Metal injection molding method for reducing gap pollution of titanium alloy product
By constructing a multivariate regression model to optimize powder configuration and sintering temperature, combined with the hydrogenation-dehydrogenation method, the gap pollution problem of porous titanium alloy in metal injection molding process is solved, the porosity and tensile strength control is improved, and high Manufacturing of porous titanium alloys with precision.
Patent Information
- Application Number
- CN202410952032.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-16
AI Technical Summary
Existing porous titanium alloys are susceptible to gap contamination in metal injection molding processes, resulting in long demolding time, difficult to control porosity and pore size, poor mechanical properties, and unstable process.
By constructing a multivariate regression model, the relationship between powder particle size and sintering temperature is determined, the powder configuration and production process are optimized, the porosity is reduced and the tensile strength is improved, and the irregular shape of Ti–6Al is obtained by using the hydrogenation-dehydrogenation method. –4V powder and polyformaldehyde adhesive, combined with the crushing and sintering process, adjusting the powder size and sintering temperature to reduce gap contamination.
Effectively reduces gap pollution of titanium alloy products, improves the control accuracy of porosity and tensile strength, enhances the mechanical properties of the material, simplifies the process flow, and reduces the use of space brackets. It is suitable for the manufacture of high-precision porous titanium alloy products. .
Smart Images

Figure CN118905223A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of titanium alloy product processing, and in particular to a metal injection molding method for reducing gap contamination of titanium alloy products. Background Art
[0002] Metal Injection Molding (MIM) is a process that involves mixing metal powder and a binder, performing injection molding and degreasing processes, and then performing a high-density sintering process. Metal injection molding has been widely used in the manufacturing of different industries such as medical, automotive, and aerospace. Titanium alloys, as key industrial metal materials, have the advantages of non-magnetic properties, gorgeous appearance, excellent chemical resistance, excellent strength-to-weight ratio, and good biocompatibility. MIM processes have been widely commercialized in portable electronics, healthcare, and shipbuilding. MIM products have higher strength, high precision, and complexity than products produced by other processes such as die casting, investment casting, sand casting, and molding routes. Ti-6Al-4V is a commonly used metal powder for processing, but titanium is a highly active metal that can react with almost all elements. At high temperatures, it can also react with gaseous compounds such as CO, CO2, water vapor, NH4, and many volatile organic compounds. During the heating process, the reaction of metal elements with the titanium surface results in surface contamination and changes in chemical composition. Some gas elements not only form compounds on the titanium surface, but also enter the metal lattice to form interstitial solid solutions, affecting the quality of the finished product. Among them, porous Ti-6Al-4V alloy has been widely used in industry as a structural or functional material because of its unique corrosion resistance. Porous titanium alloys can reduce the density of titanium alloys, and the presence of micropores can promote their application in biomedical devices. However, this porous titanium alloy is prone to collapse or deformation under mechanical force, resulting in reduced mechanical strength, weak structural integrity, and difficulty in manufacturing. In addition, during processing, the pores may be contaminated by cutting fluids and debris, causing material degradation over time. The size and distribution of micropores are also difficult to adjust in practical applications, and it is even more challenging to manufacture microporous metal parts with complex geometries and high precision.
[0003] Existing porous titanium alloys are mostly processed by using volatiles such as sugars, salts and polymers as space supports. The traditional method of producing porous Ti-6Al-4V using space supports through metal injection molding (MIM) has some disadvantages. In order to remove the space supports, salt-based materials are usually removed by dissolution, evaporation and sublimation. However, the dissolution process can be time-consuming, taking up to 72 hours, and causes the titanium alloy to expand. On the other hand, methods such as evaporation or sublimation using vacuum furnaces may contaminate the vacuum chamber, causing the space holder material to condense in the vacuum pump, and the titanium alloy gap contamination is more serious.
[0004] In summary, for porous Ti-6Al-4V alloy, its demolding time is long, it is susceptible to gap contamination in the sintering furnace, the porosity and pore size cannot be controlled, the mechanical properties are poor, the process is unstable, etc. Therefore, how to reduce the gap contamination of Ti-6Al-4V alloy in MIM processing and improve the mechanical properties of the product is an urgent problem to be solved.
[0005] SUMMARY OF THE INVENTION
[0006] In view of the above technical problems, the present invention provides a metal injection molding method for reducing gap contamination of titanium alloy products, including: including powder configuration and manufacturing process, determining the relationship between powder particle size, sintering temperature, porosity and tensile strength by constructing a multivariate regression model, inferring the particle size of the powder and the sintering temperature used in the manufacturing process according to the required tensile strength and porosity requirements of the titanium alloy product, and then processing the configured powder into a titanium alloy product through the manufacturing process, wherein the multivariate regression model reflects that the increase in powder size and the decrease in sintering temperature increase the porosity and pore size, resulting in a decrease in tensile strength;
[0007] The porosity is represented by Y1, the powder size is represented by X1, and the sintering temperature is represented by X2. The dependence after fitting is:
[0008] Y1=-0.0072×X1 2 -0.0001×X2 2 +0.0004×X1×X2+1.031X1+0.185X2-50.9(1)
[0009] The formula represents the relationship between porosity (Y1) and powder size (X1) and sintering temperature (X2), where -0.0072×X1 2 represents the effect of the square of powder size on porosity, 0.00041×X1×X2 represents the effect of the interaction between powder size and sintering temperature on porosity, 1.031X1 represents the linear effect of powder size on porosity, 0.185X2 represents the linear effect of sintering temperature on porosity, and -50.9 represents the intercept of the model;
[0010] The tensile strength is expressed as Y2, and the dependence after fitting is:
[0011]
[0012] Furthermore, the powder material includes irregularly shaped Ti-6Al-4V powder obtained by a hydrogenation-dehydrogenation method and a polyoxymethylene binder, wherein the hydrogenation-dehydrogenation process includes hydrogenation of sponge titanium, crushing of generated brittle hydride, and dehydrogenation to obtain the powder.
[0013] Furthermore, the P value is used to measure the possibility of observing the data if there is no relationship between porosity or tensile strength and the variables. A low P value indicates the sufficiency of the strong correlation between the variables. The P values of equation (1) and equation (2) are both less than 0.001.
[0014] Furthermore, the R-sq is used to measure the degree of fit of the regression model. A high R-sq indicates that the model fits the data well. The R-sq of equation (1) is 97.5%, and the R-sq of equation (2) is 97.79%.
[0015] Furthermore, the manufacturing process includes powder particle mixing and crushing, injection molding, degreasing, sintering and post-processing. The manufacturing process also includes setting the powder particle size and sintering temperature according to the required tensile strength and porous porosity requirements. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] The present invention will be further described below in conjunction with the accompanying drawings.
[0017] Figure 1 (a) is the relationship between powder size, sintering temperature and porosity;
[0018] Figure 1 (b) Construction sequence for the porosity model;
[0019] Figure 1 (c) is the statistically significant relationship between Y1 and X variables;
[0020] Figure 1 (d) is the R-sq accuracy of the model;
[0021] Figure 1 (e)-(g) are the relationship diagrams between porosity and powder size and sintering temperature, respectively;
[0022] Figure 2 (a) Relationship between powder size, sintering temperature and tensile strength.
[0023] Figure 2 (b) Construction sequence for tensile strength model;
[0024] Figure 2 (c) is the statistically significant relationship between Y2 and X variables;
[0025] Figure 2 (d) is the R-sq accuracy of the model;
[0026] Figure 2 (e)-(g) are the relationship diagrams of tensile strength, powder size and sintering temperature, respectively. DETAILED DESCRIPTION
[0027] Various aspects of the present invention are described in further detail below.
[0028] Unless otherwise defined or indicated, all professional and scientific terms used herein have the same meaning as those familiar to those skilled in the art. In addition, any method and material similar or equivalent to the described content can be applied to the method of the present invention.
[0029] The present invention provides a metal injection molding method for reducing gap contamination of titanium alloy products, including powder configuration and manufacturing process, by constructing a multivariate regression model to determine the relationship between powder particle size, sintering temperature, porosity and tensile strength, according to the required tensile strength and porosity requirements of the titanium alloy product, the powder particle size and the sintering temperature used in the manufacturing process are inferred, and then the configured powder is processed into a titanium alloy product through the manufacturing process, such as Figure 1 (a) shows the relationship between powder size, sintering temperature and porosity. When the initial powder size (expressed as D50) decreases and the sintering temperature increases, the porosity of the sample decreases. When the powder with D50 = 100 μm is sintered at 1000 °C, a high porosity of 74% can be achieved. Figure 1 (b) shows the order of model construction. Powder size has a greater effect on porosity than sintering temperature. The multivariate regression model shows that as powder size increases and sintering temperature decreases, porosity and pore size increase, resulting in a decrease in tensile strength. Porosity is represented as Y1, powder size is represented as X1, and sintering temperature is represented as X2. The P value measures the likelihood of observing the data if there is no relationship between the Y and X variables. A low P value indicates the adequacy of the strong association between Y1 and the X variables (X1 and X2). Figure 1 (c) indicates that there is a statistically significant relationship between Y1 and X variables (p <
[0030] 0.001), the dependence after fitting is:
[0031] Y1=-0.0072×X1 2 -0.0001×X2 2 +0.0004×X1×X2+1.031X1+0.185X2-50.9(1)
[0032] The formula represents the relationship between porosity (Y1) and powder size (X1) and sintering temperature (X2), where -0.0072×1 2 represents the effect of the square of powder size on porosity, 0.00041×X1×X2 represents the effect of the interaction between powder size and sintering temperature on porosity, 1.031X1 represents the linear effect of powder size on porosity, 0.185X2 represents the linear effect of sintering temperature on porosity, and -50.9 represents the intercept of the model;
[0033] Figure 1 (d) shows that this model can achieve an R-sq of 97.5%, demonstrating the accuracy of the model. The predicted porosity variation as a function of the two X variables powder size and sintering temperature is plotted in Figure 1 (e)-(g). It can be seen that the porosity has a positive / negative correlation with the powder size and sintering temperature, respectively. This can be understood as the increase in temperature increases the size of the sintering neck, which may reduce the porosity. On the contrary, the larger powder size with irregular shapes leads to poor connection between particles and smaller specific surface area, requiring more energy to form sintering necks, resulting in increased porosity.
[0034] like Figure 2 As shown in (a), higher sintering temperature and smaller powder size promote the formation and growth of intergranular sintering necks, enhance intergranular bonding, reduce the porosity of the material, and ultimately lead to higher tensile strength. The highest tensile strength of 457MPa was achieved under the conditions of powder size D50 = 32μm and sintering temperature of 1200℃. Figure 2 (b) shows the order in which the model was built, demonstrating the order in which the variables were added. Powder size has a greater effect on tensile strength than sintering temperature.
[0035] The tensile strength is expressed as Y2, and the dependence after fitting is:
[0036]
[0037] Figure 2 (c) shows the statistical significance of the relationship between Y2 and X (X1 and X2) variables, with a P value less than 0.001. Figure 2 As shown in (d), an R-sq of up to 97.79% was achieved in this regression model, indicating that the regression model is very accurate and almost all the changes in Y2 can be explained by the changes in the X variable. The predicted dependence of the tensile strength on powder size and sintering temperature is given by equation (2), as Figure 2As shown in (e)-(g), it is clear from the data that there is a negative correlation between powder size and tensile strength, which means that larger powder sizes result in lower tensile strength. This is because larger powder particles will result in larger pores after sintering, reducing the effective cross-sectional area of the material under tensile loads and creating stress concentration points that can initiate and propagate cracks, leading to premature failure. In contrast, sintering temperature has a positive correlation with tensile strength, which means that as the sintering temperature increases, the tensile strength also increases. This is because higher sintering temperatures result in better densification and bonding of the powder particles, increasing the effective cross-sectional area of the material under tensile loads, reducing the size and number of pores, reducing stress concentration points that can initiate and propagate cracks, and improving material properties. In order to maintain the tensile strength of the Ti-6Al-4V MIM sample, it is necessary to minimize the porosity and ensure that any remaining pores are small and sealed. The model can be used to predict the optimal values of powder size and sintering temperature to achieve the desired porosity and tensile strength, or to evaluate the impact of these variables on material properties. Equations (1) and (2) provide an empirical model for the correlation between two key properties (porosity, tensile strength) and two controllable variables (powder size and sintering temperature), which can facilitate the in-house customized design of industrial porous Ti-6Al-4V materials. The model can be used to predict the optimal powder size and sintering temperature values for the desired porosity and tensile strength, or to evaluate the impact of changes in these variables on material properties.
[0038] The sintered density and relative density are negatively correlated with the porosity for different powder sizes. Therefore, for all powder sizes, the sintered density and relative density increase with increasing sintering temperature, which indicates that the pore size decreases and sintering at higher temperatures helps improve the density of the material. The sintered density and relative density also increase with decreasing powder size, which means that smaller particles have higher surface energy and shorter diffusion distances, which accelerates the densification process. Similar to the tensile strength, the 10% compressive strength is also affected by the powder size and sintering temperature of the porous Ti-6Al-4V material. In general, higher density leads to higher strength. Smaller particles tend to form finer grains and more evenly distributed pores, thereby enhancing strength. The sample with the highest compressive strength is the sample with a powder size of 32μm and a sintering temperature of 1200℃, which has the highest density. The content of interstitial elements such as carbon, nitrogen, and especially oxygen after sintering is also affected by particle size and sintering temperature. Smaller particles have a larger specific surface area and more interstitial element adsorption. Higher temperatures also facilitate the diffusion of interstitial elements into the metal matrix. The best conditions for reducing the interstitial element content are to use larger powder size and lower sintering temperature.
[0039] Therefore, by using the processing method of the present invention, various properties in the processing are predicted and reversed, and porous Ti-6Al-4V titanium alloy products with suitable porosity can be processed without the need for a spatial support, which can be used in the field of medical implants.
[0040] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. A metal injection molding method for reducing gap contamination of titanium alloy products, characterized in that: Including powder configuration and manufacturing process, by constructing a multivariate regression model to determine the relationship between powder particle size, sintering temperature, porosity and tensile strength, according to the required tensile strength and porosity requirements of the titanium alloy product, the powder particle size and the sintering temperature used in the manufacturing process are inferred, and then the configured powder is processed into a titanium alloy product through the manufacturing process. The multivariate regression model shows that the increase in powder size and the decrease in sintering temperature increase the porosity and pore size, resulting in a decrease in tensile strength; The porosity is represented by Y1, the powder size is represented by X1, and the sintering temperature is represented by X2. The dependence after fitting is: Y1=-0.0072×X1 2 -0.0001×X2 2 +0.0004×X1×X2+1.031X1+0.185X2-50.9(1) The formula represents the relationship between porosity (Y1) and powder size (X1) and sintering temperature (X2), where -0.0072×X1 2 represents the effect of the square of powder size on porosity, 0.00041×X1×X2 represents the effect of the interaction between powder size and sintering temperature on porosity, 1.031X1 represents the linear effect of powder size on porosity, 0.185X2 represents the linear effect of sintering temperature on porosity, and -50.9 represents the intercept of the model; The tensile strength is expressed as Y2, and the dependence after fitting is:
2. A metal injection molding method for reducing gap contamination of titanium alloy products as claimed in claim 1, characterized in that: The powder material comprises irregularly shaped Ti-6Al-4V powder obtained by a hydrogenation-dehydrogenation method and a polyoxymethylene binder. The hydrogenation-dehydrogenation process comprises hydrogenation of titanium sponge, crushing of generated brittle hydride and dehydrogenation to obtain the powder.
3. A metal injection molding method for reducing gap contamination of titanium alloy products as claimed in claim 2, characterized in that: The P value is used to measure the probability of observing the data if there is no relationship between porosity or tensile strength and the variables. A low P value indicates the sufficiency of a strong association between the variables. The P values of equation (1) and equation (2) are both less than 0.
001.
4. A metal injection molding method for reducing gap contamination of titanium alloy products as claimed in claim 3, characterized in that: The R-sq is used to measure the degree of fit of the regression model. A high R-sq indicates that the model fits the data well. The R-sq of equation (1) is 97.5%, and the R-sq of equation (2) is 97.79%.
5. A metal injection molding method for reducing gap contamination of titanium alloy products as claimed in claim 1, characterized in that: The manufacturing process includes powder particle mixing and crushing, injection molding, degreasing, sintering and post-processing.
6. A metal injection molding method for reducing gap contamination of titanium alloy products as claimed in claim 5, characterized in that: The manufacturing process also includes setting the crushing particle size of the powder and the sintering temperature of the sintering according to the required tensile strength and porous porosity requirements.
Citation Information
Patent Citations
Foamed metal porosity measuring method
CN108470110A
Temperature measuring ring and method for calibrating temperature of injection molding titanium alloy sintering furnace
CN117182077A
Injection-molded high-strength titanium alloy and preparation method thereof
CN118060542A
Method for fabricating biocompatible porous titanium
US20140348688A1
Manufacture of near-net shape titanium alloy articles from metal powders by sintering with presence of atomic hydrogen
WO2016205263A1