Electrodepositable coating composition

By using polyols, film-forming polymers containing ionic salt groups and coating compositions, the problem of pit defects in coatings under oil pollution is solved, and a coating with high oil pollution resistance and smoothness is achieved. Reduced additional processing steps.

CN118900902APending Publication Date: 2024-11-05PPG INDUSTRIES OHIO INC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202380027477.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-21
Filing Date
2023-03-20
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

Existing electrodepositable coating techniques are prone to pit defects in oil-contaminated environments, affecting the smoothness and appearance of the coating, and require additional processing steps to achieve the desired finish.

Method used

The coating composition consisting of a polyol, a film-forming polymer containing ionic salt groups and a curing agent is applied and partially cured by electrophoresis to form an oil-contamination-resistant coating.

Benefits of technology

Improves the oil pollution resistance of the coating, reduces additional processing steps, and enhances the smoothness and appearance quality of the coating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005041920900000021
    Figure BDA0005041920900000021
  • Figure BDA0005041920900000022
    Figure BDA0005041920900000022
  • Figure BDA0005041920900000061
    Figure BDA0005041920900000061
Patent Text Reader

Abstract

The present disclosure relates to an electrodepositable coating composition comprising: (a) a polyol comprising a residue of ethylene oxide and a residue of butylene oxide; (b) a film-forming polymer containing ionic salt groups; and (c) a curing agent. A method of coating a substrate and a coated substrate are also disclosed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to an electrodepositable coating composition, a method of coating a substrate, and the treated substrate. Background Art

[0002] As a coating application method, electrodeposition involves depositing a film-forming composition onto a conductive substrate under the influence of an applied potential. Compared to non-electrophoretic coating methods, electrodeposition is increasingly popular in the coating industry because it provides higher coating utilization, excellent corrosion resistance, and low environmental pollution. Both cationic and anionic electrodeposition processes are used commercially. Oil contamination on the substrate surface is problematic for electrodepositable coating compositions. Oil deposits, such as the oil used in automobile assembly lines, cause defects in the form of pits to form in the cured coating. These pits are formed when the electrodepositable coating composition is dehumidified around the area where the oil is deposited, and the coating may solidify around the oil deposits. The formation of pits affects both the smoothness and appearance of the cured coating, and requires additional processing steps such as polishing to achieve the desired coating finish. It is desirable to provide an electrodepositable coating composition that is resistant to oil contamination. Summary of the invention

[0003] The present disclosure provides an electrodepositable coating composition comprising: (a) a polyol comprising residues of ethylene oxide and butylene oxide; (b) a film-forming polymer containing ionic salt groups; and (c) a curing agent.

[0004] The present disclosure also provides a method of coating a substrate, the method comprising electrophoretically applying one of the electrodepositable coating compositions described herein to at least a portion of the substrate, and at least partially curing the coating composition to form a coating.

[0005] The present disclosure also provides a substrate coated with one of the electrodepositable coating compositions disclosed herein in an at least partially cured state.

[0006] The present disclosure also provides a substrate, the substrate comprising a coating, the coating comprising (a) a polyol, the polyol comprising residues of ethylene oxide and butylene oxide; (b) a film-forming polymer containing an ionic group; and (c) a curing agent. DETAILED DESCRIPTION

[0007] The present disclosure relates to an electrodepositable coating composition comprising: (a) a polyol comprising residues of ethylene oxide and butylene oxide; (b) a film-forming polymer containing ionic salt groups; and (c) a curing agent.

[0008] According to the present disclosure, the term "electrodepositable coating composition" refers to a composition that is capable of being deposited onto a conductive substrate under the influence of an applied electric potential.

[0009] Polyols

[0010] The electrodepositable coating composition of the present disclosure may include a polyol including a residue of ethylene oxide and a residue of butylene oxide. As used herein, the term "polyol" means a compound including one or more hydroxyl groups. The polyol of the present disclosure at least partially includes the following: a constituent unit including a residue of ethylene oxide and a constituent unit including a residue of butylene oxide. As used herein, the term "ethylene oxide" refers to an organic compound having the formula C2H4O and the following structure:

[0011]

[0012] As used herein, the term "butylene oxide" refers to an organic compound having the formula C4H8O and the following structure:

[0013]

[0014] As used herein, the term "constituent unit comprising a monomer residue" means a portion of the polyol structure attributable to the residue of a single monomer after the monomer reacts during polymerization to form a portion of a polymer or a structural unit of a polymer.

[0015] The polyol may comprise, consist essentially of, or consist of constituent units comprising residues of ethylene oxide and constituent units comprising residues of butylene oxide. The polyol may comprise constituent units comprising residues of ethylene oxide in a ratio of at least 9:1, such as at least 4:1, such as at least 1:1, such as at least 2:1. The polyol may comprise constituent units comprising residues of ethylene oxide in a ratio of no more than 1:9, such as no more than 1:7, such as no more than 1:5, such as no more than 1:4. The polyol may include constituent units including residues of ethylene oxide to constituent units including residues of butylene oxide in a ratio of 9:1 to 1:9, such as 4:1 to 1:9, such as 2:1 to 1:9, such as 1:1 to 1:9, such as 9:1 to 1:7, such as 4:1 to 1:7, such as 2:1 to 1:7, such as 1:1 to 1:7, such as 9:1 to 1:5, such as 4:1 to 1:5, such as 2:1 to 1:5, such as 1:1 to 1:5, such as 9:1 to 1:4, such as 4:1 to 1:4, such as 2:1 to 1:4, such as 1:1 to 1:4.

[0016] The polyol may be polymerized from a mixture of monomers comprising, substantially consisting of, or consisting of ethylene oxide and butylene oxide. The mixture of monomers may include a molar ratio of ethylene oxide to butylene oxide of at least 9:1, such as at least 4:1, such as at least 1:1, such as at least 2:1. The mixture of monomers may include a molar ratio of ethylene oxide to butylene oxide of no more than 1:9, such as no more than 1:7, such as no more than 1:5, such as no more than 1:4. The mixture of monomers may include a molar ratio of ethylene oxide to butylene oxide of 9:1 to 1:9, such as 4:1 to 1:9, such as 2:1 to 1:9, such as 1:1 to 1:9, such as 9:1 to 1:7, such as 4:1 to 1:7, such as 2:1 to 1:7, such as 1:1 to 1:7, such as 9:1 to 1:5, such as 4:1 to 1:5, such as 2:1 to 1:5, such as 1:1 to 1:5, such as 9:1 to 1:4, such as 4:1 to 1:4, such as 2:1 to 1:4, such as 1:1 to 1:4.

[0017] Polyols can include at least two hydroxyl groups, and can be difunctional, trifunctional, tetrafunctional or have higher functionality. As used herein, "hydroxyl functional group" refers to -OH groups. As used herein, when used relative to the number of hydroxyl functional groups, "difunctional" means that each molecule of a specific monomer or polymer includes two (2) hydroxyl functional groups, is generally composed of two hydroxyl functional groups, or is composed of two hydroxyl functional groups. As used herein, when used relative to the number of hydroxyl functional groups, "trifunctional" means that each molecule of a monomer or polymer includes three (3) hydroxyl functional groups, is generally composed of three hydroxyl functional groups, or is composed of three hydroxyl functional groups. As used herein, when used relative to the number of hydroxyl functional groups, "tetrafunctional" means that each molecule of a monomer or polymer includes four (4) hydroxyl functional groups, is generally composed of four hydroxyl functional groups, or is composed of four hydroxyl functional groups. For clarity, polyols can include additional functional groups in addition to hydroxyl functional groups.

[0018] The theoretical hydroxyl equivalent weight of the polyol may be at least 500 g / hydroxyl group ("OH"), such as at least 600 g / OH, such as at least 700 g / OH, such as at least 750 g / OH. The theoretical hydroxyl equivalent weight of the polyol may be no more than 2,000 g / OH, such as no more than 1,750 g / OH, such as no more than 1,500 g / OH, such as no more than 1,250 g / OH. The theoretical hydroxyl equivalent weight of the polyol may be from 500 g / OH to 2,000 g / OH, such as from 500 g / OH to 1,750 g / OH, such as from 500 g / OH to 1,500 g / OH, such as from 500 g / OH to 1,250 g / OH, such as from 600 g / OH to 2,000 g / OH, such as from 600 g / OH to 1,750 g / OH, such as from 600 g / OH to 1,500 g / OH, such as from 600 g / OH to 1,25 0g / OH, such as 700g / OH to 2,000g / OH, such as 700g / OH to 1,750g / OH, such as 700g / OH to 1,500g / OH, such as 700g / OH to 1,250g / OH, such as 750g / OH to 2,000g / OH, such as 750g / OH to 1,750g / OH, such as 750g / OH to 1,500g / OH, such as 750g / OH to 1,250g / OH.

[0019] The hydroxyl value of the polyol can be at least 35 mg KOH / gram of polyol, such as at least 40 mg KOH / gram of polyol, such as at least 45 mg KOH / gram of polyol, such as at least 50 mg KOH / gram of polyol. The hydroxyl value of the polyol can be no more than 115 mg KOH / gram of polyol, such as no more than 100 mg KOH / gram of polyol, such as no more than 75 mg KOH / gram of polyol, such as no more than 60 mg KOH / gram of polyol. The hydroxyl value of the polyol can be 35 to 115 mg KOH / gram of polyol, such as 35 to 100 mg KOH / gram of polyol, such as 35 to 75 mg KOH / gram of polyol, such as 35 to 60 mg KOH / gram of polyol, such as 40 to 115 mg KOH / gram of polyol, such as 40 to 100 mg KOH / gram of polyol, such as 40 to 75 mg KOH / gram of polyol, such as 40 to 60 mg KOH / gram of polyol, such as 45 to 115 mg KOH / gram of polyol, such as 45 to 100 mg KOH / gram of polyol, such as 45 to 75 mg KOH / gram of polyol, such as 45 to 60 mg KOH / gram of polyol, such as 50 to 115 mg KOH / gram of polyol, such as 50 to 100 mg KOH / gram of polyol, such as 50 to 75 mg KOH / gram of polyol, such as 50 to 60 mg KOH / gram of polyol. As used herein, the term "hydroxyl value" generally refers to the number of milligrams of potassium hydroxide (KOH) required to neutralize acetic acid absorbed by one gram of a chemical containing free hydroxyl groups during acetylation, and is determined herein by theoretically calculating the number of free hydroxyl groups theoretically present in one gram of polyol.

[0020] The theoretical molecular weight of polyol can be at least 1,000g, such as at least 1,250g, such as at least 1,500g. The theoretical molecular weight of polyol can be no more than 3,000g, such as no more than 2,750g, such as no more than 2,500g. The theoretical molecular weight of polyol can be from 1,000g to 3,000g, such as from 1,000g to 2,750g, such as from 1,000g to 2,500g, such as from 1,250g to 3,000g, such as from 1,250g to 2,750g, such as from 1,250g to 2,500g, such as from 1,500g to 3,000g, such as from 1,500g to 2,750g, such as from 1,500g to 2,500g. As used herein, the term "theoretical molecular weight" means the molecular weight calculated using the following equation:

[0021] (1)

[0022] 56,100 mg is the molecular weight of KOH. "Hydroxyl Number" is the hydroxyl number as described above. "Total # Equivalent OH Groups" is the total number of equivalent hydroxyl groups present on one polyol molecule.

[0023] Based on the weight of resin solids, the above polyols can be present in the electrodepositable coating composition in an amount of at least 0.5 wt %, such as at least 0.6 wt %, such as at least 0.8 wt %, such as at least 1 wt %, such as at least 5 wt %. Based on the weight of resin solids, the above polyols can be present in the electrodepositable coating composition in an amount of no more than 15 wt %, such as no more than 12 wt %, such as no more than 10 wt %, such as no more than 8 wt %. The above polyols can be present in the electrodepositable coating composition in an amount of 0.5 wt % to 15 wt %, such as 0.5 wt % to 12 wt %, such as 0.5 wt % to 10 wt %, such as 0.5 wt % to 8 wt %, such as 0.6 wt % to 15 wt %, such as 0.6 wt % to 12 wt %, such as 0.6 wt % to 10 wt %, such as 0.6 wt % to 8 wt %, such as 0.8 wt % to 15 wt %, such as 0.8 wt % to 12 wt %, such as 0.8 wt % to 10 wt %, such as 0.8 wt % to 8 wt %, such as 1 wt % to 15 wt %, such as 1 wt % to 12 wt %, such as 1 wt % to 10 wt %, such as 1 wt % to 8 wt %, such as 5 wt % to 15 wt %, such as 5 wt % to 12 wt %, such as 5 wt % to 10 wt %, such as 5 wt % to 8 wt %.

[0024] Film-forming polymers containing ionic salt groups

[0025] According to the present disclosure, the electrodepositable coating composition may further include a film-forming polymer containing an ionic salt group. The film-forming polymer containing an ionic salt group may be different from the above-mentioned polyol.

[0026] According to the present disclosure, the film-forming polymer containing ionic salt groups may include the film-forming polymer containing cationic salt groups. The film-forming polymer containing cationic salt groups can be used in the coating composition of cationic electrodeposition. As used herein, the term "film-forming polymer containing cationic salt groups" refers to the polymer containing the cationic groups at least partially neutralized such as the sulfonium groups and ammonium groups that impart positive charge. As used herein, the term "polymer" covers but is not limited to oligomers and homopolymers and copolymers. The film-forming polymer containing cationic salt groups may include active hydrogen functional groups. As used herein, the term "active hydrogen functional group" refers to those groups determined by the Zerewitinoff test (Zerewitinofftest) described in "Journal of the American Chemical Society", Vol. 49, p. 3181 (1927) with reactivity to isocyanate, and includes, for example, hydroxyl, primary amine or secondary amine and thiol groups. The cationic salt group-containing film-forming polymer including an active hydrogen functional group may be referred to as an active hydrogen-containing, cationic salt group-containing film-forming polymer.

[0027] Examples of polymers suitable for use as the cationic salt group-containing film-forming polymer in the present disclosure include, but are not limited to, alkyd polymers, acrylics, polyepoxides, polyamides, polyurethanes, polyureas, polyethers, polyesters, and the like.

[0028] More specific examples of suitable active hydrogen-containing, cationic salt group-containing film-forming polymers include polyepoxide-amine adducts such as polyglycidyl ethers of polyphenols (e.g., bisphenol A) and primary and / or secondary amines, such as described in U.S. Pat. No. 4,031,050 at column 3, line 27 to column 5, line 50, U.S. Pat. No. 4,452,963 at column 5, line 58 to column 6, line 66, and U.S. Pat. No. 6,017,432 at column 2, line 66 to column 6, line 26, portions of which are incorporated herein by reference. A portion of the amine reacted with the polyepoxide may be a ketimine of a polyamine, such as described in U.S. Pat. No. 4,104,147 at column 6, line 23 to column 7, line 23, the cited portions of which are incorporated herein by reference. Ungelled polyepoxide-polyoxyalkylene polyamine resins are also suitable, such as those described in U.S. Pat. No. 4,432,850 at column 2, line 60 to column 5, line 58, the cited portion of which is incorporated herein by reference. In addition, cationic acrylic resins such as those described in U.S. Pat. No. 3,455,806 at column 2, line 18 to column 3, line 61 and U.S. Pat. No. 3,928,157 at column 2, line 29 to column 3, line 21, portions of which are incorporated herein by reference, may be used.

[0029] In addition to the resin containing amine salt groups, the resin containing quaternary ammonium salt groups can also be used as the film-forming polymer containing cationic salt groups in the present disclosure. Examples of these resins are those resins formed by the reaction of organic polyepoxides with tertiary amine acid salts. Such resins are described in U.S. Patent No. 3,962,165, Column 2, Line 3 to Column 11, Line 7, U.S. Patent No. 3,975,346, Column 1, Line 62 to Column 17, Line 25, and U.S. Patent No. 4,001,156, Column 1, Line 37 to Column 16, Line 7, and these parts of the U.S. Patent No. are incorporated herein by reference. Examples of other suitable cationic resins include resins containing ternary sulfonium salt groups, such as those containing ternary sulfonium salt groups described in U.S. Patent No. 3,793,278, Column 1, Line 32 to Column 2, Line 20, and this part of the U.S. Patent No. is incorporated herein by reference. Furthermore, it is also possible to employ cationic resins which cure by a transesterification mechanism, as described in European Patent Application No. 12463 B1, page 2, line 1 to page 6, line 25, this part of which is incorporated herein by reference.

[0030] Other suitable film-forming polymers containing cationic salt groups include those film-forming polymers that can form an electrodepositable coating composition that resists photodegradation. Such polymers include polymers including cationic amine salt groups, which are derived from pendant amino groups and / or terminal amino groups disclosed in paragraphs

[0064] to

[0088] of U.S. Patent Application Publication No. 2003 / 0054193A1, which is incorporated herein by reference in this section. Also suitable are active hydrogen-containing, cationic salt group-containing resins derived from polyglycidyl ethers of polyphenols that are substantially free of aliphatic carbon atoms bonded to more than one aromatic group, which are described in paragraphs

[0096] to

[0123] of U.S. Patent Application Publication No. 2003 / 0054193A1, which are incorporated herein by reference in this section.

[0031] The active hydrogen-containing, cationic salt-containing film-forming polymer is made cationic and water-dispersible by at least partially neutralizing with an acid. Suitable acids include organic acids and inorganic acids. Non-limiting examples of suitable organic acids include formic acid, acetic acid, methanesulfonic acid, and lactic acid. Non-limiting examples of suitable inorganic acids include phosphoric acid and aminosulfonic acid. "Aminosulfonic acid" means aminosulfonic acid itself or a derivative thereof, such as those aminosulfonic acids or derivatives thereof having the following formula:

[0032]

[0033] wherein R is hydrogen or an alkyl group having 1 to 4 carbon atoms. Mixtures of the above mentioned acids may also be used in the present disclosure.

[0034] The degree of neutralization of the film-forming polymer containing cationic salt groups can vary with the specific polymer involved. However, sufficient acid should be used to fully neutralize the film-forming polymer containing cationic salt groups so that the film-forming polymer containing cationic salt groups can be dispersed in the aqueous dispersion medium. For example, the amount of acid used can provide at least 20% of the total theoretical neutralization. It is also possible to use an excess of acid that exceeds the amount required for 100% total theoretical neutralization. For example, based on the total amine in the film-forming polymer containing active hydrogen and cationic salt groups, the amount of acid used to neutralize the film-forming polymer containing cationic salt groups can be ≤100%. The total amount of acid used to neutralize the film-forming polymer containing cationic salt groups can range between any combination of the values ​​stated in the preceding sentences (including the stated values). For example, based on the total amine in the film-forming polymer containing cationic salt groups, the total amount of acid used to neutralize the film-forming polymer containing active hydrogen and cationic salt groups can be 20%, 35%, 50%, 60% or 80%.

[0035] According to the present disclosure, based on the total weight of the resin solids of the electrodepositable coating composition, the film-forming polymer containing cationic salt groups can be present in the cationic electrodepositable coating composition in the following amount: at least 40% by weight, such as at least 50% by weight, such as at least 60% by weight. Based on the total weight of the resin solids of the electrodepositable coating composition, the film-forming polymer containing cationic salt groups can be present in the cationic electrodepositable coating composition in the following amount: not more than 90% by weight, such as not more than 80% by weight, such as not more than 75% by weight. Based on the total weight of the resin solids of the electrodepositable coating composition, the film-forming polymer containing cationic salt groups can be present in the cationic electrodepositable coating composition in the following amount: 40% to 90% by weight, such as 40% to 80% by weight, such as 40% to 75% by weight, such as 50% to 90% by weight, such as 50% to 80% by weight, such as 50% to 75% by weight, such as 60% to 90% by weight, such as 60% to 80% by weight, such as 60% to 75% by weight.

[0036] As used herein, the term "resin solids" includes the ionic salt group-containing film-forming polymer, curing agent, polyol, and any additional water-dispersible, unpigmented components present in the electrodepositable coating composition.

[0037] According to the present disclosure, the film-forming polymer containing ionic salt groups can include the film-forming polymer containing anionic salt groups. As used herein, the term "film-forming polymer containing anionic salt groups" refers to anionic polymers including at least partially neutralized anionic functional groups (such as carboxylic acid groups and phosphoric acid groups that impart negative charge). The film-forming polymer containing anionic salt groups can include active hydrogen functional groups. The film-forming polymer containing anionic salt groups including active hydrogen functional groups can be referred to as a film-forming polymer containing active hydrogen and anionic salt groups. The film-forming polymer containing anionic salt groups can be used in anion electrodepositable coating compositions.

[0038] Film-forming polymers containing anionic salt groups may include alkali-soluble, carboxylic acid group-containing film-forming polymers, such as reaction products or adducts of drying oils or semi-drying fatty acid esters with dicarboxylic acids or anhydrides; and reaction products of fatty acid esters, unsaturated acids or anhydrides with any additional unsaturated modifying materials further reacted with polyols. Also suitable are at least partially neutralized interpolymers of hydroxy-alkyl esters of unsaturated carboxylic acids, unsaturated carboxylic acids and at least one other ethylenically unsaturated monomer. Still another suitable anionic electrodepositable resin includes an alkyd resin-aminoplast vehicle, i.e., a vehicle containing an alkyd resin and an amine-aldehyde resin. Another suitable anionic electrodepositable resin composition includes mixed esters of resin polyols. Other acid-functional polymers may also be used, such as phosphated polyepoxides or phosphated acrylic polymers. Exemplary phosphatized polyepoxides are disclosed in U.S. Patent Application Publication No. 2009 / 0045071, paragraphs

[0004] to

[0015] and U.S. Patent Application Serial No. 13 / 232,093, paragraphs

[0014] to

[0040] , the cited portions of which are incorporated herein by reference. Also suitable are resins comprising one or more pendant carbamate functional groups, such as those described in U.S. Patent No. 6,165,338.

[0039] According to the present disclosure, based on the total weight of the resin solids of the electrodepositable coating composition, the film-forming polymer containing anionic salt groups can be present in the anionic electrodepositable coating composition in the following amount: at least 50% by weight, such as at least 55% by weight, such as at least 60% by weight. Based on the total weight of the resin solids of the electrodepositable coating composition, the film-forming polymer containing anionic salt groups can be present in the anionic electrodepositable coating composition in the following amount: not more than 90% by weight, such as not more than 80% by weight, such as not more than 75% by weight. Based on the total weight of the resin solids of the electrodepositable coating composition, the film-forming polymer containing anionic salt groups can be present in the anionic electrodepositable coating composition in the following amount: 50% by weight to 90% by weight, such as 50% by weight to 80% by weight, such as 50% by weight to 75% by weight, such as 55% by weight to 90% by weight, such as 55% by weight to 80% by weight, such as 55% by weight to 75% by weight, such as 60% by weight to 90% by weight, such as 60% by weight to 80% by weight, such as 60% by weight to 75% by weight.

[0040] According to the present disclosure, based on the total weight of the resin solids of the electrodepositable coating composition, the film-forming polymer containing ionic salt groups can be present in the electrodepositable coating composition in an amount of at least 39.5 wt %, such as at least 50 wt %, such as at least 55 wt %, such as at least 60 wt %. Based on the total weight of the resin solids of the electrodepositable coating composition, the film-forming polymer containing ionic salt groups can be present in the electrodepositable coating composition in an amount of no more than 90 wt %, such as no more than 80 wt %, such as no more than 75 wt %. The film-forming polymer containing ionic salt groups can be present in the electrodepositable coating composition in an amount of 39.5 to 90 wt %, such as 39.5 to 80 wt %, such as 39.5 to 75 wt %, such as 50 to 90 wt %, such as 50 to 80 wt %, such as 50 to 75 wt %, such as 55 to 90 wt %, such as 55 to 80 wt %, such as 55 to 75 wt %, such as 60 to 90 wt %, such as 60 to 80 wt %, such as 60 to 75 wt %, based on the total weight of the resin solids of the electrodepositable coating composition.

[0041] Curing agent

[0042] According to the present disclosure, the coating composition of the present disclosure that can be deposited can further include a curing agent. The curing agent can be reactive with polyols and film-forming polymers containing ionic salt groups. The curing agent can react with the reactive groups (such as active hydrogen groups) of the film-forming polymers containing ionic salt groups and the reactive groups of polyols to realize the curing of the coating composition to form a coating. As used herein, as used in conjunction with the coating composition that can be deposited as described herein, the term "curing", "cured" or similar terms means that at least a portion of the components of the coating composition that can be deposited are crosslinked to form a coating. Additionally, the curing of the coating composition that can be deposited refers to subjecting the composition to curing conditions (e.g., elevated temperature), thereby causing the reactive functional groups of the components of the coating composition that can be deposited to react, and causing the components of the composition to crosslink and form a coating that is at least partially cured. Non-limiting examples of suitable curing agents are at least partially blocked polyisocyanates, amino plastic resins and phenolic plastic resins, such as phenol formaldehyde condensates, including their allyl ether derivatives.

[0043] Suitable at least partially blocked polyisocyanates include aliphatic polyisocyanates, aromatic polyisocyanates and mixtures thereof. The curing agent may include at least partially blocked aliphatic polyisocyanates. Suitable at least partially blocked aliphatic polyisocyanates include, for example, fully blocked aliphatic polyisocyanates, such as those described in U.S. Pat. No. 3,984,299, column 1, line 57 to column 3, line 15, portions of which are incorporated herein by reference; or partially blocked aliphatic polyisocyanates reacted with a film-forming polymer backbone containing an ionic salt group, such as described in U.S. Pat. No. 3,947,338, column 2, line 65 to column 4, line 30, portions of which are also incorporated herein by reference. "Blocked" means that the isocyanate group has reacted with a compound so that the resulting blocked isocyanate group is stable to active hydrogen at ambient temperature, but is reactive with active hydrogen in the film-forming polymer at elevated temperatures (such as between 90° C. and 200° C.). The polyisocyanate curing agent may be a fully blocked polyisocyanate containing substantially no isocyanate groups.

[0044] The polyisocyanate curing agent may include a diisocyanate, a higher functional polyisocyanate, or a combination thereof. For example, the polyisocyanate curing agent may include an aliphatic polyisocyanate and / or an aromatic polyisocyanate. The aliphatic polyisocyanate may comprise (i) alkylene isocyanates such as trimethylene diisocyanate, tetramethylene diisocyanate, pentamethylene diisocyanate, hexamethylene diisocyanate ("HDI"), 1,2-propylene diisocyanate, 1,2-butylene diisocyanate, 2,3-butylene diisocyanate, 1,3-butylene diisocyanate, ethylene diisocyanate and butylene diisocyanate, and (ii) cycloalkylene isocyanates such as 1,3-cyclopentane diisocyanate, 1,4-cyclohexane diisocyanate, 1,2-cyclohexane diisocyanate, isophorone diisocyanate, methylene bis(4-cyclohexyl isocyanate) ("HMDI"), the cyclotrimer of 1,6-hexamethylene diisocyanate (also known as the isocyanurate trimer of HDI, available as Desmodur N3300 from Covestro AG) commercially available) and m-tetramethylxylylene diisocyanate (available as Commercially available from Allnex SA). The aromatic polyisocyanate may comprise (i) an arylene isocyanate such as m-phenylene diisocyanate, p-phenylene diisocyanate, 1,5-naphthalene diisocyanate, and 1,4-naphthalene diisocyanate, and (ii) an aralkylene isocyanate such as 4,4′-diphenylmethane (“MDI”), 2,4-tolylene diisocyanate, or 2,6-tolylene diisocyanate (“TDI”), or mixtures thereof, 4,4-toluidine diisocyanate, and xylylene diisocyanate. Triisocyanates such as triphenylmethane-4,4',4"-triisocyanate, 1,3,5-triisocyanatobenzene and 2,4,6-triisocyanatotoluene; tetraisocyanates such as 4,4'-diphenyldimethylmethane-2,2',5,5'-tetraisocyanate; and polymeric polyisocyanates such as tolylene diisocyanate dimer and trimer, etc. can also be used. The curing agent may include a blocked polyisocyanate selected from polymeric polyisocyanates (such as polymeric HDI, polymeric MDI, polymeric isophorone diisocyanate, etc.). The curing agent may also include a blocked trimer of hexamethylene diisocyanate, which can be used as Desmodur Available from Covestro AG. Mixtures of polyisocyanate curing agents may also be used.

[0045] The polyisocyanate curing agent may be at least partially blocked by the above-mentioned polyols. Alternatively or in addition to the polyols, the polyisocyanate curing agent may be at least partially blocked by at least one blocking agent selected from the following: 1,2-alkane diols, such as 1,2-propylene glycol; 1,3-alkane diols, such as 1,3-butanediol; benzyl alcohols, such as benzyl alcohol; allyl alcohols, such as allyl alcohol; caprolactam; dialkylamines, such as dibutylamine; and mixtures thereof. The polyisocyanate curing agent may be at least partially blocked by at least one 1,2-alkane diol having three or more carbon atoms (e.g., 1,2-butanediol).

[0046] Other suitable blocking agents include aliphatic, alicyclic or aromatic alkyl monoalcohols or phenolic compounds, including, for example, lower aliphatic alcohols, such as methanol, ethanol and n-butanol; alicyclic alcohols, such as cyclohexanol; aromatic alkyl alcohols, such as benzyl alcohol and methyl phenyl carbinol; and phenolic compounds, such as phenol itself and substituted phenols, such as cresol and nitrophenol, wherein the substituents do not affect the coating operation. Glycol ethers and diol amines can also be used as blocking agents. Suitable glycol ethers include ethylene glycol butyl ether, diethylene glycol butyl ether, ethylene glycol methyl ether and propylene glycol methyl ether. Other suitable blocking agents include oximes, such as methyl ethyl ketone oxime, acetone oxime and cyclohexanone oxime.

[0047] Curing agents may include aminoplast resins. Aminoplast resins are condensation products of aldehydes with substances carrying amino or amide groups. Condensation products obtained by reacting alcohols and aldehydes with melamine, urea or benzoguanamine may be used. However, condensation products of other amines and amides may also be used, for example, aldehyde condensates of alkyl and aryl substituted derivatives of triazines, diazines, triazoles, guanidines, guanamines and such compounds as alkyl-substituted and aryl-substituted ureas and alkyl-substituted and aryl-substituted melamines. Some examples of such compounds are N,N'-dimethylurea, phenylurea, dicyandiamide, formaguanamine, acetoguanamine, ammeline, 2-chloro-4,6-diamino-1,3,5-triazine, 6-methyl-2,4-diamino-1,3,5-triazine, 3,5-diaminotriazole, triaminopyrimidine, 2-mercapto-4,6-diaminopyrimidine, 3,4,6-tris(ethylamino)-1,3,5-triazine, etc. Suitable aldehydes include formaldehyde, acetaldehyde, crotonaldehyde, acrolein, benzaldehyde, furfural, glyoxal, etc.

[0048] The aminoplast resin may contain methylol groups or similar alkyl alcohol groups, and at least a portion of these alkyl alcohol groups may be etherified by reaction with an alcohol to provide a resin soluble in an organic solvent. For this purpose, any monohydric alcohol may be employed, including such alcohols as methanol, ethanol, propanol, butanol, pentanol, hexanol, heptanol, and others, as well as benzyl alcohol and other aromatic alcohols, cyclic alcohols such as cyclohexanol, monoethers of ethylene glycol such as Cello solve and Carbitol, and halogen-substituted or other substituted alcohols such as 3-chloropropanol and butoxyethanol.

[0049] A non-limiting example of a commercially available aminoplast resin is the aminoplast resin sold under the trademark ANTI-TREAT® from Allnex Belgium SA / NV. (such as CYMEL 1130 and 1156) and products from INEOS Melamines under the trademark Examples of suitable aminoplast resins also include those described in U.S. Pat. No. 3,937,679 at column 16, line 3 to column 17, line 47, portions of which are hereby incorporated by reference. As disclosed in the aforementioned portion of the '679 patent, aminoplasts may be used in combination with hydroxymethylphenol ethers.

[0050] Phenolic plastic resin is formed by the condensation of aldehyde and phenol. Suitable aldehydes include formaldehyde and acetaldehyde. Methylene releasers and aldehyde releasers (such as paraformaldehyde and hexamethylenetetramine) can also be used as aldehyde agents. Various phenols can be used, such as phenol itself, cresols or substituted phenols, in which hydrocarbon groups with straight, branched or cyclic structures replace hydrogen in the aromatic ring. Mixtures of phenols can also be used. Some specific examples of suitable phenols are p-phenylphenol, p-tert-butylphenol, p-tert-amylphenol, cyclopentylphenol and phenols substituted with unsaturated hydrocarbons, such as monobutenylphenol containing butenyl groups in the ortho, meta or para positions, and wherein double bonds appear in various positions of the hydrocarbon chain.

[0051] As described above, aminoplast resins and phenoplast resins are described in US Pat. No. 4,812,215 at column 6, line 20 to column 7, line 12, the cited portion of which is incorporated herein by reference.

[0052] The curing agent may be present in the cationic electrodepositable coating composition in an amount of at least 10 wt %, such as at least 20 wt %, such as at least 25 wt %, based on the total weight of the resin solids of the electrodepositable coating composition. The curing agent may be present in the cationic electrodepositable coating composition in an amount of no more than 60 wt %, such as no more than 50 wt %, such as no more than 40 wt %, based on the total weight of the resin solids of the electrodepositable coating composition. The curing agent may be present in the cationic electrodepositable coating composition in an amount of 10 wt % to 60 wt %, such as 10 wt % to 50 wt %, such as 10 wt % to 40 wt %, such as 20 wt % to 60 wt %, such as 20 wt % to 50 wt %, such as 20 wt % to 40 wt %, such as 25 wt % to 60 wt %, such as 25 wt % to 50 wt %, such as 25 wt % to 40 wt %.

[0053] The curing agent may be present in the anionic electrodepositable coating composition in an amount of at least 10 wt %, such as at least 20 wt %, such as at least 25 wt %, based on the total weight of the resin solids of the electrodepositable coating composition. The curing agent may be present in the anionic electrodepositable coating composition in an amount of no more than 50 wt %, such as no more than 45 wt %, such as no more than 40 wt %, based on the total weight of the resin solids of the electrodepositable coating composition. The curing agent may be present in the anionic electrodepositable coating composition in an amount of 10 wt % to 50 wt %, such as 10 wt % to 45 wt %, such as 10 wt % to 40 wt %, such as 20 wt % to 50 wt %, such as 20 wt % to 45 wt %, such as 20 wt % to 40 wt %, such as 25 wt % to 50 wt %, such as 25 wt % to 45 wt %, such as 25 wt % to 40 wt %.

[0054] The curing agent may be present in the electrodepositable coating composition in an amount of at least 10% by weight, such as at least 20% by weight, such as at least 25% by weight, based on the total weight of the resin solids of the electrodepositable coating composition. The curing agent may be present in the electrodepositable coating composition in an amount of no more than 60% by weight, such as no more than 50% by weight, such as no more than 45% by weight, such as no more than 40% by weight, based on the total weight of the resin solids of the electrodepositable coating composition. The curing agent may be present in the electrodepositable coating composition in an amount of 10% to 60% by weight, such as 10% to 50% by weight, such as 10% to 45% by weight, such as 10% to 40% by weight, such as 20% to 60% by weight, such as 20% to 50% by weight, such as 20% to 45% by weight, such as 20% to 40% by weight, such as 25% to 60% by weight, such as 25% to 50% by weight, such as 25% to 45% by weight, such as 25% to 40% by weight.

[0055] Additional components of the electrodepositable coating composition

[0056] In addition to the polyol, the film-forming polymer containing ionic salt groups, and the curing agent described above, the electrodepositable coating composition according to the present disclosure may optionally include one or more additional components.

[0057] The electrodepositable coating composition may further include a polyetheramine adduct comprising an ungelled ionic reaction product prepared from reactants, the ungelled ionic reaction product comprising: (a) a reaction product prepared from reactants comprising: (1) a polyol different from the polyols discussed above; and (2) an epoxy-functional material; and (b) a polyetheramine.

[0058] Examples of suitable polyols that can be used to form the ungelled ionic reaction product include resorcinol, dihydroxybenzenes, aliphatic, cycloaliphatic or araliphatic hydroxyl-containing compounds such as ethylene glycol, propylene glycol, bisphenol A, dihydroxycyclohexane, dimethylolcyclohexane or combinations thereof. The polyol can be present in the polyetheramine adduct in an amount, for example, of 0 to 20 weight percent, such as 0 to 15 weight percent, based on the total weight of the reactants forming the polyester reaction product.

[0059] Examples of suitable epoxy-functional materials that can be used to form the ungelled ionic reaction product contain at least one epoxy group in the molecule, such as di- or polyglycidyl ethers of polyols, such as polyglycidyl ethers of bisphenol A. Suitable epoxy-functional materials can have epoxy equivalent weights ranging, for example, from 90 to 2,000 g / equivalent of epoxide functional groups, as measured by titration with perchloric acid using methyl violet as an indicator. The epoxy-functional material can include, for example, 10 wt % to 40 wt %, such as 15 wt % to 35 wt % of the epoxy-functional material, based on the total weight of the epoxy-functional polyester, if combined or reacted with the polyethers described above to form the epoxy-functional polyester.

[0060] According to the present disclosure, polyetheramine adducts can be formed by reacting the ungelled ionic reaction product with at least one polyetheramine, such as one characterized by propylene oxide, ethylene oxide, or mixed propylene oxide and ethylene oxide repeating units in their respective structures, such as, for example, one of the Jeffamine series of products (commercially available from Huntsman Corporation). Examples of such polyetheramines include aminated propoxylated pentaerythritol (such as Jeffamine XTJ-616) and those compounds represented by Formula (I) to Formula (III).

[0061] According to formula (I) of the present disclosure, the polyetheramine may include or represent:

[0062]

[0063] Wherein y=0-39, x+z=1-68.

[0064] Suitable polyetheramines represented by formula (I) include, but are not limited to, amine-terminated polyethylene glycols, such as Jeffamine ED series from Huntsman, such as Jeffamine HK-511, Jeffamine ED-600, Jeffamine ED-900, and Jeffamine ED-2003; and amine-terminated polypropylene glycols, such as Jeffamine D series from Huntsman, such as Jeffamine D-230, Jeffamine D-400, Jeffamine D-2000, and Jeffamine D-4000.

[0065] According to formula (II) of the present disclosure, the polyetheramine may include or represent:

[0066]

[0067] wherein each p is independently 2 or 3.

[0068] Suitable polyetheramines represented by formula (II) include, but are not limited to, amine-terminated polyethylene glycol-based diamines, such as the Jeffamine EDR series from Huntsman Corporation, such as Jeffamine EDR-148 and Jeffamine EDR-176.

[0069] According to formula (III) of the present disclosure, the polyetheramine may include or represent:

[0070]

[0071] Wherein R is H or C2H5, m=0 or 1, and a+b+c=5-85.

[0072] Suitable polyetheramines represented by formula (III) include, but are not limited to, amine-terminated propoxylated trimethylolpropane or glycerol, such as Huntsman's Jeffamine T series, such as Jeffamine T-403, Jeffamine T-3000, and Jeffamine T-5000.

[0073] Additional examples of polyetheramine adducts are those described in US Pat. Nos. 4,420,574 and 4,423,166, which are incorporated herein by reference.

[0074] According to the present disclosure, the polyetheramine adduct may be present in the electrodepositable coating composition in an amount of at least 3 wt %, such as at least 5 wt %, such as at least 10 wt %, such as at least 15 wt % based on the total weight of the resin solids; and no more than 20 wt %, such as no more than 15 wt %, such as no more than 10 wt %, such as no more than 5 wt %. The polyetheramine may be present in the electrodepositable coating composition in an amount of 3 wt % to 20 wt %, such as 5 wt % to 15 wt %, such as 5 wt % to 10 wt %, based on the total weight of the resin solids.

[0075] According to the present disclosure, the coating composition that can be electrodeposited can optionally include a catalyst for catalyzing the reaction between the curing agent, the polyol and the film-forming polymer containing the ionic salt group. Examples of catalysts suitable for cationic electrodeposited coating compositions include, but are not limited to, organotin compounds (e.g., dibutyltin oxide and dioctyltin oxide) and salts thereof (e.g., dibutyltin diacetate); other metal oxides (e.g., oxides of cerium, zirconium and bismuth) and salts thereof (e.g., bismuth sulfamate and bismuth lactate) or cyclic guanidines as described in U.S. Pat. No. 7,842,762, column 1, line 53 to column 4, line 18 and column 16, line 62 to column 19, line 8, the cited portion of which is incorporated herein by reference. Examples of catalysts suitable for use in anionic electrodepositable coating compositions include latent acid catalysts, specific examples of which are identified in paragraph

[0031] of WO 2007 / 118024 and include, but are not limited to, ammonium hexafluoroantimonate, quaternary salts of SbF6 (e.g., XC-7231), tertiary amine salts of SbF6 (e.g., XC-9223), Zn salts of trifluoromethanesulfonic acid (e.g., A202 and A218), quaternary salts of trifluoromethanesulfonic acid (e.g., XC-A230) and diethylamine salt of trifluoromethanesulfonic acid (e.g., A233) (all commercially available from King Industries) and / or mixtures thereof. Latent acid catalysts can be formed by preparing derivatives of acid catalysts such as p-toluenesulfonic acid (pTSA) or other sulfonic acids. For example, a well-known group of blocked acid catalysts are amine salts of aromatic sulfonic acids, such as pyridinium p-toluenesulfonate. Such sulfonates are not as active as the free acids in promoting crosslinking. The catalyst can be activated by heating during curing.

[0076] In accordance with the present disclosure, the electrodepositable coating compositions of the present disclosure may optionally include a pit control additive that may be incorporated into the coating composition.

[0077] According to the present disclosure, the coating composition that can be electrodeposited can optionally include a silicone additive. The silicone additive can include a polyether-modified silicone compound, a polyester-modified silicone compound, a polypropylene-modified silicone compound, or any combination thereof. Non-limiting examples of polyether-modified silicone compounds include compounds in which a polyether chain is introduced into the end and / or side chain of a polysiloxane polymer. For example, a polyether-modified silicone compound can be a compound in which a polyether chain is introduced into the side chain of a polysiloxane polymer (such as polydimethylsiloxane). Non-limiting examples of polyester-modified silicone compounds include compounds in which a polyester chain is introduced into the end and / or side chain of a polysiloxane polymer. For example, a polyester-modified silicone compound can be a compound in which a polyester chain is introduced into the side chain of a polysiloxane polymer (such as polydimethylsiloxane). Non-limiting examples of polypropylene-modified silicone compounds include compounds in which a polypropylene chain is introduced into the end and / or side chain of a polysiloxane polymer. For example, a polypropylene-modified silicone compound may be a compound in which a polypropylene chain is introduced into a side chain of a polysiloxane polymer such as polydimethylsiloxane. Non-limiting examples of suitable commercially available silicone additives include those sold under the trade names Silicone additives such as those sold by Wet are commercially available from Evonik Operations GmbH, such as Wet 260, Wet 265, Wet270 and Wet 280.

[0078] The electrodepositable coating composition may optionally further include a pigment. The pigment may include any suitable pigment. Non-limiting examples of pigments include iron oxide, lead oxide, strontium chromate, carbon black, coal powder, titanium dioxide, barium sulfate, color pigments, layered silicate pigments, metallic pigments, thermally conductive electrical insulating fillers, flame retardant pigments, and color pigments (such as cadmium yellow, cadmium red, lead chrome yellow, etc.) or any combination thereof.

[0079] The pigment to binder (P: B) ratio described in the present disclosure can refer to the weight ratio of the pigment to the binder in the electrodepositable coating composition, and / or the weight ratio of the pigment to the binder in the deposited wet film, and / or the weight ratio of the pigment to the binder in the dried uncured deposited film, and / or the weight ratio of the pigment to the binder in the cured film. The pigment to binder (P: B) ratio of the pigment to the electrodepositable binder can be at least 0.05: 1, such as at least 0.1: 1, such as at least 0.2: 1, such as at least 0.30: 1, such as at least 0.35: 1, such as at least 0.40: 1, such as at least 0.50: 1, such as at least 0.60: 1, such as at least 0.75: 1, such as at least 1: 1, such as at least 1.25: 1, such as at least 1.5: 1. The pigment to binder (P:B) ratio of the pigment to the electrodepositable binder can be no more than 2.0:1, such as no more than 1.75:1, such as no more than 1.5:1, such as no more than 1.25:1, such as no more than 1:1, such as no more than 0.75:1, such as no more than 0.70:1, such as no more than 0.60:1, such as no more than 0.55:1, such as no more than 0.50:1, such as no more than 0.30:1, such as no more than 0.20:1, such as no more than 0.10:1. The pigment to electrodepositable binder may have a pigment to binder (P:B) ratio of 0.05:1 to 2.0:1, such as 0.05:1 to 1.75:1, such as 0.05:1 to 1.50:1, such as 0.05:1 to 1.25:1, such as 0.05:1 to 1:1, such as 0.05:1 to 0.75:1, such as 0.05:1 to 0.70:1, such as 0.05:1 to 0.60:1, such as 0. .05:1 to 0.55:1, such as 0.05:1 to 0.50:1, such as 0.05:1 to 0.30:1, such as 0.05:1 to 0.20:1, such as 0.05:1 to 0.10:1, such as 0.1:1 to 2.0:1, such as 0.1:1 to 1.75:1, such as 0.1:1 to 1.50:1, such as 0.1:1 to 1.25:1, such as 0.1:1 to 1:1, such as 0.1:1 to 0.75:1, such as 0.1:1 to 0.70:1, such as 0.1:1 to 0.60:1, such as 0.1:1 to 0.55:1, such as 0.1:1 to 0.50:1, such as 0.1:1 to 0.30:1, such as 0.1:1 to 0.20:1, such as 0.2:1 to 2.0:1, such as 0.2:1 to 1.75:1, such as 0.2:1 to 1.50:1, such as 0.2:1 to 1.25:1 , such as 0.2:1 to 1:1, such as 0.2:1 to 0.75:1, such as 0.2:1 to 0.70:1, such as 0.2:1 to 0.60:1, such as 0.2:1 to 0.55:1, such as 0.2:1 to 0.50:1, such as 0.2:1 to 0.30:1, such as 0.3:1 to 2.0:1, such as 0.3:1 to 1.75:1, such as 0.3:1 to 1.50:1, such as 0.3:1 to 1.25:1, such as 0.3:1 to 1:1, such as 0.3:1 to 0.75:1, such as 0.3:1 to 0.70:1, such as 0.3:1 to 0.60:1, such as 0.3:1 to 0.55:1, such as 0.3:1 to 0.50:1, such as 0.3:1 to 0.30:1, such as 0.35:1 to 2.0:1, such as 0.35:1 to 1.75:1, such as 0.35:1 to 1.50:1, such as 0.35:1 to 1.25:1, such as 0.35:1 to 1:1, such as 0.35:1 to 0.75:1, such as 0.35:1 to 0.7 0:1, such as 0.35:1 to 0.60:1, such as 0.35:1 to 0.55:1, such as 0.35:1 to 0.50:1, such as 0.4:1 to 2.0:1, such as 0.4:1 to 1.75:1, such as 0.4:1 to 1.50:1, such as 0.4:1 to 1.25:1, such as 0.4:1 to 1:1, such as 0.4:1 to 0.75:1, such as 0.4:1 to 0.70:1, such as 0.4:1 to 0.60:1, such as 0.4:1 to 0.55:1, such as 0.4:1 to 0.50:1, such as 0.5:1 to 2.0:1 , such as 0.5:1 to 1.75:1, such as 0.5:1 to 1.50:1, such as 0.5:1 to 1.25:1, such as 0.5:1 to 1:1, such as 0.5:1 to 0.75:1, such as 0.5:1 to 0.70:1, such as 0.5:1 to 0.60:1, such as 0.5:1 to 0.55:1, such as 0.6:1 to 2.0:1, such as 0.6:1 to 1.75:1, such as 0.6:1 to 1.50:1, such as 0.6:1 to 1.25:1, such as 0.6:1 to 1:1, such as 0.6:1 to 0.75:1, such as 0.6:1 to 0.70:1, such as 0.75:1 to 2.0:1, such as 0.75:1 to 1.75:1, such as 0.75:1 to 1.50:1, such as 0.75:1 to 1.25:1, such as 0.75:1 to 1:1, such as 1:1 to 2.0:1, such as 1:1 to 1.75:1, such as 1:1 to 1.50:1, such as 1:1 to 1.25:1, such as 1.25:1 to 2.0:1, such as 1.25:1 to 1.75:1, such as 1.25:1 to 1.50:1, such as 1.50:1 to 2.0:1, such as 1.50:1 to 1.75:1. .

[0080] According to the present disclosure, the coating composition that can be electrodeposited can include other optional ingredients, if desired, including various additives, such as fillers, plasticizers, antioxidants, biocides, UV light absorbers and stabilizers, hindered amine light stabilizers, defoamers, fungicides, dispersion aids, flow control agents, surfactants, wetting agents or combinations thereof. Alternatively, the coating composition that can be electrodeposited can be completely free of any optional ingredients, i.e., the optional ingredients are not present in the coating composition that can be electrodeposited. Based on the total weight of the resin solids of the coating composition that can be electrodeposited, the other additives mentioned above can be present in the coating composition that can be electrodeposited in an amount of 0.01% by weight to 3% by weight.

[0081] According to the present disclosure, the coating composition that can be electrodeposited can include water and / or one or more organic solvents. Based on the gross weight of the coating composition that can be electrodeposited, water can be, for example, present in an amount of 40% to 90% by weight, such as 50% to 75% by weight. The example of a suitable organic solvent comprises an oxidized organic solvent, such as a monoalkyl ether containing 1 to 10 carbon atoms in the alkyl group of ethylene glycol, diethylene glycol, propylene glycol and dipropylene glycol, such as the monoethyl ether and monobutyl ether of these glycols. Other examples of water-miscible solvents at least partially comprise alcohols, such as ethanol, isopropanol, butanol and diacetone alcohol. If used, based on the gross weight of the coating composition that can be electrodeposited, the organic solvent can generally be present in an amount of less than 10% by weight, such as less than 5% by weight. The coating composition that can be electrodeposited can be specifically provided in the form of a dispersion, such as an aqueous dispersion.

[0082] According to the present disclosure, the total solid content of the electrodepositable coating composition may be at least 1 wt %, such as at least 5 wt %, and may be no more than 50 wt %, such as no more than 40 wt %, such as no more than 20 wt %, based on the total weight of the electrodepositable coating composition. The total solid content of the electrodepositable coating composition may be from 1 wt % to 50 wt %, such as from 5 wt % to 40 wt %, such as from 5 wt % to 20 wt %, based on the total weight of the electrodepositable coating composition. As used herein, "total solids" refers to the non-volatile content of the electrodepositable coating composition, i.e., materials that will not volatilize when heated to 110° C. for 15 minutes.

[0083] The electrodepositable coating composition may be substantially free, substantially free, or completely free of catalytic tin. As used herein, an electrodepositable coating composition is "substantially free" of catalytic tin if the catalytic tin is present in an amount of less than 0.1 wt. %, based on the total weight of the electrodepositable coating composition. As used herein, an electrodepositable coating composition is "substantially free" of catalytic tin if the catalytic tin is present in an amount of less than 0.01 %, based on the total weight of the electrodepositable coating composition. As used herein, an electrodepositable coating composition is "completely free" of catalytic tin if the catalytic tin is present in an amount of 0.001 %, based on the total weight of the electrodepositable coating composition.

[0084] Substrate

[0085] According to the present disclosure, the coating composition that can be electrodeposited can be applied to the substrate electrophoretically. The coating composition that can be electrodeposited by cation can be deposited electrophoretically on any conductive substrate. Suitable substrates include metal substrates, metal alloy substrates and / or metallized substrates, such as nickel-plated plastics. Additionally, substrates can include non-metallic conductive materials including composite materials, such as materials including carbon fibers or conductive carbon. According to the present disclosure, metals or metal alloys can include cold-rolled steel, hot-rolled steel, steel coated with zinc metal, zinc compounds or zinc alloys, such as electrogalvanized steel, hot-dip galvanized steel, alloyed hot-dip galvanized steel (galvanealed steel) and steel plated with zinc alloys. Aluminum alloys of 2XXX, 5XXX, 6XXX or 7XXX series and clad aluminum alloys and cast aluminum alloys of A356 series can also be used as substrates. Magnesium alloys of AZ31B, AZ91C, AM60B or EV31A series can also be used as substrates. The substrate used in the present disclosure can also include titanium and / or titanium alloys. Other suitable non-ferrous metals include copper and magnesium and alloys of these materials. Suitable metal substrates for use in the present disclosure include metal substrates commonly used in the following: vehicle body assemblies (such as, but not limited to, doors, body panels, trunk lids, roof panels, hoods, roofs and / or stringers, rivets, landing gear components and / or skins used on aircraft), vehicle frames, vehicle parts, motorcycles, wheels, industrial structures and components, such as household appliances including washers, dryers, refrigerators, stoves, dishwashers, etc., agricultural equipment, lawn and garden equipment, air conditioning units, heat pump units, lawn furniture and other articles. As used herein, "vehicle" or variations thereof include, but are not limited to, civil, commercial and military aircraft and / or land vehicles, such as automobiles, motorcycles and / or trucks. The metal substrate can also be in the form of, for example, metal sheets or prefabricated parts. It should also be understood that the substrate can be pretreated with a pretreatment solution comprising a zinc phosphate pretreatment solution, such as those described, for example, in U.S. Pat. Nos. 4,793,867 and 5,588,989, or a zirconium-containing pretreatment solution, such as those described, for example, in U.S. Pat. Nos. 7,749,368 and 8,673,091.

[0086] In an example, the substrate may include a three-dimensional component formed by an additive manufacturing process such as selective laser melting, electron beam melting, directed energy deposition, binder jetting, metal extrusion, etc. In an example, the three-dimensional component may be a metal and / or resin component.

[0087] Coating method, coating and coated substrate

[0088] The present disclosure also relates to a method for coating a substrate (such as any of the conductive substrates mentioned above). According to the present disclosure, such a method may include electrophoretically applying an electrodepositable coating composition as described above to at least a portion of the substrate and curing the coating composition to form an at least partially cured coating on the substrate. According to the present disclosure, the method may include (a) electrophoretically depositing the electrodepositable coating composition of the present disclosure onto at least a portion of the substrate; and (b) heating the coated substrate to a temperature and for a time sufficient to cure the electrodeposited coating on the substrate. According to the present disclosure, the method may optionally further include (c) directly applying one or more pigmented coating compositions and / or one or more non-pigmented coating compositions to the at least partially cured electrodeposited coating to form a top coating on at least a portion of the at least partially cured electrodeposited coating, and (d) heating the coated substrate of step (c) to a temperature and for a time sufficient to cure the top coating.

[0089] According to the disclosure, the coating composition of the cationic electrodeposition of the present disclosure can be deposited on a conductive substrate by contacting the composition with a conductive cathode and a conductive anode, wherein the surface to be coated is a cathode. After contacting the composition, when enough voltages are applied between the electrodes, the adhesion film of the coating composition is deposited on the cathode. The conditions for electrodeposition are similar to the conditions used in the electrodeposition of other types of coatings. The voltage applied can vary and can be, for example, as low as one volt to as high as several thousand volts, such as between 50 volts and 500 volts. The current density can be between 0.5 ampere and 15 amperes per square foot, and tends to reduce during electrodeposition, which shows that an insulating film has been formed.

[0090] Once the cationic electrodepositable coating composition is electrodeposited on at least a portion of the conductive substrate, the coated substrate is heated to a temperature and for a time sufficient to at least partially cure the electrodeposited coating on the substrate. As used herein, the term "at least partially cured" with respect to the coating refers to forming a coating by subjecting the coating composition to curing conditions that chemically react at least a portion of the reactive groups of the components of the coating composition to form a coating. The coated substrate can be heated to a temperature in the following range: 250°F to 450°F (121.1°C to 232.2°C), such as 275°F to 400°F (135°C to 204.4°C), such as 300°F to 360°F (149°C to 180°C). The curing time can depend on the curing temperature as well as other variables, such as the film thickness of the electrodeposited coating, the level and type of the catalyst present in the composition, etc. For the purposes of this disclosure, all that is necessary is that the time is sufficient to achieve the curing of the coating on the substrate. For example, the curing time may range from 10 minutes to 60 minutes, such as 20 to 40 minutes. The thickness of the resulting cured electrodeposition coating may range from 15 to 50 microns.

[0091] According to the disclosure, the coating composition of anion electrodeposition of the present disclosure can be deposited on a conductive substrate by contacting the composition with a conductive cathode and a conductive anode, wherein the surface to be coated is an anode. After contacting the composition, when enough voltages are applied between the electrodes, the adhesion film of the coating composition is deposited on the anode. The conditions for electrodeposition are similar to the conditions used in the electrodeposition of other types of coatings. The voltage applied can vary and can be, for example, as low as one volt to as high as several thousand volts, such as between 50 volts and 500 volts. The current density can be between 0.5 ampere and 15 amperes per square foot, and tends to decrease during electrodeposition, which shows that an insulating film has been formed.

[0092] Once the anionic electrodepositable coating composition is electrodeposited on at least a portion of the conductive substrate, the coated substrate can be heated to a temperature and for a time sufficient to at least partially cure the electrodeposited coating on the substrate. As used herein, the term "at least partially cured" with respect to the coating refers to forming a coating by subjecting the coating composition to curing conditions that chemically react at least a portion of the reactive groups of the components of the coating composition to form a coating. The coated substrate can be heated to a temperature in the following range: 200°F to 450°F (93°C to 232.2°C), such as 275°F to 400°F (135°C to 204.4°C), such as 300°F to 360°F (149°C to 180°C). The curing time can depend on the curing temperature as well as other variables, such as the film thickness of the electrodeposited coating, the level and type of catalyst present in the composition, etc. For the purposes of this disclosure, all that is necessary is that the time is sufficient to achieve the curing of the coating on the substrate. For example, the curing time may range from 10 to 60 minutes, such as 20 to 40 minutes. The thickness of the resulting cured electrodeposition coating may range from 15 to 50 microns.

[0093] If desired, the electrodepositable coating compositions of the present disclosure may also be applied to substrates using non-electrophoretic coating application techniques such as flow coating, dipping, spraying, and roller coating. For non-electrophoretic coating applications, the coating compositions may be applied to conductive substrates as well as non-conductive substrates such as glass, wood, and plastic.

[0094] The present disclosure further relates to coatings formed by at least partially curing the electrodepositable coating compositions described herein.

[0095] The present disclosure further relates to a substrate at least partially coated with an electrodepositable coating composition as described herein. The coating may optionally be in an at least partially cured or fully cured state. The coated substrate may include a coating comprising a polyol comprising residues of ethylene oxide and butylene oxide; a film-forming polymer containing ionic salt groups different from the polyol; and a curing agent.

[0096] Multilayer coating composites

[0097] The electrodepositable coating composition of the present disclosure can be used for electrophoretic coating, which is a part of a multilayer coating composite material including a substrate with various coatings. The coating can include a pretreatment layer, such as a phosphate layer (e.g., a zinc phosphate layer), an electrophoretic coating produced by an aqueous resin dispersion of the present disclosure, and a suitable top coating (e.g., a base coating, a clear coating, a pigmented monocoat and a color plus clear coating composite composition). It should be understood that suitable top coatings include any top coatings in those top coatings known in the art, and can be independently water-borne, solvent-based, in the form of solid particles (i.e., a powder coating composition) or in the form of a powder slurry. The top coating generally includes a film-forming polymer, a cross-linking material, and one or more pigments (if it is a colored base coating or a monocoat). According to the present disclosure, a primer layer is placed between the electrophoretic coating and the base coating. According to the present disclosure, one or more top coatings in the top coating are applied to a substantially uncured bottom layer. For example, a clear coating can be applied to at least a portion of a substantially uncured base coating (wet-on-wet), and two layers can be cured simultaneously in a downstream process.

[0098] In addition, the top coating can be applied directly to the electrodepositable coating. In other words, the substrate lacks a primer layer. For example, the base coating can be applied directly to at least a portion of the electrodepositable coating.

[0099] It will also be understood that the topcoat can be applied to the bottom layer despite the fact that the bottom layer has not yet been fully cured. For example, a clearcoat can be applied to the basecoat even if the basecoat has not yet been subjected to a curing step. The two layers can then be cured during a subsequent curing step, thereby eliminating the need to cure the basecoat and clearcoat separately.

[0100] According to the present disclosure, other ingredients (such as colorants and fillers) can be present in various coating compositions that produce topcoat. Any suitable colorant and filler can be used. For example, colorant can be added to the coating in any suitable form such as discrete particles, dispersions, solutions and / or flakes. A single colorant or a mixture of two or more colorants can be used in the coating of the present disclosure. It should be noted that colorant can be present in a certain layer of multilayer composite material in any amount sufficient to impart desired properties, visual and / or color effects in general.

[0101] Example colorants include pigments, dyes and colorants, such as those used in the coatings industry and / or listed in the Dry Color Manufacturers Association (DCMA), and special effect compositions. Colorants can include, for example, finely divided solid powders that are insoluble but wettable under the conditions of use. Colorants can be organic or inorganic and can be agglomerated or non-agglomerated. Colorants can be incorporated into the coating by grinding or simple mixing. Colorants can be incorporated by grinding into the coating using a grinding medium such as an acrylic grinding medium, the use of which will be familiar to those skilled in the art.

[0102] Example pigments and / or pigment compositions include, but are not limited to, carbazole dioxazine crude pigments, azo, monoazo, disazo, naphthol AS, salts (salt lakes), benzimidazolone, condensates, metal complexes, isoindolinone, isoindolinone and polycyclic phthalocyanine, quinacridone, perylene, perinone, diketopyrrolopyrrole, thioindigo, anthraquinone, indanthrone, anthrapyrimidine, flavonanthrone, pyranthrone, anthraquinone, dioxazine, triaryl carbocyanine, quinophthalone pigment, diketopyrrolopyrrole red ("DPP red BO"), titanium dioxide, carbon black, zinc oxide, antimony oxide, etc., and organic or inorganic UV opaque pigments (such as iron oxide), transparent red or yellow iron oxide, phthalocyanine blue, and mixtures thereof. The terms "pigment" and "colored filler" may be used interchangeably.

[0103] Exemplary dyes include, but are not limited to, those solvent-based dyes and / or water-based dyes such as acid dyes, azo dyes, basic dyes, direct dyes, disperse dyes, reactive dyes, solvent dyes, sulfur dyes, mordant dyes, for example, bismuth vanadate, anthraquinone, perylene, aluminum, quinacridone, thiazole, thiazine, azo, indigo, nitro, nitroso, oxazine, phthalocyanine, quinoline, stilbene and triphenylmethane.

[0104] Exemplary colorants include, but are not limited to, pigments dispersed in water-based or water-miscible carriers such as AQUA-CHEM 896, commercially available from Degussa, Inc., CHARISMA colorants, and MAXITONER INDUSTRIAL COLORANTS, commercially available from the Accurate Dispersions Division of Eastman Chemical, Inc.

[0105] Coloring agent can be in the form of dispersion, including but not limited to nanoparticle dispersion.Nanoparticle dispersion can include one or more highly dispersed nanoparticle coloring agents and / or coloring agent particles that produce desired visible color and / or opacity and / or visual effect.Nanoparticle dispersion can include coloring agent, such as pigment or dye with particle size less than 150nm, such as less than 70nm, such as less than 30nm.Nanoparticles can be produced by milling raw material organic or inorganic pigment of grinding media with particle size less than 0.5mm.Example nanoparticle dispersion and its manufacturing method are identified in U.S. Patent No. 6,875,800B2, which is incorporated herein by reference.Nanoparticle dispersion can also be produced by crystallization, precipitation, gas phase condensation and chemical abrasion (that is, partial dissolution).In order to minimize the re-agglomeration of nanoparticles in the coating, the dispersion of resin-coated nanoparticles can be used.As used herein, "dispersion of resin-coated nanoparticles" refers to the continuous phase of fine "composite microparticles" as dispersed including nanoparticles and the resin coating on the nanoparticles. Exemplary dispersions of resin-coated nanoparticles and methods for making the same are identified in U.S. Patent Application No. 10 / 876,031, filed June 24, 2004, which is incorporated herein by reference, and in U.S. Provisional Patent Application No. 60 / 482,167, filed June 24, 2003, which is also incorporated herein by reference.

[0106] According to the present disclosure, the special effect composition that can be used in one or more layers in the multilayer coating composite material includes pigments and / or compositions that produce one or more appearance effects, such as reflection, pearlescence, metallic luster, phosphorescence, fluorescence, photochromism, photosensitivity, thermochromism, iridescence and / or color change. Additional special effect compositions can provide other perceptible properties, such as reflectivity, opacity or texture. For example, the special effect composition can produce a color shift so that the color of the coating changes when the coating is viewed from different angles. Example color effect compositions are identified in U.S. Patent No. 6,894,086, which is incorporated herein by reference. Additional color effect compositions can include transparent coated mica and / or synthetic mica, coated silica, coated aluminum oxide, transparent liquid crystal pigments, liquid crystal coatings and / or any composition, wherein interference comes from a refractive index difference within the material rather than because of a refractive index difference between the material surface and air.

[0107] According to the present disclosure, photosensitive compositions and / or photochromic compositions can be used in many layers of a multilayer composite material, and the color of the photosensitive compositions and / or photochromic compositions can be reversibly changed when exposed to one or more light sources. The photochromic and / or photosensitive compositions can be activated by exposure to radiation of a specific wavelength. When the composition becomes excited, the molecular structure changes and the changed structure exhibits a new color different from the original color of the composition. When the radiation exposure is removed, the photochromic and / or photosensitive composition can be restored to a static state, wherein the original color of the composition is restored. For example, the photochromic and / or photosensitive composition may be colorless in a non-excited state and exhibit color in an excited state. The complete color change can occur in a few milliseconds to several minutes, such as 20 seconds to 60 seconds. Example photochromic and / or photosensitive compositions include photochromic dyes.

[0108] According to the present disclosure, the photosensitive composition and / or photochromic composition can be associated with a polymeric material of a polymeric and / or polymerizable component and / or at least partially bound to the polymeric material of the polymeric and / or polymerizable component, such as by covalent bonding. Unlike some coatings in which the photosensitive composition can migrate out of the coating and crystallize into the substrate, the migration out of the coating of the photosensitive composition and / or photochromic composition associated with and / or at least partially bound to the polymeric and / or polymerizable component according to the present disclosure is minimal. Example photosensitive compositions and / or photochromic compositions and methods of making the same are identified in U.S. Patent Application No. 10 / 892,919, filed on July 16, 2004, which is incorporated herein by reference.

[0109] For the purpose of this detailed description, it should be understood that the present disclosure may take alternative variations and step sequences except where explicitly stated to the contrary. In addition, except in any operating examples or where otherwise indicated, all numerals representing the amount of ingredients used in the specification and claims should be understood to be modified by the term "about" in all cases. Therefore, unless otherwise indicated, the numerical parameters set forth in the following specification and the appended claims are approximate values ​​that can be changed according to the desired properties to be obtained by the present disclosure. At least, and not attempting to limit the application of the doctrine of equivalents to the scope of the claims, each numerical parameter should at least be interpreted according to the number of reported significant figures and by applying common rounding techniques.

[0110] Notwithstanding that the numerical ranges and parameters setting forth the broad scope of the disclosure are approximations, the numerical values ​​set forth in the specific examples are reported as precisely as possible. Any numerical value, however, inherently contains certain errors necessarily resulting from the standard deviation found in their respective testing measurements.

[0111] Furthermore, it should be understood that any numerical range recited herein is intended to include all subranges subsumed therein. For example, a range of "1 to 10" is intended to include all subranges between (and including) the recited minimum value of 1 and the recited maximum value of 10, i.e., having a minimum value equal to or greater than 1 and a maximum value equal to or less than 10.

[0112] As used herein, "including", "containing" and similar terms are understood to be synonymous with "comprising" in the context of this application, and are therefore open-ended and do not exclude the presence of additional undescribed or unrecited elements, materials, components, or method steps. As used herein, "consisting of" is understood to exclude the presence of any unspecified elements, ingredients, or method steps in the context of this application. As used herein, "consisting substantially of" is understood to include the specified elements, materials, ingredients, or method steps "as well as elements, materials, ingredients, or method steps that do not materially affect the basic and novel characteristics of the described content" in the context of this application.

[0113] In this application, unless otherwise specifically stated, the use of the singular includes the plural, and the plural encompasses the singular. For example, although "a" film-forming polymer containing an ionic salt group, "a" curing agent, or "a" polyol is mentioned herein, a combination of these components (i.e., a plurality of these components) may be used. In addition, in this application, unless otherwise explicitly stated, the use of "or" means "and / or", even though "and / or" may be explicitly used in certain cases.

[0114] Although specific aspects of the present disclosure have been described in detail, it will be appreciated by those skilled in the art that various modifications and alternatives to those details may be developed based on the overall teachings of the present disclosure. Therefore, the particular arrangements disclosed are intended to be illustrative only and not limiting of the scope of the present disclosure, which is given by the full scope of the appended claims and any and all equivalent forms thereof.

[0115] The following examples illustrate the present disclosure, which, however, should not be considered to limit the present disclosure to its details.Unless otherwise indicated, all parts and percentages in the following examples and throughout the specification are by weight.

[0116] Examples

[0117] Example 1: Preparation of blocked polyisocyanate curing agent

[0118] The blocked polyisocyanate curing agent comprising isocyanate groups blocked with an alcohol mixture was prepared as follows: Components 2-6 listed in Table 1 below were mixed in a flask set to total reflux by stirring under nitrogen. The mixture was heated to a temperature of 30°C, and component 1 was added dropwise so that the temperature increased due to the exothermic reaction and maintained at 100°C. After the addition of component 1 was completed, a temperature of 100°C was established in the reaction mixture, and the reaction mixture was maintained at the temperature until no residual isocyanate was detected by IR spectroscopy. Component 7 was then added, and the reaction mixture was stirred at 100°C for 30 minutes before cooling to ambient temperature.

[0119] Table 1

[0120] serial number Components Weight 1 <![CDATA[Polymeric methylene diphenyl diisocyanate 1 > 1206.0 2 Dibutyltin dilaurate 1.0 3 Methyl isobutyl ketone 159.6 4 2-Butoxyethanol 106.2 5 2-(2-Butoxyethoxy)ethanol 510.3 6 Methanol 158.4 7 Methyl isobutyl ketone 122.4

[0121] 1 Rubinate M, available from Huntsman Corporation.

[0122] Examples 2 to 5: Preparation of cationic amine functionalized polyepoxide-based resins

[0123] Each of Examples 2 to 5 was prepared as follows: a cationic amine functionalized polyepoxide-based polymer resin was prepared in the following manner. Components 1-6 listed in Table 2 below were mixed in a flask set to total reflux by stirring under nitrogen. The mixture was heated to a temperature of 130°C and allowed to exotherm (maximum 175°C). A temperature of 145°C was established in the reaction mixture, and the reaction mixture was then maintained at said temperature for 2 hours. Components 7-9 were slowly introduced while the mixture was cooled to 125°C, followed by addition of component 10. A temperature of 105°C was established, and then components 11 and 12 were quickly added (sequentially added) to the reaction mixture, and the reaction mixture was allowed to exotherm. A temperature of 120°C was established, and the reaction mixture was maintained for 1 hour.

[0124] Then, a portion of the resin synthesis product (component 13) was poured into the premixed solution of components 14 and 15 to form a resin dispersion, and the resin dispersion was stirred for 1 hour. Then, component 16 was introduced within 30 minutes to further dilute the resin dispersion, followed by the addition of component 17. MIBK in the resin dispersion was removed from the dispersion under vacuum at a temperature of 60-70°C.

[0125] The solids content of the resulting resin dispersion was determined by adding a certain amount of the resin dispersion to a tared aluminum pan, recording the initial weight of the resin dispersion, heating the resin dispersion in the pan in an oven at 110° C. for 60 minutes, allowing the pan to cool to ambient temperature, reweighing the pan to determine the amount of non-volatile content remaining, and calculating the solids content by dividing the weight of the remaining non-volatile content by the initial resin dispersion weight and multiplying by 100. Table 2 reports the solids content of Resin Dispersions 2-5.

[0126] Table 2

[0127]

[0128]

[0129] 1 EPON 828, available from Hexion Corporation.

[0130] 2 Newpol EB-2000, available from SANAM Corporation. A polyol consisting of ethylene oxide:butylene oxide units in a ratio of 30%:70% with a molecular weight of 2,000±500.

[0131] 3 The diketimine reaction product of 1 equivalent of diethylenetriamine and 2 equivalents of MIBK, 72.7 wt% (in MIBK).

[0132] Example 6: Preparation of polyetheramine adducts

[0133] Table 3

[0134]

[0135]

[0136] 1 Aliphatic epoxy resin, available from Dow Chemical Co.

[0137] 2 EPON 828, available from Hexion Corporation.

[0138] 3 Available as MAZON 1651 from BASF Corporation.

[0139] 4Polyoxypropylene diamine, available from Huntsman Corporation.

[0140] The polyetheramine adduct was prepared from the components listed in Table 3 according to the following procedure: Components 1, 2 and 3 were charged into a suitably equipped round-bottom flask. The mixture was heated to 130°C and material 4 was added. The reaction mixture was maintained at 150°C until the epoxide equivalent weight of the mixture was 1361. Then, materials 5 and 6 were added and the mixture was cooled to 98°C. Materials 7-8 were added and the reaction was maintained at 95°C for 30 minutes. Then, charge 9 was added and maintained at 100°C until the Gardner-Holdt viscosity of the resin sample diluted 50 / 50 in methoxypropanol remained unchanged for 30 minutes. The resin was poured into the mixture of charges 10 and 11 and mixed for 30 minutes. Then, charge 12 was added and mixed for at least 1 hour. The measured solid content of the final aqueous dispersion was 42.0%.

[0141] Example 7: Synthesis of a polymer dispersant containing cationic salt groups

[0142] Table 4

[0143]

[0144]

[0145] 1 2,2'-Azobis(2-methylbutyronitrile) free radical initiator, available from The Chemours Company.

[0146] According to the following procedure, a polymer dispersant containing cationic salt groups was prepared from the components listed in Table 4: Charge 1 was added to a 4-necked flask equipped with a thermocouple, a nitrogen sparger and a mechanical stirrer. Under nitrogen blanketing and stirring, the flask was heated to reflux with a temperature setting point of 100°C. Charges 2 and 3 were added dropwise through an addition funnel over 150 minutes and then kept for 30 minutes. After the temperature was raised to 120°C, charge 4 was then added over 15 minutes and then kept for 10 minutes. The temperature was reduced to 110°C while charge 5 was added to help cool the reaction. Charge 6 was added and the temperature was kept at 115°C for 3 hours. During the holding period, charge 7 was heated to approximately 35-40°C in a separate container equipped with a mechanical stirrer. After holding, the contents in the reactor were poured into a container containing charge 7 under rapid stirring and then kept for 60 minutes. As the dispersion continued to cool to ambient temperature (about 25°C), charge 8 was added under stirring. The solids content of the resulting aqueous dispersion of cationic polymer dispersant was 16.70%.

[0147] The weight average molecular weight (Mw) and z-average molecular weight (Mz) were determined by gel permeation chromatography (GPC). For polymers with z-average molecular weights less than 900,000, GPC was performed using a Waters 2695 separation module with a Waters 410 differential refractometer (RI detector), polystyrene standards with molecular weights ranging from approximately 500 g / mol to 900,000 g / mol, dimethylformamide (DMF) with 0.05 M lithium bromide (LiBr) at a flow rate of 0.5 ml / min as eluent, and an Asahipak GF-510HQ column for separation. For polymers with z-average molecular weight (Mz) greater than 900,000 g / mol, GPC was performed using a Waters 2695 separation module with a Waters 410 differential refractometer (RI detector), polystyrene standards with molecular weights ranging from approximately 500 g / mol to 3,000,000 g / mol, a flow rate of 0.5 ml / min of dimethylformamide (DMF) with 0.05 M lithium bromide (LiBr) as eluent, and an Asahipak GF-7M HQ column for separation. All molecular weight measurements included in the molecular weight measurements in the examples followed this procedure. It was determined that the weight average molecular weight of the cationic polymer dispersant was 207,774 g / mol, and the z-average molecular weight was 1,079,872 g / mol.

[0148] Example 8: Synthesis of cationic polymers

[0149] Table 5

[0150]

[0151]

[0152] The aqueous dispersion of Example 8 is formed from the ingredients contained in the table. Example 8 contains a cationic polymer dispersant and an ethylenically unsaturated monomer composition having 10 wt% of a hydroxyl-functional (meth) acrylate (2-hydroxypropyl methacrylate) based on the weight of the ethylenically unsaturated monomer composition. Example 8 is prepared as follows: Charge 1 is added to a 4-necked flask equipped with a thermocouple, a nitrogen sparger, and a mechanical stirrer. The flask is heated to 25°C under a nitrogen blanket and vigorous stirring. At 25°C, the solution is sparged under nitrogen for another 30 minutes. Charge 2 is then added to the reaction vessel within 10 minutes. Charge 3 is then added to the reaction vessel within 2-3 minutes. The components of Charge 4 are mixed together and added to the reactor via an addition funnel within 30 minutes. During the addition of Charge 4, the reaction is allowed to exotherm. After the addition is complete, the reactor is heated to 50°C and maintained at said temperature for 30 minutes. Charges 5 and 6 are added dropwise and maintained at 50°C for 30 minutes. The reactor was then cooled to ambient temperature.

[0153] The solid content of the resulting aqueous dispersion of Example 8 was determined using the method described in Examples 2-5. The measured solid content was 19.23%. The weight average molecular weight of Example 8 was 655,838 g / mol, and the z average molecular weight of Example 8 was 1,395,842 g / mol, as measured according to the method described in Example 7.

[0154] Example 9: Surfactant Blends

[0155] Table 6

[0156] Material# describe Weight 1 2-Butoxyethanol 31.26 2 Surfynol 104 31.26 3 <![CDATA[Amine C 1 > 32.46 4 Water containing 75% acetic acid 5.01

[0157] 1 4,5-Dihydro-1H-imidazole-1-ethanol, available from Ciba Geigy.

[0158] Materials 1-4 were blended in order.

[0159] Example 10: Preparation of Electrodepositable Coating Compositions AD

[0160] Table 7

[0161]

[0162] 1 Available as MAZON 1651 from BASF.

[0163] 2 A 40% solids cationic epoxy resin dispersion containing 0.84% ​​bismuth (by total weight) is available from PPG Industries.

[0164] 3 Pigment paste E6478, available from PPG, consists of 52% solids at a p:b of 1.22 and contains 1.28% by weight of the total catalyst described in US Pat. No. 7,842,762, available from PPG Industries.

[0165] Charges 1-8 from Table 6 were added sequentially to a plastic container and stirred for 15 minutes. Charges 9 and 10 were added and stirred for a minimum of 1 hour. The subtotal of Charges 1-8 represents the total weight of the resin blend. The solids content of the bath composition was 21.5%, and the ratio of pigment to binder was 0.15 / 1.0 (by weight).

[0166] Coated panels were prepared from baths containing the cationic electrodepositable coating compositions after 25% ultrafiltration (and reconstitution with deionized water).

[0167] Evaluation of coating compositions AD

[0168] Oil spot pollution resistance test

[0169] The above-described electrodepositable coating compositions were then electrodeposited onto cold rolled steel test panels, 4 x 6 x 0.031 inches, pretreated with CHEMFOS C700 / DI (CHEMFOS C700 is a zinc phosphate immersion pretreatment composition available from PPG Industries). These panels were available from ACT Laboratories of Hillside, Mich. The panels were electrophoresed in a manner well known in the art by immersing them in a stirred bath at 30-34° C., with the cathode of a DC rectifier connected to the panel, and the anode of the rectifier connected to a stainless steel tube for circulating cooling water to control the bath temperature. The voltage was increased from 0 to a set point voltage of 190 V over a period of 30 seconds, and then maintained at the voltage for an additional 120 seconds. This combination of time, temperature, and voltage provided a cured dry film thickness of 20 microns for all coatings.

[0170] After electrodeposition, the panels were removed from the bath, rinsed vigorously with deionized water spray, and cured by baking in an electric oven at 177°C for 25 minutes.

[0171] Substrate panels including electrodeposited coatings were subjected to an oil spot contamination resistance test, which evaluates the ability of electrodeposited coatings to resist pit formation when cured. The oil spot pitting resistance of the electrodeposited coatings was tested by locally contaminating the dried coating with three common oils: Ferrocote 6130 (Quaker Chemical Corporation, F), LubeCon Series O lubricant (Castrol Industrial North America Inc., L) or Molub- Alloy Chain Oil 22 Spray (Castrol Industrial North America Inc., M). Using 40 wt % LubeCon Series O lubricant isopropanol solution, 40 wt % or Molub- Alloy Chain Oil 22 Spray isopropanol solution or 40 wt % Ferrocote 6130 isopropanol / butanol (75 wt % / 25 wt %) solution and a micropipette (Scilogex), the oil was deposited on the dried coating in the form of droplets (<0.1 μL). The oily spot substrate panels were then cured as described above (baked in an electric oven at 177°C for 20 minutes).

[0172] Use Keyence VR3200 3D macro microscope to scan each substrate panel to check the depth of pit defects in the cured coating. The difference (pit depth, Δ) between the highest peak and the lowest pit point of each pit in the pits produced in each coating is averaged (at least 4 pits per coating) to quantify the results of the oil spot test. This test is referred to as the pit depth test method in this article. The results are summarized in Table 8 below.

[0173] Appearance test

[0174] The coatings were applied to 4 x 6 x 0.031 inch electrogalvanized (EZG) panels and pretreated with CHEMFOS C700 / DI (CHEMFOS C700 is a zinc phosphate immersion pretreatment composition available from PPG Industries). These panels are available from ACT Laboratories in Hillside, Michigan. After electrodeposition, the panels were removed from the bath, rinsed vigorously with deionized water spray, and cured by baking in an electric oven at 177°C for 25 minutes. The texture of the coated panels was evaluated using a Mitutoyo Surftest SJ-402 non-slip stylus profilometer equipped with a 4mN detector and a diamond stylus tip with a 90° cone and a 5μm tip radius. The scan length, measurement speed, and data sampling interval were 48mm, 1 mm / sec, and 5μm, respectively. The sample data was transferred to a personal computer using the USB port located on the profilometer, and the raw data was first filtered into a roughness curve according to ISO 4287-1997 3.1.6 using the Lc parameter of 2.5 mm and the Ls parameter of 8 μm, and then summarized into the Ra metric according to ISO 4287-1997 4.2.1, hereinafter referred to as Ra (2.5 mm). Table 8 reports the Ra values ​​for compositions AD.

[0175] The gloss of the coated panels was also evaluated. 20° and 60° gloss was measured according to ASTM D523 using a BYK-Gardner haze meter (Cat. No. 4601).

[0176] Adhesion test

[0177] The white alkyd resin adhesion test evaluates the ability of the second cured coating to adhere to the cured electrodeposited coating below. The viscosity of the white alkyd resin coating C354-W404 available from PPG Industries was reduced to 100 centipoise, as measured by a Brookfield DV-I Prime viscometer equipped with a cone and plate attachment at 20 rpm. The diluting solvent (reducing solvent) is butyl acetate. The E-coated test panel was prepared as described and baked in an electric oven at 155°C or 175°C for 25 minutes, or baked in an electric oven at 195°C for 50 minutes. The wet white alkyd resin coating was applied to the cured e-coating using a #55 (0.055 inch diameter wire) wire wound coating rod available from RD Specialties. After flashing the white alkyd resin coating for 10 minutes under ambient conditions, the panel was cured by baking horizontally in an electric oven at 150°C for 30 minutes. After the panel cooled to ambient temperature (about 25° C.), a crosshatch test was performed on it.

[0178] The cross-hatch test uses a scribing tool with a tooth spacing of 2 mm, which cuts the coating system onto the metal substrate. By two such vertical cuts, a "cross-hatch" is obtained, which is then tested with Scotch 898 tape. Failure is considered as the loss of adhesion between the alkyd coating and the electrodeposition coating. The cross-hatch adhesion results are tested on a scale of 0 to 10, with 0 being the worst and 10 being the best, and are reported in the following table. A score of 0 represents that the cured alkyd coating has been completely removed by the tape from the scribing area. A score between 0 and 10 represents that the tape gradually removes the alkyd coating with a lower degree of cure from the scribing area, and the coating is usually removed from the corner where two scribing lines intersect. A score of 10 represents that there is no evidence that the cured alkyd coating is removed by the tape from any corner of the corner where two scribing lines intersect. As used herein, this test is called the white alkyd adhesion test.

[0179] Table 8

[0180]

[0181] The results in Table 8 demonstrate that incorporating the polymers of the present invention into an electrodepositable composition improves the performance of the Pit Depth Test Method and the White Alkyd Adhesion Test without significantly increasing the Ra (2.5 mm) value. In addition, the gloss value is also reduced without affecting the roughness of the coating.

[0182] Those skilled in the art will appreciate that, based on the above disclosure, many modifications and variations are possible without departing from the broad inventive concepts described and illustrated herein. Therefore, it should be understood that the foregoing disclosure is only an illustration of various exemplary aspects of the present application, and those skilled in the art can easily make many modifications and variations within the spirit and scope of the present application and the appended claims.

Claims

1. An electrodepositable coating composition, include: (a) a polyol comprising residues of ethylene oxide and butylene oxide; (b) a film-forming polymer containing ionic salt groups; as well as (c) Curing agent.

2. An electrodepositable coating composition according to claim 1, wherein the molar ratio of ethylene oxide to butylene oxide is at least 9:1, or at least 4:1, or at least 1:1, or at least 2:1 and / or no more than 1:9, or no more than 1:7, or no more than 1:5, or no more than 1:

4.

3. An electrodepositable coating composition according to claim 1 or claim 2, wherein the molar ratio of ethylene oxide to butylene oxide is 9:1 to 1:9, or 4:1 to 1:9, or 2:1 to 1:9, or 1:1 to 1:9, or 9:1 to 1:7, or 4:1 to 1:7, or 2:1 to 1:7, or 1:1 to 1:7, or 9:1 to 1:5, or 4:1 to 1:5, or 2:1 to 1:5, or 1:1 to 1:5, or 9:1 to 1:4, or 4:1 to 1:4, or 2:1 to 1:4, or 1:1 to 1:

4.

4. An electrodepositable coating composition according to any one of the preceding claims, wherein the polyol has a theoretical molecular weight of at least 1,000 g, or at least 1,250 g, or at least 1,500 g and / or no more than 3,000 g, or no more than 2,750 g, or no more than 2,500 g.

5. An electrodepositable coating composition according to any one of the preceding claims, wherein the polyol has a theoretical molecular weight of 1,000 g to 3,000 g, or 1,000 g to 2,750 g, or 1,000 g to 2,500 g, or 1,250 g to 3,000 g, or 1,250 g to 2,750 g, or 1,250 g to 2,500 g, or 1,500 g to 3,000 g, or 1,500 g to 2,750 g, or 1,500 g to 2,500 g.

6. An electrodepositable coating composition according to any one of the preceding claims, wherein the polyol has a theoretical hydroxyl equivalent weight of at least 500 g / OH, or at least 600 g / OH, or at least 700 g / OH, or at least 750 g / OH and / or no more than 2,000 g / OH, or no more than 1,750 g / OH, or no more than 1,500 g / OH, or no more than 1,250 g / OH.

7. An electrodepositable coating composition according to any one of the preceding claims, wherein the polyol has a theoretical hydroxyl equivalent weight of 500 g / OH to 2,000 g / OH, or 500 g / OH to 1750 g / OH, or 500 g / OH to 1,500 g / OH, or 500 g / OH to 1,250 g / OH, or 600 g / OH to 2,000 g / OH, or 600 g / OH to 1,750 g / OH, or 600 g / OH to 1,500 g / OH. g / OH, or 600g / OH to 1,250g / OH, or 700g / OH to 2,000g / OH, or 700g / OH to 1750g / OH, or 700g / OH to 1500g / OH, or 700g / OH to 1250g / OH, or 750g / OH to 2000g / OH, or 750g / OH to 1750g / OH, or 750g / OH to 1500g / OH, or 750g / OH to 1250g / OH.

8. An electrodepositable coating composition according to any one of the preceding claims, wherein the polyol has a hydroxyl value of at least 35 mg KOH / gram of polyol, or at least 40 mg KOH / gram of polyol, or at least 45 mg KOH / gram of polyol, or at least 50 mg KOH / gram of polyol and / or no more than 115 mg KOH / gram of polyol, or no more than 100 mg KOH / gram of polyol, or no more than 75 mg KOH / gram of polyol, or no more than 60 mg KOH / gram of polyol.

9. An electrodepositable coating composition according to any one of the preceding claims, wherein the polyol has a hydroxyl value of 35 to 115 mg KOH / gram of polyol, or 35 to 100 mg KOH / gram of polyol, or 35 to 75 mg KOH / gram of polyol, or 35 to 60 mg KOH / gram of polyol, or 40 to 115 mg KOH / gram of polyol, or 40 to 100 mg KOH / gram of polyol, or 40 to 75 mg KOH / gram of polyol, or 40 to 60 mg KOH / gram of polyol, or 45 to 115 mg KOH / gram of polyol, or 45 to 100 mg KOH / gram of polyol, or 45 to 75 mg KOH / gram of polyol, or 45 to 60 mg KOH / gram of polyol, or 50 to 115 mg KOH / gram of polyol, or 50 to 100 mg KOH / gram of polyol, or 50 to 75 mg KOH / gram of polyol, or 50 to 60 mg KOH / gram of polyol. KOH / g polyol.

10. An electrodepositable coating composition according to any one of the preceding claims, wherein the polyol comprises two hydroxyl functional groups.

11. An electrodepositable coating composition according to any one of the preceding claims, wherein the polyol is present in the electrodepositable coating composition in an amount of at least 0.5 wt %, or at least 0.6 wt %, or at least 0.8 wt %, or at least 1 wt %, or at least 5 wt % and / or no more than 15 wt %, or no more than 12 wt %, or no more than 10 wt %, or no more than 8 wt %, based on the weight of resin solids.

12. An electrodepositable coating composition according to any one of the preceding claims, wherein the polyol is present in the electrodepositable coating composition in an amount of from 0.5 wt % to 15 wt %, or from 0.5 wt % to 12 wt %, or from 0.5 wt % to 10 wt %, or from 0.5 wt % to 8 wt %, or from 0.6 wt % to 15 wt %, or from 0.6 wt % to 12 wt %, or from 0.6 wt % to 10 wt %, based on the total weight of resin solids. , or 0.6 wt % to 8 wt %, or 0.8 wt % to 15 wt %, or 0.8 wt % to 12 wt %, or 0.8 wt % to 10 wt %, or 0.8 wt % to 8 wt %, or 1 wt % to 15 wt %, or 1 wt % to 12 wt %, or 1 wt % to 10 wt %, or 1 wt % to 8 wt %, or 5 wt % to 15 wt %, or 5 wt % to 12 wt %, or 5 wt % to 10 wt %, or 5 wt % to 8 wt %.

13. An electrodepositable coating composition according to any one of the preceding claims, wherein the electrodepositable coating composition is substantially free of catalytic tin.

14. An electrodepositable coating composition according to any one of the preceding claims, wherein the curing agent comprises a blocked polyisocyanate.

15. The electrodepositable coating composition according to claim 14, wherein the blocked polyisocyanate is at least partially blocked by the polyol as a blocking agent.

16. The electrodepositable coating composition of any one of the preceding claims, wherein the electrodepositable coating composition further comprises a polyetheramine adduct.

17. An electrodepositable coating composition according to any one of the preceding claims, wherein the film-forming polymer containing ionic salt groups comprises a film-forming polymer containing cationic salt groups.

18. The electrodepositable coating composition of any one of claims 1 to 16, wherein the film-forming polymer containing ionic salt groups comprises a film-forming polymer containing anionic salt groups.

19. An electrodepositable coating composition according to any one of the preceding claims, wherein the film-forming polymer containing ionic salt groups is present in an amount of at least 39.5 wt %, or at least 50 wt %, or at least 55 wt %, or at least 60 wt % and / or no more than 90 wt %, or no more than 80 wt %, or no more than 75 wt %, based on the total weight of resin solids.

20. An electrodepositable coating composition according to any one of the preceding claims, wherein the film-forming polymer containing ionic salt groups is present in an amount of 39.5 to 90 wt %, or 39.5 to 80 wt %, or 39.5 to 75 wt %, or 50 to 90 wt %, or 50 to 80 wt %, or 50 to 75 wt %, or 55 to 90 wt %, or 55 to 80 wt %, or 55 to 75 wt %, or 60 to 90 wt %, or 60 to 80 wt %, or 60 to 75 wt %, based on the total weight of resin solids.

21. An electrodepositable coating composition according to any one of the preceding claims, wherein the curing agent is present in an amount of at least 10 wt %, or at least 20 wt %, or at least 25 wt % and / or no more than 60 wt %, or no more than 50 wt %, or no more than 45 wt %, or no more than 40 wt %, based on the total weight of resin solids.

22. An electrodepositable coating composition according to any one of the preceding claims, wherein the curing agent is present in an amount based on the total weight of resin solids: 10 wt % to 60 wt %, such as 10 wt % to 50 wt %, such as 10 wt % to 45 wt %, such as 10 wt % to 40 wt %, such as 20 wt % to 60 wt %, such as 20 wt % to 50 wt %, such as 20 wt % to 45 wt %, such as 20 wt % to 40 wt %, such as 25 wt % to 60 wt %, such as 25 wt % to 50 wt %, such as 25 wt % to 45 wt %, such as 25 wt % to 40 wt %.

23. An electrodepositable coating composition according to any one of the preceding claims, wherein the electrodepositable coating composition comprises a pigment to binder ratio of at least 0.05: 1, or at least 0.1: 1, or at least 0.2: 1, or at least 0.30: 1, or at least 0.35: 1, or at least 0.40: 1, or at least 0.50: 1, or at least 0.60: 1, or at least 0.75: 1, or at least 1: 1, or at least 1.25: 1, or at least 1.5: 1 and / or no more than 2.0: 1, or no more than 1.75: 1, or no more than 1.5: 1, or no more than 1.25: 1, or no more than 1: 1, or no more than 0.75: 1, or no more than 0.70: 1, or no more than 0.60: 1, or no more than 0.55: 1, or no more than 0.50: 1, or no more than 0.30: 1, or no more than 0.20: 1, or no more than 0.10:

1.

24. An electrodepositable coating composition according to any one of the preceding claims, wherein the electrodepositable coating composition comprises a pigment to binder ratio of from 0.05:1 to 2.0:

1.

25. A method of coating a substrate, the method comprising electrophoretically applying an electrodepositable composition according to any one of the preceding claims to at least a portion of the substrate, and at least partially curing the coating composition to form a coating.

26. A substrate coated with an electrodepositable coating composition according to any one of claims 1 to 24 in an at least partially cured state.

27. A substrate comprising a coating, wherein the coating include: (a) a polyol comprising residues of ethylene oxide and butylene oxide; (b) a film-forming polymer containing ionic salt groups; as well as (c) Curing agent.

28. The substrate of claim 26 or claim 27, wherein the coating on the substrate has an adhesion rating of at least 8.5 as measured by the White Alkyd Adhesion Test.

29. The substrate of any one of claims 26 to 28, wherein the substrate comprises a three-dimensional component formed by an additive manufacturing process.

30. The substrate of claim 29, wherein the additive manufacturing process comprises selective laser melting, electron beam melting, directed energy deposition, metal extrusion, and / or binder jetting.

Citation Information

Patent Citations

  • Amphiphilic block copolymer-modified epoxy resin and adhesives made therefrom

    CN101864261A

  • Electrodeposition of dielectric coatings on semiconductive substrates

    CN102016131A

  • Flexible coating compositions having improved scratch resistance, coated substrates and methods related thereto

    CN1377392A

  • Electrodeposition paint

    US20050256229A1

  • Electrodepositable coating composition having improved crater control

    US20180002542A1