Sodium ion oxide solid electrolyte, preparation method and solid sodium ion battery
By introducing Al element and Al2O3 into the sodium ion oxide solid electrolyte, the secondary sintering temperature is reduced, and the problems of high sintering temperature and low conductivity of sodium ion oxide solid electrolyte are solved, and the efficient preparation of sodium ion battery electrolyte is achieved. In all solid sodium ion battery.
Patent Information
- Application Number
- CN202410936790.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-11-05
AI Technical Summary
The high secondary sintering temperature, low ionic conductivity, high production cost and difficult preparation of sodium ion oxide solid electrolytes limit their application in all-solid sodium ion batteries.
Using the chemical formula of Na5M1-xAlxSi4O12, the presence of Al elements in an amorphous phase is introduced to reduce the grain boundary resistance, and combined with the low-cost Al2O3 as a flux, the secondary sintering temperature is reduced and the room temperature ionic conductivity is improved.
It achieves high room temperature ion conductivity at low secondary sintering temperature, reduces production costs and preparation difficulty, improves the density and stability of sodium ion oxide solid electrolyte, and is suitable for all-solid sodium ion batteries.
Smart Images

Figure CN118899520A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of sodium ion batteries, and in particular to a sodium ion oxide solid electrolyte, a preparation method and a solid sodium ion battery. Background Art
[0002] Lithium-ion batteries have become the most mature and widely used battery system due to their advantages such as high conversion efficiency, high energy / power density, no memory effect, and long service life. However, due to the uneven distribution of lithium resources and scarce reserves around the world, it is difficult to meet the growing demand for energy storage. In recent years, thanks to the high reserves and uniform distribution of sodium resources in the earth's crust, there is no problem of resource scarcity, and it is estimated that the cost of sodium-ion batteries can be 30% to 40% lower than that of lithium-ion batteries. Therefore, sodium-ion batteries are considered to be a good supplement to lithium-ion batteries.
[0003] At present, the organic liquid electrolytes used in sodium-ion batteries are extremely volatile and flammable, posing great safety risks, so researchers have begun to work on developing all-solid-state sodium-ion batteries with longer cycle life, higher energy density and safety. As one of the core components of sodium-ion all-solid-state batteries, solid electrolytes are the key to achieving high-performance all-solid-state batteries. Solid electrolytes mainly include inorganic solid electrolytes (typical representatives: oxide solid electrolytes and sulfide solid electrolytes), polymer solid electrolytes and composite solid electrolytes. Compared with polymer solid electrolytes, inorganic solid electrolytes can not only better meet the application requirements of batteries in high and low temperature environments, but their high mechanical strength can also effectively inhibit the penetration of metal dendrites. Among them, oxide solid electrolytes have received widespread attention due to their excellent thermal stability and chemical / electrochemical stability. After appropriate ion doping and modification, their ionic conductivity can be increased to 10 -3 S cm -1 above.
[0004] Na5MSi4O 12 (M=Fe, In, Sc, Y, lanthanide Lu-Sm) is a type of oxide solid electrolyte with three-dimensional ion transport channels. It has good molecular structure plasticity, high ionic conductivity and wide electrochemical stability window, so it has gradually attracted the attention of researchers. However, the main preparation method of this type of material is the traditional solid-phase sintering method, which usually requires a high secondary sintering temperature and a long sintering time to reduce the grain boundary resistance. The secondary sintering temperature is generally 1000-1200℃. Due to the high secondary sintering temperature, the volatilization of the Na element during the synthesis process cannot be avoided, which greatly increases the production cost and preparation difficulty. This has also become an important challenge faced by its commercial application. Therefore, lowering its secondary sintering temperature while ensuring high room temperature ionic conductivity will further expand the possibility of its large-scale production, and will also effectively promote its application in all-solid-state sodium-ion batteries.
[0005] The purpose of the present invention is to solve the problems of high secondary sintering temperature, low ion conductivity, high production cost and great difficulty in preparation of sodium ion oxide solid electrolyte. The present invention provides a sodium ion oxide solid electrolyte, a preparation method and a solid sodium ion battery, wherein the sodium ion oxide solid electrolyte has a low secondary sintering temperature, low grain boundary resistance and high room temperature ion conductivity.
[0006] In a first aspect, an embodiment of the present invention discloses a sodium ion oxide solid electrolyte, the chemical formula of which is: Na5M 1-x Al x SiO 12 ,
[0007] Wherein, M is one or more of Sm, Eu, Gd, Sc, and Y, and the range of x is: 0.06≤x≤0.4.
[0008] By adopting the above technical scheme, the sodium ion oxide solid electrolyte provided by the present invention adopts the above-mentioned combination of M and Al elements, and the Al element can exist in an amorphous phase in the microstructure of the sodium ion oxide solid electrolyte of the present invention, thereby improving the density of the sodium ion oxide solid electrolyte, reducing the grain boundary resistance, and thus improving the room temperature ionic conductivity of the sodium ion oxide solid electrolyte. And through the mutual coordination of the elements in the above chemical formula, the sodium ion oxide solid electrolyte of the present invention has good stability.
[0009] According to another specific embodiment of the present invention, the range of x is: 0.1≤x≤0.35.
[0010] According to another specific embodiment of the present invention, M is Sm.
[0011] According to another specific embodiment of the present invention, the microstructure of the sodium ion oxide solid electrolyte is a crystalline-amorphous two-phase structure.
[0012] According to another specific embodiment of the present invention, the density of the sodium ion oxide solid electrolyte is ≥95%, and the area specific resistance of the grain boundary is ≤15Ωcm -2 , room temperature ionic conductivity is: 10 -3 ~10 -2 S cm -1 .
[0013] In a second aspect, an embodiment of the present invention discloses a method for preparing a sodium ion oxide solid electrolyte, which is used to prepare a sodium ion oxide solid electrolyte as in any embodiment of the first aspect, comprising the following steps:
[0014] Preparation of powder A: Na2CO3, SiO2, Al2O3 and M metal oxide are mixed by wet ball milling and dried to obtain powder A;
[0015] Preparation of powder B: Powder A is sintered once, and the product after the primary sintering is dry-milled to obtain powder B, and the primary sintering temperature is 750-850°C;
[0016] Preparation of sodium ion oxide solid electrolyte: After pressing powder B into a round embryo, secondary sintering is performed to obtain a sodium ion oxide solid electrolyte. The secondary sintering temperature is 800-900°C.
[0017] M metal oxide is one or more of Sm2O3, Eu2O3, Gd2O3, Sc2O3, and Y2O3.
[0018] By adopting the above technical scheme, low-cost and environmentally friendly Al2O3 is introduced into the preparation method of the present invention. Al2O3 can be used as a flux, which significantly reduces the secondary sintering temperature, so that a sodium ion oxide solid electrolyte with stable properties and high room temperature ionic conductivity can be obtained at a secondary sintering temperature of 800 to 900°C. In addition, the secondary sintering temperature in the preparation method of the present invention is low, which effectively avoids the volatilization of the Na element, reduces energy consumption and loss of raw materials, and reduces the preparation cost.
[0019] According to another specific embodiment of the present invention, in the wet ball milling mixing, Na2CO3, SiO2, Al2O3 and M metal oxide are mixed in a molar ratio of 5:8:x:1-x, wherein 0.06≤x≤0.4.
[0020] According to another specific embodiment of the present invention, anhydrous ethanol is used as a dispersant in wet ball milling, the mass ratio of the mixture of Na2CO3, SiO2, Al2O3 and M metal oxide to anhydrous ethanol is 1:(2-4), the ball-to-material ratio of wet ball milling is (10-15):1, the ball milling speed is 500-600rpm, and the ball milling time is 12-16 hours; the ball milling speed of dry ball milling is 400-500rpm, the ball-to-material ratio is (10-15):1, and the ball milling time is 1-3 hours.
[0021] According to another specific embodiment of the present invention, the heating rate of the primary sintering is 3-5°C min -1 The sintering time is 7 to 10 hours; the heating rate of the secondary sintering is 3 to 5 °C min -1 The sintering time is 20 to 30 hours, and it is quickly cooled to room temperature within 15 to 30 minutes.
[0022] In a third aspect, an embodiment of the present invention further discloses a solid-state sodium ion battery, comprising a sodium ion oxide solid electrolyte as in any embodiment of the first aspect, or comprising a sodium ion oxide solid electrolyte obtained by the preparation method as in any embodiment of the second aspect.
[0023] By adopting the above technical scheme, the sodium ion oxide solid electrolyte provided by the present invention has good practicality, can provide the ionic conductivity required for the operation of the sodium ion battery, and helps to achieve the stable circulation of the sodium ion battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 The AC impedance spectra of the sodium ion oxide solid electrolytes of Examples 1-4 of the present invention;
[0025] Figure 2 The AC impedance spectrum of the sodium ion oxide solid electrolyte of Examples 5-6 of the present invention;
[0026] Figure 3 is the AC impedance spectrum of the sodium ion oxide solid electrolyte of Example 7 of the present invention;
[0027] Figure 4 The AC impedance spectrum of the sodium ion oxide solid electrolyte of Comparative Example 1-2 of the present invention;
[0028] Figure 5 The AC impedance spectrum of the sodium ion oxide solid electrolyte of Comparative Examples 3-4 of the present invention;
[0029] Figure 6 The cycle performance of the solid-state sodium ion battery in Application Example 1 of the present invention. DETAILED DESCRIPTION
[0030] The following specific embodiments illustrate the implementation of the present invention, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. Although the description of the present invention will be introduced in conjunction with the preferred embodiment, this does not mean that the features of this invention are limited to this implementation. On the contrary, the purpose of introducing the invention in conjunction with the implementation is to cover other options or modifications that may extend based on the claims of the present invention. In order to provide a deep understanding of the present invention, the following description will include many specific details. The present invention can also be implemented without using these details. In addition, in order to avoid confusion or blurring the focus of the present invention, some specific details will be omitted in the description. It should be noted that the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.
[0031] It should be noted that in this specification, similar reference numerals and letters denote similar items in the following drawings, and therefore, once an item is defined in one drawing, it does not need to be further defined and explained in the subsequent drawings.
[0032] The terms “first”, “second”, etc. are only used for distinguishing descriptions and should not be understood as indicating or implying relative importance.
[0033] In order to make the objectives, technical solutions and advantages of the present invention more clear, the embodiments of the present invention will be further described in detail below with reference to the accompanying drawings.
[0034] The inventors carefully studied the existing sodium ion oxide solid electrolyte and its preparation method and found that the existing technology usually uses Na5MSi4O 12 (M=Fe, In, Sc, Y, lanthanide Lu-Sm) type oxide solid electrolyte, and the main preparation method of this type of material in the prior art is the traditional solid phase sintering method, which usually requires a high secondary sintering temperature and a long sintering time to reduce the grain boundary resistance of the solid electrolyte. The inventor also found that the production cost and preparation difficulty of this type of oxide solid electrolyte and preparation method in the prior art are very high, and the grain boundary resistance of this type of oxide solid electrolyte is large, which makes the room temperature ionic conductivity relatively low, and the secondary sintering temperature in the preparation process is high, which promotes the volatilization of the Na element, which also greatly increases the production cost and preparation difficulty. The inventor hopes to reduce the production cost and preparation difficulty, by reducing the secondary sintering temperature to avoid the volatilization of chemical raw materials in the synthesis, and obtain a sodium ion oxide solid electrolyte with a low secondary sintering temperature and high room temperature ionic conductivity during the preparation process.
[0035] In a first aspect, an embodiment of the present invention provides a sodium ion oxide solid electrolyte, the chemical formula of which is: Na5M 1-x Al x SiO 12 ,
[0036] Wherein, M is one or more of Sm, Eu, Gd, Sc, and Y, and the range of x is: 0.06≤x≤0.4.
[0037] The present invention initially adopted low-cost Al elements in order to replace the position of the precious metal M. However, the inventor unexpectedly discovered during the preparation process that only a small part of Al can occupy the site of M and exist in a mixed form with M, while the remaining Al elements exist in an amorphous phase in combination with elements such as Na and Si in the microstructure of the sodium ion oxide solid electrolyte of the present invention, thereby improving the density of the sodium ion oxide solid electrolyte and reducing the grain boundary resistance. And through the mutual coordination of the elements in the above chemical formula, the ionic conductivity of the sodium ion solid electrolyte is improved compared to before the addition of the Al element. However, due to the poor sodium ion transmission capacity of Al2O3 itself, when the Al element content is too high, the room temperature ionic conductivity of the sodium ion oxide solid electrolyte is greatly reduced. When the Al element content is too low, its production cost and preparation difficulty are not improved. When the range of x is set to: 0.06≤x≤0.4, it is beneficial to ensure the room temperature ionic conductivity of the sodium ion oxide solid electrolyte and reduce the production cost, so that the sodium ion oxide solid electrolyte of the present invention has a lower grain boundary resistance and reaches 10 -3 S cm -1 Room temperature ionic conductivity.
[0038] Preferably, the range of x is: 0.1≤x≤0.35. This is conducive to further improving the room temperature ionic conductivity of the sodium ion oxide solid electrolyte in the above embodiment, so that the room temperature ionic conductivity reaches 10 -3 ~10 -2 S cm -1 .
[0039] In another embodiment, M is Sm. The ionic radius of Sm is 95.8 μm. The suitable ionic radius enables the sodium ion oxide solid electrolyte of the present invention to have an optimal ion transport channel size, thereby exhibiting higher ionic conductivity, and the mutual coordination of Sm and Al elements and other elements in the above chemical formula obtains a sodium ion oxide solid electrolyte with more stable chemical properties.
[0040] In the present invention, the Al element accounts for 6% to 40% of the molar mass of M. The above range of the Al element not only ensures that the sodium ion oxide solid electrolyte of the present invention has high ionic conductivity, but also helps to reduce the secondary sintering temperature during the preparation process, so that the secondary sintering temperature can be reduced by at least 50 to 100°C.
[0041] In any of the above embodiments, the microstructure of the sodium ion oxide solid electrolyte of the present invention is a crystalline-amorphous two-phase structure. The crystalline-amorphous two-phase structure means that the microstructure of the sodium ion oxide solid electrolyte of the present invention is a two-phase composite structure composed of a crystalline phase and an amorphous phase, which is beneficial to reduce the grain boundary resistance of the sodium ion oxide solid electrolyte, thereby improving the ionic conductivity.
[0042] The density of the sodium ion oxide solid electrolyte is 95-99% (including the end value), thereby reducing the internal grain boundaries of the solid electrolyte, facilitating the continuous migration of ions, and thus achieving high room temperature ionic conductivity.
[0043] The room temperature ionic conductivity of the sodium ion oxide solid electrolyte is: 10 -3 ~10 -2 S cm -1 , specifically, the room temperature ionic conductivity is: 1×10 -3 ~4×10 -3 S cm -1 The area specific resistance of the grain boundary is 0~15Ωcm -2 (including endpoint values). The area specific resistance of the grain boundary in this embodiment specifically refers to the ratio of the resistance of the grain boundary region to its area. The smaller the area specific resistance of the grain boundary, the smaller the grain boundary resistance per unit area of the solid electrolyte, and the higher the ionic conductivity. As a result, it can better meet the application needs of the development of battery technology and is conducive to promoting its large-scale use.
[0044] In a second aspect, an embodiment of the present invention provides a method for preparing a sodium ion oxide solid electrolyte, comprising the following steps:
[0045] Preparation of powder A: Na2CO3, SiO2, Al2O3 and M metal oxide are mixed by wet ball milling and dried to obtain powder A;
[0046] Preparation of powder B: Powder A is sintered once, and the product after the primary sintering is dry-milled to obtain powder B, and the primary sintering temperature is 750-850°C;
[0047] Preparation of sodium ion oxide solid electrolyte: After pressing powder B into a round embryo, secondary sintering is performed to obtain a sodium ion oxide solid electrolyte. The secondary sintering temperature is 800-900°C.
[0048] M metal oxide is one or more of Sm2O3, Eu2O3, Gd2O3, Sc2O3, and Y2O3.
[0049] The preparation method of the sodium ion oxide solid electrolyte of the present invention: wherein, the powder A is prepared by wet ball milling to ensure the uniformity of the mixture of Na2CO3, SiO2, Al2O3 and M metal oxide, and then the pure phase solid electrolyte material powder B can be obtained by only one sintering. However, due to the generation of gas during the primary sintering process, the structure of the obtained powder B is not dense enough, and further by pressing into a round embryo for secondary sintering, the pressure of pressing into the round embryo is 10-30MPa, and a sodium ion oxide solid electrolyte with a good dense structure is obtained, which is beneficial to reduce the ion transmission distance and improve its room temperature ion conductivity. And because Al2O3 is introduced in the preparation process as a flux, the secondary sintering temperature is significantly reduced, so that the secondary sintering temperature is 800-900°C, which is 200-300°C lower than the prior art. At the same time, the introduction of Al2O3 instead of other aluminum compounds is that its structure is similar to that of M metal oxide, which is more conducive to the reaction and helps to avoid the introduction of impurities. In addition, due to the low secondary sintering temperature of the present invention, the volatilization of Na elements and the like is effectively avoided, energy consumption and loss of raw materials are reduced, and the preparation cost is reduced.
[0050] In the wet ball milling, Na2CO3, SiO2, Al2O3 and M metal oxide are mixed in a molar ratio of 5:8:x:1-x, 0.06≤x≤0.4. Thus, a sodium ion oxide solid electrolyte with stable properties and high room temperature ionic conductivity can be obtained without adding more sodium salt and a lower secondary sintering temperature.
[0051] Anhydrous ethanol is used as a dispersant in wet ball milling. The mass ratio of the mixture of Na2CO3, SiO2, Al2O3 and M metal oxide to anhydrous ethanol is 1: (2-4), the ball-to-material ratio of wet ball milling is (10-15): 1, the ball milling speed is 500-600rpm, and the ball milling time is 12-16 hours; the ball milling speed of dry ball milling is 400-500rpm, the ball-to-material ratio is (10-15): 1, and the ball milling time is 1-3 hours. Thus, the mixture is fully mixed, which promotes the preparation of sodium ion oxide solid electrolyte. And the use of anhydrous ethanol as a dispersant is conducive to full volatilization at the sintering temperature, does not participate in the reaction, and has no impurities.
[0052] Furthermore, the heating rate of the primary sintering is 3-5°C min -1 The sintering time is 7 to 10 hours; the heating rate of the secondary sintering is 3 to 5 °C min -1, the sintering time is 20 to 30 hours, and the sintering time is rapidly cooled to room temperature within 15 to 30 minutes, and the rapid cooling is performed by liquid nitrogen cooling, for example. By controlling the heating rate to ensure the stable reaction of the substance during the sintering process, it is more conducive to obtaining a sodium ion oxide solid electrolyte with stable performance. And the sintering time within the above range is conducive to reducing the grain boundary resistance of the sodium ion oxide solid electrolyte.
[0053] In a third aspect, an embodiment of the present invention further provides a solid-state sodium ion battery, comprising the above-mentioned sodium ion oxide solid electrolyte.
[0054] By adopting the above technical scheme, the sodium ion oxide solid electrolyte provided by the present invention has good practicality, can provide the ionic conductivity required for the operation of the sodium ion battery, and help to achieve the stable circulation of the solid-state sodium ion battery.
[0055] Example 1
[0056] This embodiment provides a Na5Sm 0.92 Al 0.08 SiO 12 The preparation method comprises the following steps:
[0057] (1) Preparation of powder A: Anhydrous Na2CO3, SiO2, Al2O3 and Sm2O3 were wet-milled in a molar ratio of 5:8:0.08:0.92, anhydrous ethanol was used as a dispersant for wet ball milling, the mass ratio of the mixture of Na2CO3, SiO2, Al2O3 and Sm2O3 to anhydrous ethanol was 1:2, the ball-to-material ratio was 15:1, the ball milling speed was 600 rpm, the ball milling time was 15 hours, and after ball milling, it was dried at 120°C for 12 hours to obtain powder A;
[0058] (2) Preparation of powder B: Powder A was sintered once in air at a heating rate of 5 °C min -1 The sintering temperature was 800°C and the sintering time was 8 hours. After cooling naturally to room temperature, dry ball milling was performed with a ball-to-material ratio of 15:1, a ball milling speed of 400 rpm and a ball milling time of 2 hours to obtain powder B.
[0059] (3) Preparation of sodium ion oxide solid electrolyte: Powder B was pressed into a round embryo with uniform thickness using a cylindrical tablet pressing mold at a pressure of 20 MPa; secondary sintering was performed in an air environment at a heating rate of 5 °C min -1 The sintering temperature was 900 °C, the sintering time was 20 hours, and then it was rapidly cooled to room temperature within 30 minutes to obtain Na5Sm 0.92 Al 0.08 SiO 12Sodium ion oxide solid electrolyte.
[0060] Example 2
[0061] The method was the same as that in Example 1, except that the molar ratio of anhydrous Na2CO3, SiO2, Al2O3 and Sm2O3 in step (1) was 5:8:0.15:0.85 to obtain Na5Sm 0.85 Al 0.15 SiO 12 Sodium ion oxide solid electrolyte.
[0062] Example 3
[0063] The method was the same as that in Example 1, except that the molar ratio of anhydrous Na2CO3, SiO2, Al2O3 and Sm2O3 in step (1) was 5:8:0.2:0.8 to obtain Na5Sm 0.8 Al 0.2 SiO 12 Sodium ion oxide solid electrolyte.
[0064] Example 4
[0065] The method was the same as that in Example 1, except that the molar ratio of anhydrous Na2CO3, SiO2, Al2O3 and Sm2O3 in step (1) was 5:8:0.4:0.6 to obtain Na5Sm 0.6 Al 0.4 SiO 12 Sodium ion oxide solid electrolyte.
[0066] Example 5
[0067] The same method as in Example 2 was used to prepare the product, wherein the difference from Example 2 was that the sintering temperature of the secondary sintering in step (3) was 850°C to obtain Na5Sm 0.85 Al 0.15 SiO 12 Sodium ion oxide solid electrolyte.
[0068] Example 6
[0069] The same method as in Example 3 was used to prepare the product, wherein the difference from Example 3 was that the sintering temperature of the secondary sintering in step (3) was 850°C to obtain Na5Sm 0.8 Al 0.2 SiO 12 Sodium ion oxide solid electrolyte.
[0070] Example 7
[0071] This embodiment provides a Na5Gd0.8 Al 0.2 SiO 12 The preparation method comprises the following steps:
[0072] (1) Preparation of powder A: Anhydrous Na2CO3, SiO2, Al2O3 and Gd2O3 were mixed by wet ball milling in a molar ratio of 5:8:0.2:0.8, anhydrous ethanol was used as a dispersant for wet ball milling, the mass ratio of the mixture of Na2CO3, SiO2, Al2O3 and Gd2O3 to anhydrous ethanol was 1:2, the ball-to-material ratio was 15:1, the ball milling speed was 600 rpm, the ball milling time was 15 hours, and after ball milling, it was dried at 120°C for 12 hours to obtain powder A;
[0073] (2) Preparation of powder B: Powder A was sintered once in air at a heating rate of 5 °C min -1 The sintering temperature was 850°C and the sintering time was 10 hours. After cooling naturally to room temperature, dry ball milling was performed with a ball-to-material ratio of 15:1, a ball milling speed of 400 rpm and a ball milling time of 2 hours to obtain powder B.
[0074] (3) Preparation of sodium ion oxide solid electrolyte: Powder B was pressed into a round embryo with uniform thickness using a cylindrical tablet pressing mold at a pressure of 20 MPa; secondary sintering was performed in an air environment at a heating rate of 5 °C min -1 The sintering temperature was 900 °C, the sintering time was 25 h, and then it was rapidly cooled to room temperature within 30 min to obtain Na5Gd 0.8 Al 0.2 SiO 12 Sodium ion oxide solid electrolyte.
[0075] Comparative Example 1
[0076] This comparative example provides a Na5SmSi4O 12 The preparation method comprises the following steps:
[0077] (1) Preparation of powder A: The molar ratio of anhydrous Na2CO3, SiO2, Al2O3 and Sm2O3 was 5:8:0:1, and wet ball milling was performed. Anhydrous ethanol was used as a dispersant for wet ball milling. The mass ratio of the mixture of Na2CO3, SiO2, Al2O3 and Sm2O3 to anhydrous ethanol was 1:2. The ball-to-material ratio was 15:1. The ball milling speed was 600 rpm, the ball milling time was 15 hours, and the ball milling was dried at 120°C for 12 hours to obtain powder A.
[0078] (2) Preparation of powder B: Powder A was sintered once in air at a heating rate of 5 °C min -1 The sintering temperature was 800°C and the sintering time was 8 hours. After cooling naturally to room temperature, dry ball milling was performed with a ball-to-material ratio of 15:1, a ball milling speed of 400 rpm and a ball milling time of 2 hours to obtain powder B.
[0079] (3) Preparation of sodium ion oxide solid electrolyte: Powder B was pressed into a round embryo with uniform thickness using a cylindrical tablet pressing mold at a pressure of 20 MPa; secondary sintering was performed in an air environment at a heating rate of 5 °C min -1 The sintering temperature was 900 °C, the sintering time was 20 h, and then it was rapidly cooled to room temperature within 30 min to obtain Na5SmSi4O 12 Sodium ion oxide solid electrolyte.
[0080] Comparative Example 2
[0081] The difference from Comparative Example 1 is that the sintering temperature in step (3) is 1000°C to obtain Na5SmSi4O 12 Sodium ion oxide solid electrolyte.
[0082] Comparative Example 3
[0083] The difference from Example 1 is that in step (1), the ratio of anhydrous Na2CO3, SiO2, Al2O3 and Sm2O3 is 5:8:0.05:0.95, and Na5Sm 0.95 Al 0.05 SiO 12 Sodium ion oxide solid electrolyte.
[0084] Comparative Example 4
[0085] The difference from Example 1 is that in step (1), the ratio of anhydrous Na2CO3, SiO2, Al2O3 and Sm2O3 is 5:8:0.5:0.5, and Na5Sm 0.5 Al 0.5 SiO 12 Sodium ion oxide solid electrolyte.
[0086] Application Example 1
[0087] This embodiment provides a method for preparing a solid-state sodium ion battery, and the raw materials for preparation can be purchased on the market. The preparation method comprises the following steps:
[0088] (1) Preparation of positive electrode: Na4Fe(PO4)2P2O7, Super P, sodium carboxymethyl cellulose (CMC), polyacrylonitrile (PAN) and NaClO4 were uniformly mixed in deionized water in a certain proportion to prepare a viscous slurry, which was evenly coated on aluminum foil. After the deionized water on the surface evaporated, the electrode was transferred to a 60°C vacuum oven to completely dry the electrode, and then the electrode was cut into discs with a diameter of 1.2 cm;
[0089] (2) Preparation of negative electrode: In a glove box filled with argon, the oxide layer on the surface of the sodium metal was removed, rolled into thin sheets, and then cut into sodium metal discs with a diameter of 1.3 cm;
[0090] (3) Assembly of solid-state sodium ion battery: The sodium metal disc negative electrode and the Na4Fe(PO4)2P2O7 positive electrode are pasted on the Na5Sm prepared in Example 2 of the present invention. 0.8 Al 0.2 SiO 12 The two sides of the oxide solid electrolyte are finally packaged with CR2032 button batteries to obtain Na4Fe(PO4)2P2O7 / Na5Sm 0.8 Al 0.2 SiO 12 / Na solid-state sodium-ion battery.
[0091] As shown in Table 1, after X-ray diffraction test, the sodium ion oxide solid electrolytes obtained in the above Examples 1-7 and Comparative Examples 1-4 are all generated without impurity phases, and the unit cell parameters of Examples 1-7 and Comparative Examples 3-4 are compared with Comparative Examples 1-2 without Al2O3 addition, and there is no obvious change in the unit cell parameters before and after the addition of Al2O3, indicating that the added Al 3+ It is not completely doped into the crystal lattice of the material, but exists mainly in the form of an amorphous composite phase.
[0092] Table 1 Unit cell parameters of solid electrolyte materials in different embodiments and comparative examples
[0093]
[0094] like Figure 1 As shown, the Na5Sm obtained by sintering at 900°C in Example 1, Example 2, Example 3 and Example 4 are shown. 1-x Al x SiO 12 (Corresponding x=0.08, 0.15, 0.2, 0.4) Room temperature AC impedance spectrum of solid electrolyte.
[0095] like Figure 2 As shown, they are respectively Na5Sm obtained by sintering at 850°C in Example 5 and Example 6. 1-xAl x SiO 12 (corresponding to x = 0.15, 0.2) Room temperature AC impedance spectrum of solid electrolyte. Figure 1 and Figure 2 It can be seen that even if the sintering temperature is reduced by 50° C., the impedance value of the sodium ion oxide electrolyte of the present invention does not increase significantly, that is, its grain boundary resistance does not increase significantly, and it still has a relatively high room temperature ionic conductivity.
[0096] like Figure 3 The Na5Gd obtained in Example 7 0.8 Al 0.2 SiO 12 The room temperature AC impedance spectrum of the solid electrolyte shows the versatility of the low-temperature preparation method of sodium ion oxide solid electrolyte. 3+ Radius less than Sm 3+ , the material unit cell parameters are reduced (Table 1), and the ionic conductivity is slightly reduced, so M is Sm is more preferred.
[0097] like Figure 4 As shown in FIG. 1 and FIG. 2, Na5Sm was obtained under the secondary sintering conditions of 900°C and 1000°C. 1- x Al x SiO 12 (corresponding to x=0) room temperature AC impedance spectrum. It can be seen from Example 1 and Comparative Example 1 that, under the same other preparation conditions, the addition of Al2O3 significantly reduces the grain boundary resistance of the sodium ion oxide solid electrolyte of the present invention. It can be seen from Example 1 and Comparative Example 2 that the addition of Al2O3 can effectively reduce the secondary sintering temperature of the sodium ion oxide solid electrolyte, and even if the temperature is reduced by 100°C, a solid electrolyte with good ionic conductivity can still be obtained.
[0098] like Figure 5 Na5Sm was obtained by sintering at 900°C for Comparative Examples 3 and 4. 1-x Al x SiO 12 (corresponding to x = 0.05, 0.5) Room temperature AC impedance spectrum of solid electrolyte. By comparison, it can be seen that when the Al content is too low, the ionic conductivity is only slightly improved, and the effect is not obvious; when the Al content is too high, the ionic conductivity decreases, indicating that too much Al2O3 will hinder the transmission of sodium ions. Therefore, the Al content only plays a role in significantly improving the electrolyte ionic conductivity within the preferred range, and reaches 10 -3 S cm -1 Room temperature ionic conductivity above the level of 1.
[0099] In order to further highlight the effect of the present invention, Table 2 summarizes the room temperature ionic conductivity of different embodiments of the present invention and comparative examples. As shown in Table 2, the introduction of Al2O3 can significantly improve the density of the sodium ion oxide solid electrolyte of the present invention, reduce the grain boundary resistance, and thus improve the room temperature ionic conductivity; and more than 10 -3 S cm -1 The room temperature ionic conductivity of the sodium ion oxide solid electrolyte can be obtained when the sintering temperature is reduced by 100°C. In Example 2 and Example 3, since the chemical formula of the sodium ion oxide solid electrolyte further satisfies the range of x: 0.1≤x≤0.35, the room temperature ionic conductivity of the sodium ion oxide solid electrolyte is further improved.
[0100] Table 2 Density, area specific resistance of grain boundaries and room temperature ionic conductivity of different embodiments and comparative examples
[0101]
[0102] The test methods and test standards for the unit cell parameters, density, area specific resistance of grain boundaries and ionic conductivity of the present invention are specifically introduced below.
[0103] The unit cell parameters of the solid electrolyte material are obtained by Fullprof refinement based on its powder X-ray diffraction data. The electrolyte ceramic sheet after secondary sintering is ground into powder and then radiated using Cu Kα radiation. The test range is 10~120°.
[0104] The density, i.e. the relative density of the solid electrolyte ceramic sheet, was measured in anhydrous ethanol using the Archimedes method. The resistance of the solid electrolyte was measured using the AC impedance method, with Ag as a blocking electrode coated on both sides of the ceramic sheet, the test frequency range was 0.1 to 5 MHz, and the applied bias voltage was 30 mV.
[0105] The area specific resistance of the grain boundary is the ratio of the grain boundary resistance to the electrolyte area, and the ionic conductivity is calculated by the formula σ=l / (S×R), where l is the thickness of the electrolyte, S is the area of the electrolyte, and R is the total resistance of the electrolyte ceramic sheet.
[0106] Figure 6 The Na4Fe(PO4)2P2O7 / Na5Sm in the application example 1 of the present invention 0.8 Al 0.2 SiO 12 / Na solid-state sodium ion battery cycle performance, where "Specific Capacity" represents the specific capacity and "Cycle Number" represents the number of cycles. Figure 6It can be seen that the solid-state sodium ion battery of the present invention can provide 95mAh g -1 The reversible specific capacity of the solid-state sodium ion battery can be stably cycled for 100 times with almost no capacity decay, which proves that the sodium ion oxide solid electrolyte provided by the present invention can not only provide the high ionic conductivity required for the battery operation, but also ensure good stability and compatibility with the electrodes, thereby ensuring the stable cycle of the solid-state sodium ion battery, further verifying its good practicality.
[0107] In summary, the sodium ion oxide solid electrolyte of the present invention has high density, low grain boundary resistance and high room temperature ionic conductivity, has a wide electrochemical window, has good compatibility with electrode materials, and can be applied to all-solid-state sodium ion battery systems. 1-x Al x SiO 12 In the preparation method of the sodium ion oxide solid electrolyte, Al2O3 is used as a flux to significantly reduce its secondary sintering temperature. Compared with the traditional solid phase sintering method to prepare this structure and other structure types (mainstream such as Na-β"-Al2O3, NASICON structure), its secondary sintering temperature can be reduced by more than 200°C, which significantly reduces the sintering energy consumption. In addition, the reduction of the sintering temperature of the present invention can avoid the volatilization of sodium, and there is no need to add additional Na source to supplement the high temperature loss, nor is there a need to cover the precursor powder during sintering, which helps to reduce the loss of raw materials. The sintering process of the present invention uses Al2O3 as a flux, which can improve the density of the sodium ion oxide solid electrolyte, reduce the grain boundary resistance of the sodium ion oxide solid electrolyte, and thus effectively improve the room temperature ionic conductivity. All sintering processes of the present invention can be carried out in an air environment without atmosphere control, the preparation method is simple and feasible, the selected material Al2O3 is low in cost, the production cost is low, and large-scale production is easy to achieve.
[0108] Although the present invention has been illustrated and described with reference to certain preferred embodiments of the present invention, it should be understood by those skilled in the art that the above is a further detailed description of the present invention in conjunction with specific embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. Those skilled in the art may make various changes in form and details, including making several simple deductions or substitutions, without departing from the spirit and scope of the present invention.
Claims
1. A sodium ion oxide solid electrolyte, characterized in that: The chemical formula of the sodium ion oxide solid electrolyte is: Na5M 1-x Al x SiO 12 , Wherein, M is one or more of Sm, Eu, Gd, Sc, and Y, and the range of x is: 0.06≤x≤0.
4.
2. A sodium ion oxide solid electrolyte according to claim 1, characterized in that: The range of x is: 0.1≤x≤0.
35.
3. The sodium ion oxide solid electrolyte according to claim 1, characterized in that The M is Sm.
4. The sodium ion oxide solid electrolyte according to claim 1, characterized in that The microstructure of the sodium ion oxide solid electrolyte is a crystalline-amorphous two-phase structure.
5. The sodium ion oxide solid electrolyte according to claim 1, characterized in that The density of the sodium ion oxide solid electrolyte is ≥95%, and the area specific resistance of the grain boundary is ≤15Ωcm -2 , room temperature ionic conductivity is: 10 -3 ~10 -2 Scm -1 .
6. A method for preparing a sodium ion oxide solid electrolyte, characterized in that: The method for preparing the sodium ion oxide solid electrolyte according to any one of claims 1 to 5 comprises the following steps: Preparation of powder A: Na2CO3, SiO2, Al2O3 and M metal oxide are mixed by wet ball milling and dried to obtain powder A; Preparation of powder B: sintering the powder A once, and obtaining powder B by dry ball milling the product after the primary sintering, wherein the primary sintering temperature is 750-850° C.; Preparation of sodium ion oxide solid electrolyte: After pressing the powder B into a round embryo, secondary sintering is performed to obtain the sodium ion oxide solid electrolyte, and the temperature of the secondary sintering is 800-900° C.; The M metal oxide is one or more of Sm2O3, Eu2O3, Gd2O3, Sc2O3, and Y2O3.
7. The method for preparing the sodium ion oxide solid electrolyte according to claim 6, characterized in that: In the wet ball milling mixing, the Na2CO3, SiO2, Al2O3 and M metal oxide are mixed in a molar ratio of 5:8:x:1-x, wherein 0.06≤x≤0.
4.
8. The method for preparing the sodium ion oxide solid electrolyte according to claim 6, characterized in that: Anhydrous ethanol is used as a dispersant in the wet ball milling, the mass ratio of the mixture of Na2CO3, SiO2, Al2O3 and M metal oxide to the mass ratio of the anhydrous ethanol is 1:(2-4), the ball-to-material ratio of the wet ball milling is (10-15):1, the ball milling speed is 500-600rpm, and the ball milling time is 12-16 hours; the ball milling speed of the dry ball milling is 400-500rpm, the ball-to-material ratio is (10-15):1, and the ball milling time is 1-3 hours.
9. The method for preparing a sodium ion oxide solid electrolyte according to claim 6, characterized in that: The heating rate of the primary sintering is 3-5°C min -1 The sintering time is 7 to 10 hours; the heating rate of the secondary sintering is 3 to 5 ° C min -1 The sintering time is 20 to 30 hours, and it is quickly cooled to room temperature within 15 to 30 minutes.
10. A solid-state sodium ion battery, characterized in that: It comprises the sodium ion oxide solid electrolyte as claimed in any one of claims 1 to 5, or comprises the sodium ion oxide solid electrolyte obtained by the preparation method according to any one of claims 6 to 9.
Citation Information
Cited By
Sodium ion composite solid electrolyte material and preparation method and application thereof
CN119994161A