Carbon-based confinement bimetallic monatomic catalytic material and application thereof in removal of perchlorate in drinking water
Through carbon-based limited-domain bimetallic single-atom catalytic material and formic acid strengthening treatment, the problem of low perchlorate removal efficiency in drinking water is solved, efficient and economical perchlorate removal is achieved, and national standards are met and treatment is simplified. process.
Patent Information
- Application Number
- CN202411414238.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-11
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-10-11
AI Technical Summary
The prior art has low efficiency, high cost, complex operation and insufficient anti-interference ability in drinking water, making it difficult to meet the removal requirements under the national standard (70 μg/L).
Using carbon-based limited-domain bimetallic single-atom catalytic material, through metal-nitrogen coordination structure design, use metal atoms such as Mn, Cu, Ni, Mo to achieve efficient adsorption and reduction of perchlorate, combined with formic acid strengthening treatment, optimize the material's material Surface electrical properties and chemosorption properties.
It significantly improves the removal efficiency of perchlorate, reduces operating costs, simplifies the processing process, and achieves rapid removal of low-concentration perchlorate. It also has strong material stability and recycling, reducing long-term operating costs.
Smart Images

Figure CN118904392A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of water purification treatment, in particular to a carbon-based confined bimetallic single-atom catalytic material and its application in removing perchlorate from drinking water. Background Art
[0002] Perchlorate ( ), as a compound that plays an important role in the industrial field, is widely used in fireworks manufacturing, arms and aerospace industries as a strong oxidant, and is also an essential additive in the production of leather making agents, lubricants, rubber products, and magnesium batteries. In addition, it is also involved in the synthesis of certain chemicals, acting as a catalyst. However, despite its wide application, the use and discharge of perchlorates also bring about environmental pollution problems, posing potential risks to ecosystems and human health.
[0003] Perchlorate not only comes from industrial production, but is also part of the natural chlorine cycle, which competitively inhibits the uptake and use of iodine by thyroid follicular epithelial cells. Potential effects on human health include suppressing thyroid function, disrupting metabolism and growth and development, and may even cause changes in cell structure and abnormal gene expression, posing a threat to reproductive health and embryonic development. In recent years, perchlorates discharged into the environment by human production activities and naturally produced have been widely involved in the ecological cycle and entered the food chain through the ecological cycle. Domestic and foreign studies have detected perchlorates in a variety of foods such as drinking water, beverages, wine, agricultural products and dairy products. To address this problem, my country implemented the "Standards for Drinking Water Quality" (GB5749-2022) on April 1, 2023, bringing perchlorate under supervision and setting a standard limit of 70 μg / L.
[0004] In order to reduce the content of perchlorate in drinking water, the industry has explored the application of various treatment technologies to achieve effective removal of perchlorate. At present, the treatment technologies for perchlorate in drinking water mainly include physical, chemical and biological methods. Physical methods such as activated carbon adsorption, ion exchange and membrane separation technology. Activated carbon adsorption technology has the advantages of high treatment efficiency and simple operation. It is one of the earlier water treatment technologies, but activated carbon usually has a low adsorption capacity and poor anti-interference. At the same time, surfactant treatment will increase the treatment cost and cause secondary pollution; membrane separation technology plays an important role in removing perchlorate from drinking water. Perchlorate can be removed by reverse osmosis and nanofiltration, but the production cost of nanofiltration and reverse osmosis membranes is expensive and is mainly used in small-scale drinking water plants. Microbial degradation and reduction technology that uses microorganisms to degrade perchlorate is currently a relatively mature and effective technology. Microorganisms can use perchlorate to breathe under the action of a multi-factor metal enzyme system, and then reduce perchlorate. However, the biological process is complex, difficult to operate, occupies a large area, and has a long operating time. There is also secondary pollution during the treatment process, so it is limited in drinking water treatment. Chemical methods usually reduce perchlorate to harmless chloride ions through oxygen atom transfer reactions and hydrogenation and deoxygenation reactions, but the spatial steric hindrance of perchlorate makes it difficult for chlorine atoms to directly accommodate the additional electrons of conventional reducing agents to achieve a reduction in their oxidation state. At the same time, perchlorate exhibits redox kinetic inertness, weak coordination ability and weak nucleophilicity in dilute aqueous solutions at room temperature and pressure. The activation energy of the process of reducing perchlorate to chloride ions is also very high. In order to better degrade perchlorate, it is usually necessary to introduce H2 into the reaction system or provide high temperature.
[0005] It can be seen that the removal of perchlorate in drinking water still faces challenges, and there is an urgent need to develop more efficient, rapid and cost-effective treatment technologies. Summary of the invention
[0006] In view of the shortcomings of existing perchlorate removal technologies in drinking water, such as limited adsorption capacity, complex reaction condition control, insufficient anti-interference ability, low reuse rate, and unsatisfactory practical application effects, the present invention proposes an innovative solution to provide a carbon-based confined bimetallic single-atom catalytic material with good adsorption and reduction properties, which can significantly improve the removal efficiency of perchlorate. The application of this technology can reduce the perchlorate content in drinking water to below the national drinking water hygiene standard (less than 70 μg / L) in a short period of time, while simplifying the treatment process and reducing operating costs. In addition, the stability and recyclability of the material reduce long-term operating costs and improve the practicality and economy of water treatment technology.
[0007] The first technical problem solved by the present invention is to provide a carbon-based confined bimetallic single-atom catalytic material, wherein the catalytic material has a carbon base as a skeleton and nitrogen atoms as coordinating atoms, and achieves dispersion and fixation of specific metal atoms in the form of single atoms through a metal-nitrogen (Me-N) coordination structure; the metal atoms are any two of Mn, Cu, Ni, and Mo.
[0008] In some preferred embodiments, the metal atoms are any combination of Mo-Mn, Mo-Cu, Mo-Ni, and Mo-Mo.
[0009] The second technical problem solved by the present invention is to provide a method for preparing a carbon-based confined bimetallic single-atom catalytic material, and the specific steps are as follows: (1) Preparing a precursor solution: using dimethylformamide as a solvent, preparing a solution A containing zinc nitrate and a first metal salt, and a solution B containing 2-methylimidazole; (2) Growing nanocrystals: mixing solutions A and B, keeping them warm under sealed conditions to promote the growth of nanocrystals with metal-nitrogen coordination structures, removing impurities by centrifugation and washing, and vacuum drying the precipitate to obtain nanocrystals; (3) Primary calcination: In a nitrogen atmosphere, the nanocrystals are heated to 900-1200°C for primary calcination; (4) Acid washing: The material after the primary calcination is subjected to acid washing, suction filtration, washing, and vacuum drying to obtain a carbon-based material; (5) Introduction of the second metal: fully dispersing the carbon-based material in an isopropanol solution, adding the second metal salt and melamine, ultrasonically dispersing, recovering, drying, and collecting particles; (6) Secondary calcination: In a nitrogen atmosphere, the particles are heated to 800-1000 °C for secondary calcination to obtain a carbon-based confined bimetallic single atom catalytic material.
[0010] In a preferred embodiment, the molar ratio of zinc nitrate, the first metal salt, and 2-methylimidazole in step (1) is 10-30:1:20-60.
[0011] In a preferred embodiment, in step (5), the molar ratio of the second metal salt to 2-methylimidazole is 1:1-5.
[0012] The third technical problem solved by the present invention is to provide a method for removing perchlorate in drinking water, which uses the above-mentioned carbon-based confined bimetallic single-atom catalytic material as a catalyst to remove perchlorate in drinking water.
[0013] In some specific embodiments, when the carbon-based confined bimetallic single atom catalytic material is used as a catalyst, it has a powdery, granular or carrier-supported form.
[0014] In a preferred embodiment, the treatment process is enhanced with formic acid.
[0015] In a specific embodiment, the formic acid enhanced treatment is to add the catalyst and a certain concentration of formic acid into a reactor containing the water sample to be purified in sequence, stir it sufficiently, control the residence time of the water sample in the reactor to be 5 to 30 minutes, then filter it and recover the catalyst.
[0016] In a preferred embodiment, the concentration of formic acid is 0.5-2 mM.
[0017] Compared with the prior art, the present invention has the following beneficial effects: The present invention provides an innovative carbon-based confined bimetallic single-atom material for the targeted removal of perchlorate in drinking water. Unlike other general pollutants, perchlorate is an inorganic anion. The catalytic material designed by the present invention is based on the properties and spatial size of perchlorate, and a catalytic material with rich nano-confined pore structure and high specific surface area is constructed in a direction, thereby achieving efficient adsorption and reduction of perchlorate. In addition, the characteristics of nanoscale confined adsorption also effectively isolate macromolecular substances in wastewater, reduce competition for adsorption sites, and further improve the utilization rate and removal efficiency of the material.
[0018] The transition metal-nitrogen coordination structure (Me-N) inside the material not only increases the active sites, but also the Me-N coordination environment gives the metal atom sites positive charge, enhancing the negatively charged ClO4 - The electrostatic attraction of the catalyst significantly improves the directional adsorption efficiency of perchlorate. The metal single atom Mo with good biocompatibility and catalytic activity is specially selected to use the Mo atom and ClO4 - The efficient interface bonding ability between O atoms enhances the adsorption performance of the material.
[0019] In the process of purifying drinking water, formic acid is used to strengthen the treatment process, optimize the surface electrical properties of the material, and further improve the material's adsorption capacity for perchlorate. The presence of formic acid makes the metal single atom site more positively charged, which strengthens the adsorption of ClO4 - The electrostatic attraction of formic acid promotes the formation of chemical bonds and enhances the chemical adsorption performance of the material. This enhanced treatment improves the material's anti-interference ability under complex water conditions and ensures its high efficiency and stability in practical applications. Through the enhanced effect of formic acid, while improving the removal efficiency, it also enhances the environmental adaptability and practicality of the material.
[0020] The catalytic material of the present invention has low dosage, stable structure, and the solid material is easy to transport and store, which not only saves technical costs, but also reduces the potential risk of secondary pollution, ensuring the safety of the technology. In addition, the material has high removal efficiency and rapid response ability, and can effectively remove even high-concentration perchlorates, and the residence time of the removal process is short and easy to operate. The solid material is easy to separate and recycle after failure, showing excellent cycle stability and anti-deactivation ability. Even after repeated use and regeneration treatment, it still maintains efficient adsorption performance, providing an economical and feasible solution for actual perchlorate removal. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art are briefly introduced below.
[0022] Figure 1 This is a scanning electron microscope image of the Mn-Mo-NC material prepared in Example 1. DETAILED DESCRIPTION
[0023] The invention discloses a carbon-based confined bimetallic single-atom catalytic material and application thereof in removing perchlorate from drinking water.
[0024] It should be understood that the expression "one or more of..." includes individually each object recited after the expression and various different combinations of two or more of the recited objects, unless otherwise understood from the context and usage. The expression "and / or" in combination with three or more recited objects should be understood to have the same meaning, unless otherwise understood from the context. The terms "comprising", "having" or "containing", including the use of their grammatical synonyms, should generally be understood to be open and non-restrictive, for example, other unrecited elements or steps are not excluded, unless otherwise specifically stated or understood from the context.
[0025] It should be understood that the order of steps or the order in which certain actions are performed is not important as long as the present invention remains operable. In addition, two or more steps or actions may be performed simultaneously.
[0026] In addition, the numerical ranges and parameters used to define the present invention are approximate values, and the relevant values in the specific embodiments have been presented as accurately as possible. However, any numerical value inherently inevitably contains standard deviations due to individual test methods. Therefore, unless otherwise expressly stated, it should be understood that all ranges, quantities, values and percentages used in the present invention are modified by "about". Here, "about" generally refers to the actual value within plus or minus 10%, 5%, 1% or 0.5% of a specific value or range.
[0027] Unless otherwise clearly stated, it should be understood that all percentages described in the present invention are by mass percentages.
[0028] The first technical problem that the present invention aims to solve is to propose a carbon-based confined bimetallic single-atom catalytic material. The catalytic material has a carbon base as a skeleton and nitrogen atoms as coordination atoms, and achieves the dispersion and fixation of specific metal atoms in the form of single atoms through a metal-nitrogen (Me-N) coordination structure.
[0029] Any two of manganese (Mn), copper (Cu), nickel (Ni) and molybdenum (Mo) are selected as metal atoms of the catalytic material. These metal atoms are selected based on the characteristics of perchlorate to achieve the best catalytic removal effect.
[0030] In some embodiments, the two metal atoms selected are Mn-Mo, Mn-Ni, Mo-Cu, Mo-Ni, Cu-Ni, and Mo-Mo.
[0031] In particular, when molybdenum (Mo) is used as one of the metal atoms, the prepared catalytic material exhibits excellent performance in reducing and purifying perchlorate. Molybdenum exists in multiple oxidation states in nature, such as Mo(0), Mo(III), Mo(IV), Mo(V) and Mo(VI), which makes it have a significant effect on regulating the electrons at the material interface, which is conducive to the generation of positive potential points at the material interface and strengthens its electrostatic adsorption of perchlorate; in addition, the multiple oxidation states of Mo are conducive to the transfer of valence electrons between Mo and O atoms, making it highly active in the reduction reaction. In some preferred embodiments, the two metal atoms selected are any combination of Mo-Mn, Mo-Cu, Mo-Ni, and Mo-Mo.
[0032] The second technical problem solved by the present invention is to provide a method for preparing a carbon-based confined bimetallic single-atom catalytic material, and the specific steps are as follows: (1) Preparing a precursor solution: using dimethylformamide as a solvent, preparing a solution A containing zinc nitrate and a first metal salt, and a solution B containing 2-methylimidazole; (2) Growing nanocrystals: mixing solutions A and B, keeping them warm under sealed conditions to promote the growth of nanocrystals with metal-nitrogen coordination structures, removing impurities by centrifugation and washing, and vacuum drying the precipitate to obtain nanocrystals; (3) Primary calcination: In a nitrogen atmosphere, the nanocrystals are heated to 900-1200°C for primary calcination; (4) Acid washing: The material after the primary calcination is subjected to acid washing, suction filtration, washing, and vacuum drying to obtain a carbon-based material; (5) Introduction of the second metal: fully dispersing the carbon-based material in an isopropanol solution, adding the second metal salt and melamine, ultrasonically dispersing, recovering, drying, and collecting particles; (6) Secondary calcination: In a nitrogen atmosphere, the particles are heated to 800-1000 °C for secondary calcination to obtain a carbon-based confined bimetallic single atom catalytic material.
[0033] In a preferred embodiment, the molar ratio of zinc nitrate, the first metal salt, and 2-methylimidazole in step (1) is 10-30:1:20-60.
[0034] In a preferred embodiment, the molar concentration of the first metal salt in solution A of step (1) is 0-20 mM; In a preferred embodiment, the molar concentration of 2-methylimidazole in solution B in step (1) is 30-1200 mM; In some specific embodiments, the first metal salt is one of manganese acetate dihydrate, copper acetate monohydrate, nickel acetate tetrahydrate, and molybdenum acetate.
[0035] In a specific embodiment, in step (2), solution A is slowly added dropwise to solution B under stirring to mix the two solutions evenly.
[0036] In a specific embodiment, in step (2), the insulation temperature is 110-130° C. and the insulation time is 23-25 hours. This temperature environment is conducive to the continuous growth of nanocrystals.
[0037] In a specific embodiment, in step (2), the centrifugation parameters are 8000 r / min, 25° C., and 10 min.
[0038] In a specific embodiment, in step (2), anhydrous ethanol is used as the washing liquid.
[0039] In a specific embodiment, in step (2), the vacuum drying temperature is 60°C.
[0040] In a specific embodiment, in step (3), the primary calcination is carried out under a protective atmosphere, with the temperature being raised to 1100° C. at a rate of 3-7° C. / min and kept at that temperature for 0.5-1.5 hours.
[0041] In a specific embodiment, in step (4), the acid washing treatment is to continuously stir the nanocrystals after the primary calcination in 0.3-1M H2SO4 at 50-90°C for 3-8 hours.
[0042] In some specific embodiments, in step (5), the second metal salt is one of manganese chloride, copper chloride, nickel chloride, and molybdenum chloride.
[0043] In a preferred embodiment, in step (5), the molar ratio of the second metal salt to melamine is 1:5.
[0044] In a specific embodiment, in step (6), the secondary calcination is carried out by heating the temperature to 900° C. at a rate of 3-7° C. / min and keeping the temperature for 2.5-3.5 hours.
[0045] The third technical problem solved by the present invention is to provide a method for removing perchlorate in drinking water, which uses the above-mentioned carbon-based confined bimetallic single-atom catalytic material as a catalyst to remove perchlorate in drinking water.
[0046] The specific method is to directly add the catalytic material into the water treatment system, and utilize its excellent adsorption and catalytic properties to achieve rapid removal of perchlorate.
[0047] In a preferred embodiment, the dosage of the catalytic material is 100 mg / L to 1000 mg / L.
[0048] In some specific embodiments, when the carbon-based confined bimetallic single atom catalytic material is used as a catalyst, it has a powdery, granular or carrier-loaded form to efficiently remove perchlorate.
[0049] In some preferred embodiments, the carrier is activated carbon, ceramsite, silicate balls, etc.
[0050] In some specific embodiments, the loading is to load the carbon-based confined bimetallic single atom catalytic material powder in situ on the carrier by dry powder impregnation-calcination method.
[0051] In a preferred embodiment, the treatment process adopts formic acid enhanced treatment, and the adsorption and reduction efficiency of the catalytic material to perchlorate is further improved through the strengthening effect of formic acid.
[0052] In a specific embodiment, the formic acid enhanced treatment is to add the catalyst and a certain concentration of formic acid into a reactor containing the water sample to be purified in sequence, stir it sufficiently, control the residence time of the water sample in the reactor to be 5 to 30 minutes, then filter it and recover the catalyst.
[0053] In a preferred embodiment, the concentration of formic acid is 1.0 mM. This concentration range can effectively enhance the removal performance of the catalytic material.
[0054] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0055] Example 1 Preparation of Carbon-based Confined Bimetallic Single Atom Catalytic Material (1) Preparation of precursor solution: Take 500 ml of dimethylformamide as a solvent, add zinc nitrate and manganese acetate dihydrate at room temperature, then place it on a magnetic stirrer and stir it at a speed of 800 rpm for 15 minutes until the solid is completely dissolved to obtain solution A.
[0056] Take 500 ml of dimethylformamide as solvent, add 2-methylimidazole at room temperature, then place it on a magnetic stirrer and stir at 800 rpm for 15 minutes until the solid is completely dissolved to obtain solution B. The molar ratio of zinc nitrate, manganese acetate dihydrate and 2-methylimidazole is 30:1:60.
[0057] (2) Growth of nanocrystals: Solution A was slowly added dropwise to solution B under stirring and mixed. The mixture was kept at 120°C for 25 h under sealed conditions to promote the growth of nanocrystals with metal Mn-nitrogen coordination structure. After the insulation, the mixed solution was allowed to stand at room temperature to allow the nanocrystals to fully precipitate. The precipitate was centrifuged at 8000 r / min, 25°C, and 10 min. The centrifuged precipitate was collected. The centrifuged precipitate was washed with anhydrous ethanol, placed in a vacuum drying oven, and dried at 60°C to constant weight to obtain nanocrystals.
[0058] (3) Primary calcination: In a nitrogen atmosphere, the nanocrystals obtained in step (2) were placed in a tubular furnace, heated at a rate of 5 °C / min to 1200 °C, and kept at this temperature for 1.5 h.
[0059] (4) Acid washing: The material after the primary calcination was dispersed in a 0.5 M H2SO4 solution under stirring, and acid washed at 80°C for 5 h. The filtrate was filtered, washed with at least 2 L of ultrapure water, and then dried in a vacuum drying oven at 60°C to constant weight.
[0060] (5) Introduction of the second metal: The dried carbon-based material was fully dispersed in 1000 ml of 50% isopropanol solution, molybdenum chloride and melamine were added and mixed thoroughly, ultrasonically dispersed for 2 h, filtered and recovered, placed in a vacuum drying oven at 60°C to constant weight, and the particles were collected. The molar ratio of molybdenum chloride to melamine was 1:1~5.
[0061] (6) Secondary calcination: In a nitrogen atmosphere, the particles obtained in step (5) were placed in a tube furnace, heated at a rate of 5 °C / min to 900 °C, and kept at this temperature for 1.5 h to obtain a carbon-based confined bimetallic single atom catalytic material, denoted as Mn-Mo-NC.
[0062] Figure 1 This is a scanning electron microscope image of the Mn-Mo-NC material.
[0063] Example 2 Preparation of Carbon-based Confined Bimetallic Single Atom Catalytic Material (1) Preparation of precursor solution: Take 500 ml of dimethylformamide as solvent, add zinc nitrate and copper acetate monohydrate at room temperature, then place on a magnetic stirrer and stir at a speed of 800 rpm for 15 minutes until the solid is completely dissolved to obtain solution A.
[0064] Take 500 ml of dimethylformamide as solvent, add 2-methylimidazole at room temperature, then place it on a magnetic stirrer and stir at 800 rpm for 15 minutes until the solid is completely dissolved to obtain solution B. The molar ratio of zinc nitrate, copper acetate monohydrate and 2-methylimidazole is 10:1:60.
[0065] (2) Growth of nanocrystals: Solution A was slowly added dropwise to solution B under stirring and mixed. The mixture was kept at 120°C for 25 h under sealed conditions to promote the growth of nanocrystals with metal Mn-nitrogen coordination structure. After the insulation, the mixed solution was allowed to stand at room temperature to allow the nanocrystals to fully precipitate. The precipitate was centrifuged at 8000 r / min, 25°C, and 10 min. The centrifuged precipitate was collected. The centrifuged precipitate was washed with anhydrous ethanol, placed in a vacuum drying oven, and dried at 60°C to constant weight to obtain nanocrystals.
[0066] (3) Primary calcination: In a nitrogen atmosphere, the nanocrystals obtained in step (2) were placed in a tubular furnace, heated at a rate of 5 °C / min to 1200 °C, and kept at this temperature for 1.5 h.
[0067] (4) Acid washing: The material after the primary calcination was dispersed in a 0.5 M H2SO4 solution under stirring, and acid washed at 80°C for 5 h. The filtrate was filtered, washed with at least 2 L of ultrapure water, and then dried in a vacuum drying oven at 60°C to constant weight.
[0068] (5) Introduction of the second metal: The dried carbon-based material was fully dispersed in 1000 ml of 50% isopropanol solution, molybdenum chloride and melamine were added and mixed thoroughly, ultrasonically dispersed for 2 h, filtered and recovered, placed in a vacuum drying oven at 60°C to constant weight, and the particles were collected. The molar ratio of molybdenum chloride to melamine was 1:1~5.
[0069] (6) Secondary calcination: In a nitrogen atmosphere, the particles obtained in step (5) were placed in a tube furnace, heated at a rate of 5 °C / min to 900 °C, and kept at this temperature for 1.5 h to obtain a carbon-based confined bimetallic single atom catalytic material, denoted as Cu-Mo-NC.
[0070] Example 3 Preparation of Carbon-based Confined Bimetallic Single Atom Catalytic Material (1) Preparation of precursor solution: Take 500 ml of dimethylformamide as a solvent, add zinc nitrate and nickel acetate tetrahydrate at room temperature, then place it on a magnetic stirrer and stir it at a speed of 800 rpm for 15 minutes until the solid is completely dissolved to obtain solution A.
[0071] Take 500 ml of dimethylformamide as solvent, add 2-methylimidazole at room temperature, then place it on a magnetic stirrer and stir at 800 rpm for 15 minutes until the solid is completely dissolved to obtain solution B. The molar ratio of zinc nitrate, nickel acetate tetrahydrate and 2-methylimidazole is 10:1:30.
[0072] (2) Growth of nanocrystals: Solution A was slowly added dropwise to solution B under stirring and mixed. The mixture was kept at 120°C for 25 h under sealed conditions to promote the growth of nanocrystals with metal Mn-nitrogen coordination structure. After the insulation, the mixed solution was allowed to stand at room temperature to allow the nanocrystals to fully precipitate. The precipitate was centrifuged at 8000 r / min, 25°C, and 10 min. The centrifuged precipitate was collected. The centrifuged precipitate was washed with anhydrous ethanol, placed in a vacuum drying oven, and dried at 60°C to constant weight to obtain nanocrystals.
[0073] (3) Primary calcination: In a nitrogen atmosphere, the nanocrystals obtained in step (2) were placed in a tubular furnace, heated at a rate of 5 °C / min to 1200 °C, and kept at this temperature for 1.5 h.
[0074] (4) Acid washing: The material after the primary calcination was dispersed in a 0.5 M H2SO4 solution under stirring, and acid washed at 80°C for 5 h. The filtrate was filtered, washed with at least 2 L of ultrapure water, and then dried in a vacuum drying oven at 60°C to constant weight.
[0075] (5) Introduction of the second metal: The dried carbon-based material was fully dispersed in 1000 ml of 50% isopropanol solution, molybdenum chloride and melamine were added and mixed thoroughly, ultrasonically dispersed for 2 h, filtered and recovered, placed in a vacuum drying oven at 60°C to constant weight, and the particles were collected. The molar ratio of molybdenum chloride to melamine was 1:1~5.
[0076] (6) Secondary calcination: In a nitrogen atmosphere, the particles obtained in step (5) were placed in a tube furnace, heated at 5 °C / min to 900 °C, and kept at this temperature for 1.5 h to obtain a carbon-based confined bimetallic single atom catalytic material, denoted as Ni-Mo-NC.
[0077] Example 4 Preparation of Carbon-based Confined Bimetallic Single Atom Catalytic Material (1) Preparation of precursor solution: Take 500 ml of dimethylformamide as solvent, add zinc nitrate and molybdenum acetate at room temperature, then place on a magnetic stirrer and stir at a speed of 800 rpm for 15 minutes until the solid is completely dissolved to obtain solution A.
[0078] Take 500 ml of dimethylformamide as solvent, add 2-methylimidazole at room temperature, then place it on a magnetic stirrer and stir at 800 rpm for 15 minutes until the solid is completely dissolved to obtain solution B. Wherein, the molar ratio of zinc nitrate, molybdenum acetate and 2-methylimidazole is 20:1:40.
[0079] (2) Growth of nanocrystals: Solution A was slowly added dropwise to solution B under stirring and mixed. The mixture was kept at 120°C for 25 h under sealed conditions to promote the growth of nanocrystals with metal Mn-nitrogen coordination structure. After the insulation, the mixed solution was allowed to stand at room temperature to allow the nanocrystals to fully precipitate. The precipitate was centrifuged at 8000 r / min, 25°C, and 10 min. The centrifuged precipitate was collected. The centrifuged precipitate was washed with anhydrous ethanol, placed in a vacuum drying oven, and dried at 60°C to constant weight to obtain nanocrystals.
[0080] (3) Primary calcination: In a nitrogen atmosphere, the nanocrystals obtained in step (2) were placed in a tubular furnace, heated at a rate of 5 °C / min to 1200 °C, and kept at this temperature for 1.5 h.
[0081] (4) Acid washing: The material after the primary calcination was dispersed in a 0.5 M H2SO4 solution under stirring, and acid washed at 80°C for 5 h. The filtrate was filtered, washed with at least 2 L of ultrapure water, and then dried in a vacuum drying oven at 60°C to constant weight.
[0082] (5) Introduction of the second metal: The dried carbon-based material was fully dispersed in 1000 ml of 50% isopropanol solution, molybdenum chloride and melamine were added and mixed thoroughly, ultrasonically dispersed for 2 h, filtered and recovered, placed in a vacuum drying oven at 60°C to constant weight, and the particles were collected. The molar ratio of molybdenum chloride to melamine was 1:1~5.
[0083] (6) Secondary calcination: In a nitrogen atmosphere, the particles obtained in step (5) were placed in a tube furnace, heated at a rate of 5 °C / min to 900 °C, and kept at this temperature for 1.5 h to obtain a carbon-based confined bimetallic single atom catalytic material, denoted as Mo-Mo-NC.
[0084] Example 5 Preparation of Carbon-based Confined Bimetallic Single Atom Catalytic Material (1) Preparation of precursor solution: Take 500 ml of dimethylformamide as a solvent, add zinc nitrate and manganese acetate dihydrate at room temperature, then place it on a magnetic stirrer and stir it at a speed of 800 rpm for 15 minutes until the solid is completely dissolved to obtain solution A.
[0085] Take 500 ml of dimethylformamide as solvent, add 2-methylimidazole at room temperature, then place it on a magnetic stirrer and stir at 800 rpm for 15 minutes until the solid is completely dissolved to obtain solution B. The molar ratio of zinc nitrate, manganese acetate dihydrate and 2-methylimidazole is 30:1:60.
[0086] (2) Growth of nanocrystals: Solution A was slowly added dropwise to solution B under stirring and mixed. The mixture was kept at 120°C for 25 h under sealed conditions to promote the growth of nanocrystals with metal Mn-nitrogen coordination structure. After the insulation, the mixed solution was allowed to stand at room temperature to allow the nanocrystals to fully precipitate. The precipitate was centrifuged at 8000 r / min, 25°C, and 10 min. The centrifuged precipitate was collected. The centrifuged precipitate was washed with anhydrous ethanol, placed in a vacuum drying oven, and dried at 60°C to constant weight to obtain nanocrystals.
[0087] (3) Primary calcination: In a nitrogen atmosphere, the nanocrystals obtained in step (2) were placed in a tubular furnace, heated at a rate of 5 °C / min to 1200 °C, and kept at this temperature for 1.5 h.
[0088] (4) Acid washing: The material after the primary calcination was dispersed in a 0.5 M H2SO4 solution under stirring, and acid washed at 80°C for 5 h. The filtrate was filtered, washed with at least 2 L of ultrapure water, and then dried in a vacuum drying oven at 60°C to constant weight.
[0089] (5) Introduction of the second metal: The dried carbon-based material was fully dispersed in 1000 ml of 50% isopropanol solution, nickel chloride and melamine were added and mixed thoroughly, ultrasonically dispersed for 2 h, filtered and recovered, placed in a vacuum drying oven at 60°C to constant weight, and the particles were collected. The molar ratio of nickel chloride to melamine was 1:1-5.
[0090] (6) Secondary calcination: In a nitrogen atmosphere, the particles obtained in step (5) were placed in a tube furnace, heated at a rate of 5 °C / min to 900 °C, and kept at this temperature for 1.5 h to obtain a carbon-based confined bimetallic single atom catalytic material, denoted as Mn-Ni-NC.
[0091] Example 6 Preparation of Carbon-based Confined Bimetallic Single Atom Catalytic Material (1) Preparation of precursor solution: Take 500 ml of dimethylformamide as a solvent, add zinc nitrate and manganese acetate dihydrate at room temperature, then place it on a magnetic stirrer and stir it at a speed of 800 rpm for 15 minutes until the solid is completely dissolved to obtain solution A.
[0092] Take 500 ml of dimethylformamide as solvent, add 2-methylimidazole at room temperature, then place it on a magnetic stirrer and stir at 800 rpm for 15 minutes until the solid is completely dissolved to obtain solution B. Wherein, the molar ratio of zinc nitrate, manganese acetate dihydrate and 2-methylimidazole is 10:1:20.
[0093] (2) Growth of nanocrystals: Solution A was slowly added dropwise to solution B under stirring and mixed. The mixture was kept at 120°C for 25 h under sealed conditions to promote the growth of nanocrystals with metal Mn-nitrogen coordination structure. After the insulation, the mixed solution was allowed to stand at room temperature to allow the nanocrystals to fully precipitate. The precipitate was centrifuged at 8000 r / min, 25°C, and 10 min. The centrifuged precipitate was collected. The centrifuged precipitate was washed with anhydrous ethanol, placed in a vacuum drying oven, and dried at 60°C to constant weight to obtain nanocrystals.
[0094] (3) Primary calcination: In a nitrogen atmosphere, the nanocrystals obtained in step (2) were placed in a tubular furnace, heated at a rate of 5 °C / min to 1200 °C, and kept at this temperature for 1.5 h.
[0095] (4) Acid washing: The material after the primary calcination was dispersed in a 0.5 M H2SO4 solution under stirring, and acid washed at 80°C for 5 h. The filtrate was filtered, washed with at least 2 L of ultrapure water, and then dried in a vacuum drying oven at 60°C to constant weight.
[0096] (5) Introduction of the second metal: The dried carbon-based material was fully dispersed in 1000 ml of 50% isopropanol solution, manganese chloride and melamine were added and mixed thoroughly, ultrasonically dispersed for 2 h, filtered and recovered, placed in a vacuum drying oven at 60°C to constant weight, and the particles were collected. The molar ratio of manganese chloride to melamine was 1:1-5.
[0097] (6) Secondary calcination: In a nitrogen atmosphere, the particles obtained in step (5) were placed in a tube furnace, heated at a rate of 5 °C / min to 900 °C, and kept at this temperature for 1.5 h to obtain a carbon-based confined bimetallic single atom catalytic material, denoted as Mn-Mn-NC.
[0098] Comparative Example 1 (1) Preparation of precursor solution: Take 500 ml of dimethylformamide as a solvent, add zinc nitrate and manganese acetate dihydrate at room temperature, then place it on a magnetic stirrer and stir it at a speed of 800 rpm for 15 minutes until the solid is completely dissolved to obtain solution A.
[0099] Take 500 ml of dimethylformamide as solvent, add 2-methylimidazole at room temperature, then place it on a magnetic stirrer and stir at 800 rpm for 15 minutes until the solid is completely dissolved to obtain solution B. The molar ratio of zinc nitrate, manganese acetate dihydrate and 2-methylimidazole is 30:1:60.
[0100] (2) Growth of nanocrystals: Solution A was slowly added dropwise to solution B under stirring and mixed. The mixture was kept at 120°C for 25 h under sealed conditions to promote the growth of nanocrystals with metal Mn-nitrogen coordination structure. After the insulation, the mixed solution was allowed to stand at room temperature to allow the nanocrystals to fully precipitate. The precipitate was centrifuged at 8000 r / min, 25°C, and 10 min. The centrifuged precipitate was collected. The centrifuged precipitate was washed with anhydrous ethanol, placed in a vacuum drying oven, and dried at 60°C to constant weight to obtain nanocrystals.
[0101] (3) Primary calcination: In a nitrogen atmosphere, the nanocrystals obtained in step (2) were placed in a tubular furnace, heated at a rate of 5 °C / min to 1200 °C, and kept at this temperature for 1.5 h.
[0102] (4) Acid washing: The material after the primary calcination was dispersed in a 0.5 M H2SO4 solution under stirring, and acid washed at 80°C for 5 h. The filtrate was filtered, washed with at least 2 L of ultrapure water, and then dried in a vacuum drying oven at 60°C to constant weight.
[0103] (5) Secondary calcination: In a nitrogen atmosphere, the dried material was placed in a tube furnace and heated to 900 °C at a rate of 5 °C / min and kept at this temperature for 1.5 h to obtain a carbon-based confined bimetallic single atom catalytic material, denoted as Mn-NC.
[0104] Comparative Example 2 (1) Preparation of precursor solution: Take 500 ml of dimethylformamide as solvent, add zinc nitrate and molybdenum acetate at room temperature, then place on a magnetic stirrer and stir at a speed of 800 rpm for 15 minutes until the solid is completely dissolved to obtain solution A.
[0105] Take 500 ml of dimethylformamide as solvent, add 2-methylimidazole at room temperature, then place it on a magnetic stirrer and stir at 800 rpm for 15 minutes until the solid is completely dissolved to obtain solution B. Wherein, the molar ratio of zinc nitrate, molybdenum acetate and 2-methylimidazole is 20:1:40.
[0106] (2) Growth of nanocrystals: Solution A was slowly added dropwise to solution B under stirring and mixed. The mixture was kept at 120°C for 25 h under sealed conditions to promote the growth of nanocrystals with metal Mn-nitrogen coordination structure. After the insulation, the mixed solution was allowed to stand at room temperature to allow the nanocrystals to fully precipitate. The precipitate was centrifuged at 8000 r / min, 25°C, and 10 min. The centrifuged precipitate was collected. The centrifuged precipitate was washed with anhydrous ethanol, placed in a vacuum drying oven, and dried at 60°C to constant weight to obtain nanocrystals.
[0107] (3) Primary calcination: In a nitrogen atmosphere, the nanocrystals obtained in step (2) were placed in a tubular furnace, heated at a rate of 5 °C / min to 1200 °C, and kept at this temperature for 1.5 h.
[0108] (4) Acid washing: The material after the primary calcination was dispersed in a 0.5 M H2SO4 solution under stirring, and acid washed at 80°C for 5 h. The filtrate was filtered, washed with at least 2 L of ultrapure water, and then dried in a vacuum drying oven at 60°C to constant weight.
[0109] (5) Secondary calcination: In a nitrogen atmosphere, the dried material was placed in a tube furnace and heated to 900 °C at a rate of 5 °C / min and kept at this temperature for 1.5 h to obtain a carbon-based confined bimetallic single atom catalytic material, denoted as Mo-NC.
[0110] Verification experiment: The catalytic materials obtained in Examples 1-5 and Comparative Examples 1 and 2, and activated carbon were used as catalysts to adsorb and remove perchlorate in drinking water, specifically comprising the following steps: Step (1), prepare 50 mL of perchlorate water sample with a concentration of 10 mg / L; Step (2): 0.3 g / L of catalyst was added to the water sample prepared in step (1), and the reaction was carried out at 1200 r / min using a stirrer. The reaction time was 300 s, and the perchlorate content was detected. The results are shown in Table 1.
[0111] The detection method of perchlorate is as follows: perchlorate is analyzed using a Dionex ICS-600 ion chromatograph (Thermo Fisher Scientific, USA), the analytical column model is AS19 (4 mm×250 mm), equipped with an AG 19 guard column (4mm×50 mm), the eluent is KOH, and the eluent flow rate is 1 mL / min.
[0112] Table 1. Removal efficiency of perchlorate in drinking water by different catalysts It can be seen from the test results that the carbon-based confined double single-atom catalysts constructed in the present invention can achieve effective removal of perchlorate, among which the Mn-Mo-NC catalyst can achieve 78.23% removal of perchlorate in only 300 s, and its performance is significantly higher than that of the commonly used activated carbon adsorbent (only 5.11%).
[0113] Example 6 Parameter Optimization Experiment The Mn-Mo-NC catalytic material was prepared by the same method as in Example 1, except that the ratio of metal salt to ligand organic matter added in step (1) and step (5) was different, and samples 1-3 were prepared respectively.
[0114] Samples 1-3 were used as catalysts to adsorb and remove perchlorate in drinking water, specifically including the following steps: Step (1), prepare 50 mL of perchlorate water sample with a concentration of 10 mg / L; Step (2): Add 0.3 g / L catalyst to the water sample prepared in step (1), and use a stirrer to react at 1200 r / min. The reaction time is 300 s, and the perchlorate content is tested. The results are shown in Table 2. From the test results, it can be seen that the ratio of metal salt to ligand organic matter significantly affects the characteristics of the catalyst, and thus affects the removal rate.
[0115] Table 2. Removal efficiency of perchlorate in drinking water by catalysts prepared with different addition ratios Example 7 Formic acid enhanced removal of perchlorate from drinking water Step (1), prepare 50 mL of perchlorate water sample with a concentration of 10 mg / L; Step (2), add 0.3 g / L of Mn-Mo-NC prepared in Example 1 as a catalyst to the water sample prepared in step (1), and simultaneously add formic acid of different concentrations, and use a stirrer to react at 1200 r / min. The reaction time is 30 min, and the perchlorate content is detected.
[0116] Step (3), placing the remaining reaction liquid in step (2) in a suction filtration device to recover the catalyst after the reaction; Step (4), the recovered catalytic material was put into 50 mL of NaOH solution for analytical elution, and the chloride ion content in the eluted product was detected by sampling at 30 minutes. The results are shown in Table 3.
[0117] Table 3. Effect of formic acid concentration on the removal of perchlorate from drinking water From the results, it can be seen that, on the one hand, the addition of formic acid can further enhance the removal effect of the material on perchlorate, mainly because formic acid can enhance the chemical adsorption of perchlorate. On the other hand, by adjusting the amount of formic acid used, the process of removing perchlorate is strengthened, and nearly 98.23% of perchlorate can be removed. From the detection of the eluted product, it can be further known that the catalyst can further reduce perchlorate to chloride ions.
[0118] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A carbon-based confined bimetallic single-atom catalytic material, characterized in that: The catalytic material has a carbon base as a skeleton and nitrogen atoms as coordinating atoms, and achieves dispersion and fixation of specific metal atoms in the form of single atoms through a metal-nitrogen (Me-N) coordination structure; the metal atoms are any two of Mn, Cu, Ni, and Mo.
2. A carbon-based confined bimetallic single-atom catalytic material according to claim 1, characterized in that: The metal atoms are any combination of Mo-Mn, Mo-Cu, Mo-Ni and Mo-Mo.
3. The method for preparing a carbon-based confined bimetallic single-atom catalytic material according to claim 1, characterized in that: The specific steps are as follows: (1) Preparing a precursor solution: using dimethylformamide as a solvent, preparing a solution A containing zinc nitrate and a first metal salt, and a solution B containing 2-methylimidazole; (2) Growing nanocrystals: mixing solutions A and B, keeping them warm under sealed conditions to promote the growth of nanocrystals with metal-nitrogen coordination structures, removing impurities by centrifugation and washing, and vacuum drying the precipitate to obtain nanocrystals; (3) Primary calcination: In a nitrogen atmosphere, the nanocrystals are heated to 900-1200°C for primary calcination; (4) Acid washing: The material after the primary calcination is subjected to acid washing, suction filtration, washing, and vacuum drying to obtain a carbon-based material; (5) Introduction of the second metal: fully dispersing the carbon-based material in an isopropanol solution, adding the second metal salt and melamine, ultrasonically dispersing, recovering, drying, and collecting particles; (6) Secondary calcination: In a nitrogen atmosphere, the particles are heated to 800-1000 °C for secondary calcination to obtain a carbon-based confined bimetallic single atom catalytic material.
4. The method for preparing the carbon-based confined bimetallic single-atom catalytic material according to claim 3, characterized in that: The molar ratio of zinc nitrate, the first metal salt and 2-methylimidazole in step (1) is 10-30:1:20-60.
5. The method for preparing the carbon-based confined bimetallic single atom catalytic material according to claim 3, characterized in that: In step (5), the molar ratio of the second metal salt to 2-methylimidazole is 1:1-5.
6. A method for removing perchlorate from drinking water, characterized in that: The carbon-based confined bimetallic single-atom catalytic material according to any one of claims 1 to 2 is used as a catalyst to remove perchlorate from drinking water.
7. According to a method for removing perchlorate in drinking water according to claim 6, when the carbon-based confined bimetallic single-atom catalytic material is used as a catalyst, it has a powdery, granular or carrier-loaded form.
8. A method for removing perchlorate from drinking water according to claim 7, characterized in that: The treatment process is enhanced with formic acid.
9. A method for removing perchlorate from drinking water according to claim 7, characterized in that: The catalyst and a certain concentration of formic acid are sequentially added into a reactor containing the water sample to be purified, and the mixture is stirred sufficiently. The residence time of the water sample in the reactor is controlled to be 5 to 30 minutes, and then the mixture is filtered and the catalyst is recovered.
10. A method for removing perchlorate from drinking water according to claim 8, characterized in that: The concentration of formic acid is 0.5~2 mM.
Citation Information
Patent Citations
Oxygen reduction electrocatalyst of cobalt monatomic isolated platinum nanoparticles and preparation method of oxygen reduction electrocatalyst
CN115318322A
Method for controlling disinfection by-products in drinking water through catalytic ozonation
CN117645356A
Preparation method and application of molybdenum monatomic porous carbon
CN117942966A
Method for preparing laminar zinc hydroxide organic-inorganic nanocomposites for use in the removal and degradation of dyes from textile effluents
US20190193061A1