Alloy powder, method for manufacturing a component based on said alloy, and resulting

Through metal injection molding and heat treatment technology of nickel-based alloy powder, the problem of insufficient mechanical properties of nickel-based alloy at high temperatures is solved, and components with good performance below 1000°C are produced, which are suitable for aviation components.

CN118900922APending Publication Date: 2024-11-05SAFRAN AIRCRAFT ENGINES SAS +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380023167.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-02-22
Filing Date
2023-02-20
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The existing nickel-based alloy materials are difficult to maintain mechanical properties at high temperatures, especially in turbojet engine components. The existing materials lack the working performance at above 650°C and have a strong tendency to crack, making it difficult to manufacture complex components.

Method used

Using nickel-based alloy powder, chemical composition is 14.00% to 15.25% chromium, 14.25% to 15.75% cobalt, 4.00% to 4.60% aluminum, etc., the particle size is between 3 μm and 10 μm, and the components are manufactured by metal injection molding method. , and the steps of quenching, tempering heat treatment and thermal isostatic pressing are carried out to obtain components with good tensile, fatigue and creep strength below 1000°C.

Benefits of technology

The manufacturing of nickel-based alloy parts with good mechanical properties at up to 1000°C is achieved, with controlled size and good surface finish, while being lighter than traditional nickel-based alloy parts, suitable for aviation components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118900922A_ABST
    Figure CN118900922A_ABST
Patent Text Reader

Abstract

The invention relates to nickel-based alloy powder. The nickel-based alloy powder comprises the following components in percentage by weight, the present invention relates to a copper alloy, in particular, a copper alloy, comprising 14.00% to 15.25% chromium, 14.25% to 15.75% cobalt, 4.00% to 4.60% aluminum, 0% to 0.50% iron, 0% to 0.15% manganese, 3.00% to 3.70% titanium, 3.90% to 4.50% molybdenum, 0% to 0.015% sulfur, 0% to 0.06% zirconium, 0.012% to 0.020% boron, 0% to 0.20% silicon, 0% to 0.10% copper, 0 ppm to 150 ppm carbon, 0 ppm to 0.5 ppm bismuth, 0 ppm to 5 ppm lead, 0 ppm to 1000 ppm platinum, 0 ppm to 1000 ppm palladium, 0 ppm to 50 ppm hydrogen, 0 ppm to 5 ppm silver, 0 ppm to 120 ppm nitrogen, 0 ppm to 1000 ppm rhenium, and the balance of copper. The present invention relates to a nickel-based alloy material, in particular a nickel-based alloy material, having a particle size D10 of between 3 [mu] m and 10 [mu] m, a particle size D90 of between 20 [mu] m and 40 [mu] m, a particle size D50 of between 10 [mu] m and 20 [mu] m, the values of the particle sizes D10, D50 and D90 being measured by laser diffraction according to ISO Standard 13322-2, from 0 ppm to 410 ppm of oxygen and from 0 ppm to 500 ppm of unavoidable impurities, the balance being nickel. The invention also relates to a method for manufacturing a component using said powder and to the resulting component.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a nickel-based alloy powder particularly for use in a metal injection molding manufacturing method.

[0002] The invention also relates to such a manufacturing method using this powder, and to a component, in particular for aeronautics, manufactured by this method. Background Art

[0003] In a turbojet engine, the exhaust gases generated by the combustion chamber can reach high temperatures of more than 1200° C. or even 1600° C. Therefore, turbojet engine components that come into contact with these exhaust gases, such as turbine blades, for example, must be able to maintain their mechanical properties at these high temperatures.

[0004] For this purpose, it is known that certain parts of turbojets are made of "superalloys". Superalloys, usually nickel-based, are a class of high-strength metal alloys that can operate at temperatures relatively close to their melting points (usually 0.7 to 0.9 times their melting point).

[0005] René 77 intermetallic alloys produced by casting are already used to manufacture certain turbine components. In fact, René 77 components can operate at temperatures up to 1000°C while being subjected to high fatigue, tensile and creep stresses. René 77 components also have very good oxidation and corrosion resistance at temperatures up to 1100°C.

[0006] However, nickel-based alloys that can withstand such high temperatures (eg, above 900° C.) are generally refractory materials with a strong tendency to crack.

[0007] Metal injection molding (MIM) is also known in the prior art. This method can be advantageously used to manufacture complex turbine components of desired dimensions.

[0008] Several materials are commercially available for use in manufacturing turbine components by the MIM process.

[0009] Typically, for example, nickel-based Inconel 718 is used, but the resulting components cannot operate above 650° C., which is too low for use in combustion chambers or at turbines.

[0010] Hastelloy X is another available material that allows the manufacture of components operating at temperatures up to 950°C. However, its mechanical properties are limited and it can only be used for lightly loaded components.

[0011] Therefore, there is a need to solve the above problems. Summary of the invention

[0012] An object of the present invention is therefore to propose a solution which makes it possible to obtain complex components such as, for example, turbine nozzles, turbine blades with internal channels, retaining rings or watertight components, which have controlled dimensions, are made of alloy materials having good tensile, fatigue and creep strength and oxidation / corrosion resistance up to a minimum temperature of 1000° C. and which can additionally be used in the MIM casting method.

[0013] Another object of the invention is to obtain parts for aeronautics having a good surface finish.

[0014] To this end, the present invention proposes a nickel-based alloy powder, characterized in that the nickel-based alloy powder includes, by weight percentage, 14.00% to 15.25% chromium, 14.25% to 15.75% cobalt, 4.00% to 4.60% aluminum, 0% to 0.50% iron, 0% to 0.15% manganese, 3.00% to 3.70% titanium, 3.90% to 4.50% molybdenum, 0% to 0.015% sulfur, 0% to 0.06% zirconium, 0.012% to 0.020% boron, and 0% to 0.2 0% silicon, 0% to 0.10% copper, 0 ppm to 150 ppm carbon, 0 ppm to 0.5 ppm bismuth, 0 ppm to 5 ppm lead, 0 ppm to 1000 ppm platinum, 0 ppm to 1000 ppm palladium, 0 ppm to 50 ppm hydrogen, 0 ppm to 5 ppm silver, 0 ppm to 120 ppm nitrogen, 0 ppm to 1000 ppm rhenium, 0 ppm to 410 ppm oxygen and 0 ppm to 500 ppm unavoidable impurities, the remainder being nickel, and having:

[0015] The particle size D10 is between 3 μm and 10 μm.

[0016] Particle size D90 between 20μam and 40μμm,

[0017] Particle size D50 between 10μμm and 20μμm,

[0018] The values ​​of particle size D10, D50 and D90 are measured by laser diffraction according to ISO standard 13322-2.

[0019] The chemical composition and particle size of the alloy powder are selected so that the alloy powder can be used in a powder injection molding method and at the end of the process an alloy component is obtained having good tensile, fatigue and creep strengths as well as oxidation and corrosion resistance up to 1000°C.

[0020] The invention also proposes a method for manufacturing a component, in particular for aviation, characterized in that the method comprises the following steps:

[0021] The step of mixing the nickel-based alloy powder as described above with at least one plastic binder,

[0022] a step of granulating the mixture to obtain particles of a mixture of alloy and plastic,

[0023] step of injection molding said mixture granules into a mold to obtain a green part,

[0024] a debonding step for obtaining a debonded component, and

[0025] a step of sintering the debonded component to obtain a sintered component.

[0026] This method makes it possible to obtain complex parts with controlled dimensions and good surface finish from the above alloy powders.

[0027] The process also makes it possible to obtain components with good tensile, fatigue and creep strength up to 1000°C and resistance to oxidation and corrosion, while being lighter than components made from nickel-based alloys.

[0028] According to other advantageous and non-limiting features of the invention, either alone or in combination:

[0029] The method further comprises a step of quenching the sintered component, which consists of heat treating the sintered component at a temperature between 1120°C and 1190°C, preferably between 1150°C and 1170°C, for 1 to 3 hours, preferably for 2 hours at atmospheric pressure. Preferably, the step is performed after the sintering step.

[0030] The method further comprises a tempering heat treatment step consisting of heat treating the sintered part at a temperature between 720°C and 800°C, preferably between 750°C and 770°C, for a period of between 3.5 hours and 4.5 hours, preferably 4 hours, preferably after the sintering step and the optional quenching step.

[0031] The method further comprises a hot isostatic pressing step, which consists of a heat treatment at a temperature between 1160°C and 1200°C, preferably at a temperature of 1180°C, at a pressure greater than 100 MPa and less than 200 MPa, preferably at a pressure of 110 MPa to 130 MPa, for 2 hours to 4 hours, which step is carried out after the sintering step and before the optional quenching and tempering heat treatment step.

[0032] The method further comprises a step of heat treating the sintered part at high temperature, consisting of heat treating the sintered part at atmospheric pressure at a temperature between 1200° C. and 1280° C., preferably between 1220° C. and 1240° C., for a period of between 2 hours and 6 hours, preferably for 5 hours, said step being carried out after the sintering step and after the optional hot isostatic pressing step, but before the optional multiple heat treatment steps.

[0033] The alloy volume filling ratio of the particles 3 of the mixture of plastic and alloy is between 50% and 75%, and the hot melt flow rate of the particles is between 60 cm 3 / 10 minutes to 85cm 3 / 10 minutes, and the injection temperature during the molding step is between 170°C and 200°C, the measurement of the hot melt flow rate is carried out according to ISO 1133-1.

[0034] The diameter of the particles of the mixture of alloy and plastic is between 1 mm and 5 mm.

[0035] The debonding step itself comprises two consecutive steps: a first step for primary chemical debonding of the green part, so as to obtain a partially debonded part, and a second step for thermal debonding of the partially debonded part, so as to obtain a debonded part.

[0036] The primary debonding step is catalytic debonding performed under nitrogen in the presence of nitric acid vapor at a flow rate of between 2 mL / min and 5 mL / min at a temperature between 100°C and 150°C for a period of 2 to 10 hours.

[0037] The primary detackification step is solvent detackification with demineralized water, the water being stirred at a temperature between 20°C and 100°C for a period of time between 100 hours and 300 hours.

[0038] The thermal debonding step is carried out under argon at a pressure between 200 and 500 mbar by two consecutive temperature stages, the first temperature stage lasting between 450° C. and 550° C. for 150 to 300 minutes and the second temperature stage lasting between 550° C. and 650° C. for 150 to 300 minutes.

[0039] The step of sintering the debonded part is performed by applying a temperature between 1260° C. and 1300° C. for a period of 4 to 8 hours under an argon atmosphere at a pressure of 20 to 50 mbar.

[0040] Finally, the invention relates to a nickel-based alloy component, in particular for aeronautics, characterized in that it is manufactured by a manufacturing method as described above.

[0041] According to other advantageous and non-limiting features of the invention, either alone or in combination:

[0042] The component comprises, by weight percentage, 14.00% to 15.25% chromium, 14.25% to 15.75% cobalt, 4.00% to 4.60% aluminum, 0% to 0.50% iron, 0% to 0.150% manganese, 3.00% to 3.70% titanium, 3.90% to 4.50% molybdenum, 0% to 0.015% sulfur, 0% to 0.060% zirconium, 0.012% to 0.020% boron, 0% to 0.20% silicon, 0% to 0.100% copper, and 0 ppm tantalum. to 0.5 ppm of bismuth, 0 ppm to 5 ppm of lead, 0 ppm to 1000 ppm of platinum, 0 ppm to 1000 npm of palladium, 0 ppm to 50 ppm of hydrogen, 0 ppm to 5 ppm of silver, 0 ppm to 200 ppm of nitrogen, 0 ppm to 1000 ppm of rhenium, 250 ppm to 900 ppm of carbon, 0 ppm to 500 ppm of oxygen and 0 ppm to 500 ppm of unavoidable impurities, and the remainder is nickel, and the nickel-based alloy powder also has a microstructure of metallurgical grains between ASTM 00 and ASTM 9, and the measurement of the metallurgical grain size is carried out according to ASTM E112.

[0043] The component is a turbine blade, a turbine nozzle, a retaining ring, a watertight part or a trim part. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] Other features and advantages of the present invention will be apparent from the following detailed description made with reference to the accompanying drawings, in which:

[0045] Figure 1 Shown is an electron microscope view of a René 77 component produced by casting after a series of heat treatments.

[0046] Figure 2 The various steps of the manufacturing method according to the present invention are schematically shown.

[0047] Figure 3A and Figure 3B Two optical microscope views at two different magnification scales of a component obtained at the end of the sintering step of the manufacturing method according to the invention are respectively shown.

[0048] Figure 4A and Figure 4BTwo optical microscope views at two different magnification scales of a component obtained at the end of a hot isostatic pressing (HIP) step of the manufacturing method according to the invention, which step has been carried out after a sintering step, are shown.

[0049] Figure 5A and Figure 5B Two optical microscope views at two different magnification scales of a component obtained at the end of a high-temperature heat treatment step of a manufacturing method according to the invention, which has been carried out after a hot isostatic pressing (HIP) step, are shown. DETAILED DESCRIPTION

[0050] René 77 alloy produced by casting includes, by weight, 0.05% to 0.09% carbon, 14.25% to 15.75% cobalt, 14.00% to 15.25% chromium, 4.00% to 4.60% aluminum, 3.90% to 4.50% molybdenum, 3.00% to 3.70% titanium, less than 0.50% iron, 0.012% to 0.020% boron, and 0.0 0.06% zirconium, 0 to 0.15% manganese, 0 to 0.20% silicon, 0 to 0.10% copper, 0 to 0.015% sulfur, less than 0.5 ppm bismuth, less than 5 ppm silver, less than 5 ppm lead, less than 25 ppm nitrogen, less than 1000 ppm platinum, less than 1000 ppm rhenium and less than 1000 ppm palladium, the rest being nickel as the alloy basis and unavoidable impurities.

[0051] The microstructure of René 77 produced by casting has metallurgical grains with a size less than or equal to ASTM 00. Figure 1 is a schematic diagram of the microstructure of this René 77 produced by casting, with grain measurements as ASTM 00. Figure 1 At the bottom left, one of the metallurgical grains can be distinguished in a darker grey. The measurement of metallurgical grain size was performed according to ASTM Standard E112.

[0052] The René 77 intermetallic alloy has interesting mechanical and chemical properties for applications in the turbine sector. In fact, René 77 components produced by casting maintain good mechanical, creep, fatigue and tensile strength up to 1000°C, as well as good corrosion and oxidation resistance up to 1100°C. By way of example, for temperatures below 800°C, the ultimate stress leading to tensile failure R of René 77 components produced by casting is m Greater than 650 MPa. In the same temperature range, for stresses greater than 500 MPa and elongation at break greater than 2%, the elastic limit Rp at 0.2% residual plastic deformation of the component is reached 0.2 .

[0053] On the other hand, metal powder injection molding makes it possible to obtain parts of complex shape with excellent surface finish and to finely control the dimensions of said parts. Metal powder injection molding is also a method that is notable for the speed with which it is implemented.

[0054] The present invention relates to an alloy powder and to a method, the parameters of which have been selected so as to obtain from the alloy powder, at the end of the process, a component which advantageously combines the properties of a René 77 alloy component and those of a component produced by a metal powder injection molding method.

[0055] The MIM method is a method of molding components by injecting a mixture of metal powder and plastic binder into a mold. The strength of the injection-molded component is ensured by the plastic binder. The plastic binder is removed in a subsequent step called the debinding step. The debinded component is fragile because it is very porous. An additional sintering step is necessary, during which the microparticles of the metal powder are bonded together.

[0056] Nickel Alloy Powders for Metal Powder Injection Molding

[0057] The invention relates to a nickel-based metal alloy powder. The chemical composition and particle size of the alloy powder have been selected to allow its use in a metal injection molding (MIM) process and to obtain, at the end of the process, a nickel-based alloy component whose chemical composition and mechanical properties are close to those of the cast René 77 alloy.

[0058] Chemical composition of powder

[0059] Although the plastic binder is almost completely removed during the above-mentioned debinding step, remnants of the plastic binder impregnate the metal material.The nitrogen, oxygen and carbon levels in the molded parts produced by the powder injection molding process are higher than those in the powder injected at the beginning of the process.

[0060] However, the carbon, nitrogen and oxygen levels given in the René 77 specification are relatively low compared to the expected mechanical properties. High carbon content, for example, leads to the formation of carbides at grain boundaries, which hinder the growth and movement of the grains. The component then has poor ductility and may break during use. High levels of oxygen and nitrogen also lead to reduced ductility of the component and rapid fracture under fatigue and tensile stresses.

[0061] Therefore, the contents of the various elements of the alloy powder of the present invention, particularly the contents of nitrogen, oxygen and carbon, are selected accordingly.

[0062] The alloy powder according to the present invention comprises, by weight percentage, 14.00% to 15.25% chromium, 14.25% to 15.75% cobalt, 4.00% to 4.60% aluminum, 0% to 0.50% iron, 0% to 0.15% manganese, 3.00% to 3.70% titanium, 3.90% to 4.50% molybdenum, 0% to 0.015% sulfur, 0% to 0.06% zirconium, 0.012% to 0.020% boron, 0% to 0.20% silicon, 0% To 0.10% copper, 0ppm to 150ppm carbon, 0ppm to 0.5ppm bismuth, 0ppm to 5ppm lead, 0ppm to 1000ppm platinum, 0ppm to 1000ppm palladium, 0ppm to 50ppm hydrogen, 0ppm to 5ppm silver, 0ppm to 120ppm nitrogen, 0ppm to 1000ppm rhenium, 0ppm to 410ppm oxygen and 0ppm to 500ppm unavoidable impurities, the rest is nickel.

[0063] "Unavoidable impurities" are defined as elements that are not intentionally added to the powder composition and are provided by other elements. As unavoidable impurities, for example, yttrium may be mentioned, which may come from the crucible used to atomize the powder.

[0064] The alloy powder according to the present invention includes, in terms of weight percentage, between 0 and 50 ppm of each element considered to constitute inevitable impurities.

[0065] Powder particle size

[0066] The particle size of the powder has been chosen such that the powder can be used in the manufacturing method described below, in particular during the injection molding and sintering steps.

[0067] The implementation of the powder injection molding process requires control of the powder particle size to ensure good injection of the alloy powder and plastic binder mixture into the mold of the component. In fact, small alloy powder particles cause a large contact interface between the alloy powder and the plastic binder within the alloy powder / plastic binder mixture and thus cause high friction during injection of the mixture into the mold of the component. On the contrary, too large alloy powder particles are more difficult to be carried by the plastic binder during the injection process and thus may result in uneven injection molded parts.

[0068] Furthermore, the particle size is important to obtain good sintering, during the sintering step the particles will diffuse and combine with each other to eliminate their interfaces and thus reduce their entropy. Thus, fine powders will sinter more easily, since by agglomeration the small powder particles will more strongly reduce their interfaces and their surface, causing their entropy to drop significantly.

[0069] Therefore, the particle size of the alloy powder of the present invention is defined by the range of acceptable values ​​of the particle sizes D10, D50 and D90 of the alloy powder.

[0070] The particle size D10 corresponds to a pass rate of 10%. In other words, 10% by number of the particles of the alloy powder have a diameter smaller than D10. Likewise, the particle sizes D50 and D90 correspond to pass rates of 50% and 90%, respectively.

[0071] The particle size D10 of the alloy powder according to the present invention is between 3 μm and 10 μm, the particle size D50 is between 10 μm and 20 μm, and finally, the particle size D90 is between 20 μm and 40 μm.

[0072] The values ​​of particle size D10, D50 and D90 are measured according to ISO standard 13322-2. This standard provides measurement results by laser diffraction.

[0073] Powder preparation

[0074] For example, the nickel-based alloy powder that is the subject of the present invention can be obtained from the René 77 alloy basic element by a powder atomization method. The atomization method provides the chemical composition and particle size of the alloy powder obtained. In addition, it ensures a good morphology of the powder, mainly spherical. Finally, it makes it possible to limit the risk of contamination.

[0075] Metal powder injection molding method

[0076] The invention also relates to a method for manufacturing a component, in particular a component for aeronautics, using a nickel-based alloy powder as defined above.

[0077] Typically, the method includes the sequential steps of mixing, granulation, injection molding, chemical debonding, thermal debonding, sintering and quenching. Optionally, the method may also include one or more additional heat treatment steps. Figure 2 Describe these steps in more detail.

[0078] mix

[0079] In a first mixing step E1, a nickel-based alloy powder 1 according to the invention is mixed with at least one plastic binder 2, preferably two plastic binders. This binder 2 is, for example, polyethylene (PE) or polyethylene glycol (PEG) or a mixture of both. During the mixing step E1, the temperature is set to a value that makes the plastic paste-like to allow good mixing. The temperature depends on the composition of the plastic and is, for example, between 50° C. and 150° C. During the mixing step E1, the titanium-based alloy powder 1 and the plastic binder 2 are mixed in a proportion chosen so as to obtain, at the end of the granulation step E2 described below, a mixture of plastic and alloy particles 3 having a hot melt flow rate that ensures efficient injection of said particles 3 during the molding step E3. Preferably, the mixture of alloy powder 1 and at least one plastic binder 2 comprises, by volume, between 50% and 75% of alloy powder 1 and between 50% and 25% of plastic binder 2, so that the particles 3 of the mixture have a flow rate of 1.5 to 2.5% at 60 cm 3 / 10 minutes to 85cm 3 The hot melt flow rate is measured according to ISO standard 1133-1.

[0080] Granulation

[0081] In a second step E2 of granulating the mixture of alloy powder and at least one plastic binder, the mixture from step E1 is passed through an extruder to obtain granules 3 of a mixture of plastic and alloy, which are raw materials known to those skilled in the art. The shape and size of the granules 3 of the mixture of plastic and alloy are fixed by the extruder settings. The granules 3 of the mixture of plastic and alloy are, for example, cylinders with a base diameter preferably between 1 mm and 5 mm.

[0082] forming

[0083] In a third molding step E3, the mixture of plastic and alloy granules 3 is injected into the mold of the part to be manufactured, the injection temperature being between 170° C. and 200° C. Below 170° C., the mixture is too solid and does not enter the mold. Above 200° C., the mixture is too liquid and the alloy powder and the plastic binder separate without carrying the alloy powder. Other parameters, such as injection speed, injection pressure, holding time after injection or injection time, depend on the part to be molded.

[0084] After the forming step E3, a green part 4 is obtained, which is a part of mixed alloy powder and plastic (alloy particles suspended in plastic). By adjusting the forming parameters, it is possible to obtain a part without pores. The plastic binder ensures the strength of the part.

[0085] Debonding

[0086] Debinding makes it possible to remove the plastic binder from the green part 4 previously obtained.

[0087] Two debonding steps are performed consecutively, one chemical and the other thermal.

[0088] Primary debonding

[0089] The preliminary debonding step E4 is a debonding of a chemical nature. The preliminary debonding step E4 makes it possible to obtain a partially debonded part 5 .

[0090] This debonding can be either: a debonding step using a solvent E4B, or preferably a catalytic debonding step E4A. The latter has the advantage of being faster.

[0091] The catalytic debinding step E4A consists of evaporating and then burning the plastic binder by injecting acid vapors in an oven.

[0092] For example, the catalytic debonding is performed in a nitrogen atmosphere in the presence of nitric acid vapor at a temperature of 100° C. to 150° C. for 2 to 10 hours, preferably, the nitric acid flow rate is 2 mL / min to 5 mL / min.

[0093] The debinding step E4B using a solvent consists of bathing the green part 4 in a bath of said solvent in order to dissolve the plastic.

[0094] The debinding step E4B is, for example, a water debinding, the green part 4 being immersed in a bath of demineralized water for 100 to 300 hours and stirred at a temperature ranging from 20°C to 100°C, preferably at about 60°C.

[0095] At the end of the chemical debonding step E4 , a partially debonded part 5 is obtained, the chemical debonding making it possible to remove more than 95% of the plastic binder.

[0096] Thermal debonding

[0097] Preferably, the thermal debonding step E5 is carried out under an argon atmosphere at a pressure between 200 and 500 mbar by applying two temperature stages successively to the partially debonded part 5. During the first stage, a temperature between 450° C. and 550° C. is applied for 150 to 300 minutes. During the second stage, a temperature comprised between 550° C. and 650° C. is applied for 150 to 300 minutes.

[0098] At the end of the thermal debonding step ( E5 ), which made it possible to remove the remaining plastic binder (ie less than 5% remaining), a debonded part or “brown part” 6 is obtained.

[0099] The debonded part 6 resulting from the primary debonding step E4 and the thermal debonding step E5 is a part of the same dimensions as the green part 4. However, unlike the green part 4, the debonded part 6 is very porous, since the plastic binder has been removed, and the density of the debonded part 6 is between 50% and 75% of the density of a René 77 alloy part produced by casting. In addition, the debonded part 6 is very fragile, since the plastic binder that ensures the strength of the part has been removed.

[0100] sintering

[0101] During step E6, the debonded component 6 is sintered. Sintering consists of subjecting the debonded component 6 to a temperature close to the melting point of the alloy powder, so that the powder particles bind together. During sintering, the component shrinks and its density increases.

[0102] Preferably, sintering is performed in a furnace under an argon atmosphere at a pressure of 20 to 50 mbar at a temperature of 1260 to 1300° C. for 4 to 6 hours.

[0103] Preferably, the thermal debonding step E5 and the sintering step E6 are carried out in the same furnace, since the debonded part 6 is fragile.

[0104] At the end of the sintering step E6, a more compact sintered part 7 is obtained, the density of which is preferably greater than 95% of the density of a conventional René 77 alloy from casting. The dimensions of the sintered part 7 are smaller than those of the debonded part or brown part 6. Typically, a size reduction of 14% to 18% is observed.

[0105] The sintered nickel-based alloy component 7 includes, by weight percentage, 14.00% to 15.25% chromium, 14.25% to 15.75% cobalt, 4.00% to 4.60% aluminum, 0% to 0.50% iron, 0% to 0.150% manganese, 3.00% to 3.70% titanium, 3.90% to 4.50% molybdenum, 0% to 0.015% sulfur, 0% to 0.060% zirconium, 0.012% to 0.020% boron, 0% to 0.20% silicon, and 0% to 0. 100% copper, 0ppm to 0.5ppm bismuth, 0ppm to 5ppm lead, 0ppm to 1000ppm platinum, 0ppm to 1000ppm palladium, 0ppm to 50ppm hydrogen, 0ppm to 5ppm silver, 0ppm to 200ppm nitrogen, 0ppm to 1000ppm rhenium, 250ppm to 900ppm carbon, 0ppm to 500ppm oxygen and 0ppm to 500ppm inevitable impurities, and the remainder is nickel. In particular, the sintered nickel-based alloy component 7 includes, by weight percentage, between 0 and 50ppm of each element considered to constitute inevitable impurities.

[0106] The chemical composition of the sintered component 7 is very close to that of the initial alloy powder. During the MIM process, only the carbon, oxygen and nitrogen levels increase significantly. By way of example, if the alloy powder 1 comprises 250 ppm oxygen, 20 ppm nitrogen and 700 ppm carbon, the sintered component 7 obtained from the alloy powder 1 by the method according to the invention comprises 270 ppm oxygen, 100 ppm nitrogen and 1100 ppm carbon.

[0107] The additional carbon, oxygen and nitrogen elements are residues of the plastic binder of the impregnated metal material. However, too high a proportion of said elements can have a negative impact on the mechanical properties of the alloy component produced by the MIM process. The carbon, oxygen and nitrogen content of alloy powder 1 must be much lower than the target René 77.

[0108] Figure 3A and Figure 3B Two optical microscope views at two different magnifications of a sintered component 7 obtained at the end of the sintering step according to the method of the invention are shown. Recorded after chemical etching to improve phase contrast Figure 3A and Figure 3B In the figure, the characteristic microstructure of nickel-based alloys is observed. The metallurgical grains, which appear as gray areas (the contrast of which varies from grain to grain), are bound and the material is relatively dense. However, the material also includes porosity residues (note the small round and black dots), which affect the mechanical properties of the final part. Heat treatment, such as hot isostatic pressing, can be used to eliminate the porosity residues.

[0109] In addition, the size of the metallurgical grains within the sintered component 7 is relatively small, between ASTM 5 and ASTM 9. The metallurgical grains are measured according to ASTM Standard E112. By way of example, Figure 3A and Figure 3B The grain size of the microstructure is ASTM 6. Components consisting of small metallurgical grains have good fatigue resistance, but poor creep resistance. Depending on the intended application of the manufactured component, a high temperature heat treatment can be applied to increase the size of the metallurgical grains of the component. The conditions of the treatment are selected to ensure fatigue, creep and tensile properties according to the intended application.

[0110] Hot Isostatic Pressing

[0111] Optionally, a hot isostatic pressing step E7 of the sintered part 7 can be carried out in order to fill the residual porosity, in particular if the density of the sintered part is less than 95% of the density of the René 77 alloy from casting. The hot isostatic pressing step E7 makes it possible to increase the density of the part 7 resulting from sintering to 100% of the density of the René 77 from casting and to improve the mechanical properties of said part. Furthermore, the hot isostatic pressing step reduces the dimensional scatter of the parts produced by the metal powder injection molding method.

[0112] During the hot isostatic pressing step E7, high pressure and temperature are applied simultaneously in an inert atmosphere. For example, a temperature between 1160° C. and 1200° C. (preferably a temperature of 1180° C.) and a pressure greater than 100 MPa and less than 200 MPa (preferably between 110 MPa and 130 MPa) are applied in an inert atmosphere, such as a helium atmosphere or a vacuum, preferably an argon atmosphere, for 2 to 4 hours.

[0113] Figure 4A and Figure 4B Are two optical microscope views at two different magnifications of the part obtained at the end of steps E6 and E7 of the method according to the invention. The microstructure of the nickel alloy is recognizable, but the points are no longer distinguishable. Thus, step E7 of hot isostatic pressing makes it possible to plug the last pores and obtain a perfectly healthy material.

[0114] High temperature heat treatment

[0115] Optionally, a step E8 of heat treatment at high temperature may be performed on the sintered part. If the hot isostatic pressing step E7 is performed, preferably, a high temperature heat treatment step E8 is performed after said step E7.

[0116] The high temperature heat treatment E8 consists of heating the part to a temperature sufficient to enlarge the metallurgical grains. In fact, under the effect of the temperature, the grains agglomerate, limiting their interfaces and thus reducing their potential energy. The agglomeration of the initial metallurgical grains leads to larger metallurgical grains. The temperature is a kinetic factor: the application of high temperatures increases the speed of the grain agglomeration.

[0117] The high temperature heat treatment step E8 is advantageously carried out for manufacturing parts that will be subjected to high creep stresses such as, for example, turbine blades and turbine nozzles. In fact, the larger the metallurgical grains, the easier it is for them to slide between each other under the effect of creep stresses, and therefore the better the resistance of the part to said stresses.

[0118] Preferably, the high temperature heat treatment step E8 comprises, at atmospheric pressure, under an inert atmosphere (for example under an argon atmosphere), applying a temperature between 1200°C and 1280°C, more preferably between 1220°C and 1240°C, for a period of time between 2 hours and 6 hours, more preferably for 5 hours.

[0119] After carrying out said step E8 under the conditions thus described, the size of the metallurgical grains is between ASTM 00 and ASTM 5, with an average of ASTM 2. As mentioned above, at the end of the sintering step E6, the grain size is between ASTM 5 and ASTM 9. The grain size is thus increased. Figure 5A and Figure 5B are two optical microscope views at two different magnifications of the component obtained at the end of steps E6, E7 and then E8 of the method according to the invention. Figure 5A and Figure 5B The microstructure of the component after step E7 and before step E8 of the method Figure 4A and Figure 4B By comparing the microstructure in , it can be seen that the grain size has actually increased during the high temperature heat treatment step E8. By way of example, Figure 4A and Figure 4B The grain size of the microstructure represented is ASTM 2.

[0120] Increasing the grain size during step E8 improves the creep strength of the component while ensuring good fatigue and tensile strength of the component.

[0121] Quenching

[0122] In addition, a quenching heat treatment step E9 is performed. The quenching heat treatment consists of heating the part to a temperature at which the good alloying elements constituting nickel are dissolved for a sufficient time to allow said elements to redissolve and diffuse into the crystalline solid. The part is then cooled relatively quickly so that said good alloying elements reprecipitate. This step makes it possible to obtain a part having the desired mechanical and chemical properties.

[0123] The quenching heat treatment step E9 is at a temperature between 1120° C. and 1190° C., more preferably comprised at a temperature between 1150° C. and 1170° C., for a period of time between 1 hour and 3 hours, more preferably for 2 hours. The part is finally cooled at an average rate between 47° C. / hour and 67° C. / hour until it reaches a temperature between 1070° C. and 1090° C., preferably 1080° C., and then cooled at an average rate greater than or equal to 16° C. / minute. Throughout the quenching heat treatment step E9, which consists of heating and then cooling the part, the inert atmosphere (for example an argon atmosphere) is maintained at atmospheric pressure, or the step is carried out under vacuum.

[0124] Tempering heat treatment

[0125] Finally, a tempering heat treatment step E10 is carried out. During the tempering heat treatment E10, some alloying elements are precipitated at the grain boundaries. The tempering heat treatment E10 makes it possible to obtain the desired mechanical properties of the alloy component manufactured. The treatment E10 makes it possible in particular to increase the tensile strength of the component manufactured.

[0126] The tempering heat treatment step E10 comprises applying a temperature between 720° C. and 800° C., preferably between 750° C. and 770° C., in air for between 3.5 hours and 4.5 hours, preferably for 4 hours. Exemplarily, under such conditions in which the tempering heat treatment E10 is carried out, an increase in stress intensity of 20% is observed.

[0127] The parts obtained by this method

[0128] The invention also relates to a component obtained by a manufacturing method using the alloy powder 1 according to the invention.

[0129] The component is a nickel-based alloy component, in particular comprising, in weight percentage, between 250 ppm and 900 ppm carbon, less than 200 ppm nitrogen and less than 500 ppm oxygen, the chemical composition being measured by elemental analysis, for example by inductively coupled plasma spectroscopy.

[0130] exist Figure 1 , which shows a part made of René 77 produced by casting, the latter having, as mentioned above, a microstructure with grains of size ASTM 00. If the metallurgical grain size of the René 77 alloy produced by casting is less than or equal to ASTM 00, the metallurgical grain size of the part obtained from the manufacturing method using alloy powder 1 according to the invention is between ASTM 00 and ASTM 9. For example, for a part obtained at the end of sintering step E6, its microstructure is between Figure 3A and Figure 3B As can be seen in the figure, the grain size is 6ASTM. Figure 5A and Figure 5B The parts obtained at the end of the high temperature heat treatment step E8 have a grain size of ASTM 2. Therefore, the parts obtained by the manufacturing method using the alloy powder according to the invention have a microstructure with metallurgical grains smaller than those in the René 77 alloy from casting; this gives them better tensile strength and fatigue resistance than René 77 parts produced by casting.

[0131] R m is the ultimate stress value that causes tensile failure R m , Rp0.2 is the stress value when the elastic limit is reached at a residual plastic deformation of 0.2% and a fracture elongation value of A%. R of the component manufactured according to the method using the alloy powder 1 according to the present invention m , Rp 0.2 and A% values, the method comprising steps E1 to E7, then E9 and E10 as described above, compared to the R of the René 77 part produced by casting m , Rp 0.2 As well as the A% value, it has increased by about 30%. In addition, the fatigue gain is about 20%.

[0132] R of a component manufactured according to the method using the alloy powder 1 according to the present invention m , Rp 0.2 and A% value, the method further comprising step E8 as described above, is about 15% compared to a René 77 part produced by casting. In this case, the fatigue gain is about 10%.

[0133] The invention finds particular application in the manufacture of parts for aviation, such as, for example, turbine blades, including blades with internal channels, turbine nozzles, retaining rings, watertight parts or trim parts, which are subjected to high tensile, high fatigue and high creep stresses, must resist corrosion and oxidation, and are used at high temperatures above 1000°C.

Claims

1. A nickel-based alloy powder (1), characterized in that: The nickel-based alloy powder (1) comprises, by weight percentage, 14.00% to 15.25% of chromium, 14.25% to 15.75% of cobalt, 4.00% to 4.60% of aluminum, 0% to 0.50% of iron, 0% to 0.15% of manganese, 3.00% to 3.70% of titanium, 3.90% to 4.50% of molybdenum, 0% to 0.015% of sulfur, 0% to 0.06% of zirconium, 0.012% to 0.020% of boron, 0% to 0.20% of silicon, 0% to 0.1 0% copper, 0 ppm to 150 ppm carbon, 0 ppm to 0.5 ppm bismuth, 0 ppm to 5 ppm lead, 0 ppm to 1000 ppm platinum, 0 ppm to 1000 ppm palladium, 0 ppm to 50 ppm hydrogen, 0 ppm to 5 ppm silver, 0 ppm to 120 ppm nitrogen, 0 ppm to 1000 ppm rhenium, 0 ppm to 410 ppm oxygen and 0 ppm to 500 ppm unavoidable impurities, the remainder being nickel, and having: The particle size D10 is between 3 μm and 10 μm. A particle size D90 between 20 μm and 40 μm, and Particle size D50 between 10 μm and 20 μm, The values ​​of particle size D10, D50 and D90 are measured by laser diffraction according to ISO standard 13322-2.

2. A method for manufacturing a component, in particular for aviation, characterized in that: The method comprises the following steps: step (E1) of mixing the nickel-based alloy powder according to claim 1 with at least one plastic binder (2), step (E2) of granulating the mixture to obtain particles (3) of a mixture of alloy and plastic, step (E3) of injection molding the mixture granules (3) into a mold to obtain a green part (4), a debonding step (E4A, E4B, E5) to obtain a debonded part (6), and A step (E6) of sintering the debonded part to obtain a sintered part (7).

3. The method according to claim 2, characterized in that The method further comprises a step (E9) of quenching the sintered component (7), which step (E9) consists of heat treating the sintered component (7) at atmospheric pressure at a temperature between 1120° C. and 1190° C., preferably between 1150° C. and 1170° C., for a period of 1 to 3 hours, preferably 2 hours, and this step is performed after the sintering step (E6).

4. The method according to any one of claims 2 or 3, characterized in that The method further comprises a tempering heat treatment step (E10) consisting of subjecting the sintered component (7) to a heat treatment at a temperature between 720° C. and 800° C., preferably between 750° C. and 770° C., for a period of between 3.5 hours and 4.5 hours, preferably 4 hours, this step being carried out after the sintering step (E6) and the optional quenching step (E9).

5. The method according to any one of claims 2 to 4, characterized in that The method also comprises a hot isostatic pressing step (E7), which consists of a heat treatment at a temperature between 1160°C and 1200°C, preferably at a temperature of 1180°C, at a pressure greater than 100 MPa and less than 200 MPa, preferably at a pressure of 110 MPa to 130 MPa, for 2 hours to 4 hours, this step being carried out after the sintering step (E6) and before the optional quenching step (E9) and the tempering heat treatment step (E10).

6. The method according to any one of claims 2 to 5, characterized in that The method further comprises a step (E8) of heat treating the sintered component (7) at high temperature, which step (E8) consists of heat treating the sintered component (7) at atmospheric pressure at a temperature between 1200°C and 1280°C, preferably between 1220°C and 1240°C, for a period of time between 2 hours and 6 hours, preferably 5 hours, and this step is carried out after the sintering step (E6) and after the optional hot isostatic pressing step (E7), but before the optional heat treatment step (E9) and the heat treatment step (E10).

7. The method according to any one of claims 2 to 6, characterized in that The alloy volume filling ratio of the particles (3) of the mixture of plastic and alloy is between 50% and 75%, and the hot melt flow rate of the particles (3) is between 60 cm 3 / 10 minutes to 85cm 3 / 10 minutes, and the injection temperature during the molding step (E3) is between 170°C and 200°C, the measurement of the hot melt flow rate is carried out according to ISO 1133-1.

8. The method according to any one of claims 2 to 7, characterized in that The diameter of the particles of the mixture of plastic and alloy is between 1 mm and 5 mm.

9. The method according to any one of claims 2 to 8, characterized in that The debonding step (E4A, E4B, E5) itself comprises two consecutive steps: a first step (E4A, E4B) for primary chemical debonding of the green part (4) to obtain a partially debonded part (5), and a second step (E5) for thermal debonding of the partially debonded part (5) to obtain a debonded part.

10. The method according to claim 9, characterized in that The primary debonding step is catalytic debonding (E4A) carried out under nitrogen in the presence of nitric acid vapor for a period of 2 hours to 10 hours, with a flow rate of nitric acid vapor between 2 mL / min and 5 mL / min at a temperature between 100°C and 150°C.

11. The method according to claim 9, characterized in that The primary detackification step is solvent detackification (E4B) with demineralized water, the water being stirred at a temperature between 20° C. and 100° C. for a period of time between 100 hours and 300 hours.

12. The method according to any one of claims 9 to 11, characterized in that The thermal debonding step (E5) is carried out under argon at a pressure between 200 and 500 mbar by means of two consecutive temperature stages, the first being between 450° C. and 550° C. for a duration of 150 to 300 minutes and the second being between 550° C. and 650° C. for a duration of 150 to 300 minutes.

13. The method according to any one of claims 2 to 12, characterized in that The step (E6) of sintering the debonded part is carried out by applying a temperature between 1260°C and 1300°C under an argon atmosphere at a pressure of 20 to 50 mbar for a period of time comprised between 4 and 8 hours.

14. A nickel-based alloy component, particularly for aviation, characterized in that: The component is manufactured by the manufacturing method according to any one of claims 2 to 13.

15. The component according to claim 14, characterized in that The component includes, by weight percentage, 14.00% to 15.25% chromium, 14.25% to 15.75% cobalt, 4.00% to 4.60% aluminum, 0% to 0.50% iron, 0% to 0.150% manganese, 3.00% to 3.70% titanium, 3.90% to 4.50% molybdenum, 0% to 0.015% sulfur, 0% to 0.060% zirconium, 0.012% to 0.020% boron, 0% to 0.20% silicon, 0% to 0.100% copper, 0ppm to 0.5ppm of bismuth, 0ppm to 5ppm of lead, 0ppm to 1000ppm of platinum, 0ppm to 1000ppm of palladium, 0ppm to 50ppm of hydrogen, 0ppm to 5ppm of silver, 0ppm to 200ppm of nitrogen, 0ppm to 1000ppm of rhenium, 250ppm to 900ppm of carbon, 0ppm to 500ppm of oxygen and 0ppm to 500ppm of unavoidable impurities, the remainder being nickel, and the component also has a microstructure of a metallurgical grain between ASTM00 and ASTM 9, and the measurement of the metallurgical grain size is carried out according to ASTM E112.

16. A component according to claim 14 or 15, characterized in that The component is a turbine blade, a turbine nozzle, a retaining ring, a watertight component or a trim component.