Rubber composition for heavy duty tire

The existing solution is solved by using a combination of a conjugated diene polymer with a glass transition temperature below -60°C in a heavy-duty tire rubber composition, combined with a silane coupling agent and a crosslinker, in a heavy-duty tire rubber composition. The problems of low heat generation, wear resistance and stone impact resistance in the technology have significantly improved the performance of rubber crosslinkers and are suitable for high-load tire applications.

CN118900884APending Publication Date: 2024-11-05ZEON CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380029127.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-30
Filing Date
2023-03-09
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The existing heavy-load tire rubber compositions are difficult to meet the requirements of low heat generation, wear resistance and stone impact resistance at the same time, especially the technology of Patent Document 1 is not performing well in this regard.

Method used

Using a conjugated diene polymer with a glass transition temperature below -60°C and having functional groups interacting with silica, combined with silica and carbon black, an optimized rubber composition is formed, and the silane coupling agent and cross-section is carried out. The coupling agent was crosslinked to prepare rubber crosslinked substances with excellent heat generation, wear resistance and stone impact resistance.

Benefits of technology

The heavy-load tire rubber composition has achieved a significant improvement in low heat generation, wear resistance and stone impact resistance, and is suitable for high-load application scenarios such as truck and bus tires.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005052186850000141
    Figure BDA0005052186850000141
  • Figure BDA0005052186850000151
    Figure BDA0005052186850000151
  • Figure BDA0005052186850000181
    Figure BDA0005052186850000181
Patent Text Reader

Abstract

The present invention provides a rubber composition for a heavy duty tire, the rubber composition containing a conjugated diene polymer and silica, the conjugated diene polymer having a glass transition temperature (Tg) of-60 DEG C or less and having a functional group capable of interacting with silica.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a rubber composition for heavy-load tires, which can form a rubber cross-linked product having low heat build-up, excellent wear resistance and stone chip resistance, and can be preferably used for heavy-load tires. Background Art

[0002] For heavy-duty tires used as truck and bus tires, it is important to have excellent wear resistance and stone impact resistance, so that the tire life is long. On the other hand, in recent years, due to environmental problems and resource problems, the requirement for low heat generation (low fuel consumption) has been continuously improved. In order to give low heat generation to heavy-duty tires, it has been studied to mix silica in heavy-duty tire rubber compositions, but there is a problem of reduced wear resistance.

[0003] For example, Patent Document 1 discloses a rubber composition for a heavy-duty tire, characterized in that 40 to 60 parts by mass of CTAB having an adsorption specific surface area of ​​180 to 300 m2 is added to 100 parts by mass of a rubber component composed of 55 to 70 parts by mass of natural rubber and 30 to 45 parts by mass of butadiene rubber. 2 / g of silica, 3 to 10 parts by mass of nitrogen adsorption specific surface area of ​​110 to 150 m 2 / g of carbon black, and 6 to 15% by mass of a silane coupling agent having a sulfur bond based on the amount of the above-mentioned silica.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent document 1: Japanese Patent Application Publication No. 2019-056068. Summary of the invention

[0007] Problem that the invention aims to solve

[0008] In recent years, the requirements for low heat generation, wear resistance and stone impact resistance of heavy-duty tires have been continuously improved, but the technology of Patent Document 1 cannot meet the high requirements for low heat generation, wear resistance and stone impact resistance. Therefore, from the perspective of preferably using it for heavy-duty tires, it is required to further improve the low heat generation, wear resistance and stone impact resistance.

[0009] The present invention has been made in view of such actual conditions, and an object of the present invention is to provide a rubber composition for a heavy-load tire that can form a rubber cross-linked product having low heat build-up properties, excellent wear resistance, and excellent stone chip resistance.

[0010] The present inventors have conducted intensive studies to achieve the above-mentioned object and have found that the above-mentioned object can be achieved by using a conjugated diene polymer having a glass transition temperature (Tg) of -60°C or less and having a functional group capable of interacting with silica as a conjugated diene polymer and by blending silica therein to form a rubber composition, thereby completing the present invention.

[0011] That is, according to the present invention, there is provided a rubber composition for a heavy load tire, comprising a conjugated diene polymer and silica, wherein the conjugated diene polymer has a glass transition temperature (Tg) of -60°C or lower and has a functional group capable of interacting with silica.

[0012] In the rubber composition for a heavy load tire of the present invention, it is preferred that the conjugated diene monomer units constituting the conjugated diene polymer have a vinyl bond content of 5 to 40% by weight.

[0013] In the rubber composition for a heavy-load tire of the present invention, it is preferred that the silica has a nitrogen adsorption specific surface area of ​​30 to 500 m2 as measured by a BET method. 2 / g.

[0014] In the rubber composition for a heavy load tire of the present invention, the content of the silica is preferably 10 to 200 parts by weight based on 100 parts by weight of the rubber component containing the conjugated diene polymer.

[0015] The rubber composition for a heavy-duty tire of the present invention preferably further contains carbon black. In this case, it is more preferred that the carbon black has a nitrogen adsorption specific surface area of ​​30 m2 as measured by the BET method. 2 In addition, the carbon black content is more preferably 10 to 200 parts by weight based on 100 parts by weight of the rubber component containing the conjugated diene polymer.

[0016] In the rubber composition for a heavy load tire of the present invention, the content of the conjugated diene polymer is preferably 10 to 80% by weight based on 100% by weight of the total rubber components.

[0017] The rubber composition for a heavy load tire of the present invention preferably further contains natural rubber, and the content of the natural rubber is 10 to 80% by weight based on 100% by weight of the total rubber components.

[0018] In the rubber composition for a heavy-duty tire of the present invention, it is preferred that the functional group capable of interacting with the silica in the conjugated diene polymer is a functional group having Si-OR a (Where R a A group having a structure represented by a hydrogen atom or a hydrocarbon group which may have a substituent.

[0019] The rubber composition for a heavy load tire of the present invention preferably further contains a silane coupling agent.

[0020] The rubber composition for a heavy load tire of the present invention preferably further contains a cross-linking agent.

[0021] Furthermore, according to the present invention, there is provided a cross-linked rubber obtained by cross-linking the rubber composition for a heavy load tire of the present invention.

[0022] Furthermore, according to the present invention, there is provided a heavy load tire comprising the above-mentioned rubber cross-linked product of the present invention.

[0023] Effects of the Invention

[0024] According to the present invention, there can be provided a rubber composition for a heavy load tire which can form a rubber cross-linked product having low heat build-up properties, excellent wear resistance, and excellent stone chip resistance. DETAILED DESCRIPTION

[0025] The rubber composition for a heavy load tire of the present invention contains a conjugated diene polymer and silica. The conjugated diene polymer has a glass transition temperature (Tg) of -60°C or lower and has a functional group capable of interacting with silica.

[0026] <Conjugated diene polymer>

[0027] The conjugated diene polymer used in the present invention is a polymer having a glass transition temperature (Tg) of -60°C or less and having a functional group capable of interacting with silica. In the present invention, as a conjugated diene polymer, a conjugated diene polymer having a glass transition temperature (Tg) of -60°C or less and having a functional group capable of interacting with silica described later is used, and it is combined with silica, thereby enabling the obtained rubber cross-linked product to be a rubber cross-linked product having low heat generation, wear resistance and excellent stone impact resistance.

[0028] The conjugated diene polymer having a glass transition temperature (Tg) of -60°C or less and having a functional group capable of interacting with silica (hereinafter appropriately referred to as "conjugated diene polymer") used in the present invention is mainly composed of conjugated diene monomer units and has a functional group capable of interacting with silica.

[0029] The content of the conjugated diene monomer units in all monomer units constituting the conjugated diene polymer used in the present invention is preferably 90% by weight or more, more preferably 95% by weight or more, further preferably 99% by weight or more, and particularly preferably 99.7% by weight or more. By making the content of the conjugated diene monomer units within the above range, the low heat generation, wear resistance and stone impact resistance of the obtained rubber cross-linked product can be taken into account at a higher level.

[0030] As the conjugated diene compound for forming the conjugated diene monomer unit, it is not particularly limited, and 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 2-phenyl-1,3-butadiene, 1,3-pentadiene, 2-methyl-1,3-pentadiene, 1,3-hexadiene, 4,5-diethyl-1,3-octadiene, 3-butyl-1,3-octadiene etc. can be enumerated. Among these, preferably 1,3-butadiene and isoprene, more preferably 1,3-butadiene. These conjugated diene compounds can be used alone or in combination of two or more.

[0031] The conjugated diene polymer used in the present invention preferably contains 1,3-butadiene units, more preferably 1,3-butadiene units and isoprene units as conjugated diene monomer units.

[0032] When the conjugated diene polymer used in the present invention contains 1,3-butadiene units and isoprene units, the ratio of the content ratio of 1,3-butadiene units to the content ratio of isoprene units in all monomer units constituting the conjugated diene polymer is not particularly limited, and is preferably 0.001 to 0.2, more preferably 0.005 to 0.1, and particularly preferably 0.01 to 0.05, in terms of (weight ratio of isoprene units) / (weight ratio of 1,3-butadiene units). By making the ratio of the content ratio of 1,3-butadiene units to the content ratio of isoprene units within the above range, the low heat generation property, wear resistance and stone chip resistance of the obtained rubber cross-linked product can be taken into account at a higher level.

[0033] In addition, the conjugated diene polymer used in the present invention may also contain other monomer units other than the conjugated diene monomer units. As other monomers constituting such other monomer units, aromatic vinyl monomers such as styrene, methyl styrene, ethyl styrene, tert-butyl styrene, α-methyl styrene, α-methyl-p-methyl styrene, chlorostyrene, bromostyrene, methoxystyrene, dimethylaminomethyl styrene, dimethylaminoethyl styrene, diethylaminomethyl styrene, diethylaminoethyl styrene, cyanoethyl styrene, and vinyl naphthalene can be cited; chain olefin compounds such as ethylene, propylene, and 1-butene; cyclic olefin compounds such as cyclopentene and 2-norbornene; non-conjugated diene compounds such as 1,5-hexadiene, 1,6-heptadiene, 1,7-octadiene, dicyclopentadiene, and 5-ethylidene-2-norbornene. Among these, aromatic vinyl monomers are preferred, and styrene is more preferred. These other monomers can be used alone or in combination of two or more.

[0034] The content of other monomer units in all monomer units constituting the conjugated diene polymer used in the present invention is preferably 10 wt % or less, more preferably 5 wt % or less, further preferably 1 wt % or less, particularly preferably 0.3 wt % or less.

[0035] In the case where the conjugated diene polymer used in the present invention includes other monomeric units, the lower limit of the content ratio of other monomeric units in all monomeric units constituting the conjugated diene polymer used in the present invention is not particularly limited, for example, it can be more than 0.01 weight %, and in addition, the upper limit of the content ratio of the conjugated diene monomeric units is not particularly limited, for example, it can be less than 99.99 weight %. By making the content ratio of each monomeric unit within the above range, the low heat generation, wear resistance and stone impact resistance of the obtained rubber cross-linked product can be taken into account at a higher level.

[0036] In addition, the glass transition temperature (Tg) of the conjugated diene polymer used in the present invention is below -60°C. The glass transition temperature (Tg) is not particularly limited, and is preferably -100°C to -67°C, more preferably -97°C to -74°C, further preferably -95°C to -81°C, and particularly preferably -93°C to -88°C. By making the glass transition temperature (Tg) within the above range, the low heat generation, wear resistance and stone chip resistance of the obtained rubber cross-linked product can be taken into account at a higher level. There are no particular limitations on the method for making the glass transition temperature (Tg) of the conjugated diene polymer within the above range, and examples include: a method of adjusting the vinyl bond content in the conjugated diene monomer unit constituting the conjugated diene polymer; a method of adjusting the weight average molecular weight of the conjugated diene polymer, etc.

[0037] The vinyl bond content in the conjugated diene monomer units constituting the conjugated diene polymer used in the present invention is preferably 5 to 40% by weight, more preferably 7 to 33% by weight, further preferably 9 to 25% by weight, particularly preferably 11 to 20% by weight, and most preferably 12 to 15% by weight. By making the vinyl bond content within the above range, the low heat generation, wear resistance and stone chip resistance of the obtained rubber cross-linked product can be taken into account at a higher level.

[0038] The conjugated diene polymer used in the present invention is preferably a polymer polymerized using a polymerization initiator with an organic alkali metal compound as a main catalyst, more preferably a polymer polymerized using an organic monolithium compound as a polymerization initiator, and further preferably a polymer polymerized using n-butyl lithium as a polymerization initiator. As the conjugated diene polymer, by using a polymer polymerized using the above-mentioned polymerization initiator, the low heat generation, wear resistance and stone impact resistance of the obtained rubber cross-linked product can be taken into account at a higher level.

[0039] In addition, the conjugated diene polymer used in the present invention has a functional group that can interact with silica in the polymer. The functional group that can interact with silica refers to a functional group that can form a covalent bond between the functional group and the silica surface, or can form an intermolecular force weaker than a covalent bond (e.g., ion-dipole interaction, dipole-dipole interaction, hydrogen bond, van der Waals force, etc.). As such a functional group that can interact with silica, there is no particular limitation, and nitrogen-containing functional groups, silicon-containing functional groups, oxygen-containing functional groups, etc. can be cited. Among these, from the viewpoint of high interaction with silica, preferably silicon-containing functional groups, preferably with Si-OR a (R a A group having a structure represented by a hydrogen atom or a hydrocarbon group which may have a substituent.

[0040] As the formation of R a The hydrocarbon group includes alkyl, cycloalkyl, alkenyl, aryl, aralkyl, etc., and preferably an alkyl group having 1 to 6 carbon atoms. As the alkyl group having 1 to 6 carbon atoms, methyl, ethyl, n-propyl, isopropyl, butyl, pentyl, hexyl, etc. are mentioned, and among these, methyl and ethyl are more preferred, and methyl is particularly preferred. In addition, when the hydrocarbon group has a substituent, a hydrocarbon group having a hydrocarbonoxy group as a substituent can be mentioned, and as the hydrocarbon group having a hydrocarbonoxy group as a substituent, alkoxyalkyl groups such as methoxymethyl, ethoxymethyl, and methoxyethyl; aryloxyalkyl groups such as phenoxymethyl, etc. can be mentioned.

[0041] The method for introducing a functional group capable of interacting with silica into the conjugated diene polymer used in the present invention is not particularly limited, and examples thereof include a method in which, when a monomer comprising a conjugated diene compound is polymerized to obtain a conjugated diene polymer chain having an active terminal, a modifier having a functional group capable of interacting with silica is reacted with the conjugated diene polymer chain having an active terminal, and the like.

[0042] In addition, the weight average molecular weight (Mw) of the conjugated diene polymer used in the present invention is preferably 150,000 to 3,000,000, more preferably 250,000 to 1,000,000, further preferably 350,000 to 700,000, further preferably 400,000 to 550,000, particularly preferably 430,000 to 500,000, and most preferably 450,000 to 480,000. By making the weight average molecular weight (Mw) of the conjugated diene polymer within the above range, it becomes easy to add silica to the conjugated diene polymer, which can further improve the processability of the rubber composition, and further can take into account the low heat generation, wear resistance and stone impact resistance of the obtained rubber cross-linked product at a higher level.

[0043] The molecular weight distribution represented by the ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) of the conjugated diene polymer used in the present invention is preferably 1.1 to 3.5, more preferably 1.2 to 3.0, further preferably 1.3 to 2.5, and particularly preferably 1.4 to 2.0. By making the molecular weight distribution (Mw / Mn) of the conjugated diene polymer used in the present invention within the above range, the low heat generation, wear resistance and stone impact resistance of the obtained rubber cross-linked product can be taken into account at a higher level. In addition, the weight average molecular weight (Mw) and the number average molecular weight (Mn) can be obtained as values ​​measured by gel permeation chromatography in terms of polystyrene.

[0044] Furthermore, the Mooney viscosity (ML1+4, 100°C) of the conjugated diene polymer used in the present invention is preferably 20 to 100, more preferably 35 to 90, further preferably 45 to 80, particularly preferably 50 to 70, and most preferably 55 to 65. When the conjugated diene polymer is made into an oil-extended rubber, the Mooney viscosity of the oil-extended rubber is preferably within the above range.

[0045] The content ratio of the conjugated diene polymer having a glass transition temperature (Tg) of -60°C or less and having a functional group capable of interacting with silica in the rubber composition for heavy-duty tires of the present invention is not particularly limited, and is preferably 10 to 80% by weight, more preferably 12 to 60% by weight, and further preferably 15 to 40% by weight, based on the content ratio in 100% by weight of all rubber components contained in the rubber composition for heavy-duty tires of the present invention. By making the content ratio of the conjugated diene polymer within the above range, the low heat generation, wear resistance and stone impact resistance of the obtained rubber cross-linked product can be taken into account at a higher level.

[0046] <Method for producing conjugated diene polymer>

[0047] The method for producing the conjugated diene polymer used in the present invention is not particularly limited.

[0048] The method for producing a conjugated diene polymer preferably comprises the following steps:

[0049] A polymerization step of polymerizing monomers comprising a conjugated diene polymer using a polymerization initiator in an inactive solvent to obtain a conjugated diene polymer chain having an active terminal; and

[0050] In the modification step, a modifier having a functional group capable of interacting with silica is reacted with the conjugated diene polymer chain having an active terminal obtained in the polymerization step.

[0051] (Polymerization process)

[0052] As the monomer containing a conjugated diene compound used in the polymerization step, the above-mentioned monomers can be used.

[0053] The inactive solvent used for polymerization is any of those commonly used in solution polymerization, and is not particularly limited as long as it does not hinder the polymerization reaction. Specific examples of inactive solvents include: chain aliphatic hydrocarbons such as butane, pentane, hexane, and heptane; alicyclic hydrocarbons such as cyclopentane and cyclohexane; aromatic hydrocarbons such as benzene, toluene, xylene, and ethylbenzene; ether compounds such as tetrahydrofuran and diethyl ether, etc. These inactive solvents can be used alone or in combination of two or more. The amount of the inactive solvent used is not particularly limited, and is, for example, an amount that makes the monomer concentration 1 to 50% by weight, preferably an amount that makes the monomer concentration 10 to 40% by weight.

[0054] As the polymerization initiator used for polymerization, as long as it is a polymerization initiator that can polymerize the monomer containing the conjugated diene compound to form a conjugated diene polymer chain with an active end, it is not particularly limited. As its specific examples, organic alkali metal compounds, organic alkaline earth metal compounds and polymerization initiators with lanthanide metal compounds as main catalysts can be cited. As organic alkali metal compounds, for example: organic monolithium compounds such as n-butyl lithium, sec-butyl lithium, tert-butyl lithium, hexyl lithium, phenyl lithium, distyrene lithium, etc.; organic polylithium compounds such as dilithium methane, 1,4-dilithium butane, 1,4-dilithium-2-ethylcyclohexane, 1,3,5-trilithium benzene, 1,3,5-tri(lithium methyl) benzene; organic sodium compounds such as sodium naphthalene; organic potassium compounds such as potassium naphthalene, etc. In addition, as organic alkaline earth metal compounds, for example, di-n-butyl magnesium, di-n-hexyl magnesium, diethoxy calcium, calcium distearate, di-tert-butoxy strontium, diethoxy barium, diisopropoxy barium, diethyl mercapto barium, di-tert-butoxy barium, diphenoxy barium, diethylamino barium, barium distearate, diketyl barium, etc. can be cited. As polymerization initiators with lanthanide metal compounds as main catalysts, for example, polymerization initiators with salts of lanthanide metals such as lanthanum, cerium, praseodymium, neodymium, samarium, and gadolinium and carboxylic acids and phosphorus-containing organic acids as main catalysts, polymerization initiators composed of the main catalyst and co-catalysts such as alkyl aluminum compounds, organic aluminum hydride compounds, and organic aluminum halides, etc. are preferably used in these polymerization initiators, organic monolithium compounds and organic polylithium compounds are more preferably used, and n-butyl lithium is particularly preferably used.

[0055] In addition, the organic alkali metal compound may be reacted with a secondary amine compound such as dibutylamine, dihexylamine, dibenzylamine, pyrrolidine, piperidine, hexamethyleneimine, and heptamethyleneimine to form an organic alkali metal amide compound for use. These polymerization initiators may be used alone or in combination of two or more.

[0056] The amount of the polymerization initiator used may be determined according to the molecular weight of the target conjugated diene polymer chain, and is usually in the range of 1 to 50 mmol, preferably 1.5 to 20 mmol, more preferably 2 to 15 mmol, based on 1000 g of the monomer.

[0057] The polymerization temperature is usually in the range of -80 to +150° C., preferably 0 to 100° C., and more preferably 30 to 90° C. As the polymerization method, any method such as a batch method and a continuous method can be adopted.

[0058] In addition, in the polymerization step, when the monomer containing the conjugated diene compound is polymerized, the polymerization is preferably carried out in the presence of a polar compound. Specifically, it is preferred to use 0.01 to 1.2 moles, more preferably 0.1 to 1.1 moles, and further preferably 0.1 to 1.0 moles of the polar compound relative to 1 mole of the polymerization initiator, and the polymerization is carried out in the presence of such a polar compound, thereby enabling the vinyl bond content in the conjugated diene monomer unit portion contained in the conjugated diene polymer chain obtained in the polymerization step to be appropriately adjusted to the above range.

[0059] The method of polymerizing in the presence of a polar compound is not particularly limited, and examples thereof include a method of adding a polar compound to an inert solvent used for polymerization and performing polymerization. In addition, specific examples of polar compounds include ether compounds such as dibutyl ether, tetrahydrofuran, and 2,2-di(tetrahydrofuranyl)propane; tertiary amines such as tetramethylethylenediamine; alkali metal alkoxides; phosphine compounds, and the like. Among these, ether compounds and tertiary amines are preferred, tertiary amines are more preferred, and tetramethylethylenediamine is particularly preferred. These polar compounds may be used alone or in combination of two or more.

[0060] The weight average molecular weight (Mw) of the conjugated diene polymer chain with active ends obtained in the polymerization step is not particularly limited, and is preferably 150,000 to 3,000,000, more preferably 170,000 to 2,000,000, further preferably 200,000 to 1,500,000, particularly preferably 350,000 to 650,000, and most preferably 380,000 to 520,000, as measured by gel permeation chromatography in terms of polystyrene. By making the weight average molecular weight (Mw) of the conjugated diene polymer chain with active ends within the above range, the low heat generation, wear resistance and stone chip resistance of the obtained rubber cross-linked product can be taken into account at a higher level.

[0061] In addition, the molecular weight distribution represented by the ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) of the conjugated diene polymer chain having an active terminal obtained in the polymerization step is also not particularly limited, and is preferably 1.1 to 3.5, more preferably 1.2 to 3.0, and further preferably 1.3 to 2.5. When the molecular weight distribution (Mw / Mn) of the conjugated diene polymer chain having an active terminal is within the above range, the production of the conjugated diene polymer becomes easy.

[0062] In the present invention, from the viewpoint of achieving a higher level of low heat build-up, wear resistance, and stone chip resistance in the obtained rubber cross-linked product, the polymerization step may be the following step.

[0063] That is, the polymerization step preferably includes the following steps:

[0064] A step of polymerizing a monomer containing isoprene or a monomer containing isoprene and an aromatic vinyl compound in an inert solvent by a polymerization initiator to form a polymer block (A) having an active terminal and containing 80 to 100 wt % of an isoprene monomer unit and 0 to 20 wt % of an aromatic vinyl monomer unit; and

[0065] The polymer block (A) having an active terminal obtained above is mixed with a monomer containing 1,3-butadiene and an aromatic vinyl compound, and the polymerization reaction is continued to connect the polymer block (B) containing 1,3-butadiene monomer units with the polymer block (A) to form a conjugated diene polymer chain having an active terminal.

[0066] By adopting such a process, the conjugated diene polymer chain having an active terminal obtained by the polymerization process can be made into a polymer chain having a structure formed by connecting a polymer block (A) and a polymer block (B), wherein the polymer block (A) contains 80 to 100% by weight of an isoprene monomer unit and 0 to 20% by weight of an aromatic vinyl monomer unit, and the polymer block (B) contains a 1,3-butadiene monomer unit.

[0067] Such a method will be described below.

[0068] [Polymer block (A)]

[0069] The polymer block (A) in the conjugated diene polymer chain of one embodiment of the present invention only needs to contain 80 to 100% by weight of isoprene monomer units and 0 to 20% by weight of aromatic vinyl monomer units in the polymer block (A), preferably 85 to 97% by weight of isoprene monomer units and 3 to 15% by weight of aromatic vinyl monomer units, and more preferably 89 to 95% by weight of isoprene monomer units and 5 to 11% by weight of aromatic vinyl monomer units. When the content ratio of isoprene monomer units and aromatic vinyl monomer units is within the above range, the affinity of the conjugated diene polymer with silica can be further improved, thereby achieving a higher level of low heat generation, wear resistance and stone impact resistance of the obtained rubber cross-linked product.

[0070] As the aromatic vinyl compound for constituting the aromatic vinyl monomer unit contained in the polymer block (A), the same compounds as those mentioned above can be used, and among them, styrene is preferred. In addition, these aromatic vinyl compounds may be used alone or in combination of two or more.

[0071] The polymer block (A) is preferably composed of isoprene monomer units only, or isoprene monomer units and aromatic vinyl monomer units, and may contain other monomer units in addition to isoprene monomer units, or isoprene monomer units and aromatic vinyl monomer units, as desired. Other compounds used to constitute other monomer units include: conjugated diene compounds other than isoprene such as 1,3-butadiene, 2,3-dimethyl-1,3-butadiene, 2-chloro-1,3-butadiene, 1,3-pentadiene and 1,3-hexadiene; α,β-unsaturated nitriles such as acrylonitrile and methacrylonitrile; unsaturated carboxylic acids or anhydrides such as acrylic acid, methacrylic acid and maleic anhydride; unsaturated carboxylic acid esters such as methyl methacrylate, ethyl acrylate and butyl acrylate; non-conjugated dienes such as 1,5-hexadiene, 1,6-heptadiene, 1,7-octadiene, dicyclopentadiene and 5-ethylidene-2-norbornene, etc. Among these, 1,3-butadiene is preferred. These other monomers can be used alone or in combination of two or more. The content of other monomer units in the polymer block (A) is preferably 20% by weight or less, more preferably 10% by weight or less, and further preferably 6% by weight or less.

[0072] In the present invention, the polymer block (A) in the conjugated diene polymer chain is formed by polymerizing a monomer containing isoprene or a monomer containing isoprene and an aromatic vinyl compound using a polymerization initiator in an inert solvent. The formed polymer block (A) becomes a polymer block having an active terminal.

[0073] As the inert solvent used in the polymerization of the monomer containing isoprene or the monomer containing isoprene and the aromatic vinyl compound to form the polymer block (A), the same inert solvent as the above-mentioned inert solvent can be used. The amount of the inert solvent used is preferably an amount that makes the monomer concentration 1 to 80% by weight, more preferably an amount that makes the monomer concentration 10 to 50% by weight.

[0074] The polymerization initiator used to form the polymer block (A) is not particularly limited as long as it is a polymerization initiator that can polymerize a monomer containing isoprene or a monomer containing isoprene and an aromatic vinyl compound to form a polymer chain having an active terminal. As a specific example, the same polymerization initiator as the above-mentioned polymerization initiator can be used.

[0075] The amount of the polymerization initiator used may be determined according to the target molecular weight, and is preferably in the range of 4 to 250 mmol, more preferably 6 to 200 mmol, and particularly preferably 10 to 70 mmol per 100 g of the monomer containing isoprene or the monomer containing isoprene and an aromatic vinyl compound.

[0076] The polymerization temperature when polymerizing a monomer containing isoprene or a monomer containing isoprene and an aromatic vinyl compound is preferably in the range of -80 to +150° C., more preferably 0 to 100° C., and even more preferably 20 to 90° C. As the polymerization method, any method such as a batch method and a continuous method can be adopted. In addition, as the bonding method, various bonding methods such as block, tapered, and random can be adopted.

[0077] In addition, when forming the polymer block (A), it is preferred to polymerize a monomer containing isoprene or a monomer containing isoprene and an aromatic vinyl compound in the presence of a polar compound. Specifically, it is preferred to use 0.01 to 100 moles, more preferably 0.03 to 30 moles, and even more preferably 0.05 to 1 mole of the polar compound relative to 1 mole of the polymerization initiator. By polymerizing in the presence of such a polar compound, the vinyl bond content of the isoprene monomer unit in the polymer block (A) can be appropriately adjusted. In addition, the vinyl bond of the isoprene monomer unit may be any of a 1,2-vinyl bond and a 3,4-vinyl bond.

[0078] There is no particular limitation on the method for polymerizing a monomer containing isoprene or a monomer containing isoprene and an aromatic vinyl compound in the presence of a polar compound, and examples thereof include a method of adding a polar compound to an inert solvent for polymerization, etc. In addition, as the polar compound, the same polar compound as described above can be used.

[0079] The vinyl bond content in the isoprene monomer unit in the polymer block (A) is preferably 1 to 90% by weight, more preferably 2 to 50% by weight, further preferably 3 to 30% by weight, particularly preferably 4 to 20% by weight, and most preferably 5 to 10% by weight. By making the vinyl bond content in the isoprene monomer unit within the above range, the low heat build-up property of the obtained rubber cross-linked product can be further improved. In addition, in this specification, the vinyl bond content in the isoprene monomer unit refers to the ratio of the total amount of the isoprene monomer unit having a 1,2-structure and the isoprene monomer unit having a 3,4-structure in the isoprene monomer unit.

[0080] The weight average molecular weight (Mw) of the polymer block (A) is preferably 500 to 15000, more preferably 1000 to 12000, and particularly preferably 1500 to 10000, as a value measured by gel permeation chromatography in terms of polystyrene. By setting the weight average molecular weight of the polymer block (A) within the above range, the low heat build-up property, wear resistance, and stone chip resistance of the obtained rubber cross-linked product can be achieved at a higher level.

[0081] In addition, the molecular weight distribution represented by the ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) of the polymer block (A) is preferably 1.0 to 1.5, more preferably 1.0 to 1.3. When the value (Mw / Mn) of the molecular weight distribution of the polymer block (A) is within the above range, the production of the conjugated diene polymer becomes easier.

[0082] [Polymer block (B)]

[0083] The polymer block (B) in the conjugated diene polymer chain of one embodiment of the present invention preferably contains 95% by weight or more of 1,3-butadiene monomer units in the polymer block (B), more preferably contains 99% by weight or more of 1,3-butadiene monomer units in the polymer block (B), and further preferably contains 100% by weight of 1,3-butadiene monomer units in the polymer block (B). By making the content of 1,3-butadiene monomer units within the above range, the low heat generation, wear resistance and stone chip resistance of the obtained rubber cross-linked product can be taken into account at a higher level.

[0084] The polymer block (B) may contain other monomer units in addition to 1,3-butadiene monomer units as desired. As other monomers for constituting other monomer units, compounds identical to the compounds exemplified in the above-mentioned polymer block (A) (wherein 1,3-butadiene is not included) can be used. In addition, in the polymer block (B), isoprene can also be used as other monomers. The content ratio of other monomer units in the polymer block (B) is preferably less than 5% by weight, more preferably less than 1% by weight.

[0085] In one embodiment of the present invention, the polymer block (B) in the conjugated diene polymer chain is formed by mixing the above-mentioned polymer block (A) having an active terminal with a monomer containing 1,3-butadiene and continuing the polymerization reaction to connect with the polymer block (A). The formed polymer block (B) becomes a polymer block having an active terminal. On the other hand, the active terminal disappears from the polymer block (A).

[0086] The inert solvent used in the polymerization of the polymer block (A) and the monomer containing 1,3-butadiene to form the polymer block (B) is not particularly limited, and the same inert solvents as those described above can be used.

[0087] The amount of the polymer block (A) having an active terminal used when forming the polymer block (B) may be determined according to the target molecular weight, and is preferably in the range of 0.1 to 5 mmol, more preferably 0.15 to 2 mmol, and even more preferably 0.2 to 1.5 mmol per 100 g of the monomer containing 1,3-butadiene.

[0088] The method for mixing the polymer block (A) and the monomer containing 1,3-butadiene is not particularly limited. The polymer block (A) having an active terminal may be added to a solution of the monomer containing 1,3-butadiene, or the monomer containing 1,3-butadiene may be added to a solution of the polymer block (A) having an active terminal. From the viewpoint of controlling polymerization, the method of adding the polymer block (A) having an active terminal to a solution of the monomer containing 1,3-butadiene is preferred.

[0089] The polymerization temperature when polymerizing the monomers containing 1,3-butadiene is preferably in the range of -80 to +150° C., more preferably 0 to 100° C., and even more preferably 20 to 90° C. The polymerization method may be a batch method or a continuous method.

[0090] In one embodiment of the present invention, it is preferred that, in the formation of polymer block (B), a monomer containing 1,3-butadiene is polymerized in the presence of a polar compound, similarly to the formation of polymer block (A). Specifically, it is preferred that 0.01 to 0.50 mol, more preferably 0.05 to 0.40 mol, and even more preferably 0.08 to 0.35 mol of the polar compound is used relative to 1 mol of the polymerization initiator. By polymerizing in the presence of such a polar compound, the vinyl bond content of the 1,3-butadiene monomer unit portion in the polymer block (B) can be appropriately adjusted, and as a result, the vinyl bond content of the conjugated diene monomer unit portion contained in the finally obtained conjugated diene polymer can be appropriately adjusted to the above range.

[0091] As a method for polymerizing a monomer containing 1,3-butadiene in the presence of a polar compound, there is no particular limitation, and examples thereof include a method for polymerizing by adding a polar compound to an inactive solvent for polymerization. In this case, the addition of the polar compound can be performed in such a manner that the total amount of the polar compound added when forming the polymer block (A) and the amount of the newly added polar compound becomes the above-mentioned range. Therefore, in the case of adding a polar compound sufficient to adjust the vinyl bond content of the 1,3-butadiene monomer unit portion in the polymer block (B) when forming the polymer block (A), the polar compound may not be newly added. In addition, as the polar compound, the same polar compound as the above-mentioned polar compound can be used.

[0092] In this way, a conjugated diene polymer chain with an active end having a polymer block (A) and a polymer block (B) can be obtained. In one embodiment of the present invention, from the viewpoint of productivity, the conjugated diene polymer chain with an active end is preferably composed of a polymer block (A)-polymer block (B) and the end of the polymer block (B) is an active end, but the polymer chain may also have a plurality of polymer blocks (A) and may also have other polymer blocks. For example, a conjugated diene polymer chain with an active end such as a polymer block (A)-polymer block (B)-polymer block (A) can be cited. In this case, an active end is formed at the end of the polymer block (A) formed next to the polymer block (B). In the case where the polymer block (A) is formed on the active end side of the conjugated diene polymer chain, the amount of isoprene used is preferably 10 to 100 moles, more preferably 15 to 70 moles, and particularly preferably 20 to 35 moles relative to 1 mole of the polymerization initiator used in the initial polymerization reaction (polymerization reaction for forming the first polymer block (A)).

[0093] The weight ratio of polymer block (A) to polymer block (B) in the conjugated diene polymer chain having an active terminal obtained in one embodiment of the present invention (when there are a plurality of polymer blocks (A) and polymer blocks (B), the weight ratio is based on the total weight of each) is preferably 0.001 to 0.2, more preferably 0.005 to 0.1, and particularly preferably 0.01 to 0.05, as measured by (weight of polymer block (A)) / (weight of polymer block (B)). By making the weight ratio of polymer block (A) to polymer block (B) within the above range, the low heat generation, wear resistance and stone chip resistance of the obtained rubber cross-linked product can be achieved at a higher level.

[0094] (Modification process)

[0095] Next, in the modification step, a modifier having a functional group capable of interacting with silica is reacted with the conjugated diene polymer chain having an active terminal obtained in the above-mentioned polymerization step.

[0096] The modifier having a functional group capable of interacting with silica used in the modification step is not particularly limited, as long as it is a compound capable of reacting with the conjugated diene polymer chain having an active terminal obtained in the above-mentioned polymerization step and having a functional group capable of interacting with silica. The functional group capable of interacting with silica is not particularly limited, and examples thereof include nitrogen-containing functional groups, silicon-containing functional groups, oxygen-containing functional groups, etc. Among these, silicon-containing functional groups are preferred from the viewpoint of high interaction with silica, and Si-OR functional groups are preferred. a (R a A group having a structure represented by a hydrogen atom or a hydrocarbon group which may have a substituent.

[0097] In the present invention, as a modifier having such a functional group capable of interacting with silica, a siloxane compound can be preferably used. Such a siloxane compound is not particularly limited as long as it has a structure represented by (-Si-O-Si-), and preferably an organosiloxane having an organic group in addition to the structure represented by (-Si-O-Si-), and more preferably a polyorganosiloxane represented by the following general formula (1).

[0098] [Chemical formula 1]

[0099]

[0100] In the general formula (1), R 1 ~R 8 is an alkyl group having 1 to 6 carbon atoms or an aryl group having 6 to 12 carbon atoms, and they may be the same or different. 1 and X 4 is any group selected from an alkyl group having 1 to 6 carbon atoms, an aryl group having 6 to 12 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, and an epoxy group-containing group having 4 to 12 carbon atoms, and these groups may be the same or different. 2 is an alkoxy group having 1 to 5 carbon atoms, or a group having 4 to 12 carbon atoms containing an epoxy group, and a plurality of X 2 They can be the same or different. 3 is a group containing 2 to 20 repeating units of alkylene glycol. 3 When , they may be the same as or different from each other. m is an integer of 1 to 200, n is an integer of 0 to 200, k is an integer of 0 to 200, and m+n+k is 1 or more.

[0101] In the polyorganosiloxane represented by the general formula (1), as a compound that can constitute R in the general formula (1), 1 ~R 8 , X 1 and X 4 The alkyl group having 1 to 6 carbon atoms includes, for example, methyl, ethyl, n-propyl, isopropyl, butyl, pentyl, hexyl, and cyclohexyl. The aryl group having 6 to 12 carbon atoms includes, for example, phenyl and methylphenyl. Among these, methyl and ethyl are preferred from the viewpoint of the ease of production of the polyorganosiloxane itself.

[0102] In the polyorganosiloxane represented by the general formula (1), as a member capable of constituting X 1 , X 2 and X 4 Examples of the alkoxy group having 1 to 5 carbon atoms include methoxy, ethoxy, propoxy, isopropoxy and butoxy groups. Among these, methoxy and ethoxy groups are preferred from the viewpoint of ease of production of the polyorganosiloxane itself.

[0103] Furthermore, in the polyorganosiloxane represented by the general formula (1), as a compound capable of constituting X 1 , X 2 and X 4 Examples of the epoxy group-containing group having 4 to 12 carbon atoms include groups represented by the following general formula (2).

[0104] -Z 3 -Z 4 -E 2 (2)

[0105] In the general formula (2), Z 3 is an alkylene group or an alkylarylene group having 1 to 10 carbon atoms, Z 4 is a methylene, sulfur or oxygen atom, E 2 It is a hydrocarbon group having 2 to 10 carbon atoms and having an epoxy group.

[0106] As the group represented by the general formula (2), Z is preferably 4 is an oxygen atom, more preferably Z 4 is an oxygen atom, and E 2 A group which is a glycidyl group, particularly preferably Z 3 is an alkylene group having 1 to 3 carbon atoms, Z 4 is an oxygen atom, and E 2 A glycidyl group.

[0107] In the polyorganosiloxane represented by the general formula (1), X 1 and X 4Among the above, a group having 4 to 12 carbon atoms or an alkyl group having 1 to 6 carbon atoms containing an epoxy group is preferred. 2 Among the above, groups having 4 to 12 carbon atoms and containing an epoxy group are preferred. Furthermore, X is more preferably 1 and X 4 is an alkyl group having 1 to 6 carbon atoms, X 2 It is a group having 4 to 12 carbon atoms and containing an epoxy group.

[0108] In the polyorganosiloxane represented by the general formula (1), X 3 , that is, a group containing 2 to 20 repeating units of alkylene glycol, preferably a group represented by the following general formula (3).

[0109] [Chemical formula 2]

[0110]

[0111] In the general formula (3), t is an integer of 2 to 20, and X 5 is an alkylene group or an alkylarylene group having 2 to 10 carbon atoms, R 9 is a hydrogen atom or a methyl group, X 6 is an alkoxy or aryloxy group having 1 to 10 carbon atoms. Among these, t is preferably an integer of 2 to 8, and X 5 is an alkylene group having 3 carbon atoms, R 9 is a hydrogen atom and X 6 It is a methoxy group.

[0112] In the polyorganosiloxane represented by the general formula (1), m is an integer of 1 to 200, preferably an integer of 20 to 150, and more preferably an integer of 30 to 120. When m is 1 or more, it is easy to make the coupling rate of the obtained conjugated diene polymer within the preferred range described below, as a result, the low heat generation, wear resistance and stone chip resistance of the obtained rubber cross-linked product can be taken into account at a higher level. In addition, when m is 200 or less, the preparation of the polyorganosiloxane represented by the general formula (1) itself becomes easier, and its viscosity does not become too high, and it becomes easier to handle.

[0113] In the polyorganosiloxane represented by the general formula (1), n ​​is an integer of 0 to 200, preferably an integer of 0 to 150, and more preferably an integer of 0 to 120. k is an integer of 0 to 200, preferably an integer of 0 to 150, and more preferably an integer of 0 to 130. The total of m, n and k is 1 or more, preferably 3 to 400, more preferably 20 to 300, and particularly preferably 30 to 250. When the total of m, n and k is 1 or more, the reaction of the polyorganosiloxane represented by the general formula (1) with the conjugated diene polymer chain having an active terminal proceeds easily. Furthermore, when the total of m, n and k is 400 or less, the polyorganosiloxane represented by the general formula (1) itself is easy to produce, and its viscosity does not become too high, so it is easy to handle.

[0114] The amount of the siloxane compound used in the modification step is preferably 0.1 mol or more, more preferably 0.2 mol or more, further preferably 0.5 mol or more, particularly preferably 1.0 mol or more, more preferably 1.1 mol or more, relative to 1 mol of the polymerization initiator used for polymerization in the above-mentioned polymerization step, calculated as the number of repeating units of (-Si-O-) in the siloxane compound, and is preferably 10 mol or less, more preferably 5 mol or less, further preferably 2.5 mol or less, and particularly preferably 2 mol or less. By making the amount of the siloxane compound used within the above-mentioned range, the low heat generation, wear resistance and stone chip resistance of the obtained rubber cross-linked product can be taken into account at a higher level.

[0115] In particular, it is particularly preferred that the amount of the siloxane compound used is 1 mol or more in terms of the number of repeating units of (-Si-O-) relative to 1 mol of the polymerization initiator, because substantially all of the active ends of the conjugated diene polymer chain having an active end obtained by the polymerization step can be reacted with the siloxane compound. That is, the alkyl metal group, i.e., -R - M + (R is a hydrocarbon group forming a polymer chain terminal, and M is an alkali metal atom, an alkaline earth metal atom or a lanthanide metal atom) is in a state where substantially no group remains.

[0116] There is no particular limitation on the method of reacting a siloxane compound with a conjugated diene polymer chain having an active terminal, and examples include a method of mixing them in solvents in which they are soluble. As the solvent used at this time, the solvents exemplified as the inactive solvents used in the above-mentioned polymerization step can be used. In addition, in this case, the method of adding a siloxane compound to the polymerization solution used for the polymerization to obtain a conjugated diene polymer chain having an active terminal is simple and therefore preferred. In addition, in this case, it is preferred that the siloxane compound be dissolved in an inactive solvent and added to the polymerization system, and the solution concentration is preferably in the range of 1 to 50% by weight. The reaction temperature is not particularly limited, and is usually 0 to 120°C, and the reaction time is not particularly limited, and is usually 1 minute to 1 hour.

[0117] The timing of adding the siloxane compound to the solution containing the conjugated diene polymer chain with an active terminal is not particularly limited. It is preferred that the siloxane compound be added to the solution before the polymerization reaction is completed and the solution containing the conjugated diene polymer chain with an active terminal still contains monomers. More specifically, the siloxane compound is added to the solution when the solution containing the conjugated diene polymer chain with an active terminal contains 100 ppm or more, more preferably 300 to 50,000 ppm of monomers. By adding the siloxane compound in this way, the side reaction between the conjugated diene polymer chain with an active terminal and impurities contained in the polymerization system can be suppressed, and the reaction can be well controlled.

[0118] In the modification step, a siloxane compound as a modifier is reacted with the active end of the conjugated diene polymer chain having an active end obtained in the above-mentioned polymerization step, and the active end of the conjugated diene polymer chain reacts with the silicon atom in the siloxane structure. Alternatively, a part of the active ends of the conjugated diene polymer chain reacts with the alkoxy group or epoxy group of the side chain of the polyorganosiloxane represented by the general formula (1) (in the general formula (1), the X that must be included is formed). 2 Furthermore, according to the modification step, by such a reaction, a modified structure based on siloxane is introduced into the conjugated diene polymer chain, thereby introducing a functional group capable of interacting with silica into the conjugated diene polymer.

[0119] Specifically, it is considered that by reacting the active end of the conjugated diene polymer chain with the silicon atom in the siloxane structure, a new bond is formed between the silicon atom in the siloxane structure of the conjugated diene polymer chain and the active end of the conjugated diene polymer chain, a modified structure based on siloxane is introduced to the end of the conjugated diene polymer chain, and an —O— bond is formed between the oxygen atom in the siloxane structure and the metal atom forming the active end of the conjugated diene polymer chain. - M +(M is an alkali metal atom, an alkaline earth metal atom, or a lanthanide metal atom) as their reactive residues.

[0120] Alternatively, it is considered that when the polyorganosiloxane represented by the general formula (1) is used as the siloxane compound, the active end of the conjugated diene polymer chain is reacted with the epoxy group of the side chain of the polyorganosiloxane, the epoxy group is ring-opened, a new bond is formed between the carbon atom of the ring-opened portion of the epoxy group and the active end of the conjugated diene polymer chain, a siloxane structure is introduced at the end of the conjugated diene polymer chain, and an —O— bond is formed between the oxygen atom in the epoxy group and the metal atom forming the active end of the conjugated diene polymer chain. - M + Alternatively, by reacting the active end of the conjugated diene polymer chain with the alkoxy group of the side chain of the polyorganosiloxane, the alkoxy group is separated, and a new bond is formed between the silicon atom in the siloxane structure of the conjugated diene polymer chain and the active end of the conjugated diene polymer chain, thereby introducing a siloxane structure at the end of the conjugated diene polymer chain.

[0121] In particular, in the modification step, by making the amount of the siloxane compound used be 1 mol or more in terms of the number of repeating units of (-Si-O-) relative to 1 mol of the polymerization initiator, it is possible to introduce a modified structure based on siloxane into almost all of the conjugated diene polymer chains having active terminals obtained in the polymerization step. Therefore, it is possible to make the alkyl metal group, i.e., -R - M + Almost no residue remains, and -O is formed as a reaction residue instead. - M + The group represented.

[0122] In addition, in the present invention, as a modifier having a functional group capable of interacting with silica, a compound having a protected primary amino group and an alkoxysilyl group can be used, such as N,N-bis(trimethylsilyl)aminopropylmethyldimethoxysilane, 1-trimethylsilyl-2,2-dimethoxy-1-aza-2-silacyclopentane, N,N-bis(trimethylsilyl)aminopropyltrimethoxysilane, N,N-bis(trimethylsilyl)aminopropyltriethoxysilane, N,N-bis(trimethylsilyl)aminopropylmethyldiethoxysilane, N,N-bis(trimethylsilyl)aminoethyltrimethoxysilane, N,N-bis(trimethylsilyl)aminoethyltriethoxysilane, N,N-bis(trimethylsilyl)aminoethylmethyldimethoxysilane, and N,N-bis(trimethylsilyl)aminoethylmethyldiethoxysilane.

[0123] Furthermore, in the present invention, as a modifier having a functional group capable of interacting with silica, a polyfunctional compound having two or more epoxy groups and one or more nitrogen-containing groups in the molecule can be used. More preferably, a polyfunctional compound represented by the following general formula (4) is used.

[0124] [Chemical formula 3]

[0125]

[0126] In the above general formula (4), R 10 and R 11 is a hydrocarbon group having 1 to 10 carbon atoms or a hydrocarbon group having 1 to 10 carbon atoms having an ether structure and / or a tertiary amine, R 12 and R 13 is hydrogen, a hydrocarbon group having 1 to 20 carbon atoms, or a hydrocarbon group having 1 to 20 carbon atoms having an ether and / or a tertiary amine, R 14 It is a hydrocarbon group having 1 to 20 carbon atoms or a hydrocarbon group having 1 to 20 carbon atoms having at least one of an ether structure, a tertiary amine, an epoxy group, a carbonyl group and a halogen group; and s is 1-6.

[0127] In addition, in the present invention, as a modifier having a functional group capable of interacting with silica, a compound having a silyl group substituted with two or more alkoxy groups and one or more nitrogen atoms can be used. Such a compound includes a compound represented by the following general formula (5), or a hydrocarbyloxysilane having a cyclic amino group containing two or more nitrogen atoms represented by the following general formula (6), a hydrocarbyloxysilane containing other functional groups such as cyclic amines, non-cyclic amines, imines, isocyanates, and cyclic azasilanes, and the like.

[0128] [Chemical formula 4]

[0129]

[0130] (In the above general formula (5), R 15 , R 16 Each independently represents an alkyl group or an aryl group having 1 to 20 carbon atoms, R 17 is an alkylene group having 1 to 20 carbon atoms, R 18 , R 19 is a hydrocarbon group having 1 to 6 carbon atoms which may be the same or different and which forms a ring structure of five or more members together with two adjacent N atoms, R 20 is a hydrocarbon group having 1 to 20 carbon atoms or a 3-organo-substituted silyl group, and u is an integer of 2 or 3.

[0131] [Chemical formula 5]

[0132]

[0133] (In the above general formula (6), R 15 ~R 20 , u have the same meanings as in the above general formula (5), R 21 It is a hydrocarbon group or an organic substituted silyl group having 1 to 20 carbon atoms.

[0134] Furthermore, in the present invention, as a modifier having a functional group capable of interacting with silica, a silane-sulfide compound represented by the following general formula (7) can be used.

[0135] (R 22 O) x (R 23 ) y Si-R 24 -S-SiR 25 (7)

[0136] (In the above general formula (7), Si is silicon, S is sulfur, O is oxygen, x is an integer selected from 1, 2 and 3, y is an integer selected from 0, 1 and 2, and x+y=3. R 22 , R 23 , R 25 are the same or different alkyl groups having 1 to 16 carbon atoms, R 24 is an aryl group, an alkylaryl group or an alkyl group having 1 to 16 carbon atoms.

[0137] In the present invention, as the siloxane compound having a functional group capable of interacting with silica, a reactive polysiloxane compound represented by the following general formula (8) can be used.

[0138] Y 1 -CH2CH2-Si(R 26 )(R 27 )-{O-Si(R 26 )(R 27 )} z -CH2CH2-Y 1 (8)

[0139] In the above general formula (8), Y 1 is (X 7 ) a (R 28 ) b Si-. Here, X 7 is halogen, R 28 is a lower alkyl group having 20 or less carbon atoms. 26 , R 27It is a lower alkyl group having a carbon number of not more than 20. a is 2 or 3, b is 0 or 1, a+b=3, and z is 1 to 50,000.

[0140] In addition, in the present invention, an amide compound can be used as a terminal modifier. Examples thereof include: N-methyl-2-pyrrolidone, N-vinyl-2-pyrrolidone, N-phenyl-2-pyrrolidone, N-methyl-ε-caprolactam and other N-substituted cyclic amides; 1,3-dimethylethyleneurea, 1,3-diethyl-2-imidazolidinone and other N-substituted cyclic ureas; 4,4'-bis(dimethylamino)benzophenone, 4,4'-bis(diethylamino)benzophenone and other N-substituted aminoketones; diphenylmethanediol; Aromatic isocyanates such as isocyanate and 2,4-toluene diisocyanate; N,N-disubstituted aminoalkyl methacrylamides such as N,N-dimethylaminopropyl methacrylamide; N-substituted aminoaldehydes such as 4-N,N-dimethylaminobenzaldehyde; N-substituted carbodiimides such as dicyclohexylcarbodiimide; Schiff bases such as N-ethylethyleneimine and N-methylbenzylideneimine; pyridyl-containing vinyl compounds such as 4-vinylpyridine.

[0141] When a siloxane compound is used as a modifier having a functional group capable of interacting with silica, it is preferred to further react a compound represented by the following general formula (9) with the conjugated diene polymer chain reacted with the siloxane compound.

[0142] [Chemical formula 6]

[0143]

[0144] In the general formula (9), R 29 A is a hydrocarbon group, 1 A is a group that can react with the alkyl metal group as the active terminal of the conjugated diene polymer chain having an active terminal, or a group that can react with the reaction residue generated by the reaction of the conjugated diene polymer chain having an active terminal and the siloxane compound, 2 is a group containing a nitrogen atom, p is an integer of 0 to 2, q is an integer of 1 to 3, r is an integer of 1 to 3, and p+q+r=4.

[0145] Here, it is considered that the compound represented by the general formula (9) and the alkyl metal group, i.e., -R - M + , or -O as a reaction residue generated by reaction with a siloxane compound - M + (including -O - M +The group represented by is hydrolyzed and converted into a hydroxyl group) and the group represented by is reacted. Furthermore, the amount of the siloxane compound used is 1 mol or more in terms of the number of repeating units of (-Si-O-) relative to 1 mol of the polymerization initiator, and -R - M + In the case where substantially no group represented by is left, substantially all of the compound represented by the general formula (9) can be reacted with -O as a reaction residue generated by the reaction with the siloxane compound. - M + The group represented by the formula (9) can be reacted, thereby appropriately introducing a modified structure based on the compound represented by the formula (9) via a structure derived from a siloxane compound into the conjugated diene polymer chain. Moreover, thereby, the low heat generation, wear resistance and stone chip resistance of the obtained rubber cross-linked product can be taken into account at a higher level.

[0146] In the compound represented by the general formula (9), R in the general formula (9) 29 The hydrocarbon group includes, for example, an alkyl group, a cycloalkyl group, an alkenyl group, an aryl group, an aralkyl group, and the like, and preferably an alkyl group having 1 to 6 carbon atoms. Examples of the alkyl group having 1 to 6 carbon atoms include a methyl group, an ethyl group, a n-propyl group, an isopropyl group, a butyl group, a pentyl group, a hexyl group, and the like, and among these, a methyl group and an ethyl group are more preferred, and a methyl group is particularly preferred.

[0147] In the compound represented by the general formula (9), A in the general formula (9) 1 is an alkyl metal group (i.e., -R - M + ) or a reactive residue (typically -O - M + The group represented by) is preferably -OR 30 (R 30 is a hydrogen atom or a hydrocarbon group). 30 Examples of the hydrocarbon group include alkyl, cycloalkyl, alkenyl, aryl, aralkyl, etc., and from the viewpoint of reactivity with the above-mentioned alkyl metal group or reaction residue, an alkyl group having 1 to 6 carbon atoms is preferred. Examples of the alkyl group having 1 to 6 carbon atoms include methyl, ethyl, n-propyl, isopropyl, butyl, pentyl, hexyl, etc., and among these, methyl and ethyl are more preferred.

[0148] In the compound represented by the general formula (9), A in the general formula (9) 2It is a group containing a nitrogen atom. There are no particular limitations on the group as long as it is a group containing a nitrogen atom. It is preferably an organic group having a nitrogen atom. Examples thereof include 3-aminopropyl, 4-aminobutyl, 3-(2-aminoethylamino)propyl, 2-dimethylaminoethyl, 3-dimethylaminopropyl, 3-diethylaminopropyl, 3-dipropylaminopropyl, 3-dibutylaminopropyl, 3-phenylmethylaminopropyl, 3-(4-methylpiperazinyl)propyl, N,N-bis(trimethylsilyl)aminopropyl, N,N-bis(triethylsilyl)aminopropyl, N,N',N'-tris(trimethylsilyl)-N-(2-aminoethyl)-3-aminopropyl and the like. Among these, from the viewpoint of being able to achieve a higher level of low heat build-up, wear resistance and stone chip resistance of the obtained rubber cross-linked product, groups containing primary amino groups having active hydrogen atoms and / or secondary amino groups having active hydrogen atoms, such as 3-aminopropyl, 4-aminobutyl, 3-(2-aminoethylamino)propyl, are preferred. In addition, "active hydrogen atom" refers to a hydrogen atom bonded to an atom other than a carbon atom, and is preferably lower than the bond energy of the carbon-hydrogen bond of the polymethylene chain.

[0149] In the compound represented by the general formula (9), p is an integer of 0 to 2, q is an integer of 1 to 3, r is an integer of 1 to 3, and p+q+r=4. From the viewpoint of reactivity with the alkyl metal group as the active terminal of the conjugated diene polymer chain having an active terminal, or reactivity with the reaction residue generated by the reaction of the conjugated diene polymer chain having an active terminal with the siloxane compound, it is preferred that: p is an integer of 0 to 1, q is an integer of 2 to 3, and r is an integer of 1 to 2, and it is more preferred that: p=0, q=3, and r=1. In addition, when p is 2, the two R contained in one molecule of the compound represented by the general formula (9) are 29 The groups represented by may be the same or different from each other. Similarly, when q is 2 or 3, the plurality of A contained in one molecule of the compound represented by the general formula (9) may be 1 The groups represented by may be the same or different from each other. When r is 2 or 3, the number of A groups contained in one molecule of the compound represented by the general formula (9) is 2 The groups represented may be the same as or different from each other.

[0150] Specific examples of the compound represented by the general formula (9) are not particularly limited. For example, A in the general formula (9) 2The compound is a compound containing a primary amino group having an active hydrogen atom and / or a secondary amino group having an active hydrogen atom, and examples thereof include 3-aminopropyldimethylmethoxysilane, 3-aminopropylmethyldimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyldimethylethoxysilane, 3-aminopropylmethyldiethoxysilane, 3-aminopropyltriethoxysilane and the like. 2 Compounds; 4-aminobutyldimethylmethoxysilane, 4-aminobutylmethyldimethoxysilane, 4-aminobutyltrimethoxysilane, 4-aminobutyldimethylethoxysilane, 4-aminobutylmethyldiethoxysilane, 4-aminobutyltriethoxysilane, etc. having 4-aminobutyl as A 2 Compounds; 3-(2-aminoethylamino)propyldimethylmethoxysilane, 3-(2-aminoethylamino)propylmethyldimethoxysilane, 3-(2-aminoethylamino)propyltrimethoxysilane, 3-(2-aminoethylamino)propyldimethylethoxysilane, 3-(2-aminoethylamino)propylmethyldiethoxysilane, 3-(2-aminoethylamino)propyltriethoxysilane, etc. having 3-(2-aminoethylamino)propyl as A 2 of compounds, etc.

[0151] In addition, as A in the general formula (9), 2 The compound is a group other than a group containing a primary amino group having an active hydrogen atom and / or a secondary amino group having an active hydrogen atom, and examples thereof include 3-dimethylaminopropyltrimethoxysilane, 3-dimethylaminopropylmethyldimethoxysilane, 3-dimethylaminopropyldimethylmethoxysilane, 3-dimethylaminopropyltriethoxysilane, 3-dimethylaminopropylmethyldiethoxysilane, 3-dimethylaminopropyldimethylethoxysilane and the like having a 3-dimethylaminopropyl group as A. 2 Compounds; 3-diethylaminopropyltrimethoxysilane, 3-diethylaminopropylmethyldimethoxysilane, 3-diethylaminopropyldimethylmethoxysilane, 3-diethylaminopropyltriethoxysilane, 3-diethylaminopropylmethyldiethoxysilane, 3-diethylaminopropyldimethylethoxysilane, etc. having 3-diethylaminopropyl as A 2 Compounds; 3-dipropylaminopropyltrimethoxysilane, 3-dipropylaminopropylmethyldimethoxysilane, 3-dipropylaminopropyldimethylmethoxysilane, 3-dipropylaminopropyltriethoxysilane, 3-dipropylaminopropylmethyldiethoxysilane, 3-dipropylaminopropyldimethylethoxysilane, etc. having 3-dipropylaminopropyl as A 2Compounds; 3-dibutylaminopropyltrimethoxysilane, 3-dibutylaminopropylmethyldimethoxysilane, 3-dibutylaminopropyldimethylmethoxysilane, 3-dibutylaminopropyltriethoxysilane, 3-dibutylaminopropylmethyldiethoxysilane, 3-dibutylaminopropyldimethylethoxysilane, etc. having 3-dibutylaminopropyl as A 2 Compounds; 3-phenylmethylaminopropyl trimethoxysilane, 3-phenylmethylaminopropyl methyl dimethoxysilane, 3-phenylmethylaminopropyl dimethylmethoxysilane, 3-phenylmethylaminopropyl triethoxysilane, 3-phenylmethylaminopropyl methyl diethoxysilane, 3-phenylmethylaminopropyl dimethylethoxysilane, etc. having 3-phenylmethylaminopropyl as A 2 Compounds; 3-(4-methylpiperazinyl)propyltrimethoxysilane, 3-(4-methylpiperazinyl)propylmethyldimethoxysilane, 3-(4-methylpiperazinyl)propyldimethylmethoxysilane, 3-(4-methylpiperazinyl)propyltriethoxysilane, 3-(4-methylpiperazinyl)propylmethyldiethoxysilane, 3-(4-methylpiperazinyl)propyldimethylethoxysilane, etc. having 3-(4-methylpiperazinyl)propyl as A 2 Compounds of

[0152] N,N-bis(trimethylsilyl)aminopropyltrimethoxysilane, N,N-bis(trimethylsilyl)aminopropyltriethoxysilane, N,N-bis(trimethylsilyl)aminopropylmethyldimethoxysilane, N,N-bis(trimethylsilyl)aminopropylmethyldiethoxysilane, etc. have N,N-bis(trimethylsilyl)aminopropyl as A. 2 Compounds; N, N-bis (triethylsilyl) aminopropyl trimethoxysilane, N, N-bis (trimethylsilyl) aminopropyl triethoxysilane, N, N-bis (triethylsilyl) aminopropyl methyl dimethoxysilane, N, N-bis (triethylsilyl) aminopropyl methyl diethoxysilane, etc. having N, N-bis (triethylsilyl) aminopropyl as A 2 Compounds; N, N', N'-tris (trimethylsilyl) -N- (2-aminoethyl) -3-aminopropyl trimethoxysilane, N, N', N'-tris (trimethylsilyl) -N- (2-aminoethyl) -3-aminopropyl triethoxysilane, N, N', N'-tris (trimethylsilyl) -N- (2-aminoethyl) -3-aminopropyl methyl dimethoxysilane, N, N', N'-tris (trimethylsilyl) -N- (2-aminoethyl) -3-aminopropyl methyl diethoxysilane and the like having N, N', N'-tris (trimethylsilyl) -N- (2-aminoethyl) -3-aminopropyl as A 2 of compounds, etc.

[0153] The amount of the compound represented by the general formula (9) used is not particularly limited, but is preferably 0.1 to 5 moles, more preferably 0.2 to 2 moles, and still more preferably 0.4 to 1.5 moles relative to 1 mole of the polymerization initiator used in the polymerization step. By making the amount of the compound represented by the general formula (9) used within the above range, the low heat generation, wear resistance, and stone chip resistance of the obtained rubber cross-linked product can be achieved at a higher level.

[0154] The timing of adding the compound represented by the general formula (9) to the solution containing the conjugated diene polymer chain is not particularly limited as long as it is after the siloxane compound is added. For example, the compound represented by the general formula (9) can be added to the solution when the polymerization reaction is not completed and the solution containing the conjugated diene polymer chain still contains monomers. More specifically, the compound represented by the general formula (9) can be added to the solution when the solution containing the conjugated diene polymer chain contains more than 100 ppm, more preferably 300 to 50,000 ppm of monomers. By adding the compound represented by the general formula (9) at such a timing, the side reaction between the conjugated diene polymer chain and the impurities contained in the polymerization system can be suppressed, and the reaction can be well controlled. Alternatively, before adding the compound represented by the general formula (9) to the solution containing the conjugated diene polymer chain or after adding the compound represented by the general formula (9), an alcohol such as water or methanol can be added to the solution, thereby removing the -O- ... - M + The modification reaction is carried out in a state where the group represented by the general formula (9) is hydrolyzed and converted into a hydroxyl group. When the compound represented by the general formula (9) is added to a solution containing a conjugated diene polymer chain, the compound represented by the general formula (9) may be added after being dissolved in an inert solvent, or may be added directly without being dissolved in an inert solvent. The reaction temperature and reaction time may be the same as those in the case of a reaction using a siloxane compound.

[0155] Furthermore, after reacting the compound represented by the general formula (9), a known polymerization terminator is added as required to deactivate the reaction system, and then, as desired, antioxidants such as phenol stabilizers, phosphorus stabilizers, and sulfur stabilizers, agglomerating agents, and scale inhibitors are added to the reaction solution, and then the polymerization solvent is separated from the reaction solution by direct drying or steam stripping to recover the conjugated diene polymer. In addition, before separating the polymerization solvent from the reaction solution, an extender oil may be mixed in the polymerization solution to recover the conjugated diene polymer as an oil-extended rubber.

[0156] As the extender oil used when the conjugated diene polymer is recovered as an oil-extended rubber, for example, petroleum softeners such as paraffin, aromatic and cycloalkane; plant softeners; and fatty acids, etc. In the case of using a petroleum softener, it is preferred that the content of polycyclic aromatics extracted by the IP346 method (test method of the Institute of Petroleum) is less than 3%. In the case of using an extender oil, its usage amount is preferably 1 to 100 parts by weight, more preferably 2 to 60 parts by weight, and further preferably 3 to 50 parts by weight relative to 100 parts by weight of the conjugated diene polymer.

[0157] In addition, in the above, the case of using siloxane compounds and compounds represented by general formula (9) as modifiers having a functional group capable of interacting with silica is mainly exemplified. The modifier having a functional group capable of interacting with silica is not particularly limited as long as it is a compound that can react with the active end of the conjugated diene polymer chain having an active end obtained in the above-mentioned polymerization step and has a functional group capable of interacting with silica.

[0158] In addition, as a method for introducing a functional group that can interact with silica in a conjugated diene polymer, it is possible to replace a method for reacting a modifier having a functional group that can interact with silica with a conjugated diene polymer chain having an active terminal obtained in a polymerization process, or on this method, a method for selecting a functional group that can interact with silica in the above-mentioned polymerization process. Specifically, in the above-mentioned polymerization process, by copolymerizing a compound that can react with a monomer used in the polymerization process and having a functional group that can interact with silica, it is possible to introduce a functional group that can interact with silica. As a functional group that can interact with silica, it is not particularly limited, and nitrogen-containing atom functional groups, silicon-containing atom functional groups, oxygen-containing atom functional groups, etc. can be cited. Among these, from the viewpoint of high interaction with silica, silicon-containing atom functional groups are preferred.

[0159] Examples of the silicon-containing modifier used in the polymerization step include (dimethylamino)dimethylvinylsilane, (ethylmethylamino)dimethylvinylsilane, (diethylamino)dimethylvinylsilane, (ethyl-n-propylamino)dimethylvinylsilane, (ethylisopropylamino)dimethylvinylsilane, (di-n-propylamino)dimethylvinylsilane, (diisopropylamino)dimethylvinylsilane, (n-butyl-n-propylamino)dimethylvinylsilane, (di-n-butylamino)dimethylvinylsilane,

[0160] (Dimethylamino)diethylvinylsilane, (ethylmethylamino)diethylvinylsilane, (diethylamino)diethylvinylsilane, (ethyl-n-propylamino)diethylvinylsilane, (ethylisopropylamino)diethylvinylsilane, (di-n-propylamino)diethylvinylsilane, (diisopropylamino)diethylvinylsilane, (n-butyl-n-propylamino)diethylvinylsilane, (di-n-butylamino)diethylvinylsilane,

[0161] (Dimethylamino)dipropylvinylsilane, (ethylmethylamino)dipropylvinylsilane, (diethylamino)dipropylvinylsilane, (ethyl-n-propylamino)dipropylvinylsilane, (ethylisopropylamino)dipropylvinylsilane, (di-n-propylamino)dipropylvinylsilane, (diisopropylamino)dipropylvinylsilane, (n-butyl-n-propylamino)dipropylvinylsilane, (di-n-butylamino)dipropylvinylsilane,

[0162] (Dimethylamino)dibutylvinylsilane, (ethylmethylamino)dibutylvinylsilane, (diethylamino)dibutylvinylsilane, (ethyl-n-propylamino)dibutylvinylsilane, (ethylisopropylamino)dibutylvinylsilane, (di-n-propylamino)dibutylvinylsilane, (diisopropylamino)dibutylvinylsilane, (n-butyl-n-propylamino)dibutylvinylsilane, (di-n-butylamino)dibutylvinylsilane,

[0163] [Bis(trimethylsilyl)amino]dimethylvinylsilane, bis[(tert-butyldimethylsilyl)amino]dimethylvinylsilane, [bis(trimethylsilyl)amino]diethylvinylsilane, bis[(tert-butyldimethylsilyl)amino]diethylvinylsilane, bis(dimethylamino)methylvinylsilane, bis(ethylmethylamino)methylvinylsilane, bis(diethylamino)methylvinylsilane, bis(ethyl-n-propylamino)methylvinylsilane, bis(ethylisopropylamino)methylvinylsilane, bis(di-n-propylamino)methylvinylsilane, bis(diisopropylamino)methylvinylsilane, bis(n-butyl-n-propylamino)methylvinylsilane, bis(di-n-butylamino)methylvinylsilane,

[0164] Bis(dimethylamino)ethylvinylsilane, bis(ethylmethylamino)ethylvinylsilane, bis(diethylamino)ethylvinylsilane, bis(ethyl-n-propylamino)ethylvinylsilane, bis(ethylisopropylamino)ethylvinylsilane, bis(di-n-propylamino)ethylvinylsilane, bis(diisopropylamino)ethylvinylsilane, bis(n-butyl-n-propylamino)ethylvinylsilane, bis(di-n-butylamino)ethylvinylsilane,

[0165] Bis(dimethylamino)propylvinylsilane, bis(ethylmethylamino)propylvinylsilane, bis(diethylamino)propylvinylsilane, bis(ethyl-n-propylamino)propylvinylsilane, bis(ethylisopropylamino)propylvinylsilane, bis(di-n-propylamino)propylvinylsilane, bis(diisopropylamino)propylvinylsilane, bis(n-butyl-n-propylamino)propylvinylsilane, bis(di-n-butylamino)propylvinylsilane,

[0166] Bis(dimethylamino)butylvinylsilane, bis(ethylmethylamino)butylvinylsilane, bis(diethylamino)butylvinylsilane, bis(ethyl-n-propylamino)butylvinylsilane, bis(ethylisopropylamino)butylvinylsilane, bis(di-n-propylamino)butylvinylsilane, bis(diisopropylamino)butylvinylsilane, bis(n-butyl-n-propylamino)butylvinylsilane, bis(di-n-butylamino)butylvinylsilane,

[0167] Bis[bis(trimethylsilyl)amino]methylvinylsilane, bis[(tert-butyldimethylsilyl)amino]methylvinylsilane, bis[bis(trimethylsilyl)amino]ethylvinylsilane, bis[(tert-butyldimethylsilyl)amino]ethylvinylsilane, tris(dimethylamino)vinylsilane, tris(ethylmethylamino)vinylsilane, tris(diethylamino)vinylsilane, tris(ethylpropylamino)vinylsilane, tris(dipropylamino)vinylsilane, tris(butylpropylamino)vinylsilane and the like.

[0168] In addition, the compound having a functional group capable of interacting with silica used in the above-mentioned polymerization step may be any one or more selected from 4,4'-vinylidenebis(n,n-dimethylaniline), 3-(2-pyrrolidinylethyl)styrene, 4-(2-pyrrolidinylethyl)styrene and 3-(2-pyrrolidinyl-1-methylethyl)-α-methylstyrene.

[0169] In addition, in the present invention, before a modifier having a functional group capable of interacting with silica, such as a siloxane compound, is reacted with a conjugated diene polymer chain having an active terminal, a coupling agent, a modifier, etc. conventionally used may be added to the polymerization system to couple or modify a part of the active terminal of the conjugated diene polymer chain having an active terminal, within a range that does not hinder the effect of the present invention.

[0170] The coupling rate of the conjugated diene polymer used in the present invention is not particularly limited, and is preferably 10 to 90% by weight, more preferably 20 to 80% by weight, and particularly preferably 30 to 70% by weight. By making the coupling rate within the above range, the low heat generation, wear resistance and stone chip resistance of the obtained rubber cross-linked product can be taken into account at a higher level. In addition, the coupling rate is the weight percentage of the polymer molecules relative to the total amount of the conjugated diene polymer finally obtained, and the above-mentioned polymer molecules are polymer molecules with a molecular weight of 1.8 times or more of the peak molecular weight of the conjugated diene polymer chain with an active terminal before reacting with a modifier having a functional group that can interact with silica, such as a siloxane compound and a compound represented by the general formula (9), and a coupling agent or other modifier used as needed, and the molecular weight at this time is determined by gel permeation chromatography as a polystyrene-converted molecular weight.

[0171] The coupling agent used as needed in the present invention is not particularly limited, and for example, a halogenated metal compound can be used. Specifically, silicon tetrachloride, hexachlorodisilane, bis (trichlorosilyl) methane, 1,2-bis (trichlorosilyl) ethane, 1,3-bis (trichlorosilyl) propane, 1,4-bis (trichlorosilyl) butane, 1,5-bis (trichlorosilyl) pentane, 1,6-bis (trichlorosilyl) hexane, among which hexachlorodisilane, 1,2-bis (trichlorosilyl) ethane or 1,6-bis (trichlorosilyl) hexane etc. can be cited. In addition, tin tetrachloride can also be used.

[0172] <Silicon Dioxide>

[0173] The rubber composition for a heavy load tire of the present invention contains silica in addition to the conjugated diene polymer having a glass transition temperature (Tg) of -60°C or lower and having a functional group capable of interacting with silica.

[0174] The silica used in the present invention is not particularly limited, and for example, dry-process silica, wet-process silica, colloidal silica, precipitated silica, etc. can be used. In addition, a carbon-silica dual-phase filler in which silica is supported on the surface of carbon black can also be used. Among these, wet-process silica containing hydrous silicic acid as the main component is preferred. These can be used alone or in combination of two or more.

[0175] The nitrogen adsorption specific surface area of ​​silica measured by the BET method is preferably 30 to 500 m 2 / g, more preferably 50 to 400 m 2 / g, more preferably 140 to 250 m 2 / g, particularly preferably 180 to 240 m 2 / g. By using silica having a specific surface area within the above range, the low heat generation, wear resistance and stone chip resistance of the obtained rubber cross-linked product can be achieved at a higher level. In addition, the pH of silica is preferably less than 7, more preferably 5 to 6.9. In addition, the nitrogen adsorption specific surface area can be measured by the BET method according to ASTM D3037-81.

[0176] The amount of silica in the rubber composition for heavy-duty tires of the present invention is preferably 10 to 200 parts by weight, more preferably 15 to 100 parts by weight, further preferably 20 to 50 parts by weight, and particularly preferably 22 to 40 parts by weight, relative to 100 parts by weight of the rubber component in the rubber composition for heavy-duty tires. By making the amount of silica in the above range, the dispersion of silica during production can be improved, and the low heat generation, wear resistance, and stone impact resistance of the obtained rubber cross-linked product can be taken into account at a higher level.

[0177] <Carbon Black>

[0178] In addition, the rubber composition for heavy-duty tires of the present invention preferably contains carbon black in addition to the conjugated diene polymer having a glass transition temperature (Tg) of -50°C or less and having a functional group capable of interacting with silica, and silica. By further containing carbon black, the wear resistance of the obtained rubber cross-linked product can be further improved.

[0179] Examples of carbon black include furnace black, acetylene black, thermal black, channel black, and graphite. Among these, furnace black is preferably used, and specific examples thereof include SAF, ISAF, ISAF-HS, ISAF-LS, IISAF-HS, HAF, HAF-HS, and HAF-LS. These can be used alone or in combination of two or more.

[0180] The nitrogen adsorption specific surface area of ​​carbon black measured by the BET method is preferably 30 m 2 / g or more, more preferably 30 to 170 m 2 / g, more preferably 70 to 160 m 2 / g, particularly preferably 110 to 150 m 2 By using carbon black having a specific surface area within this range, the wear resistance of the obtained rubber cross-linked product can be further improved. In addition, the nitrogen adsorption specific surface area can be measured by the BET method in accordance with JIS K-6217.

[0181] The DBP absorption of carbon black measured by method A is preferably 60 to 160 cm 3 / 100g, more preferably 85 to 150cm 3 / 100g, more preferably 110 to 145cm3 By using carbon black having a DBP absorption within this range, the abrasion resistance of the obtained rubber cross-linked product can be further improved. The DBP absorption can be measured by method A according to JIS Z-8091.

[0182] The iodine adsorption of carbon black is preferably 25 to 170 mg / g, more preferably 70 to 160 mg / g, and even more preferably 110 to 150 mg / g. By using carbon black having an iodine adsorption within this range, the wear resistance of the obtained rubber cross-linked product can be further improved. In addition, the iodine adsorption can be measured according to JIS Z-8091.

[0183] The amount of carbon black in the rubber composition for heavy-duty tires of the present invention is preferably 10 to 200 parts by weight, more preferably 15 to 150 parts by weight, further preferably 20 to 100 parts by weight, and further preferably 22 to 40 parts by weight, relative to 100 parts by weight of the rubber component in the rubber composition for heavy-duty tires. By setting the amount of carbon black in the above range, the wear resistance of the obtained rubber cross-linked product can be further appropriately improved.

[0184] <Natural Rubber>

[0185] In addition, the rubber composition for heavy-duty tires of the present invention preferably contains natural rubber as a rubber component in addition to the conjugated diene polymer having a glass transition temperature (Tg) of -50°C or less and having a functional group capable of interacting with silica. As the natural rubber, in addition to the usual natural rubber, modified natural rubbers such as epoxidized natural rubber and hydrogenated natural rubber introduced with epoxy groups can be used, and they can also be used in combination. By containing natural rubber, the stone impact resistance of the obtained rubber cross-linked product can be further improved.

[0186] The content of natural rubber in the rubber composition for heavy-duty tires of the present invention is preferably 10 to 80% by weight, more preferably 30 to 70% by weight, further preferably 40 to 60% by weight, and particularly preferably 45 to 55% by weight, based on the content of 100% by weight of all rubber components contained in the rubber composition for heavy-duty tires of the present invention. By mixing natural rubber in the above ratio, the stone impact resistance of the obtained rubber cross-linked product can be further appropriately improved.

[0187] <Other rubber>

[0188] The heavy load tire rubber composition of the present invention preferably contains, in addition to the conjugated diene polymer having a glass transition temperature (Tg) of -60°C or less and having a functional group capable of interacting with silica and, if necessary, natural rubber, other rubbers as rubber components.

[0189] As such other rubbers, for example, polybutadiene rubber (which may be high cis-BR or low cis-BR. In addition, polybutadiene rubber containing crystalline fibers composed of 1,2-polybutadiene polymers may be used), polyisoprene rubber, emulsion-polymerized styrene-butadiene copolymer rubber, solution-polymerized styrene-butadiene copolymer rubber, styrene-isoprene copolymer rubber, butadiene-isoprene copolymer rubber, styrene-isoprene-butadiene copolymer rubber, acrylonitrile-butadiene copolymer rubber, acrylonitrile-styrene-butadiene copolymer rubber, cyclic olefin ring-opening polymers, hydrogenated conjugated diene polymers, etc., except for the above-mentioned conjugated diene polymers having a glass transition temperature (Tg) of -60°C or less and having a functional group capable of interacting with silica. These rubbers may be used alone or in combination of two or more.

[0190] When these other rubbers are blended, the content thereof is preferably 10 to 80% by weight, more preferably 20 to 60% by weight, and even more preferably 25 to 40% by weight based on the content ratio of all rubber components contained in the rubber composition for a heavy load tire of the present invention.

[0191] In addition, among other rubbers, styrene-butadiene copolymer rubber is preferred, and terminal-modified styrene-butadiene copolymer is more preferred, from the viewpoint that the obtained rubber cross-linked product can have low heat generation, wear resistance and stone chip resistance at a higher level. As the styrene-butadiene copolymer rubber, for example, a styrene unit content of preferably 5 to 50% by weight, more preferably 10 to 30% by weight, and a butadiene unit content of preferably 50 to 95% by weight, more preferably 70 to 90% by weight can be used.

[0192] In addition, from the viewpoint of further improving the low heat build-up property, a silane coupling agent may be further added to the rubber composition for a heavy-duty tire of the present invention. The silane coupling agent is not particularly limited, and various silane coupling agents may be used. In the present invention, a sulfide-based, mercapto-based, protected mercapto-based (e.g., a silane coupling agent having a carbonylthio group), thiocyanate-based, vinyl-based, amino-based, methacrylate-based, glycidoxy-based, nitro-based, epoxy-based, or chlorine-based silane coupling agent may be preferably used. Specific examples of the silane coupling agent include bis(3-(triethoxysilyl)propyl)disulfide, bis(3-triethoxysilylpropyl)trisulfide, bis(3-(triethoxysilyl)propyl)tetrasulfide, γ-mercaptopropyltriethoxysilane, 3-[ethoxybis(3,6,9,12,15-pentaoxacosan-1-yloxy)silyl]-1-propanethiol, 3-octanoylthio-1-propyl-triethoxysilane, 3-trimethoxysilylpropyl-N,N-dimethylthiocarbamate Acyl tetrasulfide, γ-trimethoxysilylpropylbenzothiazole tetrasulfide, 3-trimethoxysilylpropylbenzothiazole tetrasulfide, 3-thiocyanatepropyltriethoxysilane, vinyltriethoxysilane, N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane, 3-trimethoxysilylpropylmethacrylate monosulfide, γ-glycidoxypropyltriethoxysilane, 3-nitropropyltrimethoxysilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, and 3-chloropropyltrimethoxysilane, etc. In addition, NXT-Z100, NXT-Z30, NXT-Z45, NXT-Z60, NXT-Z45, NXT manufactured by Momentive Performance Materials, Si69, Si75, VP Si363 manufactured by Evonik, etc. can also be used. These silane coupling agents can be used alone or in combination of two or more. In addition, one or more of them can be oligomerized in advance and used in an oligomerized state. The amount of the silane coupling agent is preferably 0.1 to 30 parts by weight, more preferably 1 to 15 parts by weight relative to 100 parts by weight of silicon dioxide.

[0193] In addition, the rubber composition for heavy-duty tires of the present invention preferably further contains a crosslinking agent. Examples of the crosslinking agent include sulfur, sulfur halides, organic peroxides, quinone dioximes, organic polyamine compounds, and alkylphenol resins having methylol groups. Among these, sulfur is preferably used. The amount of the crosslinking agent is preferably 0.1 to 15 parts by weight, more preferably 0.5 to 5 parts by weight, and particularly preferably 1 to 4 parts by weight relative to 100 parts by weight of the rubber component in the rubber composition for heavy-duty tires.

[0194] Furthermore, in addition to the above-mentioned ingredients, the rubber composition for heavy-duty tires of the present invention may also contain required amounts of cross-linking promoters, cross-linking activators, antioxidants, fillers (excluding the above-mentioned silica and carbon black), activators, processing oils, plasticizers, lubricants, tackifiers, compatibilizers, surfactants and other compounding agents according to conventional methods.

[0195] When sulfur or a sulfur-containing compound is used as a crosslinking agent, it is preferred to use a crosslinking accelerator and a crosslinking activator together. Examples of crosslinking accelerators include: sulfonamide crosslinking accelerators; guanidine crosslinking accelerators; thiourea crosslinking accelerators; thiazole crosslinking accelerators; thiuram crosslinking accelerators; dithiocarbamic acid crosslinking accelerators; xanthogenic acid crosslinking accelerators, etc. Among these, it is preferred to include a sulfonamide crosslinking accelerator. These crosslinking accelerators can be used alone or in combination of two or more. The amount of the crosslinking accelerator is preferably 0.1 to 15 parts by weight, more preferably 0.5 to 5 parts by weight, and particularly preferably 1 to 4 parts by weight relative to 100 parts by weight of the rubber component in the rubber composition for heavy-duty tires.

[0196] As the crosslinking activator, for example, higher fatty acids such as stearic acid, zinc oxide, etc. can be cited. These crosslinking activators can be used alone or in combination of two or more. The amount of the crosslinking activator is preferably 0.05 to 20 parts by weight, particularly preferably 0.5 to 15 parts by weight, relative to 100 parts by weight of the rubber component in the rubber composition for heavy-duty tires.

[0197] As antioxidants, there can be mentioned: antioxidants that are color-changing aging stabilizers and have anti-fatigue and anti-ozone effects, such as N-isopropyl-N'-phenyl-p-phenylenediamine (IPPD), N-1,3-dimethylbutyl-N'-phenyl-p-phenylenediamine (6PPD), N-1,4-dimethylpentyl-N'-phenyl-p-phenylenediamine (7PPD), N,N'-bis-(1,4-dimethylpentyl)-p-phenylenediamine (77PD), etc.; antioxidants that are color-changing aging stabilizers and have fatigue protection but no anti-ozone effect, such as phenyl-α-naphthylamine (PAN); antioxidants that are color-changing aging stabilizers, have low anti-fatigue effect and no anti-ozone effect, such as octylated diphenylamine (ODPA); antioxidants that are non-color-changing aging stabilizers and have fatigue protection and good heat protection, such as styrenated phenol (SPH), etc. These antioxidants can be used alone or in combination of two or more. The amount of the antioxidant blended is preferably 0.1 to 15 parts by weight, more preferably 0.5 to 10 parts by weight, and particularly preferably 1 to 5 parts by weight, based on 100 parts by weight of the rubber component in the rubber composition for a heavy load tire.

[0198] In addition, in addition to the rubber component, the heavy-duty tire rubber composition of the present invention can also be mixed with resin. By mixing with resin, the heavy-duty tire rubber composition can be given adhesion or the dispersibility of the silica in the heavy-duty tire rubber composition can be improved. As a result, it is expected that the balance of the stone impact resistance, low heat generation and wear resistance of the obtained rubber cross-linked product will be improved. In addition, as the same effect as the plasticizer, the processability of the heavy-duty tire rubber composition can also be improved. As resin, for example: C5 series petroleum resin, C5 / C9 series petroleum resin, C9 series petroleum resin, dicyclopentadiene series resin, terpene series resin, terpene phenolic resin, aromatic modified terpene resin, alkylphenol-acetylene resin, rosin series resin, rosin ester resin, indene series resin, C9 series resin containing indene, α-methylstyrene-indene copolymer resin, coumarone-indene resin, farnesene series resin, polylimonene resin, etc. These resins can be modified resins or hydrogenated resins. These resins may be used alone or in combination of two or more. The blending amount of the resin is preferably 25 parts by weight or less relative to 100 parts by weight of the rubber component in the rubber composition for a heavy load tire.

[0199] In order to obtain the rubber composition for heavy-duty tires of the present invention, the components can be kneaded according to a conventional method. For example, the components used as needed, except for the heat-unstable components such as crosslinking agents and crosslinking accelerators, can be kneaded with the above-mentioned conjugated diene polymer and silica, and then the heat-unstable components such as crosslinking agents and crosslinking accelerators can be mixed into the kneaded product to obtain the target composition. The kneading temperature of the components other than the heat-unstable components with the conjugated diene polymer and silica is preferably 80 to 200° C., more preferably 120 to 180° C., and the kneading time is preferably 30 seconds to 30 minutes. In addition, the mixing of the kneaded product and the heat-unstable components is usually carried out after cooling to below 100° C., preferably after cooling to below 80° C.

[0200] <Rubber cross-linked product>

[0201] The cross-linked rubber of the present invention is obtained by cross-linking the above-mentioned rubber composition for a heavy load tire of the present invention.

[0202] The crosslinking method when crosslinking the rubber composition for heavy-duty tires of the present invention is not particularly limited, and can be selected according to the shape, size, etc. of the crosslinked rubber product. The crosslinking can be performed while molding by filling the rubber composition for heavy-duty tires in a metal mold and heating it, or the crosslinking can be performed by heating the pre-molded rubber composition for heavy-duty tires. The crosslinking temperature is preferably 100 to 200°C, more preferably 130 to 190°C, and the crosslinking time is preferably 1 minute to 24 hours, more preferably 2 minutes to 12 hours, and further preferably 3 minutes to 6 hours.

[0203] Furthermore, depending on the shape and size of the cross-linked rubber, even if the surface is cross-linked, the inside may not be fully cross-linked. Therefore, further heating may be performed to perform secondary cross-linking.

[0204] As the heating method, any method generally used for cross-linking of rubber, such as press heating, steam heating, oven heating, and hot air heating, may be appropriately selected.

[0205] The cross-linked rubber of the present invention is obtained by using the above-mentioned rubber composition for heavy-duty tires of the present invention, and therefore has excellent low heat generation, wear resistance and stone impact resistance. Therefore, the cross-linked rubber of the present invention can be preferably used for various tire applications, especially for heavy-duty tires installed on trucks (including tractors, trailers), buses, construction vehicles (such as dump trucks, graders), etc. In addition, in such tires, the cross-linked rubber of the present invention can be used in various parts of the tire such as the tread portion, the carcass portion, the sidewall portion, and the bead portion, and is particularly preferably used in the tread portion. Furthermore, it is also preferably used in the tread portion of a tread retread tire for replacing a worn and deteriorated tread portion.

[0206] Example

[0207] Below, based on detailed embodiment, the present invention is further described, but the present invention is not limited to these embodiments.In addition, below, as long as there is no special explanation, "part" is a weight basis.In addition, various tests and evaluations are carried out according to the following method.

[0208] [Weight average molecular weight, molecular weight distribution, coupling ratio]

[0209] The weight average molecular weight (Mw), molecular weight distribution (Mw / Mn) and coupling ratio were determined based on a graph obtained by gel permeation chromatography (GPC) based on molecular weights converted to polystyrene. Specific measurement conditions of gel permeation chromatography are as follows.

[0210] Measuring instrument: High performance liquid chromatograph (manufactured by Tosoh Corporation, trade name "HLC-8320")

[0211] Chromatographic column: Two polystyrene columns manufactured by Tosoh Corporation, trade name “GMH-HR-H”, connected in series.

[0212] Detector: Differential refractometer

[0213] Eluent: Tetrahydrofuran

[0214] Column temperature: 40°C

[0215] The coupling rate is determined by taking the area ratio of the peak portion having a peak top molecular weight 1.8 times or more of the peak top molecular weight of the minimum molecular weight peak to the total elution area in the elution curve obtained by gel permeation chromatography under the above conditions as the value of the coupling rate.

[0216] [Vinyl bond content]

[0217] Vinyl bond content 1 The measurement was performed by H-NMR.

[0218] [Mooney viscosity (ML (1+4) 100℃)]

[0219] The measurement was performed using a Mooney viscometer (manufactured by Shimadzu Corporation) in accordance with JIS K6300-1 (2013).

[0220] [Glass transition temperature (Tg)]

[0221] The measurement was performed in accordance with JIS K6240 (2011) using a differential scanning calorimeter (manufactured by PerkinElmer, trade name "DSC8500") in a helium atmosphere (gas flow rate: 20.0 mL / min). The peak top temperature of the differential curve of the obtained DSC curve was determined as the glass transition temperature (Tg).

[0222] [Low heat generation of cross-linked rubber]

[0223] The low heat build-up property of the cross-linked rubber was evaluated by measuring the tan δ value at 60°C for a test piece having a length of 50 mm, a width of 12.7 mm, and a thickness of 2 mm under the conditions of a dynamic strain of 2.5% and 10 Hz using ARES-G2 manufactured by TA Instruments. The low heat build-up property was obtained as an index with the measured value of Comparative Example 1 being 100. The larger the index, the better the low heat build-up property.

[0224] [Abrasion resistance of cross-linked rubber]

[0225] The wear resistance of the cross-linked rubber was evaluated by measuring a test piece having an outer diameter of 50 mm, an inner diameter of 15 mm, and a thickness of 10 mm using an FPS wear tester (manufactured by Ueshima Seisakusho Co., Ltd.) at a load of 10 N and a slip rate of 15%. The wear resistance was determined as an index with the measured value of Comparative Example 1 being 100. The larger the index, the better the wear resistance.

[0226] [Stone impact resistance]

[0227] Regarding the low heat build-up of the cross-linked rubber, a tensile test was performed using a test piece of 50 mm in length, 12.7 mm in width, and 2 mm in thickness in accordance with JIS K6301 to measure the elongation at break. Regarding the stone chip resistance, it was determined in the form of an index with the measured value of Comparative Example 1 being 100. The larger the index, the better the stone chip resistance.

[0228] [Production Example 1]

[0229] (Production of Polymer Block (A) Having Active Terminals)

[0230] 218.1 parts of cyclohexane, 7.5 parts of styrene and 0.3 parts of tetramethylethylenediamine were added to the container after nitrogen substitution, and the internal temperature of the container was adjusted to 50°C. Next, 1.64 parts of n-butyl lithium were added, and 92.5 parts of isoprene were added over 80 minutes. Then, by reacting for 15 minutes, a solution containing a polymer block (A) having an active terminal was obtained. The weight average molecular weight (Mw) of the polymer block (A) having an active terminal in the obtained solution was 6500, the molecular weight distribution (Mw / Mn) was 1.10, the styrene unit content was 7.5% by weight, the isoprene unit content was 92.5% by weight, and the vinyl bond content was 7.0%.

[0231] (Manufacture of terminal-modified polybutadiene rubber (P1))

[0232] In an autoclave with a stirrer, 596.5 parts of cyclohexane and 50.0 parts of 1,3-butadiene were added under a nitrogen environment, and then 9.0 parts (the amount of the polymer block (A) with an active terminal used was 2.7 parts) of a solution containing the polymer block (A) with an active terminal obtained in Production Example 1 were added, and polymerization was initiated at 50°C. After 30 minutes from the initiation of the polymerization, 50.0 parts of 1,3-butadiene were continuously added over 50 minutes, and further stirred for 20 minutes. The highest temperature in the polymerization reaction was 75°C. After confirming that the polymerization conversion rate reached the range of 95% to 100%, 0.015 parts of 1,6-bis(trichlorosilyl)hexane were added and reacted for 10 minutes. Then, 0.18 parts of a polyorganosiloxane represented by the following formula (10) in the state of a 40% concentration xylene solution was added and reacted for 10 minutes. Further, 0.18 parts of the polyorganosiloxane represented by the following formula (10) in the state of a 40% concentration xylene solution is added and reacted for 20 minutes. Next, 0.18 parts of 3-(2-aminoethylamino)propyltrimethoxysilane in the state of a 50% concentration xylene solution is added and reacted for 15 minutes. Then, methanol in an amount equivalent to 2 times the molar amount of the n-butyl lithium used is added as a polymerization terminator to obtain a polymer solution containing terminal-modified polybutadiene rubber (P1). Then, 0.20 parts of IRGANOX 1520L (manufactured by BASF) and IRGANOX 1076 (manufactured by BASF) are added to the polymer solution as antioxidants relative to 100 parts of the copolymer components contained in the polymer solution. Next, the solvent is removed by steam stripping, and a solid terminal-modified polybutadiene rubber (P1) is obtained by warm air drying. The weight average molecular weight, coupling ratio, vinyl bond content, Mooney viscosity and glass transition temperature of the obtained terminal-modified polybutadiene rubber (P1) were measured.

[0233] In addition, the obtained terminal-modified polybutadiene rubber (P1) is a rubber having a modified structure based on a polyorganosiloxane represented by the following formula (10) and 3-(2-aminoethylamino)propyltrimethoxysilane (including a modified structure such as a Si-OH structure and a Si-OCH3 structure) at the end of the polymer chain as a functional group capable of interacting with silica (the same applies to Production Examples 2 to 4 described later).

[0234] [Chemical formula 7]

[0235]

[0236] X 1 , X 4 , R 1 ~R 3 , R 5 ~R 8 :-CH3

[0237] [Production Example 2]

[0238] (Manufacture of terminal-modified polybutadiene rubber (P2))

[0239] In the production of the terminal-modified polybutadiene rubber (P1) of Production Example 1, 0.019 parts of tetramethylethylenediamine was added before initiating polymerization, and a solid terminal-modified polybutadiene rubber (P2) was obtained by the same method as in Production Example 1. The results of the measurement of the obtained terminal-modified polybutadiene rubber (P2) in the same manner as in Production Example 1 are shown in Table 1.

[0240] [Production Example 3]

[0241] (Manufacture of terminal-modified polybutadiene rubber (P3))

[0242] In the production of the terminal-modified polybutadiene rubber (P1) of Production Example 1, 0.038 of tetramethylethylenediamine was added before initiating polymerization, and a solid terminal-modified polybutadiene rubber (P3) was obtained by the same method as in Production Example 1. The results of the measurement of the obtained terminal-modified polybutadiene rubber (P3) in the same manner as in Production Example 1 are shown in Table 1.

[0243] [Production Example 4]

[0244] (Manufacture of terminal-modified polybutadiene rubber (P4))

[0245] In the production of the terminal-modified polybutadiene rubber (P1) of Production Example 1, 0.058 of tetramethylethylenediamine was added before initiating polymerization, and a solid terminal-modified polybutadiene rubber (P4) was obtained by the same method as in Production Example 1. The results of the measurement of the obtained terminal-modified polybutadiene rubber (P4) in the same manner as in Production Example 1 are shown in Table 1.

[0246] [Production Example 5]

[0247] (Manufacture of tin-coupled polybutadiene rubber (P5))

[0248] In an autoclave with a stirrer, 525 parts of cyclohexane and 56.8 parts of 1,3-butadiene were added under a nitrogen environment, and then 2.7 parts of n-butyl lithium were added to initiate polymerization at 50°C. After 10 minutes from the initiation of polymerization, 39.6 parts of 1,3-butadiene were continuously added over 60 minutes. Then, 3.5 parts of 1,3-butadiene were continuously added over 10 minutes and further stirred for 10 minutes. The highest temperature in the polymerization reaction was 75°C. After confirming that the polymerization conversion rate reached the range of 95% to 100%, 0.008 parts of tin tetrachloride were added and reacted for 20 minutes. Then, methanol in an amount equivalent to 2 times the mole of n-butyl lithium used was added as a polymerization terminator to obtain a polymer solution containing tin-coupled polybutadiene rubber (P5). Then, 0.25 parts of IRGANOX 1520L (manufactured by BASF) was added as an antioxidant to the polymer solution based on 100 parts of the polymer components contained in the polymer solution. Then, the solvent was removed by steam stripping and dried by warm air to obtain a solid tin-coupled polybutadiene rubber (P5).

[0249] [Production Example 6]

[0250] (Manufacture of terminal-modified polybutadiene rubber (P6))

[0251] In the production of the terminal-modified polybutadiene rubber (P1) of Production Example 1, 0.067 of tetramethylethylenediamine was added before initiating polymerization, and a solid terminal-modified polybutadiene rubber (P6) was obtained by the same method as in Production Example 1. The results of the measurement of the obtained terminal-modified polybutadiene rubber (P6) in the same manner as in Production Example 1 are shown in Table 1.

[0252] [Table 1]

[0253]

[0254] [Example 1]

[0255] In a Banbury mixer with a capacity of 250 ml, 50 parts of natural rubber, 20 parts of the terminal-modified polybutadiene rubber (P1) obtained in Production Example 1, and 30 parts of a terminal-modified styrene-butadiene copolymer (manufactured by Zeon Co., Ltd., trade name "Nipol NS612", styrene unit content 15 wt%) were masticated for 30 seconds. Next, 25 parts of silica (1) (manufactured by Solvay, trade name "Zeosil 1165MP", nitrogen adsorption specific surface area measured by BET method: 165 m 2 / g), 25 parts of carbon black (1) (manufactured by Tokai Carbon Co., Ltd., trade name "Seast 9H", nitrogen adsorption specific surface area measured by BET method: 142 m 2 / g) and 2.0 parts of a silane coupling agent: bis(3-(triethoxysilyl)propyl)tetrasulfide (manufactured by Evonik, trade name "Si69"), with a starting temperature of 110°C, after kneading for 1.5 minutes, 3 parts of zinc oxide, 2 parts of stearic acid and 2 parts of an antioxidant: N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine (manufactured by Ouchi Shinko Chemical Industry Co., Ltd., trade name "NOCRAC 6C") were added, and kneading was further performed for 2.5 minutes, and the kneaded material was discharged from the mixer. The temperature of the kneaded material at the end of kneading was 150°C. After the kneaded material was cooled to room temperature, it was kneaded again in a Banbury mixer at a starting temperature of 110°C for 3 minutes, and the kneaded material was discharged from the mixer. Next, 1.75 parts of sulfur and 1.0 parts of a crosslinking accelerator: N-(tert-butyl)-2-benzothiazole sulfonamide (manufactured by Sanshin Chemical Industry Co., Ltd., trade name "Sanceler NS-G") and 0.53 parts of a crosslinking accelerator: 1,3-diphenylguanidine (manufactured by Ouchi Shinko Chemical Industry Co., Ltd., trade name "NOCCELER D") were added to the obtained kneaded product using an open roll at 50°C and kneaded, and then the sheet-like rubber composition was taken out. The obtained rubber composition was press-crosslinked at 160°C for 7 minutes to prepare a test piece of the rubber crosslinked product, and the test piece was evaluated for low heat generation, wear resistance and stone impact resistance. The results are shown in Table 2.

[0256] [Example 2]

[0257] In Example 1, 25 parts of silica (2) (manufactured by Evonik, trade name "Ultrasil 9100GR", nitrogen adsorption specific surface area measured by BET method: 235 m 2 / g), and 25 parts of carbon black (2) (manufactured by Tokai Carbon Co., Ltd., trade name "Seast 7HM", nitrogen adsorption specific surface area measured by BET method: 126 m 2 A rubber composition was obtained in the same manner as in Example 1, and a test piece of a rubber cross-linked product was prepared and evaluated. The results are shown in Table 2.

[0258] [Examples 3 to 5]

[0259] Rubber compositions were obtained in the same manner as in Example 1, except that 20 parts of the terminal-modified polybutadiene rubber (P2) to (P4) obtained in Production Examples 2 to 4 were used in place of 20 parts of the terminal-modified polybutadiene rubber (P1) obtained in Production Example 1, and test pieces of rubber cross-linked products were prepared and evaluated. The results are shown in Table 2.

[0260] [Comparative Example 1]

[0261] A rubber composition was obtained in the same manner as in Example 1 except that 20 parts of the tin-coupled polybutadiene rubber (P5) obtained in Production Example 5 was used instead of 20 parts of the terminal-modified polybutadiene rubber (P1) obtained in Production Example 1, and a test piece of a cross-linked rubber was prepared and evaluated. The results are shown in Table 2.

[0262] [Comparative Example 2]

[0263] A rubber composition was obtained in the same manner as in Example 1 except that 20 parts of the terminal-modified polybutadiene rubber (P6) obtained in Production Example 6 was used instead of 20 parts of the terminal-modified polybutadiene rubber (P1) obtained in Production Example 1, and a test piece of a rubber cross-linked product was prepared and evaluated. The results are shown in Table 2.

[0264] [Table 2]

[0265]

[0266] As shown in Tables 1 and 2, the rubber cross-linked product obtained by using a rubber composition containing silica and a conjugated diene polymer having a glass transition temperature (Tg) of less than -60°C and having functional groups capable of interacting with silica has excellent low heat generation, wear resistance and stone impact resistance, and can be preferably used for heavy-load tire applications (Examples 1 to 5).

[0267] On the other hand, a cross-linked rubber obtained using a polybutadiene rubber having a glass transition temperature (Tg) of -60°C or less but having no functional group capable of interacting with silica had insufficient low heat build-up properties, wear resistance, and stone chip resistance (Comparative Example 1).

[0268] Furthermore, a cross-linked rubber obtained by using a polybutadiene rubber having a functional group capable of interacting with silica but having a glass transition temperature (Tg) higher than -60°C had insufficient abrasion resistance (Comparative Example 2).

Claims

1. A rubber composition for a heavy-load tire, comprising a conjugated diene polymer and silica, wherein the conjugated diene polymer has a glass transition temperature (Tg) of -60°C or lower and has a functional group capable of interacting with silica.

2. The rubber composition for a heavy load tire according to claim 1, wherein The conjugated diene monomer units constituting the conjugated diene polymer have a vinyl bond content of 5 to 40% by weight.

3. The rubber composition for a heavy load tire according to claim 1 or 2, wherein: The nitrogen adsorption specific surface area of ​​the silicon dioxide measured by the BET method is 30 to 500 m 2 / g.

4. The rubber composition for a heavy load tire according to any one of claims 1 to 3, wherein The content of the silica is 10 to 200 parts by weight relative to 100 parts by weight of the rubber component containing the conjugated diene polymer.

5. The rubber composition for a heavy load tire according to any one of claims 1 to 4, wherein The rubber composition for a heavy load tire further contains carbon black.

6. The rubber composition for a heavy load tire according to claim 5, wherein: The nitrogen adsorption specific surface area of ​​the carbon black measured by the BET method is 30 m 2 / g or above.

7. The rubber composition for a heavy load tire according to claim 5 or 6, wherein: The carbon black is contained in an amount of 10 to 200 parts by weight based on 100 parts by weight of the rubber component containing the conjugated diene polymer.

8. The rubber composition for a heavy load tire according to any one of claims 1 to 7, wherein The content of the conjugated diene polymer is 10 to 80% by weight in 100% by weight of the entire rubber component.

9. The rubber composition for a heavy load tire according to any one of claims 1 to 8, wherein The rubber composition for a heavy load tire further contains natural rubber, and the content of the natural rubber is 10 to 80% by weight based on 100% by weight of the total rubber components.

10. The rubber composition for a heavy load tire according to any one of claims 1 to 9, wherein The functional group in the conjugated diene polymer capable of interacting with the silicon dioxide is a Si-OR a The group of the structure represented by a It is a hydrogen atom or a hydrocarbon group which may have a substituent.

11. The rubber composition for a heavy load tire according to any one of claims 1 to 9, wherein The rubber composition for a heavy load tire further contains a silane coupling agent.

12. The rubber composition for a heavy load tire according to any one of claims 1 to 9, wherein The rubber composition for a heavy load tire further contains a cross-linking agent. 13 . A cross-linked rubber product obtained by cross-linking the rubber composition for a heavy load tire according to claim 1 .