Metal foil with carrier, metal-clad laminate, and printed wiring board

By controlling the thickness and tensile strength of the carrier and metal foil, combined with roughening treatment and auxiliary metal layer, the problem of fracture and cracking of the carrier metal foil at high temperature is solved, and the manufacturing stability and quality of the printed circuit board are improved.

CN118900767APending Publication Date: 2024-11-05MITSUI MINING & SMELTING CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202380023836.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-01-20
Filing Date
2023-03-14
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

During the manufacturing process of printed circuit boards, the metal foil with the carrier is prone to break or cracking at high temperatures, resulting in a connecting portion forming a joint interface between the carrier and the metal foil, which is difficult to peel off, resulting in adverse conditions of residual metal.

Method used

By controlling the thickness and tensile strength of the carrier and metal foil, it is calculated that the α value is above -500 and below 30.0 to suppress breakage or cracking of the metal foil, and a roughened layer, an anti-rust treatment layer and a silane composed of roughened particles are used. A coupling agent layer is used to improve adhesion and durability, and an auxiliary metal layer is provided between the carrier and the metal foil to stabilize the peel strength.

Benefits of technology

The breakage and cracking of metal foil are effectively suppressed, the stability and quality in the manufacturing process of printed circuit boards are improved, the generation of residual metal is reduced, and the peeling effect between the carrier and the metal foil is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118900767A_ABST
    Figure CN118900767A_ABST
Patent Text Reader

Abstract

Provided is a metal foil with a carrier capable of suppressing the occurrence of breakage or cracking of the metal foil during operation. This metal foil with a carrier is provided with a carrier, a release layer, and a metal foil in this order, and the alpha value obtained by the formula alpha = 193.07-(0.13 * CT * CF)-(0.75 * BT * BF) (in the formula, CT is the thickness ([mu] m) of the carrier, CF is the tensile strength (kgf / mm2) of the carrier, BT is the thickness ([mu] m) of the metal foil, and BF is the tensile strength (kgf / mm2) of the metal foil) is-500-30.0.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a metal foil with a carrier, a metal-clad laminate and a printed circuit board. Background Art

[0002] As a material for manufacturing printed circuit boards, metal foil with a carrier is widely used. The metal foil with a carrier typically has a structure including a carrier, a peeling layer, and a metal foil (e.g., an ultra-thin copper foil) in this order, and is laminated with an insulating resin substrate (resin layer) such as a glass-epoxy substrate, a phenolic substrate, or polyimide by hot pressing to form a metal-clad laminate (e.g., a copper-clad laminate) for the manufacture of printed circuit boards.

[0003] When a metal foil with a carrier is hot-pressed at a high temperature (e.g., above 250°C), there is a problem that the peel strength between the carrier and the metal foil increases, and it is difficult to peel the carrier from the metal foil. There are known metal foils with carriers that address the above problems. For example, Patent Document 1 (International Publication No. 2015 / 080052) discloses a copper foil with a carrier, characterized in that a copper foil with a heat treatment of 250°C × 60 minutes and a strength of 40 kgf / mm2 is used as a carrier. 2 According to the copper foil with a carrier, the formation of a connection portion at the bonding interface layer between the carrier and the copper foil can be suppressed, and the carrier can be easily peeled off from the copper foil.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: International Publication No. 2015 / 080052 Summary of the invention

[0007] However, due to efforts towards SDGs (sustainable development goals) and the promotion of carbon neutrality in recent years, the thinning of the carrier in the metal foil with a carrier is envisioned for the purpose of reducing CO2 during manufacturing. In this regard, with the thinning of the carrier, there is a concern that the risk of the metal foil breaking, cracking (cracks), etc. will increase when the metal foil with a carrier is handled. In particular, the breaking or cracking of the metal foil during handling may lead to the undesirable situation of residual metal in the printed circuit board manufacturing process, and improvement is required.

[0008] The present inventors have now found that in a metal foil with a carrier, by controlling parameters calculated based on the thickness and tensile strength of the carrier and the thickness and tensile strength of the metal foil within a predetermined range, the occurrence of breakage or cracking of the metal foil during handling can be suppressed.

[0009] Therefore, an object of the present invention is to provide a metal foil with a carrier that can suppress the occurrence of breakage or cracks in the metal foil during handling.

[0010] According to the present invention, the following aspects are provided.

[0011] [Method 1]

[0012] A metal foil with a carrier, which comprises a carrier, a peeling layer and a metal foil in this order.

[0013] The α value of the metal foil with a carrier obtained by the following formula is -500 or more and 30.0 or less:

[0014] α=193.07-(0.13×C T ×C F )-(0.75×B T ×B F )

[0015] (In the formula, C T is the thickness of the carrier (μm), C F is the tensile strength of the aforementioned carrier (kgf / mm 2 ), B T is the thickness of the metal foil (μm), B F is the tensile strength of the aforementioned metal foil (kgf / mm 2 )).

[0016] [Method 2]

[0017] The metal foil with a carrier according to aspect 1, wherein the α value is -250 or more and 25.0 or less.

[0018] [Method 3]

[0019] The metal foil with a carrier according to aspect 1 or 2, wherein both the carrier and the metal foil are copper foil.

[0020] [Method 4]

[0021] The metal foil with a carrier according to any one of aspects 1 to 3, wherein the thickness C of the carrier T It is 6 μm or more and 18 μm or less.

[0022] [Method 5]

[0023] The metal foil with a carrier according to any one of aspects 1 to 4, wherein the tensile strength C of the carrier is F 50.0kgf / mm 2 above.

[0024] [Method 6]

[0025] The metal foil with a carrier according to any one of aspects 1 to 5, wherein the thickness B of the metal foil isT It is not less than 0.1 μm and not more than 6 μm.

[0026] [Method 7]

[0027] The metal foil with a carrier according to any one of aspects 1 to 6, wherein the metal foil has a tensile strength B F 50.0kgf / mm 2 above.

[0028] [Method 8]

[0029] The metal foil with a carrier according to any one of aspects 1 to 7, further comprising at least one layer selected from the group consisting of a roughened layer formed of a plurality of roughened particles, a rust-proofing layer, and a silane coupling agent layer on the metal foil.

[0030] [Method 9]

[0031] The metal foil with a carrier according to any one of aspects 1 to 8, further comprising an auxiliary metal layer between the release layer and the carrier and / or the metal foil.

[0032] [Method 10]

[0033] A metal-clad laminate comprising the metal foil with a carrier according to any one of aspects 1 to 9.

[0034] [Method 11]

[0035] A printed wiring board comprising the metal foil with a carrier according to any one of aspects 1 to 9.

[0036] [Method 12]

[0037] A method for manufacturing a printed circuit board, characterized in that the printed circuit board is manufactured using the metal foil with a carrier according to any one of the embodiments 1 to 9. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 This is a process flow chart for producing a metal-clad laminate using a metal foil with a carrier, and is a diagram for explaining the mechanism of residual metal generated by the fractured portion formed in the metal foil.

[0039] Figure 2 It is a top view of the copper foil with a carrier cut out and used for the measurement of the number of cracks in the examples, and shows the fixing area and the test area.

[0040] Figure 3 Yes Figure 2 Flow chart of the twisting process of the copper foil with carrier.

[0041] Figure 4It is a bar graph showing the α values ​​and the number of cracks calculated in Examples 1 to 9. DETAILED DESCRIPTION

[0042] Metal foil with carrier

[0043] The metal foil with a carrier of the present invention comprises a carrier, a peeling layer and a metal foil in this order. The metal foil with a carrier is obtained by the following formula:

[0044] α=193.07-(0.13×C T ×C F )-(0.75×B T ×B F )

[0045] (In the formula, C T is the thickness of the carrier (μm), C F is the tensile strength of the carrier (kgf / mm 2 ), B T is the thickness of the metal foil (μm), B F is the tensile strength of the metal foil (kgf / mm 2 )) The α value obtained is greater than -500 and less than 30.0. In this way, in the metal foil with a carrier, by controlling the α value calculated based on the thickness and tensile strength of the carrier and the thickness and tensile strength of the metal foil within a specified range, the occurrence of breakage or cracking of the metal foil during operation can be suppressed.

[0046] As described above, the breakage or cracking of the metal foil during the handling of the metal foil with a carrier may lead to the problem of residual metal in the printed circuit board manufacturing process. Figure 1 The mechanism of residual metal generated by the breakage of metal foil, etc. is explained. Figure 1 As shown in (i), when the metal foil 10 with a carrier having a carrier 12, a peeling layer (not shown) and a metal foil 14 is handled, the metal foil 14 may be broken to form a broken portion B. A resin layer 16 (e.g., prepreg) is laminated on the surface of the metal foil 14 side of the metal foil 10 with a carrier and hot pressed to obtain Figure 1 The metal-clad laminate 20 shown in (ii) is shown in FIG. Figure 1As shown in (ii), when there is a break B in the metal foil 14, the peripheral part of the break B of the metal foil 14 may be buried in the resin layer 16. Then, in the printed circuit board manufacturing process after the metal-clad laminate is made, the carrier 12 is peeled off from the metal-clad laminate 20, and the metal foil 14 is subjected to patterning including an etching process. However, the peripheral part of the break B of the metal foil 14 is buried in the resin layer 16, so when the metal foil 14 is etched, a part of the resin layer 16 exposed on the surface over the break B of the metal foil 14 functions as an etching resist. As a result, it is difficult to remove the peripheral part of the break B in the metal foil 14 by etching, resulting in residual metal.

[0047] The inventors of the present invention have conducted research on this issue, and the results show that the breakage or cracking of the metal foil during the operation of the metal foil with a carrier is affected not only by the tensile strength of the metal foil itself, but also by the tensile strength of the carrier. It is also found that by controlling the α value calculated by the above formula that takes into account the thickness of the tensile strength of the carrier and the tensile strength of the metal foil to be less than 30.0, the breakage or cracking of the metal foil during operation can be effectively suppressed. It should be noted that the smaller the α value, the more it can suppress the breakage or cracking of the metal foil, but from the perspective of fully coping with the thinning of the carrier, etc., and the perspective of the tensile strength that can be achieved, it is realistic for the α value to be above -500.

[0048] From the viewpoint of the above-mentioned effects, the α value of the metal foil with a carrier is from -500 to 30.0, preferably from -250 to 25.0, more preferably from -100 to 15.0, further preferably from -50.0 to 10.0, particularly preferably from -15.0 to 10.0.

[0049] The carrier is a support for supporting the metal foil to improve its operability, and a typical carrier includes a metal layer. Examples of such carriers include aluminum foil, copper foil, stainless steel (SUS) foil, resin films with metal coatings on the surface such as copper, glass, etc., preferably copper foil. The copper foil can be any one of rolled copper foil and electrolytic copper foil, preferably electrolytic copper foil.

[0050] Carrier thickness C T Typically, it is 250 μm or less, more typically, it is 200 μm or less, and from the viewpoint of reducing CO2 during manufacturing, it is preferably 6 μm or more and 18 μm or less, more preferably 7 μm or more and 16 μm or less, further preferably 8 μm or more and 14 μm or less, and particularly preferably 8 μm or more and 12 μm or less. A preferred method for measuring the thickness of the carrier is shown in the examples described below.

[0051] Tensile strength of carrier CF Preferably 50.0kgf / mm 2 More preferably, 50.0 kgf / mm 2 Above and 100.0kgf / mm 2 Below, more preferably 50.0 kgf / mm 2 Above and 80.0kgf / mm 2 Below, particularly preferably 55.0 kgf / mm 2 Above and 70.0kgf / mm 2 Below, most preferably 55.0kgf / mm 2 Above and 65.0kgf / mm 2 Thus, by increasing the tensile strength C of the carrier F , the metal foil can be firmly supported to ensure stability during operation, and the occurrence of breakage and cracking of the metal foil can be more effectively suppressed. The numerical values ​​of each tensile strength in this specification refer to the values ​​measured according to IPC-TM-650 2.4.18.

[0052] The metal foil is preferably copper foil or copper alloy foil, more preferably copper foil. The metal foil may be either electrolytic foil or rolled foil, but is preferably electrolytic foil (particularly preferably electrolytic copper foil).

[0053] Thickness of metal foil B T Typically, it is less than 18 μm. From the viewpoint of circuit thinning and improved laser processability, it is preferably between 0.1 μm and 6 μm, more preferably between 0.1 μm and 4 μm, further preferably between 0.3 μm and 3.0 μm, and particularly preferably between 0.5 μm and 2.5 μm. It should be noted that in this specification, copper foil having a thickness in the above range is sometimes referred to as ultra-thin copper foil. When the metal foil with a carrier includes an auxiliary layer (such as a roughening layer, an anti-rust treatment layer, a silane coupling agent layer, an auxiliary metal layer, etc. described later) between the peeling layer and the metal foil or on the metal foil, the thickness of the auxiliary layer is included in the thickness of the metal foil. The preferred method for measuring the thickness of the metal foil is shown in the embodiments described later.

[0054] Tensile strength of metal foil B F Preferably 50.0kgf / mm 2 More preferably, 50.0 kgf / mm 2 Above and 100.0kgf / mm 2 Below, more preferably 55.0kgf / mm 2 Above and 80.0kgf / mm 2 Below, particularly preferably 60.0 kgf / mm 2 Above and 70.0kgf / mm2 Below, most preferably 60.0kgf / mm 2 Above and 65.0kgf / mm 2 By improving the tensile strength of the metal foil in this way, the durability against direct loads on the metal foil can be improved when the metal foil with a carrier is handled, and the occurrence of breakage and cracks in the metal foil can be more effectively suppressed. It should be noted that when the tensile strength of a single metal foil is difficult to measure due to its thinness, the tensile strength of the metal foil can be satisfactorily calculated by the steps shown in the examples described below.

[0055] Tensile strength of metal foil B F Tensile strength relative to carrier C F The ratio (=B F / C F ) is preferably 0.70 to 1.40, more preferably 0.80 to 1.30, further preferably 0.90 to 1.20, and particularly preferably 0.95 to 1.15. By controlling the tensile strength of both the carrier and the metal foil within this range, the occurrence of breakage and cracking of the metal foil can be more effectively suppressed.

[0056] From the viewpoint of further effectively suppressing the occurrence of breakage and cracking of the metal foil in the printed circuit board manufacturing process, the metal foil with a carrier preferably maintains a specified tensile strength of the carrier and / or the metal foil even after the heat treatment. Therefore, the tensile strength of the carrier (peel strength after heating) after the metal foil with a carrier is heated at 250°C for 60 minutes is preferably 45.0 kgf / mm 2 More preferably 45.0kgf / mm 2 Above and 95.0kgf / mm 2 Below, more preferably 45.0kgf / mm 2 Above and 75.0kgf / mm 2 Below, particularly preferably 50.0 kgf / mm 2 Above and 65.0kgf / mm 2 Below, most preferably 50.0kgf / mm 2 Above and 60.0kgf / mm 2 In addition, the tensile strength of the metal foil after heating the metal foil with a carrier at 250° C. for 60 minutes (peel strength after heating) is preferably 45.0 kgf / mm 2 More preferably 45.0kgf / mm 2 Above and 95.0kgf / mm 2 Below, more preferably 50.0 kgf / mm 2 Above and 75.0kgf / mm2 Below, particularly preferably 55.0 kgf / mm 2 Above and 65.0kgf / mm 2 Below, most preferably 55.0kgf / mm 2 Above and 60.0kgf / mm 2 the following.

[0057] As required, the surface of the metal foil can be roughened to form a roughening layer. By having a roughening layer on the metal foil, the adhesion with the resin layer during the manufacture of the metal-clad laminate or printed circuit board can be improved. The roughening layer has a plurality of roughening particles (protrusions), and these plurality of roughening particles are preferably formed by metal particles, more preferably by copper particles. Copper particles can be formed by metallic copper or by copper alloys. The roughening treatment for forming the roughening treatment surface can be preferably carried out by forming roughening particles with metal or alloy on the metal foil. For example, it is preferably roughened according to a plating method through at least 2 plating processes, and the plating process includes a sintering process for precipitating fine metal particles attached to the metal foil and a coated plating process for preventing the fine metal particles from falling off.

[0058] As required, the surface of the metal foil can be subjected to rust-proof treatment to form a rust-proof treatment layer. The rust-proof treatment preferably includes a plating treatment using zinc. The plating treatment using zinc can be any one of a galvanizing treatment and a zinc alloy plating treatment, and the zinc alloy plating treatment is particularly preferably a zinc-nickel alloy treatment. The zinc-nickel alloy treatment can be a plating treatment containing at least Ni and Zn, and can also contain other elements such as Sn, Cr, and Co. The Ni / Zn adhesion ratio in the zinc-nickel alloy plating is preferably 1.2 or more and 10 or less in terms of mass ratio, more preferably 2 or more and 7 or less, and further preferably 2.7 or more and 4 or less. In addition, the rust-proof treatment preferably also includes a chromate treatment, and the chromate treatment is more preferably performed on the surface of the zinc plating after the zinc plating treatment. Thus, the rust resistance can be further improved. A particularly preferred rust-proof treatment is a combination of a zinc-nickel alloy plating treatment and a subsequent chromate treatment.

[0059] As required, the surface of the metal foil can be treated with a silane coupling agent to form a silane coupling agent layer. This can improve moisture resistance, chemical resistance, and adhesion to adhesives, etc. The silane coupling agent layer can be formed by appropriately diluting the silane coupling agent, applying it, and drying it. Examples of silane coupling agents include epoxy-functional silane coupling agents such as 4-glycidylbutyltrimethoxysilane and 3-glycidoxypropyltrimethoxysilane, or 3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N-3-(4-(3-aminopropoxy)butoxy)propyl-3-aminopropyltrimethoxysilane, N-phenyl-3-aminopropyl The present invention can be used as the silane coupling agent of claim 1, wherein the silane coupling agent comprises an amino-functional silane coupling agent such as trimethoxy silane, a mercapto-functional silane coupling agent such as 3-mercaptopropyltrimethoxy silane, an olefin-functional silane coupling agent such as vinyltrimethoxy silane and vinylphenyltrimethoxy silane, an acrylic-functional silane coupling agent such as 3-methacryloxypropyltrimethoxy silane, an imidazole-functional silane coupling agent such as imidazole silane, or a triazine-functional silane coupling agent such as triazine silane.

[0060] Therefore, the metal foil with a carrier preferably further comprises at least one layer selected from the group consisting of a roughening layer formed by a plurality of roughening particles, a rust-proofing layer, and a silane coupling agent layer on the metal foil. For example, when the metal foil with a carrier further comprises a roughening layer, a rust-proofing layer, and a silane coupling agent layer, the order of constituting these layers is not particularly limited, and it is preferred that the roughening layer, the rust-proofing layer, and the silane coupling agent layer are sequentially stacked on the metal foil.

[0061] The metal foil with a carrier has a peeling layer on the carrier. The peeling layer is a layer that has the function of weakening the peeling strength of the carrier, ensuring the stability of the strength, and further suppressing the mutual diffusion that may occur between the carrier and the metal foil during press forming at high temperature. The peeling layer is usually formed on one side of the carrier, and can also be formed on both sides. The peeling layer can be any of an organic peeling layer and an inorganic peeling layer. Examples of organic components used in the organic peeling layer include nitrogen-containing organic compounds, sulfur-containing organic compounds, carboxylic acids, etc. Examples of nitrogen-containing organic compounds include triazole compounds, imidazole compounds, etc. Among them, triazole compounds are preferred from the perspective of easy and stable peeling properties. Examples of triazole compounds include 1,2,3-benzotriazole, carboxybenzotriazole, N',N'-bis(benzotriazolylmethyl)urea, 1H-1,2,4-triazole, and 3-amino-1H-1,2,4-triazole. Examples of sulfur-containing organic compounds include mercaptobenzothiazole, thiocyanuric acid, 2-benzimidazole mercaptan, etc. Examples of carboxylic acids include monocarboxylic acids, dicarboxylic acids, etc. On the other hand, examples of inorganic components used in the inorganic peeling layer include Ni, Mo, Co, Cr, Fe, Ti, W, P, Zn, chromate-treated films, etc. The thickness of the peeling layer is typically 1 nm or more and 1 μm or less, preferably 5 nm or more and 500 nm or less.

[0062] Other functional layers may also be provided between the peeling layer and the carrier and / or the metal foil. As examples of such other functional layers, auxiliary metal layers may be cited. The auxiliary metal layer is preferably formed of nickel and / or cobalt. By forming such an auxiliary metal layer on the surface side of the carrier and / or the surface side of the metal foil, it is possible to further suppress the mutual diffusion that may occur between the carrier and the metal foil during hot pressing at high temperature or for a long time, and ensure the stability of the peel strength of the carrier. The thickness of the auxiliary metal layer is preferably not less than 0.001 μm and not more than 3 μm.

[0063] Method for producing metal foil with carrier

[0064] The metal foil with a carrier of the present invention can be produced by (1) preparing a carrier, (2) forming a release layer on the carrier, and (3) forming the metal foil on the release layer. An example of a preferred method for producing the metal foil with a carrier of the present invention is described below.

[0065] (1) Preparation of vector

[0066] First, a carrier is prepared as a support. A typical carrier includes a metal layer. As examples of such a carrier, as described above, aluminum foil, copper foil, stainless steel (SUS) foil, resin film with a metal coating on the surface with copper or the like, glass, etc. can be cited, preferably copper foil. The copper foil can be any one of rolled copper foil and electrolytic copper foil, preferably electrolytic copper foil.

[0067] When electrolytic copper foil is used as a carrier, the conditions for electrolytic foil making are preferably as follows. That is, a sulfuric acid-based copper electrolyte solution is used in which the copper concentration is set to 60 g / L or more and 85 g / L or less (more preferably 50 g / L or more and 70 g / L or less), the sulfuric acid concentration is set to 100 g / L or more and 250 g / L or less (more preferably 200 g / L or more and 250 g / L or less), the chlorine concentration is set to 1 mg / L or more and 3 mg / L or less (more preferably 1 mg / L or more and 2 mg / L or less), and the concentration of gelatin as an additive is adjusted to 0.3 mg / L or more and 5 mg / L or less (more preferably 1 mg / L or more and 3 mg / L or less), a DSA (dimensional stability anode) is used as the anode, and the liquid temperature is 40°C or more and 60°C or less (more preferably 50°C or more and 60°C or less), and the current density is 30 A / dm 2 Above and 75A / dm 2 Below (more preferably 40A / dm 2 Above and 60A / dm 2 By electrolyzing the electrolytic copper foil with the desired tensile strength (less than 100 mg / L), it is possible to preferably obtain an electrolytic copper foil with the desired tensile strength. As an additive, potassium iodide (iodine concentration of 1 mg / L or more and 10 mg / L or less) or polyethyleneimine with a molecular weight of 3000 or more (concentration of 30 mg / L or more and 200 mg / L or less) can be used instead of gelatin. By adding gelatin or the like as an additive to the electrolyte and controlling the electrolysis conditions within the above range to carry out electrolytic foil making, it is easy to form a carrier with high tensile strength, and as a result, it is easy to control the α value within the specified range. In addition, when the copper foil with a carrier is heat-treated, the decrease in the tensile strength of the carrier can be suppressed.

[0068] (2) Formation of the peeling layer

[0069] A peeling layer is formed on a carrier. The peeling layer may be any of an organic peeling layer and an inorganic peeling layer. Preferred examples of the organic peeling layer and the inorganic peeling layer are as described above. The peeling layer may be formed by bringing a solution containing peeling layer components into contact with at least one surface of the carrier, fixing the peeling layer components on the surface of the carrier, etc. When the carrier is brought into contact with the solution containing peeling layer components, the contact may be carried out by immersing the carrier in the solution containing peeling layer components, spraying the solution containing peeling layer components, or letting the solution containing peeling layer components flow down. In addition, a method of forming a film of the peeling layer components by a vapor phase method such as evaporation or sputtering may also be used. In addition, fixing of the peeling layer components to the carrier surface may be carried out by adsorption of the solution containing the peeling layer components, drying, or electrodeposition of the peeling layer components in the solution containing the peeling layer components, etc.

[0070] (3) Formation of metal foil

[0071] A metal foil is formed on the peeling layer. For example, the metal foil can be formed by a wet film forming method such as a chemical metal plating method and an electrolytic metal plating method, a dry film forming method such as sputtering and chemical vapor deposition, or a combination thereof. The ultra-thin copper foil is preferably formed by an electrolytic copper plating method. In particular, from the viewpoint of improving the tensile strength of the ultra-thin copper foil, the conditions for electrolytically forming the ultra-thin copper foil are preferably set as follows. That is, a sulfuric acid-based copper electrolyte is used in which the copper concentration is set to 40 g / L or more and 80 g / L or less (more preferably 50 g / L or more and 70 g / L or less), the sulfuric acid concentration is set to 180 g / L or more and 260 g / L or less (more preferably 200 g / L or more and 250 g / L or less), the concentration of carboxybenzotriazole (CBTA) as an additive is adjusted to more than 0 ppm and less than 200 ppm, a DSA (dimensional stability anode) is used as an anode, and the liquid temperature is 35° C. or more and 60° C. or less (more preferably 40° C. or more and 55° C. or less), and the current density is 3 A / dm 2 Above and 80A / dm 2 Below (more preferably 5A / dm 2 Above and 80A / dm 2 Below, more preferably 6A / dm 2 Above and 75A / dm 2 The desired electrolytic copper foil can be preferably obtained by electrolyzing the electrolytic copper foil with a concentration of CBTA in the electrolyte solution (less than 0.1 ppm). The CBTA concentration in the electrolyte solution is more preferably 0.1 ppm to 100 ppm, further preferably 0.1 ppm to 50 ppm, particularly preferably 0.1 ppm to 30 ppm, and most preferably 0.1 ppm to 10 ppm. By adding carboxybenzotriazole (CBTA) as an additive to the electrolyte solution and controlling the electrolysis conditions within the above range to perform electrolytic foil making, it is easy to form a metal foil with high tensile strength, and as a result, it is easy to control the α value within the specified range. In addition, when the copper foil with a carrier is heat-treated, the decrease in the tensile strength of the metal foil can be suppressed.

[0072] If necessary, the surface of the metal foil may be subjected to a roughening treatment, a rustproofing treatment and / or a silane coupling agent treatment to form a roughening layer, a rustproofing treatment layer and / or a silane coupling agent layer formed of a plurality of roughening particles. These treatments are as described above.

[0073] Metal-clad laminate

[0074] The metal foil with a carrier of the present invention is preferably used for the production of a metal-clad laminate for a printed circuit board. That is, according to a preferred embodiment of the present invention, a metal-clad laminate (more preferably a copper-clad laminate) having the above-mentioned metal foil with a carrier is provided. The metal-clad laminate comprises: a metal foil with a carrier having a carrier, a peeling layer and a metal foil in sequence; and a resin layer disposed on the surface of the metal foil in the metal foil with a carrier (the surface of the metal foil on the opposite side of the peeling layer). The above-mentioned preferred embodiment of the metal foil with a carrier is also directly applicable to the metal foil with a carrier possessed by the metal-clad laminate. The metal foil with a carrier can be disposed on a single side of the resin layer or on both sides. The resin layer contains a resin, preferably an insulating resin. The resin layer is preferably a prepreg and / or a resin sheet. Prepreg refers to a general term for composite materials impregnated with synthetic resins in substrates such as synthetic resin plates, glass plates, glass woven fabrics, glass nonwoven fabrics, and paper. As preferred examples of insulating resins, epoxy resins, cyanate resins, bismaleimide triazine resins (BT resins), polyphenylene ether resins, phenolic resins, etc. can be cited. In addition, as examples of insulating resins constituting resin sheets, insulating resins such as epoxy resins, polyimide resins, and polyester resins can be cited. In addition, from the viewpoint of improving insulation, the resin layer may contain filler particles formed by various inorganic particles such as silica and alumina. The thickness of the resin layer is not particularly limited, preferably 1 μm or more and 1000 μm or less, more preferably 2 μm or more and 400 μm or less, and further preferably 3 μm or more and 200 μm or less. The resin layer may be composed of multiple layers. Resin layers such as prepregs and / or resin sheets may be provided on a metal foil with a carrier by means of a primer resin layer pre-coated on the surface of the metal foil.

[0075] Printed Circuit Board

[0076] The metal foil with a carrier of the present invention is preferably used for the production of printed circuit boards. That is, according to a preferred embodiment of the present invention, a printed circuit board or a method for manufacturing the same is provided. The printed circuit board of this embodiment comprises a layer structure in which a resin layer and a metal layer are sequentially stacked. In addition, regarding the resin layer, as described with respect to the metal-clad laminate. In short, the printed circuit board can adopt a known layer structure. As specific examples related to printed circuit boards, there can be listed: a single-sided or double-sided printed circuit board in which a circuit is formed after the metal foil of the present invention is bonded to one or both sides of a prepreg and cured to form a laminate, and a multilayer printed circuit board formed by multilayering them, etc. In addition, as other specific examples, flexible printed circuit boards, COFs, TAB tapes, etc. in which a circuit is formed by forming the metal foil of the present invention on a resin film can also be listed. Furthermore, as other specific examples, there can be listed: a metal foil with resin coated with the above-mentioned resin layer formed on the metal foil of the present invention, after laminating the resin layer as an insulating adhesive material layer on the above-mentioned printed circuit board, using the metal foil as all or part of the circuit layer to form a circuit by a modified semi-additive method (MSAP), a subtractive method, etc.; a build-up circuit board in which the metal foil is removed and a circuit is formed by a semi-additive method (SAP); a direct build-up wafer in which the lamination of the metal foil with resin and the formation of the circuit are repeated alternately on a semiconductor integrated circuit, etc. The metal foil with a carrier of the present invention can also be preferably used in a manufacturing method using a coreless build-up method that does not use a so-called core substrate but uses an insulating resin layer and a conductor layer to be alternately laminated.

[0077] Example

[0078] The present invention is further specifically described by the following examples.

[0079] Example 1~Example 9

[0080] Copper foil with carrier was produced and evaluated as follows.

[0081] (1) Preparation of vector

[0082] For Examples 1 to 5 and 9, a copper electrolyte solution with the following composition, a cathode and a DSA (dimensional stability anode) as an anode were used, and the electrolyte solution was subjected to a current density of 60 A / dm at a solution temperature of 50°C. 2 Electrolysis is performed under the conditions of 0.1% to obtain an electrolytic copper foil of a specified thickness as a carrier.

[0083] <Composition of copper electrolyte>

[0084] -Copper concentration: 80g / L

[0085] - Sulfuric acid concentration: 250g / L

[0086] -Chlorine concentration: 1.5mg / L

[0087] - Gelatin concentration: 2mg / L

[0088] On the other hand, for Examples 6 to 8, a copper electrolyte solution with the following composition, a cathode, and a DSA (dimensional stability anode) as an anode were used, and the electrolyte solution was subjected to a temperature of 50° C. and a current density of 70 A / dm 2 Electrolysis is performed under the conditions of 0.1% to obtain an electrolytic copper foil of a specified thickness as a carrier.

[0089] <Composition of copper electrolyte>

[0090] -Copper concentration: 80g / L

[0091] - Sulfuric acid concentration: 300g / L

[0092] -Chlorine concentration: 30mg / L

[0093] -Glue concentration: 5mg / L

[0094] (2) Formation of the peeling layer

[0095] The electrode surface of the carrier that has been acid-washed is immersed in a carboxybenzotriazole (CBTA) aqueous solution containing 1 g / L CBTA concentration, 150 g / L sulfuric acid concentration, and 10 g / L copper concentration at a liquid temperature of 30° C. for 30 seconds to allow the CBTA component to be adsorbed on the electrode surface of the carrier. In this way, a CBTA layer is formed on the electrode surface of the carrier as an organic release layer.

[0096] (3) Formation of auxiliary metal layer

[0097] The support having the organic release layer formed thereon was immersed in a solution containing 20 g / L of nickel prepared using nickel sulfate at a solution temperature of 45°C, a pH of 3, and a current density of 5 A / dm 2 Under the condition of , nickel with a deposition amount corresponding to a thickness of 0.001 μm is deposited on the organic release layer. Thus, a nickel layer is formed on the organic release layer as an auxiliary metal layer.

[0098] (4) Formation of ultra-thin copper foil

[0099] The support with the auxiliary metal layer formed thereon was immersed in a copper solution of the following composition at a solution temperature of 50°C and a current density of 5 A / dm 2 Above and 40A / dm 2 The following (Examples 1 to 8) or 70A / dm 2 (Example 9) electrolysis is performed to form an ultra-thin copper foil of a specified thickness as a metal foil on the auxiliary metal layer.

[0100] <Solution Composition>

[0101] -Copper concentration: 60g / L

[0102] - Sulfuric acid concentration: 200g / L

[0103] -CBTA concentration: 5.0 ppm (Examples 1, 3-7 and 9) or 0 ppm (Examples 2 and 8)

[0104] (5) Roughening treatment

[0105] The surface of the ultra-thin copper foil thus formed is roughened to form a roughened copper foil, thereby obtaining a copper foil with a carrier. The roughening treatment consists of a sintering process to precipitate fine copper particles on the ultra-thin copper foil and a coating process to prevent the fine copper particles from falling off. In the sintering process, 9-phenylacridine (9PA) and chlorine are added to an acidic copper sulfate solution at a temperature of 25°C containing a copper concentration of 10 g / L and a sulfuric acid concentration of 200 g / L, respectively, so that the 9PA concentration is 60 ppm and the chlorine concentration is 50 ppm, and the current density is 20 A / dm 2 In the subsequent coating plating step, an acidic copper sulfate solution containing a copper concentration of 70 g / L and a sulfuric acid concentration of 240 g / L was used at a liquid temperature of 52°C and a current density of 15 A / dm 2 Electrodeposition was carried out under smooth plating conditions.

[0106] (6) Anti-rust treatment

[0107] The roughened surface of the copper foil with carrier was subjected to rust prevention treatment including zinc-nickel alloy plating and chromate treatment. First, a solution containing 1 g / L zinc, 2 g / L nickel and 80 g / L potassium pyrophosphate was used at a temperature of 40°C and a current density of 0.5 A / dm 2 The roughened layer and the carrier were treated with zinc-nickel alloy plating under the conditions of 1.5 % and 1.5 % respectively. Then, an aqueous solution containing 1 g / L of chromic acid was used at pH 12 and a current density of 1 A / dm 2 Under the conditions of , the surface treated with zinc-nickel alloy was chromated.

[0108] (7) Silane coupling agent treatment

[0109] The silane coupling agent treatment was performed by adsorbing a commercially available aqueous solution containing a silane coupling agent on the surface of the roughened copper foil side of the copper foil with a carrier, and evaporating the water with an electric heater. At this time, the carrier side was not treated with the silane coupling agent.

[0110] (8) Evaluation

[0111] The copper foil with a carrier thus obtained was evaluated for various properties as follows.

[0112] (8a) Thickness

[0113] The thickness of the carrier and the ultra-thin copper foil of the copper foil with carrier was measured as follows. First, the copper foil with carrier was cut into 100 mm squares, and the weight W thereof was measured using an electronic balance. A Next, the carrier was peeled off from the copper foil with the carrier, and the weight W of the carrier was measured using an electronic balance. C Then, by the weight W C Calculate the thickness C of the carrier based on the specific gravity of copper T , and by the weight W A and weight W C The difference (=W A -W C ) and the specific gravity of copper to calculate the thickness of the ultra-thin copper foil B T The results are shown in Table 1.

[0114] (8b) Tensile strength

[0115] The tensile strength of the carrier and the ultra-thin copper foil was measured as follows. First, the tensile strength A of the copper foil with the carrier was measured according to IPC-TM650 2.4.18. F (kgf / mm 2 ). Next, the carrier was peeled off from the copper foil with the carrier, and the tensile strength C of the carrier was measured according to IPC-TM650 2.4.18. F (kgf / mm 2 ). The tensile strength of the ultra-thin copper foil is difficult to measure by the same method due to its thinness, so it is calculated as follows. The tensile strength A of the copper foil with a carrier F (kgf / mm 2 ), tensile strength C of the carrier F (kgf / mm 2 ) multiplied by the cross-sectional area of ​​each test piece is defined as A F '(kgf), C F '(kgf), the cross-sectional area of ​​the ultra-thin copper foil test piece is set to B A (mm 2 ), will be passed through (A F '-C F ') / B A The value calculated by the formula is set as the tensile strength B of the ultra-thin copper foil F The results are shown in Table 1.

[0116] (8c) Crack number determination

[0117] As an indicator of the damage resistance of the ultra-thin copper foil, the number of cracks was measured as follows. Figure 2As shown in FIG. 1 , the copper foil with carrier is cut into 150 mm squares. Next, one side of the cut copper foil with carrier 30 is fixed with a width of 25 mm. Then, the side opposite to the fixed side is held, and the copper foil with carrier 30 is twisted twice on each side. The twist imparts Figure 3 As shown in (i) to (iii) of FIG. 1 , the copper foil 30 with a carrier is set to a horizontal state until it is at an angle of 45° relative to the horizontal plane. After the fixation is released, the copper foil 30 with a carrier is rotated 90° and the twisting process is performed again. In this way, the twisting process is performed on all four sides of the copper foil 30 with a carrier. Then, as shown in FIG. Figure 2 As shown in the figure, the center portion of the cut copper foil 30 with a carrier, that is, 100 mm×100 mm (=1 dm 2 ) test area, and counted the number of cracks generated on the surface of the ultra-thin copper foil side using an optical microscope. The operation was performed more than 3 times for each case, and the average value was taken as the number of cracks. The results are shown in Tables 1 and Figure 4 shown.

[0118] [Table 1]

[0119] Table 1

[0120]

[0121] * indicates a comparative example.

[0122] From Table 1 and Figure 4 The results shown show that in Examples 1, 3 to 5 and 9 where the α value is less than 30.0, the number of cracks is significantly suppressed compared to Examples 2 and 6 to 8 where the α value exceeds 30.0. In addition, multiple regression analysis was performed using the number of cracks as the target variable and the thickness and tensile strength of the carrier and the thickness and tensile strength of the ultra-thin copper foil as explanatory variables. The results showed that the coefficient of determination after the degree of freedom was adjusted (corrected R 2 ) was 0.86, confirming that the reliability of the calculation formula for the α value was sufficiently high.

Claims

1. A metal foil with a carrier, comprising a carrier, a release layer and a metal foil in this order, The α value of the metal foil with a carrier obtained by the following formula is not less than -500 and not more than 30.0: α=193.07-(0.13×C T ×C F )-(0.75×B T ×B F ) In the formula, C T is the thickness of the carrier (μm), C F is the tensile strength of the carrier (kgf / mm 2 ), B T is the thickness of the metal foil (μm), B F is the tensile strength of the metal foil (kgf / mm 2 ).

2. The metal foil with a carrier according to claim 1, wherein The α value is greater than or equal to -250 and less than or equal to 25.

0.

3. The metal foil with a carrier according to claim 1 or 2, wherein The carrier and the metal foil are both copper foils.

4. The metal foil with a carrier according to claim 1 or 2, wherein The thickness C of the carrier T It is 6 μm or more and 18 μm or less.

5. The metal foil with a carrier according to claim 1 or 2, wherein The tensile strength C of the carrier F 50.0kgf / mm 2 above.

6. The metal foil with a carrier according to claim 1 or 2, wherein: The thickness B of the metal foil T It is not less than 0.1 μm and not more than 6 μm.

7. The metal foil with a carrier according to claim 1 or 2, wherein: The tensile strength B of the metal foil F 50.0kgf / mm 2 above.

8. The metal foil with a carrier according to claim 1 or 2, wherein The metal foil further includes at least one layer selected from the group consisting of a roughened layer formed by a plurality of roughened particles, a rust-proofing layer, and a silane coupling agent layer.

9. The metal foil with a carrier according to claim 1 or 2, wherein: An auxiliary metal layer is further provided between the release layer and the carrier and / or the metal foil. 10 . A metal-clad laminate comprising the metal foil with a carrier according to claim 1 or 2. 11 . A printed wiring board comprising the metal foil with a carrier according to claim 1 or 2.

12. A method for manufacturing a printed circuit board, characterized in that: A printed circuit board is produced using the metal foil with a carrier according to claim 1 or 2.

Citation Information

Patent Citations

  • Copper foil with attached carrier foil and copper-clad laminate

    CN105745360A

  • Flexible copper clad laminate, film carrier tape manufactured using the same, and method for manufacturing same, and flexible printed circuit board, and semiconductor device

    CN1972557A