Beneficiation method for recovering copper from copper flotation tailings
Through flotation, remilling and sweeping steps, combined with adjusting agents such as lime, ethioamethane and pineol oil, the copper recovery rate of copper tailings was successfully improved, the problem of low copper resource utilization was solved, and copper was realized Efficient utilization of resources.
Patent Information
- Application Number
- CN202411179267.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-08-26
AI Technical Summary
The existing technology is difficult to effectively recover copper resources in copper tailings, resulting in low copper resource utilization, hindering the rapid growth of the country's economy and the sustainable development of mines.
A method for recycling copper tailings is adopted, including flotation, remilling and sweeping steps, flotation, pre-grade, remilling and remilling by adding adjusting agents such as lime, ethylthiomidine and pineol oil, flotation, pre-grade, remilling and Improve the slurry adjustment, gradually improve the copper enrichment ratio and recovery rate, and finally obtain high-grade copper concentrate.
The copper recovery rate of 15% to 40% in copper tailings was achieved, the utilization efficiency of copper resources was improved, the copper content of tailings was reduced, and the problem of insufficient utilization of copper resources was solved.
Smart Images

Figure CN118904525A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ore dressing, and in particular relates to an ore dressing method for recovering copper from copper tailings. Background Art
[0002] At present, the consumption and use of copper have become the criterion for judging the degree of industrialization of a country. However, the increasingly scarce, fine and mixed copper resources, as well as the equipment and technology, have seriously hindered the rapid growth of the national economy. Improving the comprehensive utilization of complex mineral resources and the economic benefits of mines can not only ensure the sustainable development of the national economy, but also is a major issue of technological innovation.
[0003] The beneficiation method of copper ore usually includes grinding, flotation and other steps. First, the ore will be crushed and ground to dissociate the copper metal into monomers, and then the copper ore will be separated from other impurities through the flotation process to obtain high-purity copper concentrate. In recent years, the growth of domestic copper mine production capacity and output has been limited. Obtaining greater copper output from limited copper resources and improving copper ore beneficiation indicators have become the focus of industry attention. Affected by production costs and technical levels, useful components such as copper, gold, and silver are often left in copper tailings. As rich ore resources gradually decrease, extracting these elements from tailings will help alleviate the problem of resource shortages.
[0004] In order to further improve the comprehensive utilization rate of resources, a mineral processing method for recovering copper from copper tailings is designed to further improve the economic, social and ecological benefits of mines and promote the green and high-quality development of mines. Summary of the invention
[0005] The invention discloses a ore dressing method for recovering copper from copper tailings, so as to solve any of the above and other potential problems in the prior art.
[0006] In order to solve the above technical problems, the technical solution of the present invention is: a beneficiation method for recovering copper from copper tailings, the beneficiation method specifically comprises the following steps:
[0007] S1) flotation is performed on the copper tailings to be processed to obtain a copper rough concentrate and flotation tailings;
[0008] S2) pre-classifying the copper rough concentrate obtained in S1), mixing the pre-classified sediment obtained in the pre-classification with a certain amount of adjusting agent A and feeding it into a regrinding mill; inspecting and classifying the regrinding discharge product obtained by using a cyclone, and returning the inspected and classified sediment to the regrinding mill;
[0009] S3) The pre-classified overflow product of S2) and the inspection-classified overflow product are processed through one roughing selection and two scavenging selections, and finally a high enrichment ratio, low-yield copper concentrate and a flotation tailings with a greatly reduced copper grade are obtained, and the flotation tailings are returned to the primary flotation.
[0010] Furthermore, the specific process of the primary flotation in S1) is as follows: a certain amount of flotation adjusting agent, flotation collector and flotation frother are added during the flotation process, and after uniform mixing, the copper tailings are processed with a coarse particle flotation machine to obtain a copper rough concentrate with a copper grade of 0.5% to 1.5%.
[0011] Furthermore, the flotation adjusting agent is lime, and the addition amount is 1000-2000 g / t; the flotation collector is ethionamide, and the addition amount is 3-10 g / t; the flotation frother is pine oil, and the addition amount is 1-2 g / t.
[0012] Further, the specific steps of S2 are:
[0013] S2.1) The copper concentrate obtained in S1) is slurried into a slurry with a mass percentage concentration of 35% to 45%, and pre-classified using a hydrocyclone, and the pre-classification overflow fineness is controlled to be -0.074mm, accounting for 90% to 95%;
[0014] S2.2) The obtained pre-classified sand is fed into the regrinding mill for grinding. During the grinding process, the adjusting agent A is added. The grinding product is inspected and classified by a hydrocyclone. The inspection and classification overflow fineness is controlled to be -0.074mm, accounting for 90% to 95%. The inspection and classification sand is fed into the regrinding mill for grinding.
[0015] S2.3) The pre-classification overflow of S2.1) and the inspection classification overflow of S2.2) are taken as the total overflow of regrinding and enter the subsequent flotation operation; wherein the adjusting agent A is lime, and the addition amount is 2000-3000g / t.
[0016] Further, the total overflow of the regrind in S2.3) enters the mixing barrel, and a certain amount of regrind collector and regrind foaming agent C are added, followed by high-strength modification and slurry adjustment;
[0017] Furthermore, the regrinding collector is ethiocarbamate, and the addition amount is 20-40 g / t; the regrinding foaming agent is pine oil, and the addition amount is 5-10 g / t.
[0018] Furthermore, the first roughing and second scavenging in S3) adopt an aerated stirring flotation machine; and the copper concentrate is directly obtained from the roughing, and the concentrates from the first scavenging and second scavenging are directly returned to the stirring barrel.
[0019] Furthermore, a scavenging collector and a scavenging foaming agent are added to both the primary scavenging and the secondary scavenging; wherein the primary scavenging collector B is ethylthiocarbamate, the addition amount is 10-20 g / t, the primary scavenging foaming agent is pine oil, the addition amount is 3-5 g / t; the secondary scavenging collector B is ethylthiocarbamate, the addition amount is 5-10 g / t, the secondary scavenging foaming agent is pine oil, the addition amount is 1-3 g / t.
[0020] The copper concentrate obtained by the beneficiation method has a grade of not less than 15.00%, and a copper recovery rate of not less than 14.00%. The beneficial effects of the present invention are as follows: due to the adoption of the above technical scheme, the beneficiation method for recovering copper from copper tailings of the present invention is to enrich the copper in the coarse-grained ore in the copper tailings through a single flotation, and recover 15% to 40% of the copper in the copper tailings; then the material is evenly ground by regrinding to achieve efficient dissociation of copper minerals. The surface of the mineral is scrubbed by a reformer to achieve full mixing of copper and reagents; a single roughing directly obtains copper concentrate, and the first scavenging and second scavenging concentrates are returned to the stirring barrel to reduce the circulation of the middling ore, and the flotation tailings are reselected to further improve the copper recovery rate; the method of the present invention can effectively reduce the copper content of the tailings, solve the technical problem of insufficient utilization of copper resources, and improve the utilization efficiency of copper resources. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 The present invention is a process flow chart of a method for recovering copper from copper tailings. DETAILED DESCRIPTION
[0022] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0023] On the contrary, the present invention covers any substitution, modification, equivalent method and scheme made on the essence and scope of the present invention as defined by the claims. Further, in order to make the public have a better understanding of the present invention, some specific details are described in detail in the detailed description of the present invention below. Those skilled in the art can fully understand the present invention without the description of these details.
[0024] Example 1
[0025] This embodiment provides a method for recovering copper from copper tailings. The original ore is copper tailings from Ruichang City, Jiujiang City, Jiangxi Province. The copper grade of the tailings is 0.105%. Figure 1The separation process is as follows: (1) Pre-flotation operation: add 1500g / t lime, 8g / t ethionamide and 2g / t pine oil to the copper tailings, and pre-flotate at a mass percentage concentration of 30% to 45% to obtain a coarse concentrate with a copper grade of 1.15%. (2) Re-grinding operation of the medium ore: slurry the coarse concentrate product to a concentration of 40%, pre-grade it through a cyclone, check the overflow -0.074mm and account for 93.51%, use a regrinding machine to grind the sediment, and add 3000g / t lime. The regrinding discharge product is checked and graded through a cyclone, and the check classification overflow -0.074mm accounts for 90.63%. (3) Mixing, reforming and slurry mixing operation. Add 35g / t ethionamide and 5g / t pine oil to the mixing barrel and act for 3 minutes; the mixed product enters the reformer, the reformer speed is 40Hz, and acts for 2 minutes. (3) Copper flotation roughing: the stirred product is fed into a KYF fine flotation machine for sorting for 3 minutes to obtain copper concentrate and roughing tailings. (4) Copper primary scavenging: 20 g / t ethiocarbamate and 2 g / t pine oil are added to the roughing tailings, and fed into a KYF fine flotation machine for sorting for 3 minutes to obtain copper primary scavenging concentrate and primary scavenging tailings. (5) Copper secondary scavenging: 10 g / t ethiocarbamate and 1 g / t pine oil are added to the roughing tailings, and fed into a KYF fine flotation machine for sorting for 3 minutes to obtain copper secondary scavenging concentrate and secondary scavenging tailings. (6) The primary scavenging concentrate and secondary scavenging concentrate are returned to the stirring barrel, and the secondary scavenging tailings enter the pre-flotation. (7) The grade of the obtained copper concentrate is 18.65%, and the copper recovery rate is 18.47%.
[0026] Example 2
[0027] This embodiment provides a method for recovering copper from copper tailings. The original ore is copper tailings from Chaisang District, Jiujiang City, Jiangxi Province. The copper grade of the tailings is 0.095%. Figure 1The sorting process is as follows: (1) Pre-flotation operation: add 2000g / t lime, 10g / t ethionamide and 2g / t pine oil to the copper tailings, and pre-flotate at a mass percentage concentration of 35% to 40% to obtain a coarse concentrate with a copper grade of 0.96%. (2) Middling regrinding operation: slurry the coarse concentrate product to a concentration of 40%, pre-grade it through a cyclone, check the overflow -0.074mm and account for 94.58%, use a regrinding machine to grind the sediment, and add 2000g / t lime. The regrinding discharge product is checked and graded through a cyclone, and the check classification overflow -0.074mm accounts for 93.36%. (3) Mixing, reforming and slurry mixing operation. Add 40g / t ethionamide and 6g / t pine oil to the mixing barrel and act for 3 minutes; the stirred product enters the reformer, the reformer speed is 45Hz, and acts for 2 minutes. (3) Copper flotation roughing: the stirred product is fed into a KYF fine flotation machine for sorting for 3 minutes to obtain copper concentrate and roughing tailings. (4) Copper primary scavenging: 20 g / t ethiocarbamate and 2 g / t pine oil are added to the roughing tailings, and fed into a KYF fine flotation machine for sorting for 3 minutes to obtain copper primary scavenging concentrate and primary scavenging tailings. (5) Copper secondary scavenging: 10 g / t ethiocarbamate and 2 g / t pine oil are added to the roughing tailings, and fed into a KYF fine flotation machine for sorting for 3 minutes to obtain copper secondary scavenging concentrate and secondary scavenging tailings. (6) The primary scavenging concentrate and secondary scavenging concentrate are returned to the stirring barrel, and the secondary scavenging tailings enter the pre-flotation. (7) The grade of the obtained copper concentrate is 15.35%, and the copper recovery rate is 15.98%.
[0028] Example 3
[0029] This embodiment provides a method for recovering copper from copper tailings. The original ore is copper tailings from Dexing City, Shangrao City, Jiangxi Province. The copper grade of the tailings is 0.045%. Figure 1The separation process is as follows: (1) Pre-flotation operation: add 1200g / t lime, 5g / t ethionamide and 2g / t pine oil to the copper tailings, and pre-flotate at a mass percentage concentration of 35% to 45% to obtain a coarse concentrate with a copper grade of 0.58%. (2) Re-grinding operation of the medium ore: slurry the coarse concentrate product to a concentration of 35%, pre-grade it through a cyclone, check the overflow -0.074mm and account for 92.17%, use a regrinding machine to grind the sediment, and add 2000g / t lime. The regrinding discharge product is checked and graded through a cyclone, and the check classification overflow -0.074mm accounts for 91.58%. (3) Mixing, reforming and slurry mixing operation. Add 25g / t ethionamide and 5g / t pine oil to the mixing barrel and act for 3 minutes; the stirred product enters the reformer, the reformer speed is 45Hz, and acts for 2 minutes. (3) Copper flotation roughing: the stirred product is fed into a KYF fine flotation machine for sorting for 3 minutes to obtain copper concentrate and roughing tailings. (4) Copper primary scavenging: 10 g / t ethiocarbamate and 1 g / t pine oil are added to the roughing tailings, and fed into a KYF fine flotation machine for sorting for 3 minutes to obtain copper primary scavenging concentrate and primary scavenging tailings. (5) Copper secondary scavenging: 5 g / t ethiocarbamate and 1 g / t pine oil are added to the roughing tailings, and fed into a KYF fine flotation machine for sorting for 3 minutes to obtain copper secondary scavenging concentrate and secondary scavenging tailings. (6) The primary scavenging concentrate and secondary scavenging concentrate are returned to the stirring barrel, and the secondary scavenging tailings enter the pre-flotation. (7) The grade of the obtained copper concentrate is 15.74%, and the copper recovery rate is 14.31%.
[0030] The above is a detailed introduction to a method for recovering copper from copper tailings provided in the embodiment of the present application. The description of the above embodiment is only used to help understand the method and core idea of the present application; at the same time, for those skilled in the art, according to the idea of the present application, there will be changes in the specific implementation method and application scope. In summary, the content of this specification should not be understood as limiting the present application.
[0031] For example, certain words are used in the specification and claims to refer to specific components. Those skilled in the art should understand that hardware manufacturers may use different nouns to refer to the same component. This specification and claims do not use differences in names as a way to distinguish components, but use differences in the functions of components as the criteria for distinction. As mentioned throughout the specification and claims, "including" and "comprising" are open-ended terms, so they should be interpreted as "including / including but not limited to". "Approximately" means that within an acceptable error range, those skilled in the art can solve the technical problem within a certain error range and basically achieve the technical effect. The subsequent description of the specification is a preferred embodiment of the present application, but the description is for the purpose of illustrating the general principles of the present application, and is not used to limit the scope of the present application. The scope of protection of the present application shall be determined by the definition of the attached claims.
[0032] It should also be noted that the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a product or system including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such a product or system. In the absence of more restrictions, the elements defined by the sentence "comprises a ..." do not exclude the existence of other identical elements in the product or system including the elements.
[0033] It should be understood that the term "and / or" used in this article is only a description of the association relationship of associated objects, indicating that there can be three relationships. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in this article generally indicates that the associated objects before and after are in an "or" relationship.
[0034] The above description shows and describes several preferred embodiments of the present application, but as mentioned above, it should be understood that the present application is not limited to the form disclosed herein, and should not be regarded as excluding other embodiments, but can be used in various other combinations, modifications and environments, and can be modified within the scope of the application concept described herein through the above teachings or the technology or knowledge of the relevant field. The changes and modifications made by those skilled in the art do not deviate from the spirit and scope of the present application, and should be within the scope of protection of the claims attached to the present application.
Claims
1. A method for recovering copper from copper tailings, characterized in that: The ore dressing method specifically comprises the following steps: S1) flotation is performed on the copper tailings to be processed to obtain a copper rough concentrate and flotation tailings; S2) pre-classifying the copper rough concentrate obtained in S1), mixing the pre-classified sediment obtained in the pre-classification with a certain amount of adjusting agent A and feeding it into a regrinding mill; inspecting and classifying the regrinding discharge product obtained by using a cyclone, and returning the inspected and classified sediment to the regrinding mill; S3) The pre-classified overflow product of S2) and the inspection-classified overflow product are processed through one roughing selection and two scavenging selections, and finally a high enrichment ratio, low-yield copper concentrate and a flotation tailings with a greatly reduced copper grade are obtained, and the flotation tailings are returned to the primary flotation.
2. The ore dressing method according to claim 1, characterized in that: The specific process of the primary flotation in S1) is as follows: a certain amount of flotation regulator, flotation collector and flotation frother are added during the flotation process, mixed evenly, and then the copper tailings are processed with a coarse particle flotation machine to obtain a copper concentrate with a copper grade of 0.5% to 1.5%.
3. The ore dressing method according to claim 2, characterized in that: The flotation adjusting agent is lime, and the addition amount is 1000-2000 g / t; the flotation collector is ethionamide, and the addition amount is 3-10 g / t; the flotation frother is pine oil, and the addition amount is 1-2 g / t.
4. The ore dressing method according to claim 1, characterized in that: The specific steps of S2 are: S2.1) The copper concentrate obtained in S1) is slurried into a slurry with a mass percentage concentration of 35% to 45%, and pre-classified using a hydrocyclone, and the pre-classification overflow fineness is controlled to be -0.074mm, accounting for 90% to 95%; S2.2) The obtained pre-classified sand is fed into the regrinding mill for grinding. During the grinding process, the adjusting agent A is added. The grinding product is inspected and classified by a hydrocyclone. The inspection and classification overflow fineness is controlled to be -0.074mm, accounting for 90% to 95%. The inspection and classification sand is fed into the regrinding mill for grinding. S2.3) The pre-classification overflow of S2.1) and the inspection classification overflow of S2.2) are taken as the total overflow of regrinding and enter the subsequent flotation operation; wherein the adjusting agent is lime, and the addition amount is 2000-3000g / t.
5. The ore dressing method according to claim 4, characterized in that: The regrinding process in S2.3) is as follows: the total overflow of regrinding is now fed into a mixing barrel, a certain amount of regrinding collector and regrinding foaming agent are added, and then high-intensity modification and slurry adjustment are performed.
6. The ore dressing method according to claim 5, characterized in that: The regrinding collector is ethiocarbamate, and the addition amount is 20-40 g / t; the regrinding foaming agent is pine oil, and the addition amount is 5-10 g / t.
7. The ore dressing method according to claim 1, characterized in that: The first roughing and second scavenging in S3) adopt an aerated stirring flotation machine; and the copper concentrate is directly obtained from the roughing, and the concentrates from the first scavenging and second scavenging are directly returned to the stirring barrel.
8. The ore dressing method according to claim 7, characterized in that: A scavenging collector and a scavenging foaming agent are added during both the primary scavenging and the secondary scavenging; wherein the primary scavenging collector is ethylthiocarbamate, the addition amount is 10-20 g / t, the primary scavenging foaming agent is pine oil, the addition amount is 3-5 g / t; the secondary scavenging collector is ethylthiocarbamate, the addition amount is 5-10 g / t, the secondary scavenging foaming agent is pine oil, the addition amount is 1-3 g / t.
9. The ore dressing method according to claim 1, characterized in that: The grade of the copper concentrate obtained by the ore dressing method is not less than 15.00%, and the copper recovery rate is not less than 14.00%.
Citation Information
Patent Citations
Method for recovering indium-enriched marmatite from copper, zinc and indium coexisting polymetallic ore under low-alkaline condition
CN106622641A
Technological method for recycling copper through grading and regrinding copper flotation tailings
CN109663653A
Chalcocite-contained coarse-grain disseminated copper sulfide ore step-by-step ore grinding flotation method
CN110292984A
Beneficiation method for complex disseminated low-grade copper-sulfur ore
CN113751180A
Beneficiation method for recovering valuable metal from high-grade copper and sulfur symbiotic polymetallic ore
CN116510884A
Cited By
Method for solidifying copper tailing waste through magnesium oxychloride cement
CN120483666A