Modified solid electrolyte, preparation method thereof, solid-state battery and electric device

By distributing phase change toughener in solid electrolytes, the fragility and dendrite problems of traditional solid electrolytes are solved, the mechanical strength and conductivity of solid battery are improved, and more efficient battery performance is achieved.

CN118899518APending Publication Date: 2024-11-05CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310484801.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-04
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

Traditional solid electrolytes have fragile ceramic properties and are prone to cracking. Especially when they are combined with lithium metal negative electrodes, the formation of dendrites leads to short-circuiting and failure of solid-state batteries, making it difficult to meet the practical application needs.

Method used

Modified solid electrolytes are used to distribute phase change toughening agents in solid electrolyte substrates. The phase change toughening agents are mainly distributed along the grain boundaries and undergo phase change under external forces to improve the mechanical strength and toughness of solid electrolytes and avoid The emergence of internal defects.

Benefits of technology

It improves the toughness and battery efficiency of solid electrolytes, reduces the growth and spread of dendrites, enhances the fracture toughness and ionic conductivity of the electrolytes, and extends the service life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118899518A_ABST
    Figure CN118899518A_ABST
Patent Text Reader

Abstract

The invention relates to a modified solid electrolyte, a preparation method thereof, a solid-state battery and an electric device. The modified solid electrolyte comprises a solid electrolyte base material and a phase change toughening agent distributed in the solid electrolyte base material, in the modified solid electrolyte, the phase change toughening agent is mainly distributed at a grain boundary in the solid electrolyte; the phase change toughening agent can be subjected to phase change under the action of external force.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of battery technology, and in particular to a modified solid electrolyte and a preparation method thereof, a solid-state battery and an electrical device. Background Art

[0002] In recent years, solid-state batteries prepared with solid-state electrolytes have received increasing attention. On the one hand, solid-state batteries can avoid the flammable and explosive problems of liquid batteries due to the presence of organic electrolytes. Solid-state batteries can use metals as negative electrode materials, which can reduce the probability of side reactions occurring at high temperatures. Therefore, safety is considered to be one of the most fundamental driving forces for the development of solid-state batteries. Solid-state electrolytes give solid-state batteries the characteristics of compact structure, adjustable scale, and great design flexibility. They can be used to drive microelectronic devices as well as in the fields of power and energy storage.

[0003] Traditional solid electrolytes often have the fragile characteristics of ceramics, with poor mechanical strength and easy cracking. They are prone to cracking during use, especially when used in combination with lithium metal negative electrodes. Lithium metal will form dendrites at the solid electrolyte interface. The formation of dendrites will cause the solid electrolyte to break and even penetrate the solid electrolyte, causing short circuits and failure of the solid-state battery, making it difficult to meet actual application needs.

[0004] Therefore, the traditional technology still needs to be improved. Summary of the invention

[0005] Based on this, it is necessary to provide a modified solid electrolyte and its preparation method, a solid-state battery and an electrical device, aiming to improve the toughness of the solid-state electrolyte and thereby improve the efficiency of the solid-state battery.

[0006] The present application is implemented through the following technical solutions.

[0007] In a first aspect of the present application, a modified solid electrolyte is provided, wherein the modified solid electrolyte comprises a solid electrolyte substrate and a phase change toughening agent distributed in the solid electrolyte substrate; and in the modified solid electrolyte, the phase change toughening agent is mainly distributed at the grain boundaries in the solid electrolyte;

[0008] The phase change toughening agent can undergo phase change under the action of external force.

[0009] The above-mentioned modified solid electrolyte includes a solid electrolyte substrate and a phase change toughening agent distributed in the solid electrolyte substrate. When subjected to external force, stress will be generated inside the phase change toughening agent accordingly. Under the stimulation of stress, the phase change toughening agent will undergo a phase change. The stress transformation brought about by the phase change process can improve the mechanical strength and toughness of the solid electrolyte substrate. The phase change toughening agent is mainly distributed along the grain boundary area in the modified solid electrolyte. The grain boundary is the defect area where cracks are most likely to occur when the solid electrolyte is subjected to external stress, and it is also the area where dendrites are most likely to grow and spread. In this way, the generation of internal defects of the solid electrolyte can be more accurately avoided, and the toughness can be further improved.

[0010] In some of the embodiments, among the total number of particles of the phase change toughening agent in the modified solid electrolyte, the number of particles of the phase change toughening agent distributed at the grain boundaries in the solid electrolyte accounts for ≥50%.

[0011] In some embodiments, in the same cross section of the modified solid electrolyte, the total number of particles of the phase change toughening agent is N1, and the number of particles of the phase change toughening agent distributed at the grain boundary in the same cross section is N2, then the orientation degree of the phase change toughening agent distributed along the grain boundary is A=N2 / N1×100%, and A satisfies: A≥50%;

[0012] Optionally, A satisfies: 50%<A≤100%;

[0013] Optionally, A satisfies: 50%<A<100%.

[0014] In the above-mentioned modified solid electrolyte, on the same cross section, the orientation degree H of the phase change toughening agent along the grain boundary is ≥50%, which can be regarded as that in the modified solid electrolyte, the phase change toughening agent is mainly distributed along the grain boundary in the modified solid electrolyte. The grain boundary is the defect area where cracks are most likely to occur when the solid electrolyte is subjected to external stress, and it is also the area where dendrites are most likely to grow and spread. Therefore, the phase change toughening agent is mainly distributed along the grain boundary area in the modified solid electrolyte, which can more accurately avoid the generation of internal defects in the solid electrolyte and further improve the toughness.

[0015] In some of the embodiments, the same cross section is a cross section or a longitudinal section of the modified solid electrolyte.

[0016] Specifically, the cross section is the section formed by cutting perpendicular to the height or thickness direction, and the longitudinal section is the section formed by cutting parallel to the height or thickness direction. For example, for a cylinder, its cross section is the section formed by cutting perpendicular to the height direction, which is a circle, and its longitudinal section is the section formed by cutting parallel to the height direction, which is a rectangle. The height of the cylinder can also be called the thickness. If the height of the cylinder is relatively low, for example, the height is less than the diameter of the ground, then the cylinder is a disc, and the common height is called the thickness.

[0017] In some embodiments, the step of testing the orientation degree A comprises:

[0018] Taking the sample to be tested of the modified solid electrolyte, cutting the sample to be tested along a direction perpendicular to the thickness of the wafer, and the cutting section formed when cutting the sample to be tested is the cross section to be tested;

[0019] An X-ray spectrometer is used to mark the key elements contained in the phase change toughening agent in the cross section to be measured, so that the key elements emit signal points, and a scanning electron microscope image of the cross section to be measured is obtained:

[0020] Obtaining a total number M1 of the signal points in the scanning electron microscope image and a number M2 of the signal points contained at the grain boundaries in the scanning electron microscope image;

[0021] According to M1 and M2, we get A;

[0022] Specifically, A=M2 / M1×100%.

[0023] The key element is an element contained in the phase change toughening agent but not contained in the solid electrolyte substrate.

[0024] In some embodiments, the phase change toughening agent contains zirconium oxide, and the key element is zirconium.

[0025] In some embodiments, the phase change toughening agent further contains a stabilizer, and in the phase change toughening agent, the mass proportion of the stabilizer is 0.01% to 50%;

[0026] Optionally, the stabilizer contains at least one element selected from the group consisting of yttrium, scandium, magnesium, calcium, and cesium;

[0027] Optionally, the stabilizer includes at least one of yttrium oxide, scandium oxide, magnesium oxide, calcium oxide, and cesium oxide;

[0028] Optionally, the stabilizer comprises yttrium oxide.

[0029] Although the specific toughening mechanism of phase change toughening agents is still to be studied, technicians speculate as follows: phase change toughening agents have a metastable state, that is, phase change toughening agents exist in a high-temperature stable crystal structure at room temperature, which makes the phase change toughening material undergo phase change and volume change when receiving external force stimulation, thereby inhibiting the fracture of the solid electrolyte and playing a role in phase change toughening. For example: pure ZrO2 will generally undergo the following phase change during the cooling process from high temperature to room temperature: cubic phase (c), tetragonal phase (t) to monoclinic phase (m), among which t to m phase change will occur at around 1150°C, accompanied by a volume change of about 5%. If the t and m phase transition points of ZrO2 are stabilized to room temperature, it can produce a tm phase transition induced by external stress at room temperature, and absorb a large amount of fracture energy due to the volume effect generated by the phase change, so that the material exhibits an abnormally high fracture toughness, achieving the effect of phase change toughening.

[0030] In some embodiments, in the modified solid electrolyte, the mass proportion of the phase change toughening agent is 2% to 25%;

[0031] Optionally, the mass proportion of the phase change toughening agent is 5% to 25%;

[0032] Optionally, the mass proportion of the phase change toughening agent is 10% to 25%;

[0033] Optionally, the mass proportion of the phase change toughening agent is 15% to 25%.

[0034] The mass proportion of the phase change toughening agent is adjusted to further improve the toughness of the modified solid electrolyte.

[0035] In some embodiments, in the modified solid electrolyte, the mass of the solid electrolyte substrate is m1, the theoretical density is ρ1, the mass of the phase change toughening agent is m2, the theoretical density is ρ2, then the theoretical volume Vt of the modified solid electrolyte satisfies: Vt = [m1 / ρ1] + [m2 / ρ2];

[0036] The actual volume of the modified solid electrolyte is Vr, and the density of the modified solid electrolyte is K=Vt / Vr×100%;

[0037] Optionally, K satisfies: K≥70%; Optionally, K satisfies: 90%≤K≤100%.

[0038] It can be understood that the theoretical density ρ1 and the theoretical density ρ2 are the densities of the pure solid electrolyte substrate and the pure phase change toughening agent respectively. They can also be understood as the densities of the solid electrolyte substrate raw materials and the phase change toughening agent raw materials used in the preparation. Vt represents the volume of the modified solid electrolyte. The larger the K value, the greater the difference between its actual volume and the theoretical volume, which means that the actual distribution inside the modified solid electrolyte is more compact and dense. The above-mentioned modified solid electrolyte has a high density. When used in the preparation of solid-state batteries, it can reduce defects and pores on the surface of the electrolyte sheet / membrane, and can further improve the ionic conductivity of the modified solid electrolyte.

[0039] In some embodiments, the solid electrolyte substrate includes any one of a lithium ion solid electrolyte, a sodium ion solid electrolyte, and a potassium ion solid electrolyte.

[0040] The second aspect of the present application provides a method for preparing a modified solid electrolyte, comprising the following steps:

[0041] Mixing a solid electrolyte substrate and a phase change toughening agent to prepare a mixture;

[0042] The mixture is sintered under a protective gas atmosphere to prepare the modified solid electrolyte.

[0043] In the above preparation method, during the sintering of the mixture, the grains grow and the grain boundaries fuse with each other. At the same time, driven by the grain growth, most of the phase change toughening agent, which originally tends to be evenly distributed in the mixture, enters the grain boundary area and is distributed along the grain boundary orientation.

[0044] Furthermore, under the action of grain growth and grain boundary fusion, the defects and pores of the modified solid electrolyte are greatly reduced, and the density is improved.

[0045] In some embodiments, the sintering process satisfies at least one of the following conditions (1) to (2):

[0046] (1) The sintering treatment temperature is 90°C to 600°C, and the sintering time is 10 minutes to 120 hours;

[0047] By regulating the temperature and time of the sintering treatment, the phase change toughening agent is further promoted to enter the grain boundary area under the promotion of grain growth, and the structural stability of the solid electrolyte substrate and the phase change toughening agent is ensured.

[0048] (2) The protective gas atmosphere is formed by filling with a protective gas, wherein the protective gas comprises at least one of an inert gas and nitrogen;

[0049] Optionally, the protective gas comprises helium;

[0050] Optionally, the water content in the protective gas is <0.1 ppm and the oxygen content is <0.1 ppm.

[0051] In some of the embodiments, after the sintering process, the method further comprises the step of pressing the product obtained by the sintering process;

[0052] Optionally, the pressure T1 used in the pressing step satisfies: T1≤400MPa;

[0053] Optionally, T1 satisfies: 400MPa≤T1≤600MPa.

[0054] In some embodiments, the mixing step adopts dry mixing, and before the mixture is sintered, the following steps are also included:

[0055] The mixture is pressed into a sheet-like mixture; optionally, the thickness of the sheet-like mixture is 200 μm to 2 mm; optionally, the pressure used when the mixture is pressed into the sheet-like mixture is 400 MPa to 600 MPa; or

[0056] The mixing step adopts wet mixing, and before the mixture is sintered, the following steps are also included:

[0057] The mixture is coated and dried to form a film-like mixture; optionally, the thickness of the film-like mixture is 10 μm to 200 μm.

[0058] According to a third aspect of the present application, a solid-state battery is provided, comprising the modified solid-state electrolyte of the first aspect or a modified solid-state electrolyte prepared by the preparation method of the modified solid-state electrolyte of the second aspect.

[0059] According to a fourth aspect of the present application, an electrical device is provided, wherein the electrical device comprises the solid-state battery according to the third aspect. BRIEF DESCRIPTION OF THE DRAWINGS

[0060] Various other advantages and benefits will become apparent to those of ordinary skill in the art by reading the detailed description of the preferred embodiments below. The accompanying drawings are only for the purpose of illustrating the preferred embodiments and are not to be considered as limiting the present application. Moreover, the same reference numerals are used throughout the drawings to represent the same components. In the drawings:

[0061] Figure 1 is a schematic diagram of a solid-state battery according to one embodiment;

[0062] Figure 2 is a schematic diagram of an embodiment of a battery pack;

[0063] Figure 3 yes Figure 2 Exploded diagram of

[0064] Figure 4 is a schematic diagram of an embodiment of an electrical device using a solid-state battery as a power source;

[0065] Figure 5 This is an electron microscope image of the cross section of the modified solid electrolyte prepared in Example 1.

[0066] Description of reference numerals:

[0067] 1. Battery pack; 2. Upper box; 3. Lower box; 4. Solid-state battery; 5. Electrical device. DETAILED DESCRIPTION

[0068] In order to make the above-mentioned purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are described in detail below. In the following description, many specific details are set forth to facilitate a full understanding of the present application. However, the present application can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present application, so the present application is not limited by the specific embodiments disclosed below.

[0069] In this application, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.

[0070] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In the description of this application, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.

[0071] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art to which the present application belongs. The terms used herein in the specification of the present application are only for the purpose of describing specific embodiments and are not intended to limit the present application. The term "and / or" used herein includes any and all combinations of one or more of the related listed items.

[0072] In summary, traditional solid electrolytes often have the fragile characteristics of ceramics. In traditional technologies, technicians mainly focus on developing new solid electrolytes or improving the structure of solid-state batteries, but there has been no special breakthrough or progress so far.

[0073] The technicians of this application have found through research that the contact interface, i.e., the grain boundary, formed when crystals with different orientations in a solid electrolyte contact each other is the defect area most likely to produce cracks when the solid electrolyte is subjected to external stress, and is also the area where dendrites are most likely to grow and spread.

[0074] Based on this, the technical personnel of this application, after a lot of creative exploration, obtained the modified solid electrolyte with excellent toughness in this application.

[0075] An embodiment of the present application provides a modified solid electrolyte, characterized in that the modified solid electrolyte comprises a solid electrolyte substrate and a phase change toughening agent distributed in the solid electrolyte substrate, and in the modified solid electrolyte, the phase change toughening agent is mainly distributed at the grain boundaries in the modified solid electrolyte;

[0076] Phase change toughening agents can undergo phase change under the action of external forces.

[0077] The above-mentioned modified solid electrolyte includes a solid electrolyte substrate and a phase change toughening agent distributed in the solid electrolyte substrate. When stimulated by external forces, tensile stress is generated inside. Under the stimulation of tensile stress, the phase change toughening agent will undergo a phase change. The stress transformation brought about by the phase change process can improve the mechanical strength and toughness of the solid electrolyte substrate. The phase change toughening agent is mainly distributed along the grain boundary area in the modified solid electrolyte. The grain boundary is the defect area where cracks are most likely to occur when the solid electrolyte is subjected to external stress, and it is also the area where dendrites are most likely to grow and spread. In this way, the generation of internal defects in the solid electrolyte can be more accurately avoided and the toughness can be improved.

[0078] It can be understood that the external force in the above-mentioned "phase change toughening agent will undergo phase change under the action of external force" refers to the effect exerted on the phase change toughening agent by the external environment outside the phase change toughening agent itself. Furthermore, when the external force acts on the phase change toughening agent, it causes the phase change toughening agent to deform, and the various parts in the phase change toughening agent then generate interacting internal forces to resist the action of the external force, trying to restore the phase change toughening agent from the deformed position to the position before deformation. This internal force is stress. Driven by the stress, a phase change will occur inside the phase change toughening agent, and a large amount of fracture energy will be absorbed due to the volume change caused by the phase change, thereby achieving the effect of phase change toughening.

[0079] It can be understood that the grain boundary is the interface between grains with the same structure but different orientations. On the crystal interface, the atomic arrangement transitions from one orientation to another, so the atomic arrangement at the grain boundary is in a transitional state. When observed under the bright field of a scanning electron microscope (SEM), it can be seen that the grain boundary is dark and black.

[0080] In some of the embodiments, among the total number of phase change toughening agent particles in the modified solid electrolyte, the number of phase change toughening agent particles distributed at the grain boundaries in the solid electrolyte accounts for ≥50%.

[0081] In some of the embodiments, in the same cross section of the modified solid electrolyte, the total number of phase change toughening agent particles is N1, and the number of phase change toughening agent particles distributed at the grain boundaries in the same cross section is N2, then the orientation degree of the phase change toughening agent distributed along the grain boundaries is A=N2 / N1×100%, and A satisfies: A≥50%;

[0082] Optionally, A satisfies: 50%<A≤100%;

[0083] Optionally, A satisfies: 50%<A<100%.

[0084] In the above-mentioned modified solid electrolyte, on the same cross section, the orientation degree A of the phase change toughening agent along the grain boundary is ≥50%, which means that in the modified solid electrolyte, the phase change toughening agent is mainly distributed along the grain boundary in the modified solid electrolyte. The grain boundary is the defect area where cracks are most likely to occur when the solid electrolyte is subjected to external stress, and it is also the area where dendrites are most likely to grow and spread. Therefore, the phase change toughening agent is mainly distributed along the grain boundary area in the modified solid electrolyte, which can more accurately avoid the generation of internal defects in the solid electrolyte and further improve the toughness.

[0085] It can be understood that the distribution of the phase change toughening agent on the plane can reflect the distribution of the phase change toughening agent in the overall modified fixed electrolyte.

[0086] In the above “50%<A≤100%”, the value of A includes the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiment and the following point values: 51%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95%, 99%, 100%; or a range consisting of any two values, for example, it can be 51%~99%, 55%~99%, 60%~99%, 65%~99%, 70%~99%, 75%~99%, 80%~99%, 51%~95%, 55%~95%, 60%~95%, 65%~95%, 70%~95%, 75%~ 95%, 80%-95%, 51%-90%, 55%-90%, 60%-90%, 65%-90%, 70%-90%, 75%-90%, 80%-90%, 51%-85%, 55%-85%, 60%-85%, 65%-85%, 70%-85%, 75%-85%, 80%-85%, 51%-80%, 55%-80%, 60%-80%, 65%-80%, 70%-80%, 75%-80%, 51%-75%, 55%-75%, 60%-75%, 65%-75%, 70%-75%, 51%-70%, 55%-70%, 60%-70%, 65%-70%.

[0087] In some of the embodiments, the same cross section is a cross section or a longitudinal section of the modified solid electrolyte.

[0088] Specifically, the cross section is the section formed by cutting perpendicular to the height or thickness direction, and the longitudinal section is the section formed by cutting parallel to the height or thickness direction. For example, for a cylinder, its cross section is the section formed by cutting perpendicular to the height direction, which is a circle, and its longitudinal section is the section formed by cutting parallel to the height direction, which is a rectangle. The height of the cylinder can also be called the thickness. If the height of the cylinder is relatively low, for example, the height is less than the diameter of the ground, then the cylinder is a disc, and the common height is called the thickness.

[0089] Optionally, the same cross section is a cross section of the modified solid electrolyte. Further optionally, the modified solid electrolyte is a cylinder.

[0090] In some embodiments, the steps of testing the orientation degree A include:

[0091] Taking the disc of the modified solid electrolyte, cutting the disc along a direction perpendicular to the thickness of the disc, and the cut section formed when cutting the disc is the cross section to be measured;

[0092] An X-ray spectrometer is used to mark the key elements contained in the phase change toughening agent in the cross section to be measured, so that the key elements emit signal points, and a scanning electron microscope image of the cross section to be measured is obtained: wherein the key elements are elements contained in the phase change toughening agent but not contained in the solid electrolyte substrate;

[0093] Obtaining the total number M1 of signal points in the scanning electron microscope image and the number M2 of signal points contained in the grain boundary in the scanning electron microscope image;

[0094] Based on M1 and M2, we get A.

[0095] Specifically, A=M2 / M1×100%.

[0096] It can be understood that the total number of signal points emitted by the key elements in the scanning electron microscope image can be regarded as the total number of particles of the phase change toughening agent in the cross section to be measured;

[0097] The number of signal points emitted by the key elements contained in the grain boundaries in the scanning electron microscope image can be counted, which can be regarded as the number of particles N2 of the phase change toughening agent distributed at the grain boundaries in the cross section to be measured.

[0098] Specifically, in the electron microscope energy spectrum (SEM-EDS) analysis, the electron microscope is equipped with an EDS probe. Taking the Zr element as an example, the Zr signal comes from the SEM's EDS probe. Its mechanism of action is to emit electrons, excite surface materials, and then detect characteristic X-ray radiation. Thus, the scanning electron microscope image is divided into 1 μm square grids. The number of Zr element signal points output by the EDS in the square grid is regarded as the number of particles of the phase change toughening agent.

[0099] Specifically, an accelerating voltage of 10 kV was used for EDS scanning, and the EDS probe was Oxford Instrument AZtech One.

[0100] Optionally, the disc has a thickness of 200 μm to 2 mm.

[0101] In some of the embodiments, when the wafer is cut perpendicular to the thickness direction of the wafer, the cutting point is located at 1 / 2 thickness of the wafer.

[0102] In some of the embodiments, the magnification of the scanning electron microscope image is 1k-5k.

[0103] In some embodiments, the area of ​​the measured cross section is gridded into n unit grid areas, where n is an integer ≥ 2; each unit grid area is placed under a scanning electron microscope for observation to form a scanning electron microscope image, and then the total number of signal points emitted by the key elements in the scanning electron microscope image of each grid area and the number of signal points emitted by the key elements at the grain boundaries in the grid area are counted, and the orientation degree An corresponding to each grid area is calculated, and then the average value is taken to obtain the orientation degree A in the measured cross section:

[0104] A=(A1+…+An) / n

[0105] In some embodiments, n satisfies: 3≤n≤10, and n is an integer.

[0106] In some embodiments, n=5.

[0107] When n=5, the five-point sampling method is used for grid division to divide five grid units: that is, the midpoint of the diagonal is first determined as the central sampling point grid, and then four grid units with equal distances from the central sampling point grid are selected on the diagonal.

[0108] Furthermore, when the cross section to be measured is placed under a scanning electron microscope for observation, the placement position of the cross section to be measured can be changed multiple times to perform the above steps to obtain the orientation degrees of multiple areas of the cross section to be measured, and then the average value of the orientation degrees of multiple areas is calculated, which is regarded as the orientation degree of the phase change toughening agent along the grain boundary in the cross section to be measured.

[0109] In some of the embodiments, the phase change toughening agent contains zirconium oxide, and the key element is zirconium.

[0110] In some embodiments, the phase change toughening agent further contains a stabilizer, and the mass proportion of the stabilizer in the phase change toughening agent is 0.1% to 50%;

[0111] Optionally, the stabilizer contains at least one element selected from the group consisting of yttrium, scandium, magnesium, calcium, and cesium.

[0112] In some of these embodiments, the stabilizer component includes an oxide.

[0113] Optionally, the stabilizer includes at least one of yttrium oxide, scandium oxide, magnesium oxide, calcium oxide, and cesium oxide.

[0114] When the stabilizers are yttrium oxide, scandium oxide, magnesium oxide, calcium oxide, and cesium oxide, the toughening agents are recorded as YSZ, SSZ, MSZ, CSZ, and CsSZ, respectively.

[0115] Optionally, the stabilizer comprises yttrium oxide.

[0116] Although the specific toughening mechanism of phase change toughening agents is still to be studied, technicians speculate as follows: phase change toughening agents have a metastable state, that is, phase change toughening agents exist in a high-temperature stable crystal structure at room temperature, which makes the phase change toughening material undergo phase change and volume change when receiving external force stimulation, thereby inhibiting the fracture of the solid electrolyte and playing a role in phase change toughening. For example: pure ZrO2 will generally undergo the following phase change during the cooling process from high temperature to room temperature: cubic phase (c), tetragonal phase (t) to monoclinic phase (m), among which t to m phase change will occur at around 1150°C, accompanied by a volume change of about 5%. If the t and m phase transition points of ZrO2 are stabilized to room temperature, it can produce a tm phase transition induced by external stress at room temperature, and absorb a large amount of fracture energy due to the volume effect generated by the phase change, so that the material exhibits an abnormally high fracture toughness, achieving the effect of phase change toughening.

[0117] In the above-mentioned "0.01% to 50%", the values ​​include the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiment and the following point values: 0.01%, 0.05%, 0.1%, 1%, 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%; or a range consisting of any two values, for example, it can be 1% to 50%, 5% to 50%, 10% to 50%, 15% to 50%, 20% to 50%, 25% to 50%, 30% to 50%, 35% to 50%, 40% to 50%, 45% to 50%, 1% to 45%, 5% to 45%, 10% to 50%, 15% to 50%, 20% to 50%, 25% to 50%, 30% to 50%, 35% to 50%, 40% to 50%, 45% to 50%, %~45%, 15%~45%, 20%~45%, 25%~45%, 30%~45%, 35%~45%, 40%~45%, 1%~40%, 5%~40%, 10%~40%, 15%~40%, 20%~40%, 25%~40%, 30%~40%, 35%~40%, 1%~35%, 5%~35%, 10%~35%, 15%~35%, 20%~35%, 25%~35%, 30%~35%, 1%~30%, 5%~30%, 10%~30%, 15%~30%, 20%~30%, 1%~25%, 5%~25%, 10%~25%, 15%~25%, 20%~25%.

[0118] In some of the embodiments, in the modified solid electrolyte, the mass proportion of the phase change toughening agent is 2% to 25%;

[0119] In some embodiments, the mass percentage of the phase change toughening agent is 5% to 25%;

[0120] In some embodiments, the mass proportion of the phase change toughening agent is 10% to 25%;

[0121] In some embodiments, the mass percentage of the phase change toughening agent is 15% to 25%.

[0122] The mass proportion of the phase change toughening agent is adjusted to further improve the toughness of the modified solid electrolyte.

[0123] In the above-mentioned "2%~25%", the values ​​include the minimum and maximum values ​​of the range, and every value between such minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiment and the following point values: 2%, 5%, 10%, 15%, 20%, 25%; or a range consisting of any two numerical values, for example, it can be 2%~5%, 2%~10%, 2%~15%, 2%~20%, 2%~25%, 5%~10%, 5%~15%, 5%~20%, 5%~25%, 10%~15%, 10%~20%, 10%~25%, 15%~20%, 15%~25%, 20%~25%.

[0124] In some of the embodiments, in the modified solid electrolyte, the mass of the solid electrolyte substrate is M1, the theoretical density is ρ1, the mass of the phase change toughening agent is M2, the theoretical density is ρ2, then the theoretical volume Vt of the modified solid electrolyte satisfies: Vt = [M1 / ρ1] + [M2 / ρ2];

[0125] The real volume of the modified solid electrolyte is Vr, then the density of the modified solid electrolyte is K = Vt / Vr × 100%;

[0126] Optionally, K satisfies: K≥70%; Optionally, K satisfies: 90%≤K≤100%.

[0127] It can be understood that the theoretical density ρ1 and the theoretical density ρ2 are the densities of the pure solid electrolyte substrate and the pure phase change toughening agent respectively. They can also be understood as the densities of the solid electrolyte substrate raw materials and the phase change toughening agent raw materials used in the preparation. Vt represents the volume of the modified solid electrolyte. The larger the K value, the greater the difference between its actual volume and the theoretical volume, which means that the actual distribution inside the modified solid electrolyte is more compact and dense. The above-mentioned modified solid electrolyte has a high density. When used in the preparation of solid-state batteries, it can reduce defects and pores on the surface of the electrolyte sheet / membrane, and can further improve the ionic conductivity of the modified solid electrolyte.

[0128] In some of the embodiments, the real volume Vr of the modified solid electrolyte is obtained by measuring the actual modified solid electrolyte using the Archimedean method or a micrometer.

[0129] In some embodiments, the solid electrolyte substrate includes any one of a lithium ion solid electrolyte, a sodium ion solid electrolyte, and a potassium ion solid electrolyte.

[0130] The above-mentioned lithium-ion solid electrolytes, sodium-ion solid electrolytes, and potassium-ion solid electrolytes can be various lithium-ion solid electrolytes, sodium-ion solid electrolytes, and potassium-ion solid electrolytes commonly used in the art.

[0131] In some of the embodiments, the solid electrolyte substrate is a lithium-ion solid electrolyte.

[0132] Examples of the lithium-ion solid electrolyte are given herein, including but not limited to:

[0133] LISICON type: such as γ-Li3PO4, etc.;

[0134] NASICON type; such as Li (1+x1) Q x M (2-x1) (PO4)3, 0 ≤ x1 < 1, Q includes at least one of Al, Cr, Ba, Fe, Sc, In, Lu, Y, La;

[0135] Garnet type; such as Li (7-x2) La3Zr (2-x2) M x2 O12, etc., 0 ≤ x2 < 1, M includes at least one of Sb, Nb, Ta, Te, W;

[0136] LIPON type: such as Li x3 PO y1 N z1 ; 0 < x3 ≤ 1, 0 < y1 ≤ 1, 0 < z1 ≤ 1;

[0137] Perovskite type: such as Li3 x 4Q (2 / 3-x4) MO3, etc., 0.04 < x4 < 0.17, Q includes at least one of La, Sr, Ba, Nd, and M includes at least one of Al, Ti, Ge;

[0138] Anti-Perovskite type: such as Li3OCl, etc.; Thio-LiSICON type: such as Li (3+x5) My2A (1-y2) Q (4-z2) T z2 , where -1 < x5 < 2, 0 ≤ y2 ≤ 1, 0 ≤ z2 ≤ 2, M includes at least one of B, Al, In, Si, Ge, Sn, Ti, W, Mo, A includes at least one of P, As, Sb, Bi, Q includes at least one of S, Se, and T includes at least one of F, Cl, Br, I;

[0139] Sulfide solid electrolytes, including: Thiophosphate type: Li3PS4, etc., Argyrodite type: Li6PS5Cl, Halide type: Li3InCl6, Hydride type: at least one of 0.7Li(CB9H 10 )-0.3Li(CB 11 H 12 ); for example, Li (10+x6) M (1+y3) A (2-y3) Q (12-z3) H z3 type: where -2 < x6 < 2, 0 ≤ y3 ≤ 2, 0 ≤ z3 ≤ 2, M includes at least one of B, Al, In, Si, Ge, Sn, Ti, W, Mo; A includes at least one of P, As, Sb, Bi, Q includes at least one of S, Se, H includes at least one of F, Cl, Br, I: (100 - x7)Li2S·x7M·y4Q type: where 20 ≤ x7 ≤ 30, 0 ≤ y4 ≤ 50, M includes at least one of B2S3, Al2S3, In2S3, SiS2, GeS2, SnS2, P2S5, As2S3, Sb2S5, Bi2S3, WS2, MoS2, Q includes at least one of B2O3, Al2O3, In2O3, SiO2, GeO2, SnO2, P2O5, Sb2O5, Bi2O3, WO2, WO3, MoO2, MoO3, Fe2O3, ZnO, MgO, CuO, CaO, LiN, Li2O, LiF, LiCl, LiBr, LiI; Argyrodite type: Li (6+x8) M y5 A (1-y5) Q (5-z5) T (1+z5) , where -1 ≤ x8 ≤ 1, 0 ≤ y5 ≤ 1, -1 < z5 ≤ 1, M includes at least one of B, Al, In, Si, Ge, Sn, Ti, W, Mo, A includes at least one of P, As, Sb, Bi, Q includes at least one of S, Se, T includes at least one of F, Cl, Br, I; Halide type: Li3MJ or Li2Sc 2 / 3 J; M includes at least one of Y, Er, In, Sc, Ga, J includes at least one of F, Cl, Br, I.

[0140] When the above sulfide solid electrolyte is a sulfide-based solid electrolyte, it includes but is not limited to: thiargyrite electrolyte; binary sulfide-based solid systems such as Li2S-P2S5, Li2S-SiS2, Li2S-GeS, and Li2S-B2S3, Li2S-Me-P2S5 ternary systems, where Me is selected from Si, Ge, Sn, or Al, etc.

[0141] Specifically, the sulfide electrolyte is selected from at least one of Li2S-P2S5, Li2S-SiS2, Li2S-GeS, Li2S-B2S3, and Li2S-Me-P2S5.

[0142] The sodium solid-state electrolyte includes, but is not limited to: NASICON type: Na (1+x9+2y5) Zr (2-y5) M y5 P (3-x9) Si x9 O 12 , 0≤x9≤3, 0≤y5≤1, M includes at least one of Zn, Mg, and Ca; Na-β-Alumina type: Na2O·2Al2O3 or Na2O·3Al2O3, etc.; Na (3+x10) M y6 A (1-y6) Q (4-z6) T z6 type, where -1<x10<2, 0≤y6≤1, 0≤z6≤2, M includes at least one of B, Al, In, Si, Ge, Sn, Ti, W, and Mo, A includes at least one of P, As, Sb, and Bi, Q includes at least one of S and Se, and T includes at least one of F, Cl, Br, and I; Na (11+x11) M (2-y7) A (1+y7) Q (12-z7) T z7 type where -1<x11<1, 0≤y7≤2, 0≤z7≤2, M includes at least one of B, Al, In, Si, Ge, Sn, Ti, W, and Mo, A includes P, As, Sb, Bi; Q = at least one of S and Se, and T includes at least one of F, Cl, Br, and I; anti-perovskite type Na3OX, X includes at least one of Cl, Br, I, and BH4.

[0143] The potassium solid-state electrolyte includes, but is not limited to: β-Alumina type such as K2O·x13Al2O3, etc., where x13 takes any number from 8 to 11, Anti-Perovskite type such as K3OI, at least one of K2Fe4O7 type and KSi2P3 type.

[0144] An embodiment of the present application further provides a method for preparing a modified solid-state electrolyte, including the following steps S10 to S20.

[0145] Step S10: Mix the solid-state electrolyte substrate and the phase change toughening agent to prepare a mixture.

[0146] Step S20: sintering the mixture in a protective gas atmosphere to prepare a modified solid electrolyte.

[0147] In the above preparation method, during the sintering of the mixture, the grains grow and the grain boundaries fuse with each other. At the same time, driven by the grain growth, most of the phase change toughening agent, which originally tends to be evenly distributed in the mixture, enters the grain boundary area and is distributed along the grain boundary orientation.

[0148] Furthermore, under the action of grain growth and grain boundary fusion, the defects and pores of the modified solid electrolyte are greatly reduced, and the density is improved.

[0149] The types and further mass ratios of the solid electrolyte substrate and the phase change toughening agent are as described above and will not be elaborated here.

[0150] In some of the embodiments, the sintering temperature is 90° C. to 600° C. and the sintering time is 10 min to 120 h.

[0151] By regulating the temperature and time of the sintering treatment, the phase change toughening agent is further promoted to enter the grain boundary area under the promotion of grain growth.

[0152] In some embodiments, the sintering temperature is 90°C to 550°C.

[0153] The sintering temperature is further adjusted to ensure that most of the phase change toughening agent enters the grain boundary region while maintaining the structural stability of the solid electrolyte substrate and the phase change toughening agent.

[0154] In the above "90°C to 600°C", the temperature value includes the minimum and maximum values ​​of the range, as well as every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and the following point values: 90°C, 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, 160°C, 170°C, 180°C, 190°C, 200°C, 210°C, 220°C, 230°C, 240°C, 250°C, 260°C, 270°C, 280°C, 290°C , 300°C, 310°C, 320°C, 330°C, 340°C, 350°C, 360°C, 370°C, 380°C, 390°C, 400°C, 410°C, 420°C, 430°C, 440°C, 450°C, 460°C, 470°C, 480°C, 490°C, 500°C, 510°C, 520°C, 530°C, 540°C, 550°C, 560°C, 570°C, 580°C, 590°C, 600°C; or a range consisting of any two values, for example, it can be 100 ℃~600℃、100℃~550℃、100℃~500℃、100℃~450℃、100℃~400℃、100℃~350℃、100℃~300℃、100℃~250℃、100℃~200℃、150℃~600℃、150℃~500℃、150℃~400℃、150℃~350℃、150℃~300℃、150℃~250℃、150℃~200℃、200℃~600℃、200℃~500℃、2 00℃~400℃, 200℃~350℃, 200℃~300℃, 200℃~250℃, 250℃~600℃, 250℃~500℃, 250℃~400℃, 250℃~350℃, 250℃~300℃, 300℃~600℃, 300℃~500℃, 300℃~400℃, 300℃~350℃, 400℃~600℃, 400℃~500℃, 450℃~600℃, 450℃~500℃, 500℃~600℃.

[0155] In the above "10min~120h", the time value includes the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and the following point values: 110h, 100h, 95h, 90h, 85h, 80h, 75h, 70h, 65h, 60h, 55h, 50h, 45h, 40h, 35h, 30h, 25h, 20h, 15h, 10h, 9h, 8h, 7h, 6h, 5h, 4h, 3h, 2h, 1h, 0.5h, 20min, 10min.

[0156] In some embodiments, in the sintering step of step S20, the temperature is raised to the sintering temperature at a heating rate of 10°C / min for sintering.

[0157] It should be noted that the sintering time is counted from the time when the temperature reaches the sintering temperature.

[0158] In some of the embodiments, the protective gas atmosphere is formed by charging a protective gas, wherein the protective gas includes at least one of an inert gas and nitrogen.

[0159] Optionally, the protective gas comprises helium.

[0160] Optionally, the water content in the protective gas is <0.1 ppm and the oxygen content is <0.1 ppm.

[0161] In some of the embodiments, after the sintering process, the step of pressing the product obtained by the sintering process is also included;

[0162] Optionally, the pressure T1 used in the pressing step satisfies: T1≤400MPa;

[0163] Optionally, T1 satisfies: 400MPa≤T1≤600MPa.

[0164] Through further pressing treatment, the components of the modified solid electrolyte are distributed more densely, and the phase change toughening agent is further squeezed into the grain boundary area.

[0165] Further adjusting the pressing pressure can further increase the orientation degree A of the phase change toughening agent distributed along the grain boundary.

[0166] In some embodiments, the mixing step in step S10 is dry mixing, and before the mixture is sintered, the following steps are also included:

[0167] The mixture is compressed into a sheet-like mixture.

[0168] Optionally, the thickness of the sheet-like mixture is 200 um to 2 mm.

[0169] In some of the embodiments, the pressure used when the mixture is pressed into a sheet-like mixture is 400 MPa to 600 MPa.

[0170] In some embodiments, the mixing step in step S10 is wet mixing, and before the mixture is sintered, the following steps are also included:

[0171] The mixture is coated and dried to form a film-like mixture; optionally, the thickness of the film-like mixture is 10 μm to 200 μm.

[0172] It can be understood that dry mixing is to directly mix the solid electrolyte substrate and the phase change toughening agent in the solid state; wet mixing is to mix the solid electrolyte substrate, the phase change toughening agent, the solvent and the binder to form a mixture slurry.

[0173] Optionally, the solvent may be at least one of water, small molecule alcohol, benzene solvent and alcohol ether solvent. Further optionally, the small molecule alcohol includes ethanol, propanol, etc., and the benzene solvent includes toluene, xylene, etc.

[0174] The binder may be a commonly used binder in the art, including but not limited to: styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), carboxymethyl chitosan (CMCS), and at least one of polyvinylidene fluoride (PVDF).

[0175] Furthermore, the mixing is carried out under stirring; the stirring method can be various stirring methods commonly used in the art, such as stirring with a ball mill, and the stirring time includes but is not limited to: 0.5h~6h, and further, the stirring speed is 100rpm~300rpm.

[0176] In the drying step, the purpose is to dry the solvent in the wet film formed by coating. There is no special requirement for the drying temperature or drying time. It is sufficient to evaporate the solvent in the wet film formed by coating. Specifically, the commonly used drying methods in the art can be adopted, including but not limited to: vacuum drying, heating drying, etc.

[0177] It should be noted that the solvent in the mixture after wet mixing will evaporate during the sintering process, and the binder will carbonize and form volatilized gas during the sintering process. Therefore, the content of solvent and binder residues in the modified solid electrolyte obtained after sintering is extremely small and can be almost ignored.

[0178] One embodiment of the present application provides a solid-state battery, which includes the above-mentioned modified solid-state electrolyte.

[0179] In the above-mentioned modified solid electrolyte, the phase change toughening agent is mainly distributed along the grain boundary area in the modified solid electrolyte. The grain boundary is the defect area where cracks are most likely to occur when the solid electrolyte is subjected to external stress, and it is also the area where dendrites are most likely to grow and spread. Therefore, it can more accurately avoid the generation of internal defects in the solid electrolyte, improve toughness and inhibit dendrites from further piercing the electrode. It also has high ionic conductivity, thereby improving the efficiency of solid-state batteries.

[0180] In some of the embodiments, in the above-mentioned solid-state battery, the modified solid-state electrolyte exists in the form of a membrane; further, the above-mentioned solid-state battery also includes a positive electrode sheet and a negative electrode sheet, and the modified solid-state electrolyte membrane is arranged between the electrode sheet and the negative electrode sheet.

[0181] The positive electrode sheet and the negative electrode sheet may be those commonly used in the art, and non-limiting examples are given here to illustrate the positive electrode sheet and the negative electrode sheet.

[0182]

Negative electrode

[0183] The negative electrode sheet includes a positive electrode current collector and a negative electrode active layer loaded on the surface of the positive electrode current collector.

[0184] The components of the negative electrode active layer include a negative electrode active material.

[0185] The above negative electrode active material can be the commonly used negative electrode active material in this application, including at least one of metal lithium negative electrode material, carbon family negative electrode material, oxide negative electrode material, and silicon-based negative electrode material.

[0186] In any embodiment of the present application, the above-mentioned negative electrode active material includes metallic lithium, lithium-containing alloys, lithium-containing composites, mesophase carbon microspheres, graphite, glassy carbon, carbon nanotubes, carbon-carbon composites, carbon fibers, hard carbon, soft carbon, magnesium oxide, silicon-carbon composites, TiO2, MoO2, In2O3, Al2O3, Cu2O, VO2, SnO x 、SiO x , Ga2O3, Sb2O5, Bi2O, or at least one of the following:

[0187] In any embodiment of the present application, the mass proportion of the negative electrode active material in the negative electrode active layer is 70% to 99.5%.

[0188] In any embodiment of the present application, the components of the negative electrode active layer further include a negative electrode conductive agent and a negative electrode binder.

[0189] In any embodiment of the present application, the above-mentioned negative electrode conductive agent can be a conductive material commonly used in the art, including but not limited to: at least one of graphite, carbon nanotubes, nanofibers, carbon black and graphene. Specifically, it can be selected from SP, KS-6, acetylene black, branched Ketjen black ECP, SFG-6, vapor-grown carbon fiber VGCF, carbon nanotubes CNTs and graphene and their composite conductive agents.

[0190] The weight ratio of the negative electrode conductive agent in the negative electrode active layer is 0 to 20 wt % based on the total weight of the negative electrode active layer.

[0191] The above-mentioned negative electrode binder can be a commonly used binder in the art, and can be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), carboxymethyl chitosan (CMCS), and polyvinylidene fluoride (PVDF).

[0192] The weight ratio of the negative electrode binder in the negative electrode active layer is 0 to 30 wt % based on the total weight of the negative electrode active layer.

[0193] In any embodiment of the present application, the negative electrode active layer may further include other additives, such as thickeners, such as sodium carboxymethyl cellulose (CMC-Na), etc. Based on the total weight of the negative electrode active layer, the weight ratio of other additives in the negative electrode active layer is 0-15wt%.

[0194] In any embodiment of the present application, the current collector in the negative electrode sheet may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer material base and a metal layer formed on at least one surface of the polymer material base. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0195] In any embodiment of the present application, the negative electrode sheet can be prepared in the following manner: the above-mentioned components for preparing the negative electrode sheet, such as the negative electrode active material, the conductive agent, the binder and any other components are dispersed in a solvent (such as deionized water) to form a negative electrode slurry; the negative electrode slurry is coated on the negative electrode collector, and after drying, cold pressing and other processes, the negative electrode sheet can be obtained. The solid content of the negative electrode slurry is 30wt% to 70wt%, and the viscosity at room temperature is adjusted to 2000mPa·s to 10000mPa·s; the obtained negative electrode slurry is coated on the negative electrode collector, and after a drying process, cold pressing such as a roller, a negative electrode sheet is obtained. The negative electrode powder coating unit surface density is 75mg / m 2 ~220 mg / m 2 , the compaction density of the negative electrode is 1.2g / m 3 ~2.0g / m 3 .

[0196]

Positive electrode

[0197] The positive electrode sheet includes a positive electrode current collector and a positive electrode active layer loaded on the surface of the positive electrode current collector.

[0198] The components of the positive electrode active layer include a positive electrode active material.

[0199] In some embodiments, the mass percentage of the positive electrode active material in the positive electrode active layer is 70% to 100%.

[0200] In some embodiments, the positive electrode active material may employ a positive electrode active material for a secondary battery known in the art.

[0201] In any embodiment of the present application, the positive electrode active material includes any one of a sodium ion positive electrode active material and a lithium ion positive electrode active material.

[0202] Further, as an example, the lithium ion active material may include at least one of the following materials: lithium phosphates containing olivine structure, lithium transition metal oxides and their respective modified compounds. However, the present application is not limited to these materials, and other traditional materials that can be used as positive electrode active materials for batteries can also be used. These positive electrode active materials can be used alone or in combination of two or more. Among them, examples of lithium transition metal oxides may include, but are not limited to, lithium cobalt oxide (such as LiCoO2), lithium nickel oxide (such as LiNiO2), lithium manganese oxide (such as LiMnO2, LiMn2O4), lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide (such as LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (also referred to as NCM333), LiNi 0.5 Co 0.2 Mn 0.3 O2 (also referred to as NCM523), LiNi 0.5 Co 0.25 Mn 0.25 O2 (also referred to as NCM211), LiNi 0.6 Co 0.2 Mn 0.2 O2 (also referred to as NCM622), LiNi 0.8 Co 0.1 Mn 0.1 O2 (also referred to as NCM811), lithium nickel cobalt aluminum oxide (such as LiNi 0.85 Co 0.15 Al 0.05 O2) and its modified compounds, etc. Examples of lithium-containing phosphates with olivine structure may include, but are not limited to, at least one of lithium iron phosphate (such as LiFePO4 (also referred to as LFP)), lithium manganese phosphate (such as LiMnPO4), and lithium manganese iron phosphate.

[0203] In any embodiment of the present application, the molecular formula of the lithium ion active material is: LiFex Mn (1-x) PO4, x can be any number from 0 to 1.

[0204] It can be understood that when x is 0, LiFe x Mn (1-x) PO4 is LiMnPO4 lithium manganese phosphate. When x is 1, LiFePO4 is LiFePO4 lithium iron phosphate (LFP).

[0205] As an example, the sodium ion positive electrode active material may include at least one of the following materials: at least one of a sodium transition metal oxide, a polyanionic compound, and a Prussian blue compound. However, the present application is not limited to these materials, and other conventionally known materials that can be used as positive electrode active materials for sodium ion batteries may also be used. In any embodiment of the present application, the positive electrode active material includes at least one of a sodium transition metal oxide, a polyanionic compound, and a Prussian blue compound;

[0206] Optionally, the positive electrode active material includes at least one of a sodium transition metal oxide and a polyanionic compound.

[0207] Sodium transition metal oxides have a layered transition metal structure. Compared with the rhombohedral phase of Prussian blue compounds, theoretically, the thickness rebound rate of the layered transition metal structure will be greater. However, in actual application, since Prussian blue compounds easily absorb water to form crystal water and vacancy defects, the thickness rebound rate increases and even causes structural collapse. Therefore, when sodium transition metal oxides are used as positive electrode active materials, the thickness rebound rate of the positive electrode sheet is smaller.

[0208] The anion structural units in the polyanionic compounds are connected into a three-dimensional structure through covalent bonds, and the structural stability is good. When it is a positive electrode active material, the thickness rebound rate of the positive electrode sheet is low.

[0209] As an optional technical solution of the present application, in the sodium transition metal oxide, the transition metal includes at least one of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr and Ce. The sodium transition metal oxide is, for example, Na x MO2, wherein M includes at least one or more of Ti, V, Mn, Co, Ni, Fe, Cr and Cu, and 0<x≤1.

[0210] As an optional technical solution of the present application, the polyanionic compound can be a compound having sodium ions, transition metal ions and tetrahedral (YO4) n- A class of compounds with anionic units. Transition metals include at least one of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr and Ce; Y includes at least one of P, S and Si; n represents (YO4) n-valence state.

[0211] Polyanionic compounds can also be those with sodium ions, transition metal ions, tetrahedral (YO4) n- A class of compounds containing anion units and halogen anions. The transition metal includes at least one of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr and Ce; Y includes at least one of P, S and Si, and n represents (YO4) n- valence state; the halogen may be at least one of F, Cl and Br.

[0212] Polyanionic compounds can also be sodium ions, tetrahedral (YO4) n- Anion unit, polyhedral unit (ZO y ) m+ and an optional halogen anion. Y includes at least one of P, S and Si, and n represents (YO4) n- valence state; Z represents a transition metal, including at least one of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr and Ce; m represents (ZO y ) m+ valence state; the halogen may be at least one of F, Cl and Br.

[0213] Polyanionic compounds include NaFePO4, Na3V2(PO4)3 (sodium vanadium phosphate, abbreviated as NVP), Na4Fe3(PO4)2 (P2O7), NaM'PO4F (M' is one or more of V, Fe, Mn and Ni) and Na3(VO y )2(PO4)2F 3-2y At least one of (0≤y≤1).

[0214] Prussian blue compounds can be sodium ions, transition metal ions and cyanide ions (CN - ). The transition metal includes at least one of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr and Ce. Prussian blue compounds are, for example, Na a Me b Me' c (CN)6, wherein Me and Me' each independently include at least one of Ni, Cu, Fe, Mn, Co and Zn, 0<a≤2, 0<b<1, 0<c<1.

[0215] In any embodiment of the present application, the components of the positive electrode active layer further include a positive electrode binder, and the mass proportion of the positive electrode binder in the positive electrode active layer is 0.05% to 10%.

[0216] Optionally, the mass proportion of the positive electrode binder in the positive electrode active layer is 0.1% to 8%.

[0217] The positive electrode binder can adopt various types of binders commonly used in the art. As an example, the positive electrode binder includes polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, fluorine-containing acrylate resin, sodium carboxymethyl cellulose, hydroxypropyl cellulose, sodium hydroxymethyl cellulose, potassium hydroxymethyl cellulose, diacetyl cellulose, polyacrylic acid, sodium alginate, styrene-butadiene rubber, acrylic butadiene rubber, polypyrrole, polyaniline, epoxy resin and at least one of guardo gum.

[0218] In any embodiment of the present application, the components of the positive electrode active layer further include a positive electrode conductive agent, and the mass proportion of the positive electrode conductive agent in the positive electrode active layer is 0.05% to 8%.

[0219] Optionally, the mass proportion of the positive electrode conductive agent in the positive electrode active layer is 0.1% to 6%.

[0220] As an example, the positive electrode conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0221] The positive electrode current collector may be a metal foil or a composite current collector. For example, as the metal foil, a copper foil may be used. The composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material substrate. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0222] In some embodiments, the positive electrode sheet can be prepared in the following manner: the components for preparing the positive electrode sheet, such as the positive electrode active material, the positive electrode conductor, the positive electrode binder and any other components are dispersed in a solvent (such as N-methylpyrrolidone) to form a positive electrode slurry; the positive electrode slurry is coated on the positive electrode collector, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained.

[0223] In some of the embodiments, the solid-state battery is an all-solid-state battery or a semi-solid-state battery.

[0224] In some of the embodiments, in the solid-state battery, the modified solid electrolyte is in the form of a modified solid electrolyte membrane, which is located between the positive electrode sheet and the negative electrode sheet.

[0225] Furthermore, the solid-state battery also includes a shell for packaging the positive electrode sheet, the negative electrode sheet, and the modified solid electrolyte membrane.

[0226] In some embodiments, the shell may be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. It may also be a soft package, such as a bag-type soft package. The material of the soft package may be plastic, and examples of the plastic include polypropylene, polybutylene terephthalate, and polybutylene succinate.

[0227] The present application has no particular limitation on the shape of the battery, which may be cylindrical, square or any other shape. For example, Figure 1 A solid-state battery 4 with a square structure is shown as an example.

[0228] The present application also provides an electrical device, which includes the above-mentioned solid-state battery.

[0229] Furthermore, in the above-mentioned electrical device, the solid-state battery may exist in the form of a battery cell, or may be further assembled into a battery pack.

[0230] Figure 2 and Figure 3 The battery pack 1 is used as an example. The battery pack 1 includes a battery box and one or more solid-state batteries 4 arranged in the battery box. The battery box includes an upper box body 2 and a lower box body 3. The upper box body 2 can be covered on the lower box body 3 and form a closed space for the battery 4.

[0231] Multiple solid-state batteries 4 can be arranged in the battery box in any manner.

[0232] The above-mentioned solid-state battery or the battery pack assembled therefrom can be used as a power source for an electrical device, or as an energy storage unit for an electrical device.

[0233] The above-mentioned electrical devices may be, but are not limited to, mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc.

[0234] Figure 4 The power consumption device 5 is taken as an example. The power consumption device 5 is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle, etc. In order to meet the power consumption device 5's requirements for high power and high energy density of the battery, a battery pack can be used.

[0235] As another example, the power-consuming device may be a mobile phone, a tablet computer, a notebook computer, etc. Such a device is usually required to be thin and light, and a battery may be used as a power source.

[0236] The present application will be described below in conjunction with specific embodiments, but the present application is not limited to the following embodiments. It should be understood that the attached claims summarize the scope of the present application. Under the guidance of the concept of the present application, technical personnel in the field should realize that certain changes made to the various embodiments of the present application will be covered by the spirit and scope of the claims of the present application.

[0237] The following are specific embodiments.

[0238] Example 1

[0239] 1. Preparation of modified solid electrolyte, the specific steps are as follows:

[0240] S1: The solid electrolyte substrate (Li6PS5Cl) and the phase change toughening agent are dry mixed: a Fritsch Pulverisette planetary ball mill is used to mix at a rotation speed of 100 rpm for 0.5 h to obtain a mixture.

[0241] The phase change toughening agent includes zirconium oxide and a stabilizer. The mass of the phase change toughening agent is used as the calculation basis, and the mass proportion of the stabilizer is recorded as Y1. The total mass of the mixture is used as the calculation basis, and the mass proportion of the phase change toughening agent is recorded as Y2. For specific parameters, please see Table 1.

[0242] S2: The mixture was placed in a mold and pressed at a pressure of 500 MPa to a thickness of 1 mm and a surface area of ​​19.63 mm. 2 of a flake-shaped mixture.

[0243] S3: Place the flake mixture in an argon environment (H2O < 0.1ppm, O2 < 0.1ppm), heat to 350°C at a heating rate of 10°C / min, and sinter for 10 hours, then cool naturally to obtain a modified solid electrolyte. S4: Performance test of the modified solid electrolyte

[0244] (1) Test of the orientation degree A of the phase change toughening agent along the grain boundary in the modified solid electrolyte:

[0245] 1. Cut the disc perpendicular to the thickness of the disc. The cutting point is located at 1 / 2 of the thickness of the disc. The cutting section formed when cutting the disc is the cross section to be measured.

[0246] 2. The area of ​​the measured cross section is gridded into 5 unit grid areas, and each unit grid area is placed under a scanning electron microscope for observation to form a scanning electron microscope image; then the total number of signal points emitted by the key elements in the scanning electron microscope image of each grid area is counted respectively, which is regarded as the number of phase change toughening agent particles in each grid area, and is recorded as M11, M12, M13, M14, and M15 respectively; at the same time, the number of signal points emitted by the key elements at the grain boundaries in each grid area is counted, which is regarded as the number of phase change toughening agent particles at the grain boundaries in each grid area, and is recorded as M21, M22, M23, M24, and M25 respectively, and the orientation degree of the phase change toughening agent along the grain boundary in the modified solid electrolyte in each grid area is calculated respectively, and is recorded as A1, A2, A3, A4, and A5 respectively, and the calculation method is as follows:

[0247] A1=M 21 / M 11×100%;

[0248] A2=M 22 / M 12×100%;

[0249] A3=M23 / M13×100%;

[0250] A4=M 24 / M 14×100%;

[0251] A5=M 25 / M 15×100%;

[0252] The orientation degree A of the phase change toughening agent distributed along the grain boundary in the modified solid electrolyte is calculated according to the following formula:

[0253] A=(A1+A2+A3+A4+A5) / 5

[0254] Among them, the five-point sampling method is used for grid division to divide five grid units: that is, first determine the midpoint of the diagonal as the central sampling point grid, and then select four grid units on the diagonal that are equidistant from the central sampling point grid.

[0255] Specifically, each grid area is analyzed by electron microscope energy spectrum (SEM-EDS), and the formed scanning electron microscope image is divided into 1 μm square grids.

[0256] The number of Zr element signal points output by EDS in the square grid is regarded as the number of phase change toughening agent particles. The specific results are shown in Table 1. Among them, the EDS scan was performed using an accelerating voltage of 10 kV, and the EDS probe was Oxford Instrument AZtech One.

[0257] Among them, the scanning electron microscope image of the cross section of the modified solid electrolyte to be measured is as follows: Figure 5As shown, it can be clearly seen from the figure that the phase change toughening agent particles are mainly concentrated along the electrolyte grain boundaries.

[0258] (2) Fracture toughness test of modified solid electrolyte:

[0259] Fracture toughness is a parameter that describes the material's ability to absorb strain energy before fracture. The fracture toughness value (K IC )The higher the value, the stronger the resistance to crack propagation. Here, it also reflects the resistance of the modified solid electrolyte to cracking and short circuit caused by dendrites. Fracture toughness can be measured by four-point bending test, Vickers cone indentation test and other test methods. Here, Vickers cone indentation test is used to obtain the result. The specific process is as follows:

[0260] In an argon atmosphere, the surface of the disc of the modified solid electrolyte sheet is polished with sandpaper, from 800 mesh, to 2000 mesh, to 4000 mesh, to 8000 mesh, until the surface of the disc presents mirror properties without obvious defects, and then the polished surface is subjected to an indentation test by a Vickers cone indentation tester. The indentation tester is driven with an appropriate load P until radial cracks appear at the four corners of the cone indentation. According to the indentation load P, the extension length C of the radial cracks and the microhardness H obtained during the test, the V , the fracture toughness value K is further calculated by the following formula IC :

[0261]

[0262] Where P is the indentation load when cracks appear, in N; C is the extension length of radial cracks, in mm; H V Is the microhardness, the unit is kgf / mm 2 ; E is Young's modulus, in GPa; K IC is the fracture toughness of the solid electrolyte, the unit is MPa·m 1 / 2 .

[0263] (3) Critical current density test of modified solid electrolyte

[0264] Critical current density refers to the lowest current density at which dendrites and short circuits occur when electrochemical deposition of solid electrolyte materials is performed with corresponding alkali metal electrodes. In other words, when electrochemical deposition of modified solid electrolytes is performed at a current density lower than the critical current density, dendrites and short circuits will not occur. Critical current density is the core indicator that describes the ability of solid electrolyte materials to suppress dendrites and short circuits.

[0265] The critical current density of the modified solid electrolyte is measured by the traditional symmetric battery step-by-step increase current density cycle method. Taking lithium-ion solid electrolyte as an example, the process is as follows:

[0266] Two lithium metal discs with 8 mm long dendrites and 50 μm thickness were placed at the symmetrical center of the modified solid electrolyte disc. The lithium metal discs and the electrolyte discs were tightly fitted by mechanical pressure to form a lithium / solid electrolyte / lithium symmetrical battery. After the symmetrical battery was assembled and packaged, the symmetrical battery was made to flow from 0.25 mA / cm 2 Starting with a current of 1 mAh / cm, 1 mAh / cm 2 After lithium, the current was increased to 0.5 mA / cm 2 , maintain 1mAh / cm 2 After the surface capacity deposition and stripping, the current is increased to 0.75mA / cm 2 , 1.0mA / cm 2 , 1.25mA / cm 2 ... to 10mA / cm 2 , and monitor the voltage change during the process. The current density when the voltage suddenly drops sharply is recorded as the critical current density (Jc). The specific results are shown in Table 1.

[0267] (4) Ionic conductivity test of modified solid electrolyte

[0268] Ionic conductivity is a core indicator for measuring the ability of solid electrolytes to conduct corresponding metal ions. Ionic conductivity is generally tested by electrochemical impedance spectroscopy, and the corresponding ionic conductivity is calculated. The specific process is as follows:

[0269] A 200 nm thick nickel metal layer was deposited on both sides of the solid electrolyte wafer by magnetron sputtering PVD, and then the current collector was attached to the nickel metal layer and connected to the electrochemical workstation through the tab. 6 The solid electrolyte sheet was subjected to electrochemical impedance test under the condition of Hz~0.1Hz. The Z' coordinate value of the point closest to the Z' axis from right to left in the low-frequency band of the electrochemical impedance spectrum is taken as the resistance value R, and the ionic conductivity σ can be calculated by the following formula:

[0270]

[0271] Wherein, d is the thickness of the solid electrolyte sheet, and A is the contact area between the solid electrolyte sheet and the current collector.

[0272] (5) The density of the modified solid electrolyte material is tested as follows:

[0273] 1. The mass of the solid electrolyte substrate (Li6PS5Cl) used in the preparation is m1, the theoretical density is ρ1, the mass of the phase change toughening agent is m2, and the theoretical density is ρ2. The theoretical volume Vt of the modified solid electrolyte is calculated according to the following formula: Vt = [m1 / ρ1] + [m2 / ρ2];

[0274] Among them, m1 and m2 can both be obtained by weighing on a balance, the solid electrolyte substrate and the phase change toughening agent are both purchased commodities, and ρ1 and ρ2 are recorded in the parameter table of the commodity.

[0275] 2. The real volume Vr of the modified solid electrolyte is obtained by the Archimedean method or by measuring the actual modified solid electrolyte.

[0276] 3. The density of the modified solid electrolyte is K=Vt / Vr. Please see Table 1 for specific results.

[0277] S5: Preparation and performance testing of solid-state batteries

[0278] (1) Preparation of positive electrode sheet

[0279] The positive electrode active material NCM811, the binder nitrile rubber (NBR), the conductive agent VGCF and the electrolyte Li6PS5Cl are mixed in a mass ratio of 80:1.5:0.5:18, and p-xylene is added and stirred to form a uniformly dispersed slurry; the slurry is evenly coated on the surface of one side of the aluminum foil, and then transferred to a vacuum drying oven for complete drying; the obtained electrode sheet is rolled and then punched to obtain the positive electrode sheet.

[0280] (2) Preparation of negative electrode sheet

[0281] Lithium metal is used as the negative electrode active material, and the preparation method of the negative electrode sheet is as follows:

[0282] The lithium metal foil is rolled and thinned to a thickness of 50 μm, and the lithium metal foil is coated on one surface of the copper foil by rolling again, and then cut to obtain a negative electrode sheet.

[0283] The solid electrolyte membrane is placed between the negative electrode plate and the positive electrode plate, and they are bonded together to ensure close contact at the interface to form a solid-state battery.

[0284] (3) Maximum charging current density test: The maximum charging current density of a solid-state battery can be measured by cycling the current density in a step-by-step manner until failure: After the above-mentioned all-solid-state battery is assembled and packaged, the whole battery is charged from 0.25 mA / cm 2 At the beginning, charge and discharge were performed separately, and the capacity was controlled to be 1 mAh / cm 2 To ensure that the test surface capacity is constant during the cycle test, the current is increased to 0.5 mA / cm after the first cycle. 2, maintain 1mAh / cm 2 After the surface capacity is charged and discharged for a cycle, the 2 The gradient is 0.75 mA / cm 2 , 1.0mA / cm 2 , 1.25mA / cm 2 ... to 10mA / cm 2 Perform an all-solid-state battery cycle and record the current density at which the voltage suddenly drops sharply or shows obvious jitter as the maximum charging current density.

[0285] In fact, the maximum charging current density is similar to the critical current density of the composite solid electrolyte in physical meaning, and their values ​​are almost the same.

[0286] Example 2

[0287] Example 2 is basically the same as Example 1, except that the type of stabilizer in step S1 is different from that in Example 1. Please see Table 1 for specific conditions.

[0288] The other steps and conditions are the same as those in Example 1. The test results are shown in Table 1.

[0289] Embodiments 3 to 6

[0290] Examples 3 to 6 are substantially the same as Example 1, except that in step S1, the mass proportion of the phase change toughening agent in the mixture is denoted as Y2, which is different from Example 1. For specific conditions, see Table 1.

[0291] The other steps and conditions are the same as those in Example 1. The test results are shown in Table 1.

[0292] Embodiments 7 to 13

[0293] Examples 7 to 13 are basically the same as Example 1, and the only difference is: the temperature or time of the sintering treatment in step S3. Please see Table 1 for specific conditions.

[0294] The other steps and conditions are the same as those in Example 1. The test results are shown in Table 1.

[0295] Embodiments 14 to 16

[0296] Examples 14 to 16 are basically the same as Example 1, except that the mass proportion Y1 of the stabilizer in the phase change toughening agent in step S1 is different from that in Example 1. Please see Table 1 for specific conditions.

[0297] The other steps and conditions are the same as those in Example 1. The test results are shown in Table 1.

[0298] Comparative Example 1

[0299] Comparative Example 1 is substantially the same as Example 1, except that: Comparative Example 1 directly provides a solid electrolyte substrate (Li6PS5Cl) to perform step S4 and subsequent steps.

[0300] Comparative Example 2

[0301] Comparative Example 2 is substantially the same as Example 1, except that step S3 is not performed in Comparative Example 2. For specific conditions, see Table 1.

[0302] The remaining steps are the same as those in Example 1.

[0303] The relevant physical parameters and test results in each embodiment and comparative example are shown in Table 1, wherein the mass of the phase change toughening agent is used as the calculation basis, the mass proportion of the stabilizer is recorded as Y1, the total mass of the modified solid electrolyte is used as the calculation basis, the mass proportion of the phase change toughening agent is recorded as Y2, the orientation degree of the phase change toughening agent along the grain boundary in the modified solid electrolyte is A, KIC, Jc, σ and K are the fracture toughness, critical current density, ionic conductivity and density of the modified solid electrolyte, respectively.

[0304] Table 1

[0305]

[0306]

[0307] Note: “ / ” means that this step does not exist.

[0308] From the experimental results in the above table, analysis and comparison of the data of Example 1 and Comparative Examples 1 to 2 show that in the modified solid electrolyte of the present application, the phase change toughening agent is mainly distributed along the grain boundary region in the modified solid electrolyte, and the grain boundary is the defective region where cracks are most likely to occur when the solid electrolyte is subjected to external stress, and is also the region where dendrites are most likely to grow and spread. Therefore, the phase change toughening agent is mainly distributed along the grain boundary region in the modified solid electrolyte, which can more accurately avoid the generation of internal defects in the solid electrolyte and further improve the toughness.

[0309] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0310] The above-mentioned embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent of the present application shall be subject to the attached claims, and the description and drawings may be used to interpret the contents of the claims.

Claims

1. A modified solid electrolyte, characterized in that: The components of the modified solid electrolyte include a solid electrolyte substrate and a phase change toughening agent distributed in the solid electrolyte substrate, and in the modified solid electrolyte, the phase change toughening agent is mainly distributed at the grain boundaries in the solid electrolyte; The phase change toughening agent can undergo phase change under the action of external force.

2. The modified solid electrolyte according to claim 1, characterized in that Among the total number of particles of the phase change toughening agent in the modified solid electrolyte, the number of particles of the phase change toughening agent distributed at the grain boundaries in the solid electrolyte accounts for ≥50%.

3. The modified solid electrolyte according to claim 1, characterized in that In the same cross section of the modified solid electrolyte, the total number of particles of the phase change toughening agent is N1, and the number of particles of the phase change toughening agent distributed at the grain boundary in the same cross section is N2, then the orientation degree of the phase change toughening agent distributed along the grain boundary is A=N2 / N1×100%, and A satisfies: A≥50%; Optionally, A satisfies: 50%<A≤100%; Optionally, A satisfies: 50%<A<100%.

4. The modified solid electrolyte according to claim 3, characterized in that The same cross section is a cross section or a longitudinal section of the modified solid electrolyte.

5. The modified solid electrolyte according to claim 3, characterized in that The test steps of the orientation degree A include: Taking the sample to be tested of the modified solid electrolyte, cutting the sample to be tested along a direction perpendicular to the thickness of the sample to be tested, and the cutting section formed when cutting the sample to be tested is the cross section to be tested; An X-ray spectrometer is used to mark the key elements contained in the phase change toughening agent in the cross section to be measured, so that the key elements emit signal points, and a scanning electron microscope image of the cross section to be measured is obtained: Obtaining a total number M1 of the signal points in the scanning electron microscope image and a number M2 of the signal points contained at the grain boundaries in the scanning electron microscope image; According to M1 and M2, we get A; The key element is an element contained in the phase change toughening agent but not contained in the solid electrolyte substrate.

6. The modified solid electrolyte according to claim 5, characterized in that The phase change toughening agent contains zirconium oxide, and the key element is zirconium.

7. The modified solid electrolyte according to claim 6, characterized in that The phase change toughening agent further contains a stabilizer, and the mass proportion of the stabilizer in the phase change toughening agent is 0.01% to 50%; Optionally, the stabilizer contains at least one element selected from the group consisting of yttrium, scandium, magnesium, calcium, and cesium; Optionally, the stabilizer includes at least one of yttrium oxide, scandium oxide, magnesium oxide, calcium oxide, and cesium oxide; Optionally, the stabilizer comprises yttrium oxide.

8. The modified solid electrolyte according to any one of claims 1 to 7, characterized in that In the modified solid electrolyte, the mass proportion of the phase change toughening agent is 2% to 25%; Optionally, the mass proportion of the phase change toughening agent is 5% to 25%; Optionally, the mass proportion of the phase change toughening agent is 10% to 25%; Optionally, the mass proportion of the phase change toughening agent is 15% to 25%.

9. The modified solid electrolyte according to any one of claims 1 to 7, characterized in that In the modified solid electrolyte, the mass of the solid electrolyte substrate is m1, the theoretical density is ρ1, the mass of the phase change toughening agent is m2, the theoretical density is ρ2, then the theoretical volume Vt of the modified solid electrolyte satisfies: Vt = [m1 / ρ1] + [m2 / ρ2]; The actual volume of the modified solid electrolyte is Vr, and the density of the modified solid electrolyte is K=Vt / Vr×100%; Optionally, K satisfies: K ≥ 70%; Optionally, K satisfies: 90%≤K≤100%.

10. The modified solid electrolyte according to any one of claims 1 to 7, characterized in that: The solid electrolyte substrate includes any one of a lithium ion solid electrolyte, a sodium ion solid electrolyte and a potassium ion solid electrolyte.

11. A method for preparing a modified solid electrolyte, characterized in that: The steps include: Mixing a solid electrolyte substrate and a phase change toughening agent to prepare a mixture; The mixture is sintered under a protective gas atmosphere to prepare a modified solid electrolyte.

12. The method for preparing a modified solid electrolyte according to claim 11, characterized in that: The sintering process satisfies at least one of the following conditions (1) to (2): (1) The sintering treatment temperature is 90°C to 600°C, and the sintering time is 10 minutes to 120 hours; (2) The protective gas atmosphere is formed by filling with a protective gas, wherein the protective gas comprises at least one of an inert gas and nitrogen; Optionally, the protective gas comprises helium; Optionally, the water content in the protective gas is <0.1 ppm and the oxygen content is <0.1 ppm.

13. The method for preparing a modified solid electrolyte according to any one of claims 11 to 12, characterized in that: After the sintering process, the method further comprises the step of pressing the product obtained by the sintering process; Optionally, the pressure T1 used in the pressing step satisfies: T1 ≥ 400 MPa; Optionally, T1 satisfies: 400MPa≤T1≤600MPa.

14. The method for preparing a modified solid electrolyte according to any one of claims 11 to 12, characterized in that: The mixing step adopts dry mixing, and before the mixture is sintered, the following steps are also included: The mixture is pressed into a sheet-like mixture; optionally, the sheet-like mixture has a thickness of 200 μm to 2 mm; optionally, the pressure used when the mixture is pressed into the sheet-like mixture is 400 to 600 MPa; or The mixing step adopts wet mixing, and before the mixture is sintered, the following steps are also included: The mixture is coated and dried to form a film-like mixture; optionally, the film-like mixture has a thickness of 10 μm to 200 μm.

15. A solid-state battery, characterized in that: The solid-state battery comprises a modified solid electrolyte as described in any one of claims 1 to 10 or a modified solid electrolyte prepared by the method for preparing a modified solid electrolyte as described in any one of claims 11 to 14.

16. An electrical device, characterized in that: The electrical device comprises the solid-state battery as claimed in claim 15.

Citation Information

Cited By

  • Modified solid-state electrolyte and preparation method therefor, solid-state battery, and electric device

    EP4625580A1