Method of manufacturing and etching semiconductor device
By employing a plasma etching process with passivation orientation and etchant orientation in the dense and isolated regions of semiconductor devices, the problem of depth load difference during fin etching in the prior art is solved, appropriate trench formation is achieved, damage to epitaxial source/drain regions is avoided, and the integration density and reliability of semiconductor devices are improved.
Patent Information
- Application Number
- CN202410677765.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-07-10
- Filing Date
- 2024-05-29
- Publication Date
- 2024-11-05
AI Technical Summary
As the minimum feature size of semiconductor devices decreases, existing technologies struggle to effectively address the depth load differences between dense and isolated regions during fin etching, leading to leakage and damage in the epitaxial source/drain regions.
Plasma etching processes employing passivation orientation and etchant orientation are used to form trenches with different depths and critical dimensions in dense and isolated regions, respectively. By controlling the etching rates of the passivation orientation and etchant orientation processes, appropriate trench depths and widths are formed to avoid damage to the epitaxial source/drain regions.
This enables the formation of appropriate trench depth and width in dense and isolated regions, avoiding damage to epitaxial source/drain regions and improving the integration density and reliability of semiconductor devices.
Smart Images

Figure CN118899221A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a method of manufacturing and etching a semiconductor device. Background Art
[0002] Semiconductor devices are used in a variety of electronic applications such as, for example, personal computers, cell phones, digital cameras, and other electronic equipment. Semiconductor devices are typically manufactured by sequentially depositing insulating or dielectric layers, conductive layers, and semiconductor material layers over a semiconductor substrate and patterning the various material layers using lithography techniques to form circuit components and elements on these material layers.
[0003] The semiconductor industry continues to improve the integration density of various electronic components (e.g., transistors, diodes, resistors, capacitors, etc.) by continuously reducing the minimum feature size, thereby integrating more components into a given area. However, as the minimum feature size decreases, additional problems arise that should be solved. Summary of the invention
[0004] One aspect of the present disclosure is a method for manufacturing a semiconductor device, comprising the following steps: forming a plurality of fins in a dense area and an isolation area of a semiconductor substrate; performing a plasma etching process to remove a portion of at least one selected fin in the dense area, thereby forming a first trench in the dense area, and removing a portion of at least one selected fin in the isolation area, thereby forming a second trench in the isolation area, wherein the plasma etching process comprises the following steps: performing a passivation orientation process and an etchant orientation process; and controlling the passivation orientation process and the etchant orientation process to form the first trench having a first critical dimension and a first depth, and forming the second trench having a second critical dimension and a second depth.
[0005] Another aspect of the present disclosure is a method comprising the following steps: determining a first depth of a first trench etched in a dense region of a substrate and a second depth of a second trench etched in an isolated region of the substrate; designing a plasma dry etching process to form a first trench having a first depth and a second trench having a second depth, wherein the plasma dry etching process includes a first plasma dry etching operation and a second plasma dry etching operation, wherein the first plasma dry etching operation has a first dense etching rate in multiple dense regions and a first isolation etching rate in multiple isolated regions, and wherein the second plasma dry etching operation has a second dense etching rate in the dense region and a second isolation etching rate in the isolated region; and performing the plasma dry etching process to form a first trench having a first depth and a second trench having a second depth.
[0006] Another aspect of the present disclosure is a method for etching a semiconductor material, comprising the following steps: performing a first plasma dry etching operation with a passivation orientation; performing a second plasma dry etching operation with an etchant orientation; and repeating the first plasma dry etching operation and the second plasma dry etching operation to form a trench in the semiconductor material having a depth. BRIEF DESCRIPTION OF THE DRAWINGS
[0007] The various aspects of the present disclosure can be best understood when the following detailed description is read in conjunction with the accompanying drawings. It should be noted that, in accordance with standard practice in the industry, various features are not drawn to scale. In fact, the dimensions of various features may be arbitrarily increased or reduced for clarity of discussion.
[0008] Figure 1 is a flow chart illustrating a method according to some embodiments;
[0009] Figure 2 A top view of a gate-all-around (GAA) semiconductor device is illustrated according to some embodiments;
[0010] Figures 3 to 10 , Fig.12 , Fig.14 , Fig.16 and Fig.18 According to some embodiments, Figure 1 a cross-sectional view of the device taken along the Y-axis during a continuous manufacturing stage of the method;
[0011] Fig.11 , Fig.13 , Fig.15 , Fig.17 and Fig.19 are respectively intercepted along the Y axis according to some embodiments Fig.10 , Fig.12 , Fig.14 , Fig.16 and Fig.18 A cross-sectional view of the device at a manufacturing stage;
[0012] Fig. 20 for Fig.14 A top view of a portion of a manufacturing device in an isolation area;
[0013] Fig.21 for Fig. 20 A cross-sectional view of the device along the Y-axis after a passivation oriented etching operation;
[0014] Fig. 22 for Fig. 20 A cross-sectional view of the device along the Y-axis after an etchant oriented etching operation;
[0015] Fig.23 for Fig.14A top view of a portion of a manufacturing device in a dense area;
[0016] Fig.24 for Fig.23 A cross-sectional view of the device along the Y-axis after a passivation oriented etching operation;
[0017] Fig.25 for Fig.23 A cross-sectional view of the device along the Y-axis after an etchant oriented etching operation;
[0018] Fig.26 is a flow chart illustrating a method according to some embodiments;
[0019] Fig. 27 For similar Fig.17 A cross-sectional view of a trench formed by a plasma etching process operation is used to describe the dimensions of the trench.
[0020]
Explanation of symbols
[0021] 10, 90: Method
[0022] 100:Semiconductor device
[0023] 103:Multi-layer structure
[0024] 105, 106: Fins
[0025] 107: Gate
[0026] 109: Cutting metal gate structure
[0027] 111:CPODE structure
[0028] 201:Substrate
[0029] 202: Concave surface
[0030] 203: Multi-layer stacking
[0031] 205: First floor
[0032] 207: Second floor
[0033] 209, 1001: Quarantine Area
[0034] 211: Dummy gate dielectric
[0035] 301:Dummy gate stack
[0036] 303: dummy gate
[0037] 305: First hard mask
[0038] 307: Second hard mask
[0039] 503: epitaxial source / drain region
[0040] 505: Internal spacer
[0041] 701:Nanostructure
[0042] 703: Gate dielectric
[0043] 801: Gate cap
[0044] 901, 1003, 1091: Open
[0045] 903: Mask layer
[0046] 1002: Dense area
[0047] 1103: Groove
[0048] 1200: Mask
[0049] 1201: Bottom layer
[0050] 1202: Middle layer
[0051] 1203: Top floor
[0052] 1205: Gap
[0053] 2101, 2201: Byproducts
[0054] CW1: Channel Width
[0055] d1, d2, D1, D2: vertical depth
[0056] Da: Depth
[0057] H5, H6: Height
[0058] l, l1, l2: length
[0059] S11, S12, S13, S14, S15, S16, S17, S18, S19, S20, S21, S22, S23, S91, S92, S93, S94, S95: Steps
[0060] w, W3: width
[0061] Wa, Wb, Wc: lateral width DETAILED DESCRIPTION
[0062] The following disclosure provides many different embodiments or examples for realizing the different features of the subject matter. The specific examples of components and configurations described below are for simplifying the disclosure. Of course, these are only examples and are not intended to be limiting. For example, in the following description, forming a first feature above or on a second feature may include an embodiment in which the first feature and the second feature are directly contacted, and may also include an embodiment in which an additional feature may be formed between the first feature and the second feature so that the first feature and the second feature may not be directly in contact. In addition, the disclosure may repeat reference numerals and / or letters in various examples. This repetition is for the purpose of simplicity and clarity, and does not itself indicate the relationship between the various embodiments and / or configurations discussed.
[0063] Additionally, for ease of description, spatially relative terms such as "above," "overlying," "above," "upper," "top," "below," "underlying," "under," "beneath," "lower," "bottom," "side," and the like may be used herein to describe the relationship of one element or feature to another element or feature as illustrated in the figures. The spatially relative terms are intended to encompass different orientations of the device in use or operation in addition to the orientation depicted in the figures. The device may be otherwise oriented (rotated 90 degrees or at other orientations) and the spatially relative descriptors used herein may likewise be interpreted accordingly.
[0064] In certain embodiments herein, a "material structure" is a structure that includes at least 50 weight percent of an identified material (e.g., at least 60 weight percent of an identified material, at least 75 weight percent of an identified material, at least 90 weight percent of an identified material, at least 95 weight percent of an identified material, or at least 99 weight percent of an identified material); and is a structure formed of a "material" that includes at least 50 weight percent of an identified material (e.g., at least 60 weight percent of an identified material, at least 75 weight percent of an identified material, at least 90 weight percent of an identified material, at least 95 weight percent of an identified material, or at least 99 weight percent of an identified material). For example, in certain embodiments, each of a tungsten structure and a structure formed of tungsten is a structure that is at least 50 weight percent, at least 60 weight percent, at least 75 weight percent, at least 90 weight percent, at least 95 weight percent, or at least 99 weight percent tungsten.
[0065] For the sake of brevity, typical techniques associated with semiconductor device manufacturing may not be described in detail in this disclosure. In addition, the various tasks and processes described in this disclosure may be incorporated into a more comprehensive program or process with additional functionality not described in detail in this disclosure. In particular, the various processes for manufacturing semiconductor devices are well known, and therefore, for the sake of brevity, many typical processes will only be briefly mentioned in this disclosure or will be completely omitted without providing familiar process details. As will be readily apparent to those familiar with the art after reading this disclosure in its entirety, the structures disclosed in this disclosure can be employed with various techniques and can be incorporated into various semiconductor devices and products. In addition, it should be noted that the semiconductor device structure includes different numbers of components, and a single component shown in the description may represent multiple components.
[0066] The present disclosure presents embodiments of semiconductor devices and embodiments of methods for making such devices. The methods described in the present disclosure can be easily integrated into current process flows. In addition, the methods described in the present disclosure are related to forming an insulating structure that divides a fin into two halves, such as a Continuous Poly On Diffusion Edge (CPODE) structure. In some embodiments, a portion of a selected fin is removed and the removed portion is replaced with an insulating material.
[0067] In the embodiments of the present disclosure, a CPODE-last processing method is described, that is, during the middle-end-of-line (MEOL) processing after the metal gate is formed. However, the embodiments of the present disclosure are not limited thereto, and the embodiments of the present disclosure can be further applied to a CPODE-first processing method, that is, during the front-end-of-line (FEOL) processing before the metal gate is formed.
[0068] In embodiments of the present disclosure, a CPODE process is used to pattern transistors by plasma etching to avoid leakage current through the transistors and the silicon substrate. In addition, embodiments of the present disclosure alleviate isolation / dense depth loading and provide a tuning knob for isolation / dense depth loading. Furthermore, in embodiments of the present disclosure, CPODE etching achieves a sufficiently deep vertical depth and a sufficiently small lateral width or critical dimension (CD) to avoid leakage from and damage to the epitaxial source / drain regions, respectively. As used in the present disclosure, "source / drain region" may refer to a source region or a drain region, either alone or together, depending on the context.
[0069] Embodiments of the present disclosure provide advantages over existing technologies, but it should be understood that other embodiments may provide different advantages, not all of which must be discussed in the present disclosure, and not all embodiments require a particular advantage.
[0070] For the purpose of the following discussion, Figure 1 A flow chart of a method 10 for manufacturing a semiconductor device 100 during a semiconductor manufacturing process is provided. Figures 2 to 19 Description Method 10, Figures 2 to 19 The semiconductor device 100 is illustrated at various stages of fabrication according to the method 10 . Figure 2 A top view of an intermediate structure in forming a semiconductor device 100 , such as a gate-all-around (GAA) semiconductor device, is illustrated according to some embodiments. Figures 3 to 10 , Fig.12 , Fig.14 , Fig.16 and Fig.18 It is a cross-sectional view with the vertical direction defined by the Z-axis and the lateral direction defined by the Y-axis (ie, “transverse to the Y-axis”). Fig.11 , Fig.13 , Fig.15 , Fig.17 and Fig.19 1 is a cross-sectional view with the vertical direction defined by the Z-axis and the lateral direction defined by the X-axis (i.e., "X-axis cross-section"). It should be understood that method 10 includes steps that are characteristic of a complementary metal-oxide-semiconductor (CMOS) technology process flow, and therefore is only briefly described in this disclosure. In addition, additional steps may be performed before, after, and / or during method 10.
[0071] exist Figure 2 In the embodiment, the semiconductor device 100 includes a multilayer structure 103, which includes a plurality of nanosheets (described in the following figure) formed on a substrate 201, a fin 105 formed in the multilayer structure 103, and a plurality of gates 107 located above the fin 105. Figure 2 Further described are a plurality of cut metal gate structures 109 separating two gates 107 and a continuous polysilicon on diffusion edge (CPODE) structure 111 dividing a fin 105 into two halves and intersecting the cut metal gate structures 109 .
[0072] Despite Figure 2In the Y-axis cut diagram shown below, three fins 105 are described, but it should be understood that any suitable number of fins 105 can be formed in the multilayer structure 103 according to the desired design and number of the all-around gate semiconductor device 100 to form the desired all-around gate semiconductor device 100. In addition, any suitable number of gates 107, CPODE structures 111, and cut metal gate structures 109 can be formed to form the desired all-around gate semiconductor device 100.
[0073] exist Figure 2 , the X-axis extends through the length of the fin 105 and through the CPODE structure 111. Additionally, the Y-axis extends through the length of the gate 107 separated by the two cut metal gate structures 109, through the two cut metal gate structures 109, and through the CPODE structure 111 intersecting the two cut metal gate structures 109.
[0074] Reference Figure 1 and Figure 3 According to some embodiments, a method 10 for manufacturing a semiconductor device 100 includes, in step S11 , forming a multilayer structure 103 over a semiconductor material such as a substrate, and forming a fin 105 in the multilayer structure 103 .
[0075] In one embodiment of the present disclosure, the substrate 201 is a semiconductor substrate, which may be, for example, a silicon substrate, a silicon germanium substrate, a germanium substrate, a III-V material substrate (e.g., GaAs, GaP, GaAsP, AlInAs, AlGaAs, GaInAs, InAs, GaInP, InP, InSb and / or GaInAsP; or a combination thereof), or a substrate formed of other semiconductor materials having, for example, high band-to-band tunneling (BTBT). The substrate 201 may be doped or undoped. In some embodiments, the substrate 201 may be a bulk semiconductor substrate, such as a bulk silicon substrate as a wafer, a semiconductor-on-insulator (SOI) substrate, a multi-layer or gradient substrate, or the like.
[0076] Figure 3 The deposition process for forming the multilayer structure 103 at an intermediate stage of manufacturing the all-around gate semiconductor device 100 according to some embodiments is described. Specifically, Figure 3 A series of depositions is further illustrated to form a multilayer stack 203 of alternating materials of a first layer 205 and a second layer 207 over a substrate 201 .
[0077] According to some embodiments, the first layer 205 may be formed using a first semiconductor material having a first lattice constant, such as SiGe, Ge, Si, GaAs, InSb, GaSb, InAlAs, InGaAs, GaSbP, GaAsSb, combinations of these materials, or the like. In some embodiments, the first layer 205 of the first semiconductor material (e.g., SiGe) is epitaxially grown on the substrate 201 using a deposition technique such as epitaxial growth, vapor-phase epitaxy (VPE), molecular beam epitaxy (MBE), but other deposition processes may also be used, such as chemical vapor deposition (CVD), low pressure chemical vapor deposition (LPCVD), atomic layer chemical vapor deposition (ALCVD), ultrahigh vacuum chemical vapor deposition (UHVCVD), reduced pressure chemical vapor deposition (RPCVD), combinations of these processes, or the like. In some embodiments, the first layer 205 is formed to a thickness between about 3 nanometers and about 10 nanometers. However, any suitable thickness may be used while remaining within the scope of the embodiments.
[0078] After forming the first layer 205 over the substrate 201, the second layer 207 may be formed over the first layer 205. According to some embodiments, the second layer 207 may be formed using a second semiconductor material having a second lattice constant different from the first lattice constant of the first layer 205, such as Si, SiGe, Ge, GaAs, InSb, GaSb, InAlAs, InGaAs, GaSbP, GaAsSb, combinations of these materials, or the like. In a specific embodiment where the first layer 205 is silicon germanium, the second layer 207 is a material such as silicon. However, any combination of suitable materials may be used for the first layer 205 and the second layer 207.
[0079] In some embodiments, the second layer 207 is epitaxially grown on the first layer 205 using a deposition technique similar to the deposition technique used to form the first layer 205. However, the second layer 207 may use any deposition technique as described above for forming the first layer 205 or any other suitable technique. According to some embodiments, the second layer 207 is formed to a thickness similar to the thickness of the first layer 205. However, the second layer 207 may also be formed to a different thickness than the first layer 205. According to some embodiments, the second layer 207 may be formed to a thickness between about 5 nanometers and about 15 nanometers. However, any suitable thickness may be used.
[0080] After forming the second layer 207 over the first layer 205, the deposition process is repeated to form the remaining material layers using a series of alternating materials of the first layer 205 and the second layer 207 until the desired topmost layer of the multilayer stack 203 has been formed. According to one embodiment of the present disclosure, the first layer 205 may be formed to the same or similar first thickness, and the second layer 207 may be formed to the same or similar second thickness. However, the first layer 205 may have different thicknesses from each other and / or the second layer 207 may have different thicknesses from each other, and any combination of thicknesses used for the first layer 205 and the second layer 207 may be present. According to the present embodiment, the topmost layer of the multilayer stack 203 is formed as the second layer 207; however, in other embodiments, the topmost layer of the multilayer stack 203 may be formed as the first layer 205. In addition, although the present disclosure discloses an embodiment including three first layers 205 and three second layers 207, the multilayer stack 203 may have any suitable number of stacked layers (e.g., nanosheets). For example, the multilayer stack 203 may include two to ten nanosheets. In some embodiments, the multilayer stack 203 may include an equal number of first layers 205 and second layers 207; however, in other embodiments, the number of first layers 205 may be different from the number of second layers 207. According to some embodiments, the multilayer stack 203 may be formed to a height between about 12 nanometers and about 100 nanometers. However, any suitable height may be used.
[0081] Figure 3 The patterning process of the multilayer structure 103 and the formation of the isolation region 209 at an intermediate stage of manufacturing the all-around gate semiconductor device 100 is further described according to some embodiments. The patterning process is used to form the fins 105 in the multilayer structure 103 and to form trenches between the fins 105 in preparation for forming the isolation region 209. According to some embodiments, the patterning process for forming the fins 105 includes applying a photoresist over the multilayer stack 203, then patterning and developing the photoresist to form a mask over the multilayer stack 203. After forming the mask, the mask is then used during an etching process such as an anisotropic etching process to transfer the pattern of the mask into the underlying layer to form trenches through the multilayer stack 203 and into the substrate 201, thereby defining the fins 105, wherein the fins 105 are separated by the trenches.
[0082] Furthermore, while a single mask process has been described, this is intended to be illustrative and not limiting, as the all-around gate device structure may be patterned by any suitable method. For example, the structure may be patterned using one or more lithography processes, including double patterning or multi-patterning processes. In general, combinations of lithography processes such as double patterning or multi-patterning and self-aligned processes may form patterns having a smaller pitch than, for example, using a single direct lithography process. For example, in one embodiment of the present disclosure, a sacrificial layer is formed over substrate 201 and patterned using a lithography process. Spacers are formed adjacent to the patterned sacrificial layer using a self-aligned process. The sacrificial layer is then removed and the remaining spacers may be used to pattern the all-around gate structure.
[0083] In an exemplary embodiment, the isolation region 209 is formed as a shallow trench isolation region by depositing a dielectric material in the trench. According to some embodiments, the dielectric material used to form the isolation region 209 may be, for example, an oxide material (e.g., a flowable oxide), a high-density plasma (HDP) oxide, or the like. After the trench is selectively cleaned and lined, a dielectric material may be formed using any of a chemical vapor deposition method (e.g., a HARP process), a high-density plasma chemical vapor deposition method, or other suitable formation methods to fill or overfill the area around the fin 105. In some embodiments, a post-placement annealing process (e.g., oxide densification) is performed to densify the material of the isolation region 209 and reduce its wet etch rate. Chemical mechanical polishing, etching, a combination of these processes, or the like may be performed to remove any excess material of the isolation region 209.
[0084] After depositing the dielectric material to fill or overfill the area around the fin 105, the dielectric material may then be recessed from the surface of the fin 105 to form the isolation region 209. The recessing may be performed to expose at least a portion of the sidewall of the fin 105 adjacent to the top surface of the fin 105. The dielectric material may be recessed by immersing the top surface of the fin 105 in an etchant that is selective to the dielectric material and using a wet etch, although other methods such as reactive ion etching, dry etching, chemical oxide removal, or dry chemical cleaning may also be used.
[0085] Figure 3Further illustrating the formation of a dummy gate dielectric 211 over the exposed portion of the fin 105. After the isolation region 209 has been formed, the dummy gate dielectric 211 may be formed by thermal oxidation, chemical vapor deposition, sputtering, or any other method known and used in the art for forming a gate dielectric. Depending on the technique of gate dielectric formation, the thickness of the dummy gate dielectric 211 at the top may be different from the thickness of the dummy dielectric on the sidewalls. In some embodiments, the dummy gate dielectric 211 may be formed by depositing a material such as silicon and oxidizing or nitriding the silicon layer to form the dummy gate dielectric 211, thereby forming a dielectric such as silicon dioxide or silicon oxynitride. In such embodiments, the dummy gate dielectric 211 may be formed to be between about 100 Å and 200 Å. (angstrom) Between (e.g. about ) in thickness. In other embodiments, the dummy gate dielectric 211 may also be made of a dielectric having a thickness between about About Between (e.g. about The dummy gate dielectric 211 is formed of a high-k material with an equivalent oxide thickness of 100 Å (0.1 Å) or less, such as lanthanum oxide (La2O3), aluminum oxide (Al2O3), hafnium oxide (HfO2), hafnium oxynitride (HfON) or zirconium oxide (ZrO2) or a combination thereof. In addition, any combination of silicon dioxide, silicon oxynitride and / or high-k materials may also be used for the dummy gate dielectric 211.
[0086] Cross Reference Figure 1 and Figure 4 According to some embodiments, the method 10 may continue in step S12 to form a sacrificial or dummy gate stack 301 above the fin 105. According to some embodiments, the dummy gate stack 301 includes a dummy gate dielectric 211, a dummy gate 303 located above the dummy gate dielectric 211, a first hard mask 305 located above the dummy gate 303, and a second hard mask 307 located above the first hard mask 305.
[0087] In some embodiments, the dummy gate 303 includes a conductive material, and the conductive material may include polysilicon, tungsten (W), aluminum (Al), copper (Cu), AlCu, titanium (Ti), TiAlN, TaC, TaCN, TaSiN, manganese (Mn), zirconium (Zr), TiN, tantalum (Ta), TaN, cobalt (Co), nickel (Ni), combinations of these materials, or the like. The dummy gate 303 may be deposited by chemical vapor deposition, sputtering deposition, or other techniques known in the art and used to deposit conductive materials. The thickness of the dummy gate 303 may be between about 1000 Å and about 2000 Å. About The top surface of the dummy gate 303 may have a non-flat top surface, and may be flattened before patterning or gate etching of the dummy gate 303. At this time, ions may be introduced into the dummy gate 303, or ions may not be introduced into the dummy gate 303. For example, ions may be introduced by ion implantation technology.
[0088] After forming the dummy gate 303, the dummy gate dielectric 211 and the dummy gate 303 may be patterned. In one embodiment of the present disclosure, the patterning may be performed by initially forming a first hard mask 305 over the dummy gate 303 and a second hard mask 307 over the first hard mask 305.
[0089] According to some embodiments, the first hard mask 305 includes a dielectric material such as silicon nitride (SiN), oxide (OX), silicon oxide (SiO), titanium nitride (TiN), silicon oxynitride (SiON), a combination of these materials, or the like. The first hard mask 305 may be formed using processes such as chemical vapor deposition, plasma enhanced chemical vapor deposition, atomic layer deposition, or the like. However, any other suitable materials and formation methods may be used. The first hard mask 305 may be formed to be between about About Between (e.g. about ) thickness.
[0090] The second hard mask 307 includes a dielectric material that is separate from the material of the first hard mask 305. The second hard mask 307 may include any material and use any process suitable for forming the first hard mask 305, and may be formed to the same or similar thickness as the first hard mask 305. In an embodiment where the first hard mask 305 includes silicon nitride (SiN), the second hard mask 307 may be, for example, oxide (OX). However, any suitable dielectric material, process, and thickness may be used to form the second hard mask 307.
[0091] After forming the first hard mask 305 and the second hard mask 307, the first hard mask 305 and the second hard mask 307 may be patterned. The patterning of the first hard mask 305 and the second hard mask 307 is performed in the X dimension, that is, in and out of the cross-sectional view. Figures 3 to 12 Thereafter, various processes may be performed to form the desired structure, etch the dummy gate material to form different dummy gate stacks, form spacers, etch openings for source / drain regions, epitaxially grow source / drain regions, implant processes, and other typical gate processing.
[0092] Cross Reference Figure 1 and Figure 5, the method 10 may continue to remove the first hard mask 305 and the second hard mask 307 in step S13. According to some embodiments, one or more etching processes and / or chemical mechanical planarization may be used to remove the first hard mask 305 and the second hard mask 307. Therefore, after removing the first hard mask 305, the dummy gate 303 is exposed.
[0093] Cross Reference Figure 1 and Figure 6 The method 10 may continue to remove the dummy gate 303 and the dummy gate dielectric 211 in step S14 . Figure 6 A line release process for forming nanostructures 701 (ie, vertically spaced nanosheets) from the second layer 207 is further described according to some embodiments. Figure 6 According to some embodiments, a gate dielectric 703 is further formed over the nanostructure 701 .
[0094] After exposure by removing the first hard mask 305, the dummy gate 303 can be removed to expose the underlying dummy gate dielectric 211. In one embodiment of the present disclosure, the dummy gate 303 is removed using, for example, one or more wet etching processes or dry etching processes that use an etchant that is selective to the material of the dummy gate 303. However, any suitable removal process may be used.
[0095] After the dummy gate dielectric 211 has been exposed by removing the dummy gate 303, the dummy gate dielectric 211 may be removed. In an embodiment, the dummy gate dielectric 211 may be removed using, for example, a wet etching process, however, any suitable etching process may be used.
[0096] After removing the dummy gate dielectric 211 (which also exposes the side of the first layer 205), the first layer 205 can be removed from the substrate 201 and from between the second layer 207 in a line release process step. The line release process step may also be referred to as a sheet release process step, a sheet formation process step, a nanosheet formation process step, or a line formation process step. In one embodiment of the present disclosure, the first layer 205 can be removed using a wet etching process that selectively removes the material of the first layer 205 (e.g., SiGe) without significantly removing the material of the substrate 201 and the material of the second layer 207 (e.g., Si). However, any suitable removal process may be used.
[0097] For example, in one embodiment of the present disclosure, an etchant such as high temperature HCl may be used to selectively remove the material of the first layer 205 (e.g., SiGe) without substantially removing the material of the substrate 201 and / or the material of the second layer 207 (e.g., Si). In addition, the wet etching process may be performed at a temperature between about 400° C. and about 600° C. (e.g., about 560° C.) for a time between about 100 seconds and about 600 seconds (e.g., about 300 seconds). However, any suitable etchant, process parameters, and time may be used.
[0098] By removing the material of the first layer 205, the second layer 207 ( Figure 6 10 ) are exposed. According to some embodiments, the nanostructures 701 are vertically separated or spaced apart from each other by a spacing between about 5 nanometers and about 15 nanometers, such as about 10 nanometers. The nanostructure 701 includes a channel region between opposing source / drain regions in the source / drain region and has a channel length (in the X direction into and out of the drawing) between about 5 nanometers and about 180 nanometers, such as about 10 nanometers, and a channel width CW1 in the Y direction between about 8 nanometers and about 100 nanometers, such as about 30 nanometers. In one embodiment of the present disclosure, the nanostructure 701 is formed to have the same thickness as the original thickness of the second layer 207, such as between about 3 nanometers and about 15 nanometers, such as about 8 nanometers, but the thickness can also be reduced using an etching process.
[0099] In some embodiments, the line release step may include a selective step of partially removing the material of the second layer 207 (e.g., by overetching) during the removal of the first layer 205. As a result, the thickness of the nanostructure 701 is formed to have a reduced thickness compared to the original thickness of the second layer 207. Therefore, the thickness of the nanostructure 701 may be less than the thickness of the original second layer 207.
[0100] although Figure 6 The formation of three of the nanostructures 701 is described, but any suitable number of nanostructures 701 may be formed by the nanosheets disposed in the multilayer stack 203. For example, the multilayer stack 203 may be formed to include any suitable number of first layers 205 and any suitable number of second layers 207. Therefore, after removing the first layer 205, the multilayer stack 203 including fewer first layers 205 and fewer second layers 207 forms one or two of the nanostructures 701. However, after removing the first layer 205, the multilayer stack 203 including many first layers 205 and many second layers 207 forms four or more nanostructures 701.
[0101] Figure 6According to some embodiments, a gate dielectric 703 is further described as being formed over the nanostructure 701. In one embodiment of the present disclosure, the gate dielectric 703 comprises a high dielectric constant material (e.g., a dielectric constant greater than or equal to 9) deposited by a process such as atomic layer deposition, chemical vapor deposition, or the like, such as Ta2O5, Al2O3, Hf oxide, Ta oxide, Ti oxide, Zr oxide, Al oxide, La oxide (e.g., HfO2, HfSiO, HfSiON, HfTaO, HfTiO, HfZrO, LaO, ZrO, TiO), combinations of these materials, or the like. In some embodiments, the gate dielectric 703 comprises a nitrogen-doped oxide dielectric that is initially formed prior to forming a dielectric material having a metal content high dielectric constant (e.g., a dielectric constant greater than 13). The gate dielectric 703 may be deposited to a thickness between about 1 nanometer and about 3 nanometers, however, any suitable material and thickness may be used. In an exemplary embodiment, gate dielectric 703 surrounds nanostructure 701 to form a channel region between source / drain regions.
[0102] Cross Reference Figure 1 and Figure 7 , the method 10 may continue to form a metal gate over the fin 105 in step S15. For example, according to some embodiments, the method 10 includes forming a gate 107 and a gate cap 801. After forming the gate dielectric 703, the gate 107 is formed around the nanostructure 701. For example, the inter-sheet portion of the metal gate is located between the nanostructures 701.
[0103] In some embodiments, multiple layers are used to form the gate 107, each layer being sequentially deposited adjacent to each other using a highly conformal deposition process such as atomic layer deposition, however, any suitable deposition process may be used. According to some embodiments, the gate 107 may include a capping layer, a barrier layer, an n-type metal work function layer, a p-type metal work function layer, and a fill material.
[0104] The capping layer may be formed adjacent to the gate dielectric 703 and may be formed of a metallic material such as TaN, Ti, TiAlN, TiAl, Pt, TaC, TaCN, TaSiN, Mn, Zr, TiN, Ru, Mo, WN, other metal oxides, metal nitrides, metal silicates, transition metal oxides, transition metal nitrides, transition metal silicates, metal oxynitrides, metal aluminates, zirconium silicate, zirconium aluminate, combinations of these materials, or the like. The metallic material may be deposited using a deposition process such as atomic layer deposition, chemical vapor deposition, or the like, however, any suitable deposition process may be used.
[0105] The barrier layer may be formed adjacent to the capping layer and may be formed of a different material than the capping layer. For example, the barrier layer may be formed of one or more layers of a metallic material such as TiN, TaN, Ti, TiAlN, TiAl, Pt, TaC, TaCN, TaSiN, Mn, Zr, Ru, Mo, WN, other metal oxides, metal nitrides, metal silicates, transition metal oxides, transition metal nitrides, transition metal silicates, metal oxynitrides, metal aluminates, zirconium silicate, zirconium aluminate, combinations of these materials, or the like. The barrier layer may be deposited using a deposition process such as atomic layer deposition, chemical vapor deposition, or the like, however, any suitable deposition process may be used.
[0106] The n-type metal work function layer may be formed adjacent to the barrier layer. In one embodiment of the present disclosure, the n-type metal work function layer may be, for example, W, Cu, AlCu, TiAlC, TiAlN, TiAl, Pt, Ti, TiN, Ta, TaN, Co, Ni, Ag, Al, TaAl, TaAlC, TaC, TaCN, TaSiN, Mn, Zr, other suitable n-type work function materials, or combinations thereof. For example, the first n-type metal work function layer may be deposited using an atomic layer deposition (ALD) process, a chemical vapor deposition process, or the like. However, any suitable material and process may be used to form the n-type metal work function layer.
[0107] The p-type metal work function layer may be formed adjacent to the n-type metal work function layer. In one embodiment of the present disclosure, the first p-type metal work function layer may be formed of a metal material, such as W, Al, Cu, TiN, Ti, TiAlN, TiAl, Pt, Ta, TaN, Co, Ni, TaC, TaCN, TaSiN, TaSi2, NiSi2, Mn, Zr, ZrSi2, TaN, Ru, AlCu, Mo, MoSi2, WN, other metal oxides, metal nitrides, metal silicates, transition metal oxides, transition metal nitrides, transition metal silicates, metal oxynitrides, metal aluminates, zirconium silicate, zirconium aluminate, combinations of these materials, or the like. In addition, the p-type metal work function layer may be deposited using a deposition process such as atomic layer deposition, chemical vapor deposition, or the like, however, any suitable deposition process may be used.
[0108] After forming the p-type metal work function layer, a filling material is deposited to fill the remaining portion of the opening. In one embodiment of the present disclosure, the filling material may be, for example, tungsten, Al, Cu, AlCu, W, Ti, TiAlN, TiAl, Pt, TaC, TaCN, TaSiN, Mn, Zr, TiN, Ta, TaN, Co, Ni, a combination of these materials, or the like, and may be formed using a deposition process such as electroplating, chemical vapor deposition, atomic layer deposition, physical vapor deposition, a combination of these processes, or the like. However, any suitable material may be used.
[0109] After filling the opening left by removing the dummy gate 303, the material of the gate 107 and the gate dielectric 703 can be planarized to remove any material except for this opening. In certain embodiments, a planarization process such as chemical mechanical polishing can be used for removal, however, any suitable planarization and removal process can be used. According to some embodiments, the gate can be formed to a length between about 8 nanometers and about 30 nanometers. However, any suitable length can be used.
[0110] After the gate 107 is formed, the gate 107 may be recessed. According to some embodiments, an etching process such as wet etching, dry etching, a combination of the above, or the like may be used to recess the gate 107. After the gate 107 is recessed, the gate 107 located above the top nanostructure in the nanostructure 701 has a height H5 between about 8 nanometers and about 30 nanometers. However, any suitable height may be used.
[0111] The gate cap 801 may be formed by initially depositing a dielectric material over the gate 107 to fill and / or overfill the recess. In some embodiments, the gate cap 801 may be formed using a dielectric material such as silicon nitride (SiN), oxide (OX), silicon oxynitride (SiON), silicon oxycarbonitride (SiOCN), silicon carbonitride (SiCN), or the like. According to some embodiments, the gate cap 801 may be formed using a metal oxide such as zirconium (Zr), hafnium (Hf), aluminum (Al), or the like. In addition, the gate cap 801 may be formed using a suitable deposition process such as chemical vapor deposition, atomic layer deposition, physical vapor deposition (PVD), a combination of such processes, or the like. However, any suitable material and deposition process may be used. After deposition, the gate cap 801 may be planarized using a planarization process such as a chemical mechanical polishing process. After the gate cap 801 is planarized, the gate cap 801 has a height H6 between about 10 nanometers and about 30 nanometers. However, any suitable height may be used.
[0112] Cross Reference Figure 1 and Figure 8 According to some embodiments, the method 10 may continue to form an opening 901 in the cut metal gate process in step S16. After the gate cap 801 is planarized, a mask layer 903 may be deposited over the planar surface of the gate cap 801. After the mask layer 903 is deposited, the mask layer 903 is patterned to expose the underlying material including the gate cap 801 at the desired location of the cut metal gate structure 109 to be formed.
[0113] After the mask layer 903 is patterned, the mask layer 903 is used as an etching mask to etch the underlying material to form an opening 901 (e.g., a trench, recess, channel, or the like). In the etching process, an anisotropic etching process is used to etch the material of the gate cap 801 and the gate 107. In an exemplary embodiment, the etching process continues through the gate dielectric 703 and into the isolation region 209. The opening 901 may be formed between adjacent fins 105 and may be formed to cut through one or more gates 107. According to some embodiments, two openings 901 are formed to cut through two adjacent gates 107 and are located on opposite sides of one of the fins 105 (e.g., a selected fin 106), such as Figure 1 After the opening 901 is formed, the mask layer 903 is removed.
[0114] Cross Reference Figure 1 and Fig. 9 According to some embodiments, the method 10 may continue to form a cut metal gate structure 109 in step S17. After the opening 901 is formed, the cut metal gate structure 109 is formed by initially depositing a dielectric material to fill and overfill the opening 901. According to some embodiments, the cut metal gate structure 109 is formed using any dielectric material and deposition process suitable for forming the gate cap 801. In some embodiments, the dielectric material used to form the cut metal gate structure 109 is the same as the dielectric material used to form the gate cap 801, however, the dielectric material may also be different. For example, in an embodiment where silicon nitride (SiN) is used to form the gate cap 801, the cut metal gate structure 109 may also be formed using silicon nitride (SiN) in a deposition process such as atomic layer deposition. However, any suitable dielectric material and deposition process may be used. For example, the cut metal gate structure 109 may be formed as a silicon nitride (SiN) layer and a silicon (Si) layer. According to some embodiments, the cut metal gate structure 109 is formed to have a width W3 between about 5 nanometers and about 50 nanometers, such as about 10 nanometers. However, any suitable width may be used.
[0115] The cut metal gate structure 109 divides the two relatively long gates 107 into a plurality of relatively short segmented gates 107 and isolates the segmented gates 107 from each other. In addition, the excess dielectric material of the cut metal gate structure 109 outside the opening 901 can be retained and used as a mask layer in the continuous poly on diffusion edge (CPODE) process.
[0116] Cross Reference Figure 1 and Figure 10 to Figure 11 According to some embodiments, method 10 may continue with the initial step of forming a continuous poly on diffusion edge (CPODE) structure 111. CPODE structure 111 may also be referred to as an isolation structure, a cut poly structure, or a cut-PODE structure in the present disclosure, and is similar to the following Figure 1 It should be noted that the gate cap 801 is shown as being combined with the cut metal gate structure 109 because both can be considered as hard masks. In step S18, the method 10 performs Fig.10 and Fig.11 The mask 1200 is patterned over a portion of the semiconductor device 100 .
[0117] As shown, mask 1200 may include multiple layers such as a bottom layer 1201, a middle layer 1202, and a top layer 1203. In some embodiments, bottom layer 1201 is a carbon-based layer. In some embodiments, middle layer 1202 is an oxide-based layer. In some embodiments, top layer 1203 is a photosensitive mask (e.g., photoresist).
[0118] As shown, the photoresist is patterned to include a slit 1205 aligned with a portion of the selected fin 106 for removal.
[0119] Cross Reference Figure 1 and Figure 12 to Figure 13 According to some embodiments, the method 10 may continue to the next step of forming a continuous poly on diffusion edge (CPODE) structure 111. Specifically, in step S19, the method 10 etches and cuts the metal gate structure 109 (or hard mask) through the gap 1205 to form an opening 1091. Thereafter, the mask 1200 may be removed.
[0120] Cross Reference Figure 1 and Figure 14 to Figure 15, the method 10 may continue in step S20 to form a void or opening 1003 over the portion of the selected fin 106 for removal. In an exemplary embodiment, forming the opening 1003 includes selectively removing the section of the metal gate 107 located over the selected fin 106. For example, the process may remove all of the metal gate 107 between the cut metal gate structures 109.
[0121] According to some embodiments, the etching process may terminate at the gate dielectric 703. Thus, the gate dielectric 703 and the nanostructures 701 remain at the bottom of the opening 1003. According to some embodiments, the etching process used to form the opening 1003 may be an isotropic etching process (e.g., a wet etching process) using an etchant that terminates at the gate dielectric 703. However, other suitable etching processes may also be used, including an anisotropic etching process (e.g., a dry etching process or a reactive ion etching (RIE) process), a combination of isotropic and anisotropic etching, or the like.
[0122] After the opening 1003 is formed to expose the gate dielectric 703, another etching process is performed to remove the material of the gate dielectric 703 in the opening 1003 and expose the nanostructure 701, the fin 106 and the isolation region 209 in the opening 1003. According to some embodiments, wet etching, dry etching, a combination thereof or the like may be used to remove the material of the gate dielectric 703. However, any suitable etching process may be used.
[0123] Cross Reference Figure 1 and Figure 16 to Figure 17 , the method 10 may continue with the intermediate steps of the CPODE process in step S19, including removing the nanostructure 701 and recessing the selected fin 106 to form a trench 1103. Specifically, after exposing the nanostructure 701 and a portion of the fin 106 protruding above the isolation region 209, a further etching process may be used to remove the material of the nanostructure 701 and recess the fin 106. In an exemplary embodiment, the fin 106 is removed and a portion of the underlying substrate 201 is etched. As a result, the upper surface of the substrate 201 is recessed into a recessed surface 202. In an exemplary embodiment, the etching process is a plasma etch as described below.
[0124] Cross Reference Figure 1 and Figure 18 to Figure 19, the method 10 may continue in step S22 to complete the CPODE process by forming a CPODE structure 111. For example, an insulator material or a dielectric material may be deposited to fill and / or overfill the trench 1103. The CPODE structure 111 or the insulating region may be formed using a dielectric material such as silicon nitride (SiN), oxide (OX), silicon oxynitride (SiON), silicon oxycarbonitride (SiOCN), silicon carbonitride (SiCN), or the like. According to some embodiments, the CPODE structure 111 may be formed using a metal oxide such as zirconium (Zr), hafnium (Hf), aluminum (Al), or the like. In addition, the CPODE structure 111 may be formed using a suitable deposition process such as chemical vapor deposition, atomic layer deposition, physical vapor deposition, a combination of these processes, or the like. The CPODE structure 111 may be formed using any dielectric material and process suitable for forming the cut metal gate structure 109. According to some embodiments, the dielectric material used to form the CPODE structure 111 is the same as the dielectric material used to form the cut metal gate structure 109, however, the dielectric material may be different. For example, in an embodiment where silicon nitride (SiN) is used to form the cut metal gate structure 109, the CPODE structure 111 may be formed using silicon nitride (SiN) via a deposition process such as chemical vapor deposition, atomic layer deposition, sputtering, or the like.
[0125] After the dielectric material of the CPODE structure 111 is deposited, excess dielectric material outside the opening 1003 may be removed by a chemical mechanical planarization process. According to some embodiments, the chemical mechanical planarization process may be continued to planarize the surface of the CPODE structure 111 having the gate 107. After the surface of the CPODE structure 111 is planarized, the CPODE structure 111 located above the fin 105 has a height between about 55 nanometers and about 140 nanometers (e.g., about 70 nanometers). However, any suitable height may be used. The gate cap 801 has a height between about 10 nanometers and about 30 nanometers (e.g., about 15 nanometers). However, any suitable height may be used. In addition, the cut metal gate structure 109 has a height between about 50 nanometers and about 120 nanometers (e.g., about 60 nanometers). However, any suitable height may be used.
[0126] like Figure 1 As shown in , method 10 may continue in step S23 to complete further processing of semiconductor device 100. For example, according to some embodiments, further processing may include: forming interlayer dielectric and metallization layers; forming source / drain contacts with source / drain regions; and forming source / drain vias and gate vias.
[0127] Reference Figure 20 to Figure 22 and Figure 23 to Figure 25, the plasma etching process of step S21 is described in more detail.
[0128] Fig. 20 The metal gate structure 109 that is not cut in the isolation region 1001 (for example, Fig.14 1001). In the isolation region 1001, the fin 105 may be spaced a minimum distance of 500 nanometers from another fin in the Y direction, such as 1000 nanometers (1 micrometer) or 10,000 nanometers (10 micrometers). In other words, the spacing or interval may be at least 500 nanometers, at least 1000 nanometers, or at least 10,000 nanometers. Fig. 20 As shown, the opening 1003 cut in the metal gate structure 109 around the selected portion of the fin 105 has a length l1 in the X direction. In some embodiments, the length l1 is greater than or equal to 1000 nanometers (1 micrometer). In addition, the isolation region 1001 has a length l in the X direction and a width w in the Y direction.
[0129] Fig.21 The etching operation of the passivation orientation in the isolation region 1001 is described. The etching operation of the passivation orientation etches the trench 1103 to a vertical depth d1. Fig.21 As shown, the passivation-oriented etching operation forms a byproduct 2101 on the cut metal gate structure 109 and in the trench 1103. For example, the byproduct 2101 can be a polymer film.
[0130] For a passivation-oriented etching operation in the isolation region 1001, the total reaction area A1 is equal to the width w times the length l plus the vertical depth d1 times twice the length l1:
[0131] A1≈(w×l)+2(d1×l1).
[0132] It can be seen that in isolation regions such as isolation region 1001 , the passivation oriented etching operation forms trenches 1103 having a relatively shallow vertical depth d1 .
[0133] Fig. 22 The etching operation of the etchant orientation in the isolation region 1001 is described. The etching operation of the etchant orientation etches the trench 1103 to a vertical depth D1. Fig. 22 As shown, the passivation-oriented etching operation forms a byproduct 2201 on the cut metal gate structure 109 and in the trench 1103. For example, the byproduct 2201 can be a polymer film.
[0134] It can be seen that in isolation regions such as isolation region 1001, the etching operation oriented by the etchant forms trenches 1103 having a relatively deep vertical depth D1. Fig.21 and Fig. 22, it can be seen that the vertical depth D1 is greater than the vertical depth d1.
[0135] Fig.23 The metal gate structure 109 that is not cut in the dense area 1002 (for example, Fig.14 1002 ). In the dense region 1002 , the fins 105 may be spaced apart from one another in the Y direction by a maximum distance of 100 nanometers, such as 60 nanometers or 50 nanometers. For example, the spacing or pitch may be no more than 100 nanometers, such as no more than 60 nanometers or no more than 50 nanometers. Fig. 20 As shown, each opening 1003 cut in the metal gate structure 109 around a respective selected portion of the fin 105 has a length l2 in the X direction. In some embodiments, the length l2 is greater than or equal to 1000 nanometers (1 micrometer). In addition, the isolation region 1001 has a length l in the X direction and a width w in the Y direction.
[0136] Fig.24 The etching operation of the passivation orientation in the dense area 1002 is illustrated. The etching operation of the passivation orientation etches the trench 1103 to a vertical depth d2. Fig.24 As shown, the passivation-oriented etching operation forms a byproduct 2101 on the cut metal gate structure 109 and in the trench 1103. For example, the byproduct 2101 can be a polymer film.
[0137] For a passivation-oriented etch operation in the dense region 1002, the total reaction area A2 is equal to the width w times the length l plus n times the vertical depth d2 times twice the length l2, where n is the number of fins in the dense region:
[0138] A2≈(w×l)+n×2(d2×l2).
[0139] It can be seen that in dense regions such as dense region 1002, the passivation oriented etching operation forms trenches 1103 having a relatively deep vertical etch depth d2.
[0140] Fig.25 The etching operation of the etchant orientation in the dense area 1002 is illustrated. The etching operation of the etchant orientation etches the trench 1103 to a vertical depth D2. Fig.25 As shown, the passivation-oriented etching operation forms a byproduct 2201 on the cut metal gate structure 109 and in the trench 1103. For example, the byproduct 2201 can be a polymer film.
[0141] It can be seen that in dense areas such as dense area 1002, the etching operation oriented by the etchant forms trenches 1103 having a relatively shallow vertical etching depth D2. Fig.24 and Fig.25, it can be seen that the vertical depth D2 is smaller than the vertical depth d2.
[0142] Therefore, the passivation-oriented etching operation forms a trench 1103 having a relatively deep vertical etching depth d2 in the dense region 1002 and a trench 1103 having a relatively shallow vertical etching depth d1 in the isolation region 1001, while the etchant-oriented etching operation forms a trench 1103 having a relatively shallow vertical etching depth D2 in the dense region 1002 and a trench 1103 having a relatively deep vertical etching depth D1 in the isolation region 1001. In addition, since the generated reaction areas A1 and A2 are larger, this phenomenon is more prominent in the case of longer patterns (longer lengths l1 and l2). In addition, this phenomenon is more prominent when the difference in the lateral spacing between the isolation region 1001 and the dense region 1002 is larger.
[0143] As used herein, a passivation-oriented etch operation refers to an etch operation in which the etch rate is limited and / or primarily determined by the passivation effect, while an etchant-oriented etch operation refers to an etch operation in which the etch rate is not limited by the passivation effect.
[0144] In the etching operation of the passivation orientation, a large amount of polymer and byproduct 2201 are generated to passivate the sidewalls of the trench 1103. In some embodiments, the byproduct 2201 is positive, and the etching operation can still etch the semiconductor material. In some embodiments, the byproduct 2201 is negative, so that the etching of the semiconductor material is stopped by the byproduct 2201.
[0145] The etching rate (ER) can be defined by the following formula:
[0146]
[0147] where S is the adhesion coefficient, Y is the yield, and Γ is the flux.
[0148] In addition, the desorption rate of the byproduct 2201 can affect the etching rate. The following table presents the boiling points (BP) of the byproduct 2201 of selected etchants at 1 atmosphere pressure.
[0149]
[0150]
[0151] As shown in Table 1, the byproduct desorption rate of SiF4 is greater than that of SiCl4, which is greater than that of SiBr4. Therefore, HBr-based etching operations result in severe accumulation of byproduct 2201, leading to a passivation-oriented process. On the other hand, Cl / F-based etching operations result in rapid removal of byproduct 2201 via desorption, leading to an etchant-oriented process. It should be noted that the pressure in the etching chamber can be much lower than 1 atmosphere; however, it is expected that the trend of the byproduct desorption rate will remain unchanged.
[0152] In one embodiment of the present disclosure, the passivation-oriented etching operation is performed using a hydrogen bromide (HBr) etchant, and the etchant-oriented etching operation is performed using a chlorine-based etchant or a fluorine-based etchant.
[0153] Reference Fig.26 A flow chart of method 90 is provided. Method 90 includes, in step S91, determining a desired first depth of a first trench to be etched in a dense region of a substrate and a desired second depth of a second trench to be etched in an isolation region.
[0154] Furthermore, the method 90 may include determining a desired length of the trench 1103 to be formed in step S92 .
[0155] In step S93 , the method 90 includes determining the spacing of the densely populated areas and the spacing of the isolated areas.
[0156] In step S94 , method 90 may include determining widths and lengths of dense regions and isolated regions.
[0157] In view of the desired trench depth, the desired trench length, the spacing between the dense area and the isolation area, and the width and length of the dense area and the isolation area, the method 90 may include designing a plasma dry etching process in step S95 to form a first trench having a first depth and a second trench having a second depth, wherein the plasma dry etching process includes a first plasma dry etching operation and a second plasma dry etching operation, wherein the first plasma dry etching operation has a first dense etching rate in the dense area and a first isolation etching rate in the isolation area, and wherein the second plasma dry etching operation has a second dense etching rate in the dense area and a second isolation etching rate in the isolation area. The design of the plasma dry etching process may include setting the duration of each first plasma dry etching operation and each second plasma dry etching operation; setting the number of cycles of the first plasma dry etching operation and the second plasma dry etching operation; and / or setting the conditions of each repetition of the first plasma dry etching operation and the conditions of each repetition of the second plasma dry etching operation.
[0158] In S96, method 90 includes performing a plasma etching process to form a first trench having a first depth and a second trench having a second depth. For example, although different results are obtained through certain operations on the dense area and the isolated area, the wafer including the dense area and the isolated area can be processed using the same plasma etching process to form appropriate trenches 1103 in the dense area and the isolated area.
[0159] Performing the plasma etching process may include controlling the process as designed in step S95 .
[0160] Fig. 27 Further description is given of various sizes of the trench 1103 in which the CPODE structure 111 may be formed. Fig. 27 As shown, the trench 1103 is formed so that the inner spacer 505 remains between the trench 1103 and the epitaxial source / drain region 503. Therefore, damage to the epitaxial source / drain region 503 can be avoided. In other words, the critical dimension or lateral width of the trench 1103 is carefully controlled to avoid damage to the epitaxial source / drain region 503. Fig. 27 , a lateral width Wa is defined at the uppermost nanosheet, a lateral width Wb is defined at the second nanosheet, and a lateral width Wc is defined at the lowermost nanosheet. In addition, trench 1103 is formed to a depth Da measured from the top of the uppermost nanosheet.
[0161] In the dense region, the trench 1103 is formed by an etchant-directed etching operation with an average uppermost nanosheet lateral width Wa of 16.3 nanometers, a maximum uppermost nanosheet lateral width Wa of 17.9 nanometers, and a minimum uppermost nanosheet lateral width Wa of 14.4 nanometers. In the dense region, the trench 1103 is formed by an etchant-directed etching operation with an average second nanosheet lateral width Wb of 15.3 nanometers, a maximum second nanosheet lateral width Wb of 17.3 nanometers, and a minimum second nanosheet lateral width Wb of 13.9 nanometers. In the dense region, the trench 1103 is formed by an etchant-directed etching operation with an average lowermost nanosheet lateral width Wc of 15.5 nanometers, a maximum lowermost nanosheet lateral width Wc of 17.6 nanometers, and a minimum lowermost nanosheet lateral width Wc of 13.4 nanometers. In the dense region, the trench 1103 is formed by an etchant-oriented etching operation with an average depth Da of 147.6 nanometers, a maximum depth Da of 154.8 nanometers, and a minimum depth Da of 140.0 nanometers.
[0162] In the isolation region, trench 1103 is formed by an etchant-oriented etching operation with an average uppermost nanosheet lateral width Wa of 18.4 nanometers, an average second nanosheet lateral width Wb of 14.6 nanometers, an average lowermost nanosheet lateral width Wc of 14.9 nanometers, and an average depth Da of 178.9 nanometers.
[0163] In the dense region, the trench 1103 was formed by a passivation-oriented etching operation with an average uppermost nanosheet lateral width Wa of 17.3 nanometers, a maximum uppermost nanosheet lateral width Wa of 19.6 nanometers, and a minimum uppermost nanosheet lateral width Wa of 16.2 nanometers. In the dense region, the trench 1103 was formed by a passivation-oriented etching operation with an average second nanosheet lateral width Wb of 17.2 nanometers, a maximum second nanosheet lateral width Wb of 18.9 nanometers, and a minimum second nanosheet lateral width Wb of 15.3 nanometers. In the dense region, the trench 1103 was formed by a passivation-oriented etching operation with an average lowermost nanosheet lateral width Wc of 22.3 nanometers, a maximum lowermost nanosheet lateral width Wc of 25.8 nanometers, and a minimum lowermost nanosheet lateral width Wc of 18.3 nanometers. In the dense region, trenches 1103 are formed by a passivation-oriented etching operation with an average depth Da of 136.0 nanometers, a maximum depth Da of 154.9 nanometers, and a minimum depth Da of 99.4 nanometers.
[0164] In the isolation region, trench 1103 is formed by a passivation-oriented etching operation with an average uppermost nanosheet lateral width Wa of 20.8 nanometers, an average second nanosheet lateral width Wb of 19.0 nanometers, an average lowermost nanosheet lateral width Wc of 19.0 nanometers, and an average depth Da of 114.3 nanometers.
[0165] In one embodiment, a method for manufacturing a semiconductor device 100 is provided, comprising the following steps: forming a plurality of fins in a dense area and an isolation area of a semiconductor substrate; performing a plasma etching process to remove a portion of at least one selected fin in the dense area, thereby forming a first trench in the dense area, and removing a portion of at least one selected fin in the isolation area, thereby forming a second trench in the isolation area, wherein the plasma etching process comprises the following steps: performing a passivation orientation process and an etchant orientation process; and controlling the passivation orientation process and the etchant orientation process to form the first trench having a first critical dimension and a first depth, and forming the second trench having a second critical dimension and a second depth.
[0166] In some embodiments of the method, the passivation-oriented process etches using a bromide-based etchant; and the etchant-oriented process etches using a chloride-based etchant or a fluoride-based etchant.
[0167] In some embodiments of the method, the passivation oriented process etches using a hydrogen bromide etchant; and the etchant oriented process etches using a carbon fluoride etchant, a silicon fluoride etchant, a chloride etchant, or a boron chloride etchant.
[0168] In some embodiments of this method, the passivation oriented process forms a silicon bromide polymer; and the etchant oriented process forms a fluoride polymer, a chloride polymer, or a boride polymer.
[0169] In some embodiments of the method, the passivation-oriented process forms a first byproduct having a first boiling point; the etchant-oriented process forms a second byproduct having a second boiling point; and the first boiling point is higher than the second boiling point.
[0170] In some embodiments of the method, the passivation-oriented process forms a first byproduct having a first boiling point; the etchant-oriented process forms a second byproduct having a second boiling point; and the first boiling point is higher than twice the second boiling point.
[0171] In some embodiments of the method, the passivation oriented process forms byproducts 2201 on the selected fins at a first rate; the etchant oriented process forms byproducts 2201 on the selected fins at a second rate; and the first rate is greater than the second rate.
[0172] In some embodiments of the method, the process of controlling the orientation of the passivation and the process of controlling the orientation of the etchant are performed such that the first depth is greater than the second depth.
[0173] In some embodiments of the method, the process of controlling the orientation of the passivation and the process of controlling the orientation of the etchant are performed such that the first depth is less than the second depth.
[0174] In some embodiments of the method, a process for controlling the orientation of the passivation agent and a process for controlling the orientation of the etchant agent are performed such that the first critical dimension is greater than the second critical dimension.
[0175] In some embodiments of the method, a process for controlling the orientation of the passivation agent and a process for controlling the orientation of the etchant agent are performed such that the first critical dimension is smaller than the second critical dimension.
[0176] In another embodiment, a method is provided, comprising the following steps: determining a first depth of a first trench etched in a dense area of a substrate and a second depth of a second trench etched in an isolated area of the substrate; designing a plasma dry etching process to form a first trench having a first depth and a second trench having a second depth, wherein the plasma dry etching process includes a first plasma dry etching operation and a second plasma dry etching operation, wherein the first plasma dry etching operation has a first dense etching rate in multiple dense areas and a first isolation etching rate in multiple isolated areas, and wherein the second plasma dry etching operation has a second dense etching rate in the dense areas and a second isolation etching rate in the isolated areas; and performing a plasma dry etching process to form a first trench having a first depth and a second trench having a second depth.
[0177] In some embodiments of the method, the first plasma dry etching operation forms a first byproduct having a first boiling point; the second plasma dry etching operation forms a second byproduct having a second boiling point; and the first boiling point is higher than the second boiling point.
[0178] In some embodiments of the method, the first depth is greater than the second depth.
[0179] In some embodiments of the method, the first depth is less than the second depth.
[0180] In some embodiments of the method, the first plasma dry etching operation is a passivation oriented process; and the second plasma dry etching operation is an etchant oriented process.
[0181] In another embodiment, a method for etching a semiconductor material is provided, comprising the following steps: performing a first plasma dry etching operation with a passivation orientation; performing a second plasma dry etching operation with an etchant orientation; and repeating the first plasma dry etching operation and the second plasma dry etching operation to form a trench 1103 in the semiconductor material having a depth.
[0182] In some embodiments of the method, the first plasma dry etching operation in the passivation orientation uses a bromide-based etchant for etching; and the second plasma dry etching operation in the etchant orientation uses a chloride-based etchant or a fluoride-based etchant for etching.
[0183] In some embodiments of the method, the first plasma dry etch operation in the passivation orientation forms a silicon bromide polymer; and the second plasma dry etch operation in the etchant orientation forms a fluoride polymer, a chloride polymer, or a boride polymer.
[0184] In some embodiments of the method, the first plasma dry etching operation in the passivation orientation forms first byproducts having a first boiling point; the second plasma dry etching operation in the etchant orientation forms second byproducts having a second boiling point; and the first boiling point is higher than the second boiling point.
[0185] The foregoing summarizes the features of several embodiments so that those skilled in the art can better understand the various aspects of the present disclosure. Those skilled in the art should understand that they can easily use the present disclosure as a basis for designing or modifying other processes and structures for achieving the same purposes and / or achieving the same advantages of the embodiments introduced herein. Those skilled in the art should also recognize that such equivalent constructions do not depart from the spirit and scope of the present disclosure, and various changes, substitutions and modifications can be made herein without departing from the spirit and scope of the present disclosure.
Claims
1. A method for manufacturing a semiconductor device, It is characterized in that The following steps are involved: forming a plurality of fins in a dense region and an isolation region of a semiconductor substrate; A plasma etching process is performed to remove a portion of the at least one selected fin in the dense area to form a first trench in the dense area, and to remove a portion of the at least one selected fin in the isolated area to form a second trench in the isolated area, wherein the plasma etching process comprises the following steps: Performing a passivation orientation process and an etchant orientation process; as well as The passivation orientation process and the etchant orientation process are controlled to form the first trench having a first critical dimension and a first depth, and to form the second trench having a second critical dimension and a second depth.
2. The method according to claim 1, It is characterized in that in: The passivation alignment process forms a first byproduct having a first boiling point; The etchant orientation process forms a second byproduct having a second boiling point; as well as The first boiling point is higher than the second boiling point.
3. The method according to claim 1, It is characterized in that in: The passivation orientation process forms a byproduct on the selected fin at a first rate; The etchant orientation process forms a byproduct on the selected fin at a second rate; as well as The first rate is greater than the second rate.
4. The method according to claim 1, It is characterized in that The first depth is made greater than the second depth by controlling the passivation orientation process and the etchant orientation process.
5. The method according to claim 1, It is characterized in that The first critical dimension is made larger than the second critical dimension by controlling the passivation orientation process and the etchant orientation process.
6. A method for etching a semiconductor device, It is characterized in that The following steps are involved: Determining a first depth of a first trench etched in a dense region of a substrate and a second depth of a second trench etched in an isolated region of the substrate; Designing a plasma dry etching process to form the first trench having the first depth and the second trench having the second depth, wherein the plasma dry etching process includes a first plasma dry etching operation and a second plasma dry etching operation, wherein the first plasma dry etching operation has a first dense etching rate in a plurality of dense regions and a first isolation etching rate in a plurality of isolated regions, and wherein the second plasma dry etching operation has a second dense etching rate in the plurality of dense regions and a second isolation etching rate in the plurality of isolated regions; as well as The plasma dry etching process is performed to form the first trench having the first depth and the second trench having the second depth.
7. The method according to claim 6, It is characterized in that in: The first plasma dry etching operation forms a first byproduct having a first boiling point; The second plasma dry etching operation forms a second byproduct having a second boiling point; and The first boiling point is higher than the second boiling point.
8. The method according to claim 6, It is characterized in that in: The first plasma dry etching operation is a passivation orientation process; and The second plasma dry etching operation is an etchant orientation process.
9. A method for etching a semiconductor material, It is characterized in that The following steps are involved: Performing a first plasma dry etching operation for passivation orientation; Performing a second plasma dry etching operation of etchant orientation; and The first plasma dry etching operation and the second plasma dry etching operation are repeated to form a trench having a depth in the semiconductor material.
10. The method according to claim 9, It is characterized in that in: The first plasma dry etching operation in the passivation orientation forms a first byproduct having a first boiling point; The second plasma dry etching operation of the etchant orientation forms a second byproduct having a second boiling point; as well as The first boiling point is higher than the second boiling point.