Anisotropic conductive film

By using low-polar oxetane compounds in anisotropic conductive films in combination with alicyclic epoxy compounds, and using quaternary ammonium salt-based heat acid generators as cationic polymerization initiators, the conductive films are solved and stored and The problems of stability and reliability during the connection process achieve better shelf life and bonding characteristics.

CN118895092APending Publication Date: 2024-11-05DEXERIALS CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410926876.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2016-05-13
Filing Date
2017-02-10
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The existing anisotropic conductive films have problems with extended time, reduced storage stability and connection reliability during commercial transactions and storage, especially in warehouses without air conditioning, and have poor adhesive characteristics.

Method used

Use low-polar oxetane compounds and alicyclic epoxy compounds to combine with quaternary ammonium salt-based heat acid generators as cationic polymerization initiators to form adhesives including film-forming components, cationic polymerizable components and conductive particles. The mixture composition ensures curing temperature and connection reliability while improving shelf life.

Benefits of technology

While maintaining the curing temperature and connection reliability, the shelf life of the anisotropic conductive film is significantly improved, and the adhesion characteristics and reaction stability are enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004938464310000091
    Figure BDA0004938464310000091
Patent Text Reader

Abstract

Provided is a cationically polymerizable anisotropic conductive film using an alicyclic epoxy compound, which has a better storage life than conventional films while ensuring the same curing temperature and connection reliability as conventional films. The anisotropic conductive film contains a binder composition containing a film-forming component and a cationically polymerizable component, a cationic polymerization initiator, and conductive particles. The anisotropic conductive film uses a quaternary ammonium salt-based thermal acid generator as a cationic polymerization initiator, and contains an alicyclic epoxy compound and a low-polarity oxetane compound as cationically polymerizable components.
Need to check novelty before this filing date? Find Prior Art

Description

This application is a divisional application of a patent application with the original application date of February 10, 2017, application number 201780010511.3 (international application number PCT / JP2017 / 004887), and invention name “Anisotropic Conductive Film”. Technical Field

[0001] The present invention relates to an anisotropic conductive film. Background Art

[0002] In the past, when electronic components such as IC chips are mounted on wiring substrates, anisotropic conductive films in which conductive particles are dispersed in an insulating adhesive composition containing a polymerizable compound are widely used. For such anisotropic conductive films, in order to achieve low-temperature rapid curing properties, it has been proposed to use alicyclic epoxy compounds with higher cationic polymerization reactivity than general glycidyl ether compounds as polymerizable compounds, and to use sulfonium salt-based thermal acid generators that generate protons by heat as polymerization initiators that do not inhibit oxygen-based polymerization and show dark reactivity (Patent Documents 1 to 3). Such conventional anisotropic conductive films containing alicyclic epoxy compounds and sulfonium salt-based thermal acid generators have shown relatively low curing temperatures (e.g., around 100°C).

[0003] Prior art literature Patent Literature Patent Document 1: Japanese Patent Application Publication No. 9-176112 Patent Document 2: Japanese Patent Application Publication No. 2008-308596 Patent document 3: International Publication No. 2012 / 018123. Summary of the invention

[0004] Problems to be solved by the invention However, with regard to the anisotropic conductive film as described above, there is a problem that the time from manufacturing to actual use becomes longer due to the internationalization of commercial transactions, and there is a problem that there is a possibility of storage in warehouses without air conditioning, and there is a risk of reduced storage stability (shelf life) from the perspective of temporary sticking or indentation, and reduced connection reliability from the perspective of adhesive properties.

[0005] An object of the present invention is to achieve a better shelf life than before, while maintaining the same curing temperature and connection reliability as before, for a cationically polymerizable anisotropic conductive film using an alicyclic epoxy compound.

[0006] Means for solving problems The present inventors have found that, by using a low-polarity oxetane compound as a cationically polymerizable compound in a specific ratio in addition to an alicyclic epoxy compound, and by using a quaternary ammonium salt-based thermal acid generator instead of a sulfonium salt-based thermal acid generator as a cationic polymerization initiator, while maintaining the same curing temperature and connection reliability as before, a better shelf life than before can be achieved, thereby completing the present invention.

[0007] That is, the present invention provides an anisotropic conductive film comprising: a binder composition containing a film-forming component and a cationically polymerizable component, a cationic polymerization initiator, and conductive particles. The cationic polymerization initiator is a quaternary ammonium salt-based thermal acid generator, and the cationic polymerizable component contains an alicyclic epoxy compound and a low-polarity oxetane compound.

[0008] The present invention also provides a connection structure in which a first electronic component and a second electronic component are anisotropically conductively connected using the above-mentioned anisotropic conductive film.

[0009] Effects of the Invention The anisotropic conductive film of the present invention comprises a binder composition containing a film-forming component and a cationically polymerizable component, a cationic polymerization initiator, and conductive particles, uses a quaternary ammonium salt-based thermal acid generator as a cationic polymerization initiator, and contains an alicyclic epoxy compound and a low-polarity oxetane compound as a cationically polymerizable component. Therefore, while ensuring the same curing temperature and connection reliability as before, a better shelf life than before can be achieved. DETAILED DESCRIPTION

[0010] An example of the present invention is described in detail below.

[0011] <Anisotropic Conductive Film> The anisotropic conductive film of the present invention comprises a binder composition containing a film-forming component and a cationically polymerizable component, a cationic polymerization initiator, and conductive particles.

[0012] (Adhesive composition) In the present invention, the binder composition that contains and holds the conductive particles contains a film-forming component and a cationically polymerizable component.

[0013] (Film-forming ingredient) The film-forming component is a component used to make the anisotropic conductive film into a film, and is a component having film-forming ability. As such a film-forming component, phenoxy resin, epoxy resin, unsaturated polyester resin, saturated polyester resin, polyurethane resin, butadiene resin, polyimide resin, polyamide resin, polyolefin resin, etc. can be mentioned, and two or more of them can be used in combination. Among these, phenoxy resin can be preferably used from the viewpoint of film-forming property, processability, and connection reliability.

[0014] The content of the film-forming component in the adhesive composition is preferably 10 to 70% by mass, more preferably 20 to 50% by mass. Within this range, sufficient film-forming ability can be exhibited.

[0015] (Cationically polymerizable component) The cationic polymerizable component is a component that cures the anisotropic conductive film, and contains an alicyclic epoxy compound and a low-polarity oxetane compound. The amount of the cationic polymerizable component in the adhesive composition is preferably 10 to 80% by mass, and more preferably 20 to 60% by mass. If it is within this range, an adhesive composition with a higher curing speed can be provided.

[0016] (Alicyclic Epoxides) The reason for using alicyclic epoxy compounds is that, by utilizing their higher reactivity than general glycidyl ether-type epoxy compounds, good low-temperature rapid curing properties are imparted to the anisotropic conductive film. As such alicyclic epoxy compounds, preferably alicyclic epoxy compounds having two or more epoxy groups in the molecule can be cited. They can be liquid or solid. Specifically, hexahydrobisphenol A diglycidyl ether, 3,4-epoxycyclohexenylmethyl-3',4'-epoxycyclohexene formate (ester), dicyclohexyl diepoxide (ジエポキシビシクロヘキシル), etc. Among them, from the viewpoint of ensuring that the light transmittance of the cured product is excellent and the rapid curing properties are also excellent, hexahydrobisphenol A diglycidyl ether, especially dicyclohexyl diepoxide, can be preferably used.

[0017] (Low polarity oxetane compounds) In the present invention, a low polarity oxetane compound is used together with an alicyclic epoxy compound. The low polarity oxetane compound is an oxetane compound having a dipole moment of less than 3.0d, and has a relatively low surface tension, which can impart good leveling properties to the film of the anisotropic conductive film, and as a result, the shelf life of the anisotropic conductive film can be improved. On the other hand, the low polarity oxetane compound has the effect of increasing the reaction start temperature and the reaction end temperature of the anisotropic conductive film derived from the alicyclic epoxy compound as measured by a differential scanning calorimeter (DSC). As such a low polarity oxetane compound, there can be cited: 3-ethyl-3-(2-ethylhexyloxymethyl)oxetane, 3-ethyl-3-hydroxymethyloxetane, di[1-ethyl(3-oxetane)]methyl ether, 4,4′-bis[(3-ethyl-3-oxetane)methoxymethyl]biphenyl, etc. Among them, 3-ethyl-3-(2-ethylhexyloxymethyl)oxetane, particularly 4,4′-bis[(3-ethyl-3-oxetanyl)methoxymethyl]biphenyl is preferred because of its low surface tension and excellent wettability.

[0018] The blending ratio of the alicyclic epoxy compound and the low polarity oxetane compound is preferably 25:75 to 60:40, more preferably 45:55 to 60:40, and particularly preferably 50:50 to 55:45 in terms of mass standard. If the blending amount of the low polarity oxetane compound is increased than this range, there is a tendency to increase the reaction start temperature and the reaction end temperature. On the contrary, if it is reduced than this range, there is a tendency to reduce the shelf life. Therefore, by adjusting the blending ratio of the alicyclic epoxy compound and the low polarity oxetane compound, the reaction start temperature and the reaction end temperature of the anisotropic conductive film can be controlled. In addition, by adjusting the temperature rise rate during the reaction, the reaction time can also be controlled.

[0019] The adhesive composition may contain, as required: bisphenol A type epoxy resin, bisphenol F type epoxy resin, novolac type epoxy resin, other epoxy resins such as their modified epoxy resins, silane coupling agents, fillers, softeners, co-catalysts, anti-aging agents, colorants (pigments, dyes), organic solvents, ion trapping agents, etc. In addition, (meth)acrylate compounds and free radical polymerization initiators may be contained as required. Here, as (meth)acrylate compounds, conventionally known (meth)acrylate monomers may be used. For example, monofunctional (meth)acrylate monomers and difunctional or higher multifunctional (meth)acrylate monomers may be used. Here, (meth)acrylates include acrylates and methacrylates. In addition, as free radical polymerization initiators, known free radical polymerization initiators such as organic peroxides and azobisbutyronitrile may be contained.

[0020] (Conductive particles) In order to achieve anisotropic conductive connection, the anisotropic conductive film of the present invention contains conductive particles in the adhesive composition. As conductive particles, they can be appropriately selected from conductive particles used in conventionally known anisotropic conductive films. For example, metal particles such as nickel, cobalt, silver, copper, gold, palladium, alloy particles such as solder, metal-coated resin particles, etc. can be mentioned. Two or more kinds can also be used in combination.

[0021] The average particle size of the conductive particles is preferably 2.5 μm to 30 μm, more preferably 3 μm to 9 μm, in order to cope with the deviation of the wiring height, suppress the increase of the on-resistance, and suppress the occurrence of short circuits. The particle size of the conductive particles can be measured by a general particle size distribution measuring device, and the average particle size can also be obtained using a particle size distribution measuring device.

[0022] It should be noted that when the conductive particles are metal-coated resin particles, the particle hardness (20% K value; compression elastic deformation characteristics K 20 ), in order to obtain good connection reliability, preferably 100 to 1000 kgf / mm 2 , more preferably 200 to 500 kgf / mm 2 About the compressive elastic deformation characteristics K 20 For example, it can be measured at a measurement temperature of 20° C. using a micro compression tester (MCT-W201, manufactured by Shimadzu Corporation).

[0023] Regarding the amount of conductive particles present in the anisotropic conductive film, in order to suppress the reduction of the conductive particle capture efficiency and suppress the occurrence of short circuits, it is preferably more than 50 and less than 100,000 per 1 square mm, and more preferably more than 200 and less than 70,000. The determination of the amount can be carried out by observing the film of the material with an optical microscope. It should be noted that before the anisotropic conductive connection, since the conductive particles in the anisotropic conductive film are present in the adhesive composition, it is difficult to observe with an optical microscope. In this case, the anisotropic conductive film after the anisotropic conductive connection can also be observed. In this case, the change in film thickness before and after the connection can be considered to infer the amount.

[0024] It should be noted that the amount of conductive particles in the anisotropic conductive film can also be expressed as a mass standard. In this case, when the total mass of the anisotropic conductive film is taken as 100 parts by mass, the amount of conductive particles in the 100 parts by mass is preferably 1 part by mass or more and 30 parts by mass or less, and more preferably 3 parts by mass or more and 10 parts by mass or less.

[0025] (Cationic polymerization initiator) As a cationic polymerization initiator, the anisotropic conductive film of the present invention contains a quaternary ammonium salt-based thermal acid generator, rather than a sulfonium salt-based thermal acid generator. This is to improve the shelf life. As such a quaternary ammonium salt-based thermal acid generator, salts of quaternary ammonium cations and the following anions can be cited: hexafluoroantimonate anion, hexafluorophosphate anion, trifluoromethanesulfonate anion, perfluorobutanesulfonate anion, dinonylnaphthalenesulfonate anion, p-toluenesulfonate anion, dodecylbenzenesulfonate anion or tetrakis(pentafluorophenyl)borate anion. In addition, as a quaternary ammonium cation, NR1R2R3R4 can be cited. + Here, R1, R2, R3 and R4 are linear, branched or cyclic alkyl or aryl groups having 1 to 12 carbon atoms, and may each have a hydroxyl group, a halogen group, an alkoxy group, an amino group, an ester group or the like.

[0026] Specific examples of the quaternary ammonium salt-based thermal acid generator include CXC-1612, CXC-1733, CXC-1738, TAG-2678, CXC-1614, TAG-2689, TAG-2690, TAG-2700, CXC-1802-60, and CXC-1821 manufactured by King Industries, Inc. These are available from Kusumoto Chemicals Co., Ltd.

[0027] The thickness of the anisotropic conductive film of the present invention is preferably 3 to 50 μm, more preferably 5 to 20 μm.

[0028] (Manufacturing of anisotropic conductive film) The anisotropic conductive film of the present invention can be produced by dissolving the conductive particles, the cationic polymerization initiator, and the above-mentioned binder composition in an organic solvent such as toluene to prepare a coating material, and forming the coating material into a film using a known film forming method.

[0029] It should be noted that the anisotropic conductive film of the present invention may be a single layer, but in order not to reduce the particle capture property during anisotropic conductive connection, reduce the amount of conductive particles used to reduce the manufacturing cost and save the filling operation of the bottom filler, an insulating resin layer may be laminated. In this case, the anisotropic conductive film of the present invention becomes a two-layer structure containing a conductive particle layer / insulating resin layer. Such an insulating resin layer can basically be formed by the following composition: a composition in which a cationic polymerization initiator is mixed without making the conductive particles contained in the adhesive composition used for the anisotropic conductive film.

[0030] Regarding the anisotropic conductive film of the present invention, from the viewpoint of reaction rate control, it is preferred that the reaction start temperature of the reaction peak measured by a differential scanning calorimeter is adjusted to 60 to 80° C., and the reaction end temperature is adjusted to 155 to 185° C. These adjustments can be made by adjusting the blending ratio of the alicyclic epoxy compound and the low-polarity oxetane compound.

[0031] <Connection structure> The anisotropic conductive film of the present invention can be preferably used for anisotropically conductively connecting a first electronic component such as an IC chip, an IC module, or an FPC to a second electronic component such as a plastic substrate, a glass substrate, a rigid substrate, a ceramic substrate, or an FPC. A connection structure in which a first electronic component and a second electronic component are anisotropically conductively connected using the anisotropic conductive film of the present invention is also a part of the present invention. It should be noted that as a method for connecting electronic components using an anisotropic conductive film, a known method can be used. Example

[0032] The present invention is specifically described below by way of examples.

[0033] Example 1 (Formation of Conductive Particle-Containing Layer) 60 parts by mass of a phenoxy resin (YP-50, Nippon Steel & Sumitomo Chemical Co., Ltd.), 10 parts by mass of a dicyclohexyl diepoxide (CELLOXIDE 8000, Daicel Co., Ltd.) as an alicyclic epoxy compound, 20 parts by mass of a low-polarity oxetane compound (OXBP, Ube Industries, Ltd.), 2 parts by mass of a thermal cationic polymerization initiator (quaternary ammonium salt-based thermal acid generator, trade name CXC-1612, Kusumoto Chemical Co., Ltd.), and 50 parts by mass of conductive particles having an average particle size of 3 μm (Ni / Au-plated resin particles, AUL704, Sekisui Chemical Co., Ltd.) were added to toluene to prepare a mixed solution having a solid content of 50% by mass.

[0034] The obtained mixed liquid was applied onto a polyethylene terephthalate release film (PET release film) having a thickness of 50 μm to a dry thickness of 6 μm, and dried in an oven at 60° C. for 5 minutes to form a conductive particle-containing layer.

[0035] (Formation of Insulating Resin Layer) The same raw materials as those used to form the conductive particle-containing layer were added to toluene except that no conductive particles were used, to prepare a mixed liquid having a solid content of 50% by mass.

[0036] The obtained mixed liquid was applied on a PET release film having a thickness of 50 μm to a dry thickness of 12 μm, and dried in an oven at 60° C. for 5 minutes to form an insulating resin layer.

[0037] (Fabrication of anisotropic conductive film) The insulating resin layer was laminated on the conductive particle-containing layer at 60° C. and 5 MPa, thereby obtaining an anisotropic conductive film sandwiched between a pair of PET release films having a thickness of 50 μm.

[0038] Embodiments 2 to 4 An anisotropic conductive film was obtained in the same manner as in Example 1, except that the blending amounts (ratios) of the alicyclic epoxy compound (CELLOXIDE 8000, Daicel) and 4,4′-bis[(3-ethyl-3-oxetanyl)methoxymethyl]biphenyl (OXBP, Ube Industries, Ltd.) as a low-polarity oxetane compound in the conductive particle-containing layer and the insulating resin layer were changed as shown in Table 1.

[0039] Comparative Examples 1 to 4 Anisotropic conductive films were prepared in the same manner as in Examples 1 to 4 except that the thermal cationic polymerization initiator in the conductive particle-containing layer and the insulating resin layer was replaced with a sulfonium salt-based thermal acid generator (SI-60L, Sanshin Chemical Industry Co., Ltd.) as shown in Table 1.

[0040] Examples 5 to 13, Comparative Example 5 An anisotropic conductive film was prepared in the same manner as in Example 1, except that the blending amounts (ratios) of the alicyclic epoxy compound (CELLOXIDE 8000, Daicel) and the low-polarity oxetane compound (OXBP, Ube Industries, Ltd.) in the conductive particle-containing layer and the insulating resin layer were changed as shown in Table 1.

[0041] <<Evaluation>> The anisotropic conductive films obtained in the respective Examples and Comparative Examples were tested, measured, and evaluated for “shelf life characteristics”, “curing temperature”, “adhesion characteristics”, and “reaction time” as described below.

[0042] <Shelf Life Characteristics> The anisotropic conductive film sandwiched between a pair of PET release films was placed in a constant temperature and humidity chamber set at 40% humidity and 25°C or 30°C. After placement, samples were taken every 24 hours, and the following temporary attachment evaluation and pressure bonding evaluation were performed. Based on these evaluation results, the shelf life characteristics were comprehensively evaluated. The obtained results are shown in Table 1.

[0043] (Temporary evaluation) The PET release film on the conductive particle layer side of the anisotropic conductive film was peeled off, and the anisotropic conductive film was attached to a plain glass from the conductive particle layer side to produce a laminate of plain glass and anisotropic conductive film. The laminate was placed in such a way that the plain glass side was in contact with a hot plate set at 45°C, and pressure was applied by hand from the anisotropic conductive film side, and then cooled to room temperature. After cooling, the PET release film on the insulating resin layer side of the laminate was peeled off to confirm whether only the PET release film was peeled off from the plain glass and the anisotropic conductive film was not peeled off.

[0044] (Pressure Evaluation) An anisotropic conductive film was sandwiched between a test IC chip and a test substrate so that the insulating resin layer was disposed on one side of the IC chip, and heat and pressurization (120°C, 60 MPa, 5 seconds) was performed to produce an evaluation connection. The indentation state of the produced connection was confirmed to confirm whether the indentation remained without becoming thinner or disappearing.

[0045] (Shelf life characteristics evaluation) The shelf life was determined as the time when the anisotropic conductive film peeled off from the plain glass in the temporary bonding evaluation. In addition, when the anisotropic conductive film did not peel off from the plain glass in the temporary bonding evaluation, the shelf life was determined as the time when the indentation became thinner (disappeared) in the press bonding evaluation.

[0046] <Curing Temperature> The anisotropic conductive film was sandwiched between the test IC chip and the test substrate in such a way that the insulating resin layer was arranged on one side of the IC chip, and heating and pressing (80°C, 90°C, 100°C, 110°C or 120°C, 60MPa, 5 seconds) were performed to obtain an evaluation connection. The reaction rate of the anisotropic conductive film in the connection was measured as follows, and the curing temperature was determined based on the measurement results. The obtained results are shown in Table 1.

[0047] (Reaction rate determination) The IC chip of the evaluation connection was peeled off by hand to expose the cured anisotropic conductive film and sample the anisotropic conductive film. The obtained sample was dissolved in acetonitrile to a concentration of 0.1 g / mL. In addition, the anisotropic conductive film before curing was dissolved in acetonitrile to the same concentration, and the peak intensity of each monomer was confirmed using HPLC-MS (WaterS Company) under the following conditions. The reaction rate at each temperature was calculated by the reduction in peak intensity after curing, and the temperature with a reaction rate of 80% or more was taken as the curing temperature.

[0048] Solvent: A mixed solvent obtained by mixing 40 parts by mass of acetonitrile with 60 parts by mass of a water / acetonitrile mixed solution (90 / 10) Flow rate: 0.4 mL / min Column: 10cm, 40°C Injection volume: 5μL Analysis wave: 210-410nm <Adhesion Characteristics> Between the test IC chip and the test substrate, the anisotropic conductive film was clamped in such a way that the insulating resin layer was arranged on one side of the IC chip, and heating and pressing (120°C, 60MPa, 5 seconds) were performed to obtain an evaluation connection. For the connection, the pressure cooker test (Pressure Cooker Test, PCT) was implemented using the model EHS-411M of ETAC. Specifically, for the obtained evaluation connection, the connection was put into a constant temperature and humidity tank set to 121°C, 2atm, and a saturated water vapor atmosphere, and the following adhesion evaluation was performed every 24 hours. The results obtained are shown in Table 1.

[0049] (Adhesion Evaluation) The appearance of the connected product subjected to the PCT test was checked, and it was visually observed whether or not peeling occurred between the anisotropic conductive film and the IC chip or the substrate layer.

[0050] Grade Standard ○: After IC lamination, no peeling was observed even after 48 hours of PCT △: After IC lamination, no peeling was observed during 24-hour PCT test, but peeling was observed during 48-hour PCT test. ×: After IC lamination, peeling was observed before PCT or after 24 hours of PCT <Reaction time> A sample of about 5 mg cut out from the obtained anisotropic conductive film was placed in aluminum PAN (TA Instruments Inc.), which was placed in a DSC measuring device (Q2000, TA Instruments Inc.), and a differential scanning calorimeter (DSC) was measured from 30°C to 250°C at a heating rate of 10°C / min. According to the obtained DSC chart, the temperature at the time point when the exothermic peak rises is read as the reaction start temperature, and the temperature at the time point when the exothermic peak changes to the baseline is read as the reaction end temperature. In addition, the reaction time was calculated according to the following formula. The results obtained are shown in Table 1.

[0051] Reaction time (minutes) = (reaction end temperature (°C) - reaction start temperature (°C)) / 10 [°C / minute] [Table 1] <<Review of Evaluation Results>> According to the results in Table 1 (comparison between Example 1 and Comparative Example 1, comparison between Example 2 and Comparative Example 2, comparison between Example 3 and Comparative Example 3, and comparison between Example 4 and Comparative Example 4), it can be seen that if a quaternary ammonium salt-based thermal acid generator is used instead of a sulfonium salt-based thermal acid generator, the shelf life can be greatly improved without changing the curing temperature or the adhesive properties that are an evaluation index of connection reliability, even if the blending ratio between the alicyclic epoxy compound and the low-polarity oxetane compound is changed.

[0052] In addition, from the comparison of Examples 1, 5 to 7 and Comparative Example 5, it can be seen that the shelf life tends to be improved as the blending ratio of the low-polarity oxetane compound to the alicyclic epoxy compound increases, but if the blending amount of the alicyclic epoxy compound is relatively reduced, the adhesive properties tend to decrease. On the contrary, from the comparison of Examples 8 to 13, it can be seen that the shelf life tends to decrease as the blending ratio of the low-polarity oxetane compound to the alicyclic epoxy compound decreases.

[0053] It is to be noted that, from the comparison of the DSC measurement results performed in Example 1, Examples 5 to 13, and Comparative Example 5, it is found that increasing the blending amount of the low-polarity oxetane compound tends to increase the reaction start temperature and the reaction end temperature.

[0054] Industrial Applicability The anisotropic conductive film of the present invention using the cationic polymerization of an alicyclic epoxy compound can achieve a curing temperature and connection reliability equivalent to those of a conventional anisotropic conductive film using a sulfonium salt-based thermal acid generator, while also achieving a better shelf life than before. Therefore, it can be used for anisotropic conductive connection to a wiring substrate of electronic components such as IC chips.

Claims

1. An anisotropic conductive film comprising: an adhesive composition containing a film-forming component and a cationically polymerizable component, a cationic polymerization initiator, and conductive particles; in, The cationic polymerization initiator is a quaternary ammonium salt-based thermal acid generator, and the cationic polymerizable component contains an alicyclic epoxy compound and a low-polarity oxetane compound. The reaction peak measured by a differential scanning calorimeter showed a reaction initiation temperature of 60 to 80° C., and a reaction time of 8.5 to 11 minutes.

2. The anisotropic conductive film according to claim 1, wherein The blending ratio of the alicyclic epoxy compound to the low-polarity oxetane compound is 25:75 to 60:40 based on the mass standard.

3. The anisotropic conductive film according to claim 1, wherein The blending ratio of the alicyclic epoxy compound to the low-polarity oxetane compound is 45:55 to 60:40 based on the mass standard.

4. The anisotropic conductive film according to any one of claims 1 to 3, wherein The quaternary ammonium salt-based thermal acid generator is a salt of a quaternary ammonium cation and the following anions: hexafluoroantimonate anion, hexafluorophosphate anion, trifluoromethanesulfonate anion, perfluorobutanesulfonate anion, dinonylnaphthalenesulfonate anion, p-toluenesulfonate anion, dodecylbenzenesulfonate anion or tetrakis(pentafluorophenyl)borate anion.

5. The anisotropic conductive film according to claim 4, wherein Quaternary ammonium cation is NR1R2R3R4 + In the cation represented by, R1, R2, R3 and R4 are linear, branched or cyclic alkyl or aryl groups having 1 to 12 carbon atoms.

6. The anisotropic conductive film according to any one of claims 1 to 5, wherein The alicyclic epoxy compound is hexahydrobisphenol A diglycidyl ether or dicyclohexyl diepoxide, and the low-polarity oxetane compound is 3-ethyl-3-(2-ethylhexyloxymethyl)oxetane or 4,4′-bis[(3-ethyl-3-oxetane)methoxymethyl]biphenyl.

7. The anisotropic conductive film according to any one of claims 1 to 6, wherein The film-forming component is a phenoxy resin.

8. The anisotropic conductive film according to any one of claims 1 to 7, wherein The reaction peak measured by a differential scanning calorimeter had a reaction start temperature of 60 to 80°C and a reaction end temperature of 155 to 185°C.

9. An anisotropic conductive film comprising: an adhesive composition containing a film-forming component and a cationically polymerizable component, a cationic polymerization initiator, and conductive particles, in, The cationic polymerization initiator is a quaternary ammonium salt-based thermal acid generator, and the cationic polymerizable component contains an alicyclic epoxy compound and a low-polarity oxetane compound. The blending ratio of the alicyclic epoxy compound to the low polarity oxetane compound is 1:8 to 2:1 according to the mass standard. The reaction start temperature of the reaction peak measured by a differential scanning calorimeter is 65° C. or higher and 90° C. or lower, and the reaction end temperature is 150° C. or higher and 200° C. or lower.

10. An anisotropic conductive film comprising: an adhesive composition containing a film-forming component and a cationically polymerizable component, a cationic polymerization initiator, and conductive particles, in, The cationic polymerization initiator is a quaternary ammonium salt-based thermal acid generator, and the cationic polymerizable component contains an alicyclic epoxy compound and a low-polarity oxetane compound. The shelf life is more than 5 days and the temporary sticking property is satisfied at 45°C.

11. A connection structure formed by anisotropically conductively connecting a first electronic component and a second electronic component using the anisotropic conductive film according to any one of claims 1 to 10.

12. A method for manufacturing a connection structure, comprising: A first electronic component and a second electronic component are anisotropically conductively connected using the anisotropic conductive film according to any one of claims 1 to 10.