Plastic particle for processing plastic tray, plastic tray and manufacturing method of plastic tray

By using specific ratios of plastic particles, including polyolefins, fillers, compatibilizers, crosslinkers, flow aids and modifiers, the welding interface problems caused by additive migration are solved, and the welding interface problems are improved. The reliability and stability of welding ensure the strength and quality of the pallet structure.

CN118895026AInactive Publication Date: 2024-11-05JIANGSU PALETTE NEW MATERIAL TECH CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411401705.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-09
Publication Date
2024-11-05
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

During the manufacturing process of plastic trays, additives such as flame retardants, lubricants, colorants and fillers migrate at high temperatures, resulting in residual and aggregation of welding interfaces, affecting the firmness and stability of welding and reducing structural strength.

Method used

Using specific ratios of plastic tray processing plastic particles, including polyolefins, fillers, compatible agents, crosslinking agents, flow aids, antioxidants and modifiers, modifiers are prepared through specific synthetic methods to significantly reduce heat Migration of additives during fusion welding improves welding quality.

Benefits of technology

显著减少了焊缝不连续、气孔等问题,提高了焊接的牢靠性和稳定性,确保托盘结构的强度和质量。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention discloses a plastic particle for processing a plastic tray. The plastic particle comprises the following raw materials: 100 parts of polyolefin, 10-15 parts of a filler, 1-5 parts of a compatilizer, 1-2.5 parts of a cross-linking agent, 1-2 parts of a flow promoter, 1-1.5 parts of an antioxidant, 1-1.5 parts of a coloring agent and 1-1.5 parts of a modifier. The weight ratio of the compatilizer to the cross-linking agent to the modifier is 1: (0.5-1): (0.3-1); the plastic tray prepared from the plastic particles is high in tensile strength, has few welding quality problems caused by migration of auxiliaries, and has excellent welding fastness. The invention correspondingly discloses a plastic tray taking the plastic particles as raw materials and a manufacturing method of the plastic tray.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of plastic pallets, and in particular to plastic particles for processing plastic pallets, a plastic pallet and a manufacturing method thereof. Background Art

[0002] Plastic pallets are used to facilitate cargo loading and unloading, transportation, storage and distribution. The load surface is used in conjunction with forklift sockets and is an essential storage equipment for food, aquatic products, medicine, chemicals and other industries. Plastic pallets are mainly made of PP or PE raw materials. The process of manufacturing plastic pallets usually includes the process of forming the top plate by thermoforming extruded sheets, the process of forming the bottom plate by injection molding, and the process of hot-melt welding to make the top and bottom plates firmly connected.

[0003] According to the use scenario requirements and processing needs of the pallet, the raw materials often contain a certain amount of flame retardants, lubricants, colorants and fillers. These additives are often small molecular organic matter or inorganic particles insoluble in the polyolefin polymer system. In the process of molten welding, the molecular movement will inevitably intensify due to heat and the migration in the polymer material system will intensify, which may lead to the formation of residues / aggregates at the welding interface, affecting the firmness and stability of the welding and causing the structural strength of the pallet to decrease. Summary of the invention

[0004] In order to inhibit the migration of additives and improve welding quality, the present invention provides plastic particles for processing a plastic pallet, a plastic pallet and a manufacturing method thereof.

[0005] In a first aspect, the present invention provides a plastic particle for processing a plastic pallet, which specifically adopts the following technical solution.

[0006] A plastic particle for processing a plastic pallet, wherein the raw material comprises, by weight, 100 parts of polyolefin, 10-15 parts of filler, 1-5 parts of compatibilizer, 1-2.5 parts of crosslinking agent, 1-2 parts of flow aid, 1-1.5 parts of antioxidant, 1-1.5 parts of colorant and 1-1.5 parts of modifier; The polyolefin is polyethylene, polypropylene or a mixture of the two; The weight ratio of the compatibilizer, the crosslinking agent and the modifier is 1:(0.5-1):(0.3-1); The modifier is prepared by the following method: S1. Add bisphenol A and chloroform into an alkaline solution, heat to 80-100°C and react for 4-6 hours; S2, adding the product obtained in step S1 and 1,4-dihydroxynaphthalene monobenzoate to the acidic solution, heating to 80-100° C. and reacting for 4-6 hours; S3, heating the obtained product of step S2 and naphthoic acid or naphthoic acid ester under reflux for 5-8h in the presence of a catalyst; washing the reaction system with saturated brine first, then with methanol, and vacuum rotary drying to obtain the aforementioned modifier.

[0007] By adopting the above technical solution, the modifier prepared by a specific method and the compatibilizer and the cross-linking agent are compounded according to the above ratio, which can significantly reduce the migration of the additive during hot melt welding, and is conducive to reducing the problems of weld discontinuity, pores, welds, etc. caused by the residue / aggregation of the migration of the additive at the welding interface. The plastic pallet processed with the plastic particles for plastic pallet processing of the present invention as raw materials has excellent welding reliability and stability.

[0008] Furthermore, the compatibilizer is maleic anhydride grafted POE and / or glycidyl methacrylate grafted POE.

[0009] Furthermore, the polyolefin is a mixture of high-density polyethylene and polypropylene.

[0010] Furthermore, the weight ratio of the high-density polyethylene to the polypropylene is 1:(3-6).

[0011] Furthermore, the alkaline solution in step S1 is a sodium hydroxide aqueous solution with a mass concentration of 10%, and the acidic solution in step S2 is a sulfuric acid aqueous solution with a mass concentration of 50%.

[0012] Furthermore, the catalyst in step S3 is a Lewis acid catalyst. The Lewis acid catalyst can be boron trifluoride (BF 3 ), aluminum chloride (AlCl 3 ), titanium chloride (TiCl 4 ), zinc chloride (ZnCl 2 ), tin chloride (SnCl 4 )、Zirconium chloride(ZrCl 4 ), iron chloride (FeCl 3 ), scandium chloride (ScCl 3 ), indium chloride (InCl 3 )wait.

[0013] Furthermore, the cross-linking agent is diisopropyl peroxide or distearoyl peroxide.

[0014] Furthermore, the flow aid is diffusion oil.

[0015] Furthermore, the filler is one or more of aluminum hydroxide, magnesium hydroxide, antimony oxide, zinc borate, calcium carbonate, talc, kaolin, titanium dioxide and aluminum oxide.

[0016] In a second aspect, the present invention provides a plastic pallet using the aforementioned plastic particles for processing plastic pallets as raw materials. This type of pallet is not prone to welding quality problems due to the migration of additives during the welding process and has excellent welding reliability and stability.

[0017] The third invention provides a method for manufacturing a plastic pallet, and the specific steps are: first, the plastic particles for processing the plastic pallet are used as raw materials for thermoforming to obtain a panel and a base of the pallet; then, the butt joint surfaces of the panel and the base are heated by a hot melt welding machine to melt the butt joint surfaces of the two; finally, the panel and the base are pressed tightly together and cooled to obtain a plastic pallet. The processed plastic pallet has excellent welding reliability and stability. DETAILED DESCRIPTION

[0018] The present invention is described in further detail below.

[0019] [Preparation Example] Preparation of modifier: S1. Add 0.4 mol bisphenol A (purity 99.8%) and 0.8 mol chloroform to 300 ml of 10% sodium hydroxide aqueous solution, heat to 80-100°C and react for 4-6 hours; then, neutralize with dilute hydrochloric acid to pH about 7, add 140 ml of ether for extraction, repeat the extraction three times, and vacuum rotary dry the organic phase; S2, adding 0.2 mol of the product obtained in step S1 and 0.2 mol of 1,4-dihydroxynaphthalene monobenzoate (purity 99%, Alpha Chemical, USA) to 100 ml of a 50% sulfuric acid aqueous solution, heating to 80-100° C. and reacting for 4-6 hours; then, washing the reaction system with 100 ml of methanol, repeating the washing 3 times, and vacuum-drying the reaction solution; S3, 0.1 mol of the product obtained in step S2 and 0.2 mol of naphthoate were dissolved in 60 ml of xylene, and 0.05 mol of catalyst AlCl 3 , heated under reflux at 95-100°C for 5-8h; the reaction system was first washed with 30ml saturated brine, repeated three times; then washed with 20ml methanol, repeated three times; vacuum rotary drying was performed to obtain a modifier.

[0020] <Preparation Examples 1-3> Preparation Examples 1-3 all involve a modifier, which is prepared by the aforementioned method, except that the process parameters of each step are different, as shown in Table 1.

[0021] Table 1. Process parameters of preparation examples Example

[0022] <Raw Materials and Reagents> High-density polyethylene: ExxonMobil™ high-density polyethylene (HDPE), from ExxonMobil Chemical; Polypropylene: ExxonMobil™ polypropylene (PP) from ExxonMobil Chemical; Aluminum hydroxide: purity 99%, from Nantong Zhonghe Chemical New Materials Co., Ltd.; Maleic anhydride grafted POE: grafting rate 2.5%, from Nanjing Feiteng New Materials Technology Co., Ltd.; Glycidyl methacrylate grafted POE: grafting rate 2.5%, from Dongguan Shenghao Plastic Raw Materials Co., Ltd.; Diisopropyl peroxide (DCP): purity 98%, from Sigma-Aldrich; Distearoyl peroxide: purity 98%, from Shaanxi Didu Pharmaceutical Chemical Co., Ltd.; Diffuser oil: Diffuser oil TSF-96-500, from Dongguan Shengbang Polymer Materials Co., Ltd.; Antioxidant 1010: purity 98%, from Qingdao Zhenguang Functional Materials Technology Co., Ltd. Phthalocyanine blue BS: CIPIGMENT BLUE 15:1, from Meikalun Pigments.

[0023] It should be noted that the above raw materials can be made by yourself or obtained through commercial channels. The selection of specific specifications and models is only an exemplary description. Raw materials of other specifications and models can also be selected when implementing the present invention according to actual needs. At the same time, in order to facilitate the description of the specific implementation methods of the present invention, the following examples only select aluminum hydroxide as a filler, diffusion oil as a flow aid, antioxidant 1010 as an antioxidant, and phthalocyanine blue BS as a colorant for exemplary description, which is not a limitation of the present invention.

[0024] <Examples 1-5> Examples 1-5 all relate to plastic particles for processing plastic pallets, which are obtained by mixing and granulating the raw materials in the proportions shown in Table 2.

[0025] Table 2. Raw material ratios of Examples 1-5 (by weight)

[0026] When actually processing and preparing plastic particles, the actual amount of materials added is calculated according to the ratio in the above table. Among them, the modifiers used in Examples 1-5 are all prepared in Preparation Example 1.

[0027] <Example 6> The difference between Example 6 and Example 3 is only that: diisophenylpropene peroxide is replaced by an equal amount of distearoyl peroxide.

[0028] <Examples 7-8> The only difference between Example 7-8 and Example 3 is that the source of the modifier is different.

[0029] The modifier in Example 7 was prepared by Preparation Example 2; and the modifier in Example 8 was prepared by Preparation Example 3.

[0030] <Examples 9-12> Examples 9-12 are all based on Example 7, except that the composition of the compatibilizer is different.

[0031] In Example 9, compared to every 100 parts of polyolefin (mixture of HDPE and PP), the amount of maleic anhydride grafted POE is 4 parts, and the amount of glycidyl methacrylate grafted POE is 1 part; In Example 10, compared to every 100 parts of polyolefin (mixture of HDPE and PP), the amount of maleic anhydride grafted POE is 3 parts, and the amount of glycidyl methacrylate grafted POE is 3 parts; In Example 11, compared to every 100 parts of polyolefin (mixture of HDPE and PP), the amount of maleic anhydride grafted POE is 1 part, and the amount of glycidyl methacrylate grafted POE is 4 parts; In Example 12, an equal amount of glycidyl methacrylate-grafted POE was used to replace maleic anhydride-grafted POE.

[0032] <Examples 13-15> Examples 13-15 are all based on Example 11, with the difference being that the composition of the cross-linking agent is different.

[0033] In Example 13, compared to every 100 parts of polyolefin (mixture of HDPE and PP), the amount of diisopropyl peroxide used is 1.5 parts and the amount of distearoyl peroxide used is 1 part; In Example 14, compared to every 100 parts of polyolefin (mixture of HDPE and PP), the amount of diisopropyl peroxide used is 1 part and the amount of distearoyl peroxide used is 1.5 parts; In Example 15, the amount of diisopropyl peroxide is 0.5 parts and the amount of distearoyl peroxide is 2 parts per 100 parts of polyolefin (mixture of HDPE and PP).

[0034] [Comparative Example] <Comparative Example 1> The only difference between Comparative Example 1 and Example 3 is that the raw material does not contain a modifier.

[0035] <Comparative Example 2> The difference between Comparative Example 2 and Example 3 is that an equal amount of maleic anhydride-grafted POE is used to replace the modifier.

[0036] <Comparative Example 3> The difference between Comparative Example 3 and Example 3 is that the modifier is replaced by an equal amount of diisopropyl peroxide.

[0037] <Comparative Examples 4-7> The difference between Comparative Examples 4-7 and Example 3 is that the sum of the amounts of maleic anhydride grafted POE, diisopropyl peroxide and modifier remains unchanged, but the weight ratios of the three raw materials are different.

[0038] In Comparative Example 4, the weight ratio of maleic anhydride grafted POE, diisopropyl peroxide and modifier is 1:0.1:0.3; in Comparative Example 5, the weight ratio of maleic anhydride grafted POE, diisopropyl peroxide and modifier is 1:1.5:0.3.

[0039] In Comparative Example 6, the weight ratio of maleic anhydride grafted POE, diisopropyl peroxide and modifier is 1:0.5:0.1; in Comparative Example 7, the weight ratio of maleic anhydride grafted POE, diisopropyl peroxide and modifier is 1:0.5:1.5.

[0040] [Application Examples] A method for manufacturing a plastic pallet, using the plastic particles for processing plastic pallets of Examples 1-15 as raw materials, and the specific manufacturing steps are: First, the panel and base of the pallet are obtained by extrusion molding the plastic particles for processing the plastic pallet as raw materials; then, the butt surfaces of the panel and the base are heated by a hot melt welding machine to melt the butt surfaces of the two; finally, the panel and the base are pressed tightly together and cooled to obtain a plastic pallet. The processed plastic pallet has excellent welding reliability and stability.

[0041] [Comparative application example] The difference between the comparative application example and the application example is that the plastic particles of comparative examples 1-7 are used as raw materials respectively.

[0042] [Performance test] <Appearance inspection> The pallets made from the corresponding use cases and comparative application examples are manually inspected for appearance to check whether the welding area is flat, whether there are obvious welding defects such as discontinuous welds, pores, cracks, etc., and pallets with a total of ≥3 visible pores, pits, cracks, etc. are considered unqualified. Unqualified rate = number of unqualified products / number of sampled products*100%, and the unqualified rate is calculated, as shown in Table 3.

[0043] <Tensile test> The plastic particles of each embodiment and comparative example are used as raw materials, hot melt extruded to form a material plate, cut into samples, and two samples of the same size are melt-welded at 210°C to obtain a rectangular test sample of 200mm*15mm*5mm. The prepared test sample is placed at room temperature for 24 hours before being used for the tensile test. During the test, the prepared test sample is placed in the upper and lower wedge clamps of the universal tensile testing machine to ensure that both ends of the sample are firmly clamped. The sample is stretched at a tensile speed of 35mm / min, and the deformation of the sample is tracked throughout the process by an extensometer until it breaks. After the test, the average tensile strength of multiple tests is recorded as the test result, as shown in Table 3.

[0044] Table 3. Performance test results

[0045] From the test data in the above table, we can see that: The plastic pallet made of plastic particles prepared by compounding the compatibilizer, cross-linking agent and modifier and other components in the weight ratio of 1: (0.5-1): (0.3-1) of the present invention as raw materials has a welding failure rate of ≤0.25%; comparing the results of Example 3 and the comparative example, it can be seen that when the weight ratio of the compatibilizer, cross-linking agent and modifier is not in the aforementioned range or does not contain the modifier, the failure rate of the welded pallet increases significantly. From the tensile test results, it can be seen that the sample made of the plastic particles of the present invention has a tensile strength of ≥15.1MPa after hot melt welding, and the tensile strength decreases to varying degrees when the weight ratio of the compatibilizer, cross-linking agent and modifier is not in the aforementioned range or does not contain the modifier. Therefore, it can be reasonably inferred that the plastic pallet prepared with the plastic particles of the present invention has excellent welding fastness, and the possible reason is that the compatibilizer, cross-linking agent and modifier in the weight ratio of 1: (0.5-1): (0.3-1) synergistically inhibit the migration of the auxiliary agent and improve the welding quality.

[0046] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.

Claims

1. A plastic particle for processing plastic pallets, It is characterized in that The raw material contains 100 parts of polyolefin, 10-15 parts of filler, 1-5 parts of compatibilizer, 1-2.5 parts of crosslinking agent, 1-2 parts of flow aid, 1-1.5 parts of antioxidant, 1-1.5 parts of colorant and 1-1.5 parts of modifier by weight; The polyolefin is polyethylene, polypropylene or a mixture of the two; The weight ratio of the compatibilizer, the crosslinking agent and the modifier is 1:(0.5-1):(0.3-1); The modifier is prepared by the following method: S1. Add bisphenol A and chloroform into an alkaline solution, heat to 80-100°C and react for 4-6 hours; S2, adding the product obtained in step S1 and 1,4-dihydroxynaphthalene monobenzoate to the acidic solution, heating to 80-100° C. and reacting for 4-6 hours; S3, heating the obtained product of step S2 and naphthoic acid or naphthoic acid ester under reflux for 5-8h in the presence of a catalyst; washing the reaction system with saturated brine first, then with methanol, and vacuum rotary drying to obtain the aforementioned modifier.

2. The plastic particles for processing plastic pallets according to claim 1, Features: The compatibilizer is maleic anhydride grafted POE and / or glycidyl methacrylate grafted POE.

3. The plastic particles for processing plastic pallets according to claim 1, Features: The polyolefin is a mixture of high-density polyethylene and polypropylene.

4. The plastic particles for processing plastic pallets according to claim 3, Features: The weight ratio of the high-density polyethylene to the polypropylene is 1:(3-6).

5. The plastic particles for processing plastic pallets according to any one of claims 1 to 4, Features: The alkaline solution in step S1 is a sodium hydroxide aqueous solution with a mass concentration of 10%, and the acidic solution in step S2 is a sulfuric acid aqueous solution with a mass concentration of 50%.

6. The plastic particles for processing plastic pallets according to any one of claims 1 to 4, Features: The catalyst in step S3 is a Lewis acid catalyst.

7. The plastic particles for processing plastic pallets according to any one of claims 1 to 4, Features: The cross-linking agent is diisophenylpropene peroxide or distearoyl peroxide.

8. The plastic particles for processing plastic pallets according to any one of claims 1 to 4, Features: The flow aid is diffusion oil.

9. A plastic pallet, made from the plastic particles for plastic pallet processing according to any one of claims 1 to 8 as raw materials.

10. A method for manufacturing a plastic pallet, It is characterized in that The specific steps are: first, the plastic particles for processing plastic pallets as described in any one of claims 1-8 are used as raw materials for thermoforming to obtain the panel and base of the pallet; then, the butt joint surfaces of the panel and the base are heated by a hot melt welding machine to melt the butt joint surfaces; finally, the panel and the base are pressed tightly together and cooled to obtain a plastic pallet.

Citation Information

Patent Citations

  • Large and medium-sized HDPE container special-purpose material composition

    CN102311572A

  • Method for preparing polypropylene and rice hull powder foamed composite tray

    CN103772819A

  • Plastic pallet and manufacturing method thereof

    CN108688935A

  • Active ester compound and preparation method thereof

    CN111116369A

  • Thermoplastic plastic pipe and preparation method thereof

    CN117624763A