A method for preparing a black niobium oxide photocatalytic material and the product obtained therefrom

The NbOyHx+NbO2.5 biphase niobium oxide photocatalyst was prepared by solvothermal reaction and low-temperature calcination, which solved the problem of the difficulty in preparing black niobium oxide photocatalysts in the prior art and achieved a high efficiency improvement in photocatalytic performance.

CN118904326BActive Publication Date: 2026-11-17JINGDEZHEN CERAMIC UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410953275.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2026-11-17
Estimated Expiration
2044-07-16

AI Technical Summary

Technical Problem

Existing technologies make it difficult to prepare efficient black niobium oxide photocatalysts easily and quickly, especially since H doping in niobium oxide materials is difficult to achieve, resulting in low visible light absorption and insufficient photocatalytic efficiency.

Method used

Using niobium oxide nanopowder, NbCl5, NaH, or CaH2 as raw materials, a biphase niobium oxide photocatalytic material with a structure of NbOyHx+NbO2.5 was prepared through solvothermal reaction and low-temperature calcination. By changing the reactant ratio and heat treatment under a hydrogen atmosphere, its photocatalytic activity was significantly improved.

Benefits of technology

The photocatalytic activity of niobium oxide photocatalyst was significantly improved, making its hydrogen evolution rate 25 to 35 times that of pure NbO2.5, and the preparation method is simple and easy to implement.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118904326B_ABST
    Figure CN118904326B_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing a black niobium oxide photocatalytic material and the product obtained therefrom. Using niobium oxide nanopowder, NbCl5, NaH, or CaH2 as raw materials, NbCl5 is reacted with NaH or CaH2 via a solvothermal reaction to form NbH... x Cl 5‑x NbO was prepared by uniformly depositing niobium oxide on the surface of nano-sized particles, followed by hydrolysis and ethanol washing, and then calcining the resulting precipitate at low temperature in a hydrogen atmosphere. y H2+NbO 2.5 The biphase structure of niobium oxide photocatalyst significantly improves the photocatalytic activity of niobium oxide materials. The preparation method of this invention is simple, rapid, and operates under mild conditions, making it easy to implement and providing a new approach for the preparation of black niobium oxide photocatalysts.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of photocatalyst materials technology, and in particular to a method for preparing H-doped black niobium oxide photocatalyst material and the product obtained therefrom. Background Technology

[0002] Niobium oxide is a wide-bandgap intrinsic semiconductor, appearing as a white powder. It is a non-toxic and highly efficient photocatalyst, capable of decomposing water to produce hydrogen or organic matter in the air (formaldehyde, toluene, etc.). To narrow the bandgap of niobium oxide and improve its photocatalytic efficiency, enabling it to respond to visible light, various synthetic methods have been used to prepare niobates (such as KNbO3 and InNbO3), and niobium oxide has been modified by doping with various ions, with the effects tested. Numerous studies have shown that (1) wide-bandgap niobates have very weak absorption of visible light; (2) doping niobium oxide with anions can effectively narrow its bandgap. For example, when N is doped into niobium oxide at a certain concentration, it can turn niobium oxide yellow, effectively improving its absorption rate of visible light; when H is doped into niobium oxide at a certain concentration, it can turn niobium oxide into blue-gray (near black), narrowing the bandgap of niobium oxide to 0.5 eV, greatly improving the photoelectric conversion efficiency of niobium oxide. Hydrogen doping of oxides, such as titanium dioxide and niobium oxide, can not only improve their conductivity and significantly reduce their band gap, but also significantly improve their photoelectric conversion efficiency. Currently, high-pressure hydrogen reaction is widely used industrially to prepare hydrides such as MgH2, CaH2, TiH2, and ZrH2. High-pressure hydrogen doping of titanium dioxide has been very successful, producing black titanium dioxide with good photocatalytic performance in the ultraviolet region. However, when this method is applied to niobium oxide, hydrogen doping is difficult to achieve (the Nb-O chemical bond is relatively stable). Currently, a palladium reduction method for preparing black niobium oxide photocatalysts has been reported abroad, but its efficiency is low due to limitations in equipment or preparation conditions. Therefore, a simple, rapid, and easily implemented new method for preparing black niobium oxide photocatalysts is needed. Summary of the Invention

[0003] The purpose of this invention is to overcome the shortcomings of the prior art and provide a method for preparing a black niobium oxide photocatalytic material. Using niobium oxide nanopowder, NbCl5, NaH, or CaH2 as raw materials, a solvothermal reaction is performed where NbCl5 reacts with NaH or CaH2 to form NbH... x Cl 5-x NbO was prepared by uniformly depositing niobium oxide on the surface of nano-sized particles, followed by hydrolysis and ethanol washing, and then calcining the resulting precipitate at low temperature in a hydrogen atmosphere. y H2+NbO 2.5A dual-phase niobium oxide photocatalytic material is provided to significantly improve the photocatalytic activity of niobium oxide materials. Another object of the present invention is to provide a product prepared using the above-described method.

[0004] The objective of this invention is achieved through the following technical solution:

[0005] The present invention provides a method for preparing a black niobium oxide photocatalytic material, comprising the following steps:

[0006] (1) Niobium oxide nanopowder : NbCl5 : NaH or CaH2 : anhydrous toluene = 10-30g : 1-5g : 0.2-1g : 100-200mL, and mix at room temperature to obtain a reaction solution;

[0007] (2) The reaction solution is placed in a reaction vessel and subjected to a solvothermal reaction at 180–220°C for 5–15 h, allowing NbCl5 to dissolve in anhydrous toluene and react with NaH or CaH2. After the reaction is complete, the solution is filtered and collected to obtain NbH2. x Cl 5-x (x = 0.1~2) Precursor powder uniformly deposited on the surface of niobium oxide particles;

[0008] (3) The precursor powder is added to an aqueous solution of NH3 with a concentration of 0.5–2 mol / L, so that NbH x Cl 5-x (x = 0.1–2) Hydrolysis was performed, and the resulting precipitate was washed with anhydrous ethanol and then transferred to a hydrogen furnace for heat treatment at 250–350 °C in a hydrogen atmosphere for 1–2 hours to obtain NbO. y H x +NbO 2.5 (x=0.1~2) Biphase structure niobium oxide photocatalytic material.

[0009] The product prepared using the above-described method for preparing black niobium oxide photocatalytic material, wherein the NbO y H x +NbO 2.5 In the photocatalytic water splitting reaction to produce hydrogen, the hydrogen evolution rate of the biphase niobium oxide photocatalyst is higher than that of pure NbO. 2.5 25 to 35 times.

[0010] The present invention has the following beneficial effects:

[0011] This invention utilizes a simple solvothermal reaction and chemical precipitation method. By altering the ratio of NbCl5, NaH or CaH2, and niobium oxide nanoparticles in the reactants, and through low-temperature calcination under a hydrogen atmosphere, a biphase structure of black niobium oxide nanocatalyst is prepared, significantly improving the photocatalytic activity of niobium oxide. The preparation method of this invention is simple, rapid, and operates under mild conditions, providing a new approach for the preparation of black niobium oxide photocatalysts. Attached Figure Description

[0012] The present invention will now be described in further detail with reference to the embodiments and accompanying drawings:

[0013] Figure 1 The NbO prepared according to the embodiments of the present invention y H2+NbO 2.5 Transmission electron microscope image of a biphase niobium oxide photocatalytic material;

[0014] Figure 2 It is pure NbO 2.5 and NbO y H 0.5 NbO y H, NbO y XRD spectrum of H2;

[0015] Figure 3 It is ω%NbO y H2+NbO 2.5 XRD patterns of two-phase structure powders (ω = 0, 3, 5) (ω = 3: Example 1, Example 3; ω = 5: Example 2);

[0016] Figure 4 The NbO prepared according to the embodiments of the present invention y H2+NbO 2.5 High-resolution Nb3d XPS spectra of biphase niobium oxide photocatalysts;

[0017] Figure 5 The NbO prepared according to the embodiments of the present invention y H2+NbO 2.5 The UV-Vis absorption spectrum of a two-phase niobium oxide photocatalyst material. (3% NbO) y H2+NbO 2.5 Example 1 and Example 3; 5% NbO y H2+NbO 2.5 Example 2) Detailed Implementation

[0018] Example 1:

[0019] This embodiment describes a method for preparing a black niobium oxide photocatalytic material, the steps of which are as follows:

[0020] (1) Add 13.3g of niobium oxide nanopowder, 1.8g of NbCl5 and 0.5g of NaH to 100mL of anhydrous toluene and mix at room temperature to obtain a reaction solution;

[0021] (2) The above reaction solution was loaded into a reaction vessel lined with polytetrafluoroethylene, and then placed in an oven at 180°C for 10 hours to allow NbCl5 to dissolve in anhydrous toluene and react with NaH. After the reaction was completed, the mixture was filtered and collected to obtain precursor powder with NbH2Cl3 uniformly deposited on the surface of niobium oxide particles.

[0022] (3) The above precursor powder was added to a 1 mol / L NH3 aqueous solution to hydrolyze NbH2Cl3. The resulting precipitate was washed with anhydrous ethanol and then transferred to a hydrogen furnace for heat treatment at 300°C in a hydrogen atmosphere for 1 hour to obtain NbO. y H2+NbO 2.5 Two-phase structure niobium oxide photocatalytic material.

[0023] Example 2:

[0024] This embodiment describes a method for preparing a black niobium oxide photocatalytic material, the steps of which are as follows:

[0025] (1) Add 13.3g of niobium oxide nanopowder, 3g of NbCl5 and 0.8g of NaH to 100mL of anhydrous toluene and mix at room temperature to obtain a reaction solution;

[0026] (2) The above reaction solution was loaded into a reaction vessel lined with polytetrafluoroethylene, and then placed in an oven at 200°C for 8 hours to allow NbCl5 to dissolve in anhydrous toluene and react with NaH. After the reaction was completed, the mixture was filtered and collected to obtain precursor powder with NbH2Cl3 uniformly deposited on the surface of niobium oxide particles.

[0027] (3) The above precursor powder was added to a 1 mol / L NH3 aqueous solution to hydrolyze NbH2Cl3. The resulting precipitate was washed with anhydrous ethanol and then transferred to a hydrogen furnace for heat treatment at 350°C in a hydrogen atmosphere for 1.5 h to obtain NbO. y H2+NbO 2.5 Two-phase structure niobium oxide photocatalytic material.

[0028] Example 3:

[0029] This embodiment describes a method for preparing a black niobium oxide photocatalytic material, the steps of which are as follows:

[0030] (1) Add 13.3g of niobium oxide nanopowder, 1.8g of NbCl5 and 0.7g of CaH2 to 100mL of anhydrous toluene and mix at room temperature to obtain a reaction solution;

[0031] (2) The above reaction solution was loaded into a reaction vessel lined with polytetrafluoroethylene, and then placed in an oven at 220°C for 8 hours to allow NbCl5 to dissolve in anhydrous toluene and react with CaH2. After the reaction was completed, the mixture was filtered and collected to obtain precursor powder with NbH2Cl3 uniformly deposited on the surface of niobium oxide particles.

[0032] (3) The above precursor powder was added to a 1 mol / L NH3 aqueous solution to hydrolyze NbH2Cl3. The resulting precipitate was washed with anhydrous ethanol and then transferred to a hydrogen furnace for heat treatment at 300°C in a hydrogen atmosphere for 2 hours to obtain NbO. y H2+NbO 2.5 Two-phase structure niobium oxide photocatalytic material.

[0033] NbO prepared according to the embodiments of the present invention y H2+NbO 2.5 Dual-phase niobium oxide photocatalysts, such as Figure 1 As shown, the photocatalytic water splitting reaction for hydrogen production was tested as follows:

[0034] At 20℃, using a 300W xenon lamp as the light source, 100mL of 20% (v / v) methanol aqueous solution and 0.3g of catalyst were added to a 150mL quartz reactor. The distance between the light source and the quartz tube was 8cm, and the stirring speed was 500rpm. After irradiation for 4h, samples were taken and analyzed by gas chromatography. The reaction data are listed in Table 1.

[0035] Table 1. Photocatalytic materials and pure NbO in embodiments of the present invention 2.5 Photocatalytic hydrogen production activity

[0036]

[0037] The above results indicate that the hydrogen evolution rate of the niobium oxide photocatalytic material in the embodiments of the present invention is higher than that of pure NbO. 2.5 25 to 35 times.

[0038] Figure 2 The image shown is of pure NbO. 2.5 and NbO y H 0.5 NbO y H, NbO y The XRD pattern of H2 shows that pure NbO 2.5The crystal form is intact, and the diffraction peaks are in agreement with the standard card JCPDS 027-1003; NbO prepared by solvothermal assisted heat treatment method y H 0.5 NbO y H, NbO y H2 has a complete crystal structure, and its diffraction peaks are consistent with those of monoclinic NbO in the standard card (JCPDS 30–0872). 2.5 The diffraction peaks of the (100), (011), (013), (113), and (202) crystal planes are consistent. This indicates that H doping makes NbO... 2.5 The crystal structure has changed. Furthermore, with increasing H doping, NbO... 2.5 The crystal structure is gradually destroyed until an amorphous structure (such as NbO) is formed. y H2). For example Figure 3 As shown, a small amount of amorphous NbO y H2 coated onto NbO 2.5 niobium oxide catalyst surface for NbO 2.5 The crystal structure was not affected.

[0039] like Figure 4 As shown, Nb 3d 5 / 2 and Nb 3d 3 / 2 The binding energies are 207.5 eV and 210.1 eV, respectively, indicating that Nb in the sample exhibits a +5 bond. However, a small splitting peak is clearly observed at approximately 206.2 eV, which may be due to the Nb-H bond (Nb 3d in pure NbH2). 5 / 2 The binding energy is located at 203 eV. The ultraviolet-visible absorption spectrum of the product obtained in the embodiments of the present invention is as follows: Figure 5 As shown, the prepared black niobium oxide exhibits strong absorption of visible light (absorbance of 0.8–0.9).

Claims

1. A method for preparing a black niobium oxide photocatalytic material, characterized in that... Includes the following steps: (1) Niobium oxide nanopowder : NbCl5 : NaH or CaH2 : anhydrous toluene = 10-30g : 1-5g : 0.2-1g : 100-200mL, and mix at room temperature to obtain a reaction solution; (2) The reaction solution is placed in a reaction vessel and subjected to a solvothermal reaction at 180–220°C for 5–15 h, allowing NbCl5 to dissolve in anhydrous toluene and react with NaH or CaH2. After the reaction is complete, the solution is filtered and collected to obtain NbH2. x Cl 5-x Precursor powder uniformly deposited on the surface of niobium oxide particles, wherein x = 0.1 to 2; (3) The precursor powder is added to an ammonia solution with a concentration of 0.5–2 mol / L, so that the NbH x Cl 5-x Hydrolysis was performed, and the resulting precipitate was washed with anhydrous ethanol and then transferred to a hydrogen furnace for heat treatment at 250–350 °C in a hydrogen atmosphere for 1–2 hours to obtain NbO. y H x +NbO 2.5 A two-phase structure niobium oxide photocatalytic material, wherein x = 0.1 to 2.

2. The product obtained by the preparation method of the black niobium oxide photocatalytic material according to claim 1.

3. The product according to claim 2, characterized in that: The NbO y H x +NbO 2.5 In the photocatalytic water splitting reaction to produce hydrogen, the hydrogen evolution rate of the biphase niobium oxide photocatalyst is higher than that of pure NbO. 2.5 25 to 35 times.

Citation Information

Patent Citations

  • Process for manufacturing metal containing powder

    CN105392734A

  • Black cerium dioxide nano-material and preparation method thereof

    CN111268714A