Epoxy acrylate with adjustable molecular weight and high cost performance and preparation method thereof
By controlling the molar ratio and addition order of acrylic acid, epoxy chlorohydrin and phthalic anhydride, simplifying the process and reducing the cost of raw materials, the problem of insufficient flexibility of epoxy resin is solved, and the preparation of epoxy acrylate with adjustable molecular weight and high cost performance is realized. Suitable for a variety of application scenarios.
Patent Information
- Application Number
- CN202410945139.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-11-05
AI Technical Summary
The existing epoxy acrylates are insufficient in flexibility after curing, and the multi-part modification process is complex, the molecular weight is difficult to control, and the raw material cost is high.
By controlling the molar ratio and addition sequence of acrylic acid, epoxy chlorohydrin and phthalic anhydride, continuous ring opening reactions are carried out to prepare cost-effective epoxy acrylate with adjustable molecular weight, simplifying the process and reducing raw material costs.
It realizes flexible control of the molecular weight of epoxy resin, simple process, low raw material cost, good product flexibility, light appearance and color, good compatibility with other resins, and is suitable for different application scenarios.
Smart Images

Figure BDA0004945410300000101
Abstract
Description
Technical field:
[0001] The invention relates to the technical field of epoxy resins, and in particular to a molecular weight-adjustable epoxy acrylate with high cost performance and a preparation method thereof. Background technology:
[0002] Epoxy acrylate is the most widely used photocurable prepolymer. From the structural point of view, it can be divided into bisphenol A epoxy acrylate, novolac epoxy acrylate, epoxidized oil acrylate and modified epoxy acrylate. As a main resin, the coating film of epoxy acrylate has good adhesion, chemical resistance and strength after curing, but it also has disadvantages, such as insufficient flexibility and high brittleness of the cured film. Therefore, in order to meet the needs of different fields, (physical and / or chemical) modification of epoxy acrylate has become one of the research hotspots in this field. For example, polyol modification, acid, anhydride modification, polyurethane modification, etc.
[0003] Physical modification is to add nanoparticles to epoxy acrylate to improve the performance during the curing process; chemical modification is to use the epoxy or hydroxyl groups in epoxy acrylate to react with the functional groups in other modifying substances to prepare modified products with different properties.
[0004] The raw material cost of the epoxy acrylate mentioned above is relatively high, and the multi-part modification processes such as polyol modification and polyurethane modification take a long time to synthesize, are complex, and the molecular weight is difficult to control. The unmodified epoxy acrylate has a high hardness and insufficient flexibility. Summary of the invention:
[0005] The present invention solves the problems existing in the prior art and provides a cost-effective epoxy acrylate with adjustable molecular weight and a preparation method thereof. The preparation method of the epoxy acrylate provided by the present invention can adjust the molecular weight according to application requirements, and at the same time has low raw material cost, simple process, light appearance color, good compatibility with other resins, and can solve the disadvantage of insufficient flexibility of ordinary epoxy resin.
[0006] The first object of the present invention is to provide a method for preparing epoxy acrylate with adjustable molecular weight and high cost performance, which specifically comprises the following steps:
[0007] (1) adding 1-18 parts by weight of acrylic acid, 0.02-0.04 parts by weight of a polymerization inhibitor, 0.2-0.4 parts by weight of a catalyst, 0.01-0.03 parts by weight of an antioxidant and 5-7 parts by weight of epichlorohydrin into a reaction vessel, heating the vessel to 90° C.-100° C. and reacting the vessel for 0.5-1.5 hours to obtain a polymer having a hydroxyl group;
[0008] (2) adding 18-30 parts by weight of phthalic anhydride to the polymer with hydroxyl groups obtained in step (1) in several portions, and then adding 17-21 parts by weight of epichlorohydrin in several portions, and maintaining the temperature at 100° C. to 110° C. for 3.5-4.5 hours;
[0009] (3) Detecting the change of the acid value in the reaction container. When the acid value is less than 4 mgKOH / g, adding 18-30 parts by weight of phthalic anhydride at one time, and then adding 15-19 parts by weight of epichlorohydrin several times. During the addition of epichlorohydrin, confirming that the temperature rises and falls each time epichlorohydrin is added, and then adding the second epichlorohydrin. Maintaining the temperature of 100° C.-110° C. for reaction for 2-4 hours; monitoring the change of the acid value in the reaction container. When the acid value is less than 4 mgKOH / g, the epoxy acrylate with high cost performance is obtained.
[0010] Preferably, during the entire reaction process, the molar ratio of the total amount of acrylic acid, epichlorohydrin, and phthalic anhydride added is 1:n:n-1, and 2≤n≤20, where n is a positive integer.
[0011] The reaction mechanism of synthesizing the epoxy acrylate with adjustable molecular weight and high cost performance proposed by the present invention is as follows: acrylic acid and epichlorohydrin undergo ring-opening polymerization reaction under the action of a catalyst to generate a polymer P1 with hydroxyl groups, phthalic anhydride is added to cause the polymer P1 to undergo ring-opening polymerization reaction with the phthalic anhydride to generate a polymer P2 with carboxyl groups, and then epichlorohydrin is added to cause the polymer P2 to undergo ring-opening polymerization reaction with the epichlorohydrin to generate a polymer P3 with hydroxyl groups, and the polymer P3 can undergo ring-opening polymerization reaction with the phthalic anhydride to generate a polymer P4 with carboxyl groups. In this way, the molecular weight of the epoxy acrylate finally generated is controlled by controlling the weight of the epichlorohydrin and the phthalic anhydride and the number and sequence of additions, so as to obtain the epoxy acrylate with adjustable molecular weight and high cost performance.
[0012] The invention can flexibly control the degree of continuous ring-opening reaction by controlling the weight of epichlorohydrin and phthalic anhydride and the number and sequence of input, and can produce epoxy resins with different molecular weights and different properties to meet different application requirements.
[0013] The preparation method proposed by the present invention controls the molar ratio of the total added amount of acrylic acid, epichlorohydrin and the total added amount of phthalic anhydride to be 1:n:n-1, and 2≤n≤20, so that acrylic acid, epichlorohydrin and phthalic anhydride form a continuous ring-opening reaction structure under the action of a catalyst, and controls the added amount and addition order of epichlorohydrin and phthalic anhydride to obtain cost-effective epoxy acrylate through multi-step continuous ring-opening reaction.
[0014] Further preferably, the inhibitor in step (1) is p-hydroxyanisole, the catalyst is tetraethylammonium bromide, tetrapropylammonium bromide or tetrabutylammonium bromide, and the antioxidant is antioxidant 1076.
[0015] Further preferably, the specific steps of step (1) are: adding 1.52-17.78 parts by mass of acrylic acid, 0.02-0.04 parts by mass of a polymerization inhibitor, 0.2-0.4 parts by mass of a catalyst, 0.01-0.03 parts by mass of an antioxidant and 5.86-6.85 parts by mass of epichlorohydrin into a reaction container, heating to 95° C. and reacting for 1.0 hour to obtain a polymer with a hydroxyl group.
[0016] Further preferably, the specific steps of step (2) are: adding 18.28-29.71 parts by weight of phthalic anhydride to the polymer with hydroxyl groups obtained in step (1) in several portions, controlling the temperature below 105° C. each time phthalic anhydride is added, and then adding 17.58-20.55 parts by weight of epichlorohydrin in several portions, maintaining the temperature at 100° C.-110° C. for reaction for 3.5-4.5 hours.
[0017] Further preferably, the specific steps of step (3) are: detecting the change of the acid value in the reaction container, when the acid value is less than 4 mgKOH / g, adding a total amount of 18.28-29.71 parts by mass of phthalic anhydride at one time, and then adding a total amount of 15.63-18.27 parts by mass of epichlorohydrin in 5-8 times, and adding epichlorohydrin for the second time after confirming that the temperature of each addition of epichlorohydrin rises and falls during the addition of epichlorohydrin, and maintaining the temperature of 100°C-110°C for reaction for 3 hours; monitoring the change of the acid value in the reaction container, when the acid value is less than 4 mgKOH / g, obtaining the epoxy acrylate with high cost performance.
[0018] The second object of the present invention is to provide epoxy acrylate with high cost performance obtained by the preparation method, wherein the molecular weight of the epoxy acrylate is 400-5000.
[0019] The molecular weight of the epoxy acrylate obtained by the preparation method proposed in the present invention is adjustable. By controlling the number and sequence of adding epichlorohydrin and phthalic anhydride, the molecular weight of the epoxy resin can be controlled to vary within the range of 400-5000, thereby meeting different application scenarios.
[0020] The present invention also protects the application of the epoxy acrylate in the field of photocuring.
[0021] Preferably, the light-cured area is nail polish glue or wood coating.
[0022] Compared with the prior art, the present invention has the following advantages:
[0023] 1. The molecular weight of the epoxy acrylate obtained by the preparation method proposed in the present invention is adjustable. By controlling the number and sequence of adding epichlorohydrin and phthalic anhydride, the molecular weight of the epoxy resin can be controlled to vary within the range of 400-5000, thereby meeting different application scenarios.
[0024] 2. The raw material cost used in the preparation method proposed by the present invention is low. Epichlorohydrin, acrylic acid and phthalic anhydride are all low-priced raw materials, and the material cost is low.
[0025] 3. The preparation method proposed in the present invention has a simple process. The production process mainly controls the temperature, time, acid value and other conditions. The process is simple and can be mass-produced.
[0026] 4. The epoxy acrylate obtained by the preparation method proposed in the present invention has a light color and a Gardner color value of less than 1.
[0027] 5. The epoxy acrylate obtained by the preparation method proposed in the present invention has good compatibility with other resins.
[0028] 6. The epoxy acrylate obtained by the preparation method proposed in the present invention has good flexibility and can be folded in half 5 times without breaking after curing. Specific implementation method:
[0029] The following examples are provided to further illustrate the present invention, rather than to limit the present invention.
[0030] Unless otherwise defined, all professional terms used hereinafter have the same meaning as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention. Unless otherwise specified, the experimental materials and reagents herein are conventional commercial products in the art, and phthalic anhydride refers to phthalic anhydride.
[0031] Example 1
[0032] A method for preparing epoxy acrylate comprises the following steps:
[0033] (1) adding 17.78 parts by mass of acrylic acid, 0.02 parts by mass of p-hydroxyanisole, 0.2 parts by mass of tetrabutylammonium bromide, 0.01 parts by mass of antioxidant 1076 and 6.85 parts by mass of epichlorohydrin into a reaction kettle, heating the kettle to 95° C. for reaction for about 1 hour to obtain a polymer;
[0034] (2) adding 18.28 parts by weight of phthalic anhydride to the polymer obtained in step (1) in 5 portions, with the temperature being controlled below 105° C. each time the phthalic anhydride is added, and after the phthalic anhydride is added, adding 20.55 parts by weight of epichlorohydrin in 5 portions, maintaining the temperature at 100° C.-110° C. for about 4 hours;
[0035] (3) Detecting the change of the acid value in the reaction kettle, when the acid value is less than 4 mgKOH / g, adding 18.28 parts by weight of phthalic anhydride at one time, and then adding 18.27 parts by weight of epichlorohydrin in five portions after adding the phthalic anhydride, confirming that the temperature rises and falls each time before adding the second portion, and maintaining the temperature at 100° C.-110° C. for about 3 hours; monitoring the change of the acid value in the reaction kettle, when the acid value is less than 4 mgKOH / g, obtaining a transparent and light-colored epoxy acrylate resin.
[0036] In this embodiment, the molar ratio of acrylic acid:epichlorohydrin:phthalic anhydride is 1:2:1.
[0037] Example 2
[0038] A method for preparing epoxy acrylate comprises the following steps:
[0039] (1) adding 6.39 parts by weight of acrylic acid, 0.02 parts by weight of p-hydroxyanisole, 0.3 parts by weight of tetrabutylammonium bromide, 0.02 parts by weight of antioxidant 1076, and 6.16 parts by weight of epichlorohydrin into a reaction kettle, heating the kettle to 95° C. for a first reaction, and reacting for about 1 hour to obtain a polymer;
[0040] (2) adding 26.28 parts by weight of phthalic anhydride to the polymer obtained in step (1) in 6 portions, with the temperature being controlled below 105° C. each time the phthalic anhydride is added, and after the phthalic anhydride is added, adding 18.47 parts by weight of epichlorohydrin in 6 portions, maintaining the temperature at 100° C.-110° C. for a reaction for about 4 hours;
[0041] (3) Detecting the change of the acid value in the reaction kettle, when the acid value is less than 4 mg KOH / g, adding phthalic anhydride in a total amount of 26.28 parts by weight at one time, and then adding epichlorohydrin in a total amount of 16.42 parts by weight in 6 portions after adding the phthalic anhydride, confirming that the temperature rises and falls each time before adding the second portion, and maintaining the temperature at 100° C.-110° C. for about 3 hours; monitoring the change of the acid value in the reaction kettle, when the acid value is less than 4 mg KOH / g, obtaining a transparent light-colored epoxy acrylate resin.
[0042] In this embodiment, the molar ratio of acrylic acid:epichlorohydrin:phthalic anhydride is 1:5:4.
[0043] Example 3
[0044] A method for preparing epoxy acrylate comprises the following steps:
[0045] (1) adding 3.90 parts by weight of acrylic acid, 0.03 parts by weight of p-hydroxyanisole, 0.4 parts by weight of tetrapropylammonium bromide, 0.02 parts by weight of antioxidant 1076, and 6.00 parts by weight of epichlorohydrin into a reaction kettle, heating the kettle to 95° C. for a first reaction, and reacting for about 1 hour to obtain a polymer;
[0046] (2) adding 28.04 parts by weight of phthalic anhydride to the polymer obtained in step (1) in 6 portions, with the temperature being controlled below 105° C. each time the phthalic anhydride is added, and after the phthalic anhydride is added, adding 18.01 parts by weight of epichlorohydrin in 6 portions, maintaining the temperature at 100° C.-110° C. for a reaction for about 4 hours;
[0047] (3) Detecting the change of the acid value in the reaction kettle, when the acid value is less than 4 mgKOH / g, adding phthalic anhydride in a total amount of 28.04 parts by weight at one time, and then adding epichlorohydrin in a total amount of 16.01 parts by weight in 6 portions after adding the phthalic anhydride, confirming that the temperature rises and falls each time before adding the second portion, and maintaining the temperature at 100° C.-110° C. for about 3 hours; monitoring the change of the acid value in the reaction kettle, when the acid value is less than 4 mgKOH / g, obtaining a transparent and light-colored epoxy acrylate resin.
[0048] In this embodiment, the molar ratio of acrylic acid:epichlorohydrin:phthalic anhydride is 1:8:7.
[0049] Example 4
[0050] A method for preparing epoxy acrylate comprises the following steps:
[0051] (1) adding 2.80 parts by weight of acrylic acid, 0.03 parts by weight of p-hydroxyanisole, 0.4 parts by weight of tetrapropylammonium bromide, 0.02 parts by weight of antioxidant 1076, and 5.94 parts by weight of epichlorohydrin into a reaction kettle, heating the kettle to 95° C. for a first reaction, and reacting for about 1 hour to obtain a polymer;
[0052] (2) adding 28.81 parts by weight of phthalic anhydride to the polymer obtained in step (1) in 7 portions, with the temperature being controlled below 105° C. each time the phthalic anhydride is added, and after the phthalic anhydride is added, adding 17.81 parts by weight of epichlorohydrin in 7 portions, maintaining the temperature at 100° C.-110° C. for about 4 hours;
[0053] (3) Detecting the change of the acid value in the reaction kettle, when the acid value is less than 4 mgKOH / g, adding phthalic anhydride in a total amount of 28.81 parts by mass at one time, and after adding phthalic anhydride, adding epichlorohydrin in a total amount of 15.83 parts by mass in 7 times, confirming that the temperature rises and falls each time before adding the second time, and maintaining the temperature at 100° C.-110° C. for about 3 hours; monitoring the change of the acid value in the reaction kettle, when the acid value is less than 4 mgKOH / g, obtaining a transparent and light-colored epoxy acrylate resin.
[0054] In this embodiment, the molar ratio of acrylic acid:epichlorohydrin:phthalic anhydride is 1:11:10.
[0055] Example 5
[0056] A method for preparing epoxy acrylate comprises the following steps:
[0057] (1) adding 2.19 parts by weight of acrylic acid, 0.03 parts by weight of p-hydroxyanisole, 0.4 parts by weight of tetraethylammonium chloride, 0.02 parts by weight of antioxidant 1076, and 5.90 parts by weight of epichlorohydrin into a reaction kettle, heating the kettle to 95° C. to carry out a first reaction for about 1 hour to obtain a polymer;
[0058] (2) adding 29.24 parts by weight of phthalic anhydride to the polymer obtained in step (1) in 7 portions, with the temperature being controlled below 105° C. each time the phthalic anhydride is added, and after the phthalic anhydride is added, adding 17.70 parts by weight of epichlorohydrin in 7 portions, maintaining the temperature at 100° C.-110° C. for about 4 hours;
[0059] (3) Detecting the change of the acid value in the reaction kettle, when the acid value is less than 4 mgKOH / g, adding phthalic anhydride in a total amount of 29.24 parts by weight at one time, and then adding epichlorohydrin in a total amount of 15.73 parts by weight in 7 portions after adding the phthalic anhydride, confirming that the temperature rises and falls each time before adding the second portion, and maintaining the temperature at 100° C.-110° C. for about 3 hours; monitoring the change of the acid value in the reaction kettle, when the acid value is less than 4 mgKOH / g, obtaining a transparent light-colored epoxy acrylate resin.
[0060] In this embodiment, the molar ratio of acrylic acid:epichlorohydrin:phthalic anhydride is 1:14:13.
[0061] Example 6
[0062] A method for preparing epoxy acrylate comprises the following steps:
[0063] (1) adding 1.79 parts by weight of acrylic acid, 0.04 parts by weight of p-hydroxyanisole, 0.4 parts by weight of tetraethylammonium chloride, 0.03 parts by weight of antioxidant 1076, and 5.88 parts by weight of epichlorohydrin into a reaction kettle, heating the kettle to 95° C. to carry out a first reaction for about 1 hour to obtain a polymer;
[0064] (2) adding 29.51 parts by weight of phthalic anhydride to the polymer obtained in step (1) in 8 portions, with the temperature being controlled below 105° C. each time the phthalic anhydride is added, and after the phthalic anhydride is added, adding 17.63 parts by weight of epichlorohydrin in 8 portions, maintaining the temperature at 100° C.-110° C. for about 4 hours;
[0065] (3) Detecting the change of the acid value in the reaction kettle, when the acid value is less than 4 mgKOH / g, adding phthalic anhydride in a total amount of 29.51 parts by weight at one time, and then adding epichlorohydrin in a total amount of 15.67 parts by weight in 8 portions after adding the phthalic anhydride, confirming that the temperature rises and falls each time before adding the second portion, and maintaining the temperature at 100° C.-110° C. for about 3 hours; monitoring the change of the acid value in the reaction kettle, when the acid value is less than 4 mgKOH / g, obtaining a transparent and light-colored epoxy acrylate resin.
[0066] In this embodiment, the molar ratio of acrylic acid:epichlorohydrin:phthalic anhydride is 1:17:16.
[0067] Example 7
[0068] A method for preparing epoxy acrylate comprises the following steps:
[0069] (1) adding 1.52 parts by weight of acrylic acid, 0.04 parts by weight of p-hydroxyanisole, 0.4 parts by weight of tetraethylammonium chloride, 0.03 parts by weight of antioxidant 1076, and 5.86 parts by weight of epichlorohydrin into a reaction kettle, heating the kettle to 95° C. for a first reaction, and reacting for about 1 hour to obtain a polymer;
[0070] (2) adding 29.71 parts by weight of phthalic anhydride to the polymer obtained in step (1) in 8 portions, with the temperature being controlled below 105° C. each time the phthalic anhydride is added, and after the phthalic anhydride is added, adding 17.58 parts by weight of epichlorohydrin in 8 portions, maintaining the temperature at 100° C.-110° C. for a reaction for about 4 hours;
[0071] (3) Detecting the change of the acid value in the reaction kettle, when the acid value is less than 4 mgKOH / g, adding phthalic anhydride in a total amount of 29.71 parts by mass at one time, and then adding epichlorohydrin in a total amount of 15.63 parts by mass in 8 portions after adding the phthalic anhydride, confirming that the temperature rises and falls each time before adding the second time, and maintaining the temperature at 100° C.-110° C. for about 3 hours; monitoring the change of the acid value in the reaction kettle, when the acid value is less than 4 mgKOH / g, obtaining a transparent and light-colored epoxy acrylate resin.
[0072] In this embodiment, the molar ratio of acrylic acid:epichlorohydrin:phthalic anhydride is 1:20:19.
[0073] The epoxy acrylate resin obtained in Examples 1-7 and Allnex bisphenol A epoxy resin acrylate product EBECRYL-600 were used as a control group for the following comparison:
[0074] 1. Compare the appearance color and transparency.
[0075] 2. According to the ratio of 80% epoxy acrylate resin + 20% other resins / monomers, each group was mixed evenly with four conventional dilution monomers: epoxy acrylate product 7622, amine-modified polyether acrylate product 8600, dipropylene glycol diacrylate (DPGDA), 1,6-hexanediol diacrylate (HDDA), trimethylolpropane ethoxy triacrylate (TMPEOTA), and tripropylene glycol diacrylate (TPGDA) of Zhaoqing Baojun Chemical Co., Ltd. The transparency was observed. Clear and transparent means good compatibility.
[0076] 3. Each group of resins was cured by adding 5 parts of photoinitiator TPO and irradiated with 365nm UV lamp. The toughness data are shown in Table 1 below:
[0077] Table 1
[0078]
[0079] From the above comparative data, it can be concluded that the molecular weight of the epoxy acrylate obtained by the present invention is adjustable, and the molecular weight of the epoxy resin can be controlled to vary in the range of 400-5000, thereby meeting different application scenarios. The epoxy acrylate obtained by the present invention is light in color and has good compatibility with other resins and conventional dilution monomers. The epoxy acrylate obtained by the present invention has good flexibility and does not break after being folded 5 times after curing. The performance is comparable to bisphenol A epoxy resin acrylate on the market, but because the present invention uses epichlorohydrin, acrylic acid, and phthalic anhydride as low-priced raw materials, the cost is lower and the cost performance is higher.
[0080] The description of the above embodiments is only used to help understand the technical solution and core ideas of the present invention. It should be pointed out that for technicians in this technical field, several improvements and modifications can be made to the present invention without departing from the principles of the present invention. These improvements and modifications also fall within the scope of protection of the claims of the present invention.
Claims
1. A method for preparing epoxy acrylate with adjustable molecular weight and high cost performance, characterized in that: The specific steps include: (1) adding 1-18 parts by weight of acrylic acid, 0.02-0.04 parts by weight of a polymerization inhibitor, 0.2-0.4 parts by weight of a catalyst, 0.01-0.03 parts by weight of an antioxidant and 5-7 parts by weight of epichlorohydrin into a reaction vessel, heating the vessel to 90° C.-100° C. and reacting the vessel for 0.5-1.5 hours to obtain a polymer having a hydroxyl group; (2) adding 18-30 parts by weight of phthalic anhydride to the polymer with hydroxyl groups obtained in step (1) in several portions, and then adding 17-21 parts by weight of epichlorohydrin in several portions, and maintaining the temperature at 100° C. to 110° C. for 3.5-4.5 hours; (3) Detecting the change of the acid value in the reaction container. When the acid value is less than 4 mgKOH / g, adding 18-30 parts by weight of phthalic anhydride at one time, and then adding 15-19 parts by weight of epichlorohydrin several times. During the addition of epichlorohydrin, confirming that the temperature rises and falls each time epichlorohydrin is added, and then adding the second epichlorohydrin. Maintaining the temperature of 100° C.-110° C. for reaction for 2-4 hours; monitoring the change of the acid value in the reaction container. When the acid value is less than 4 mgKOH / g, the epoxy acrylate with high cost performance is obtained.
2. The preparation method according to claim 1, characterized in that: During the entire reaction process, the molar ratio of the total amount of acrylic acid, epichlorohydrin, and phthalic anhydride added is 1:n:n-1, and 2≤n≤20.
3. The preparation method according to claim 1 or 2, characterized in that: The inhibitor described in step (1) is p-hydroxyanisole, the catalyst is tetraethylammonium bromide, tetrapropylammonium bromide or tetrabutylammonium bromide, and the antioxidant is antioxidant 1076.
4. The preparation method according to claim 1 or 2, characterized in that: The specific steps of step (1) are: adding 1.52-17.78 parts by weight of acrylic acid, 0.02-0.04 parts by weight of a polymerization inhibitor, 0.2-0.4 parts by weight of a catalyst, 0.01-0.03 parts by weight of an antioxidant and 5.86-6.85 parts by weight of epichlorohydrin into a reaction container, heating to 95° C. and reacting for 1.0 hour to obtain a polymer with a hydroxyl group.
5. The preparation method according to claim 1 or 2, characterized in that: The specific steps of step (2) are as follows: adding 18.28-29.71 parts by weight of phthalic anhydride to the polymer with hydroxyl groups obtained in step (1) in several portions, controlling the temperature below 105° C. each time phthalic anhydride is added, and then adding 17.58-20.55 parts by weight of epichlorohydrin in several portions, maintaining the temperature at 100° C.-110° C. for reaction for 3.5-4.5 hours.
6. The preparation method according to claim 1 or 2, characterized in that: The specific steps of step (3) are as follows: detecting the change of the acid value in the reaction container, when the acid value is less than 4 mg KOH / g, adding a total amount of 18.28-29.71 parts by weight of phthalic anhydride at one time, and then adding a total amount of 15.63-18.27 parts by weight of epichlorohydrin in 5-8 portions, and adding epichlorohydrin for the second time after confirming that the temperature of each addition of epichlorohydrin rises and falls during the addition of epichlorohydrin, and maintaining the temperature of 100° C.-110° C. for reaction for 3 hours; monitoring the change of the acid value in the reaction container, when the acid value is less than 4 mg KOH / g, obtaining the epoxy acrylate with high cost performance.
7. The cost-effective epoxy acrylate obtained by the preparation method according to any one of claims 1 to 6, characterized in that: The molecular weight of the epoxy acrylate is 400-5000.
8. Use of the epoxy acrylate according to claim 7 in the field of photocuring.
9. The use according to claim 8, characterized in that: The light curing field is nail polish glue or wood coating.