounting for 3% of the mass ratio of the standard sand; after standing for 10 minutes, a calcium chloride solution accounting for 2% of the mass ratio of the standard sand is infused; after standing for 10 minutes, a urea solution accounting for 2% of the mass ratio of the standard sand is finally infused, and the sand is infused at 25°C for curing to obtain a sand solidification test block; In step 3, the calcium chloride solution is 90 g / L; The urea solution in step 3 is 90 g / L.

Citation Information

Cited By

  • Method for solidifying sandy soil by inducing calcium carbonate precipitation through urease

    CN119145397A

  • Sandy soil improvement liquid combining microorganisms and waste concrete, preparation method and improvement method

    CN119875650A

  • Method for immobilizing fine-grained tailings with different particle sizes through carboxymethyl chitosan mediated biomineralization

    CN120920482A

  • Preparation method and application of EICP (Expanded Inductively Coupled Plasma) slurry for reinforcing macroporous stratum

    CN121470850A

  • Ground source heat pump EICP mortar backfill material and preparation method and application thereof

    CN122426971A