Green cementing material as well as preparation method and application thereof

By using low-calcium solid waste fly ash, coal gasification slag and coal gangue and other materials, high-strength green gelling materials are prepared, which solves the durability of traditional cement slurry in water-rich environments and The retention rate problem has improved the utilization rate of solid waste, and is suitable for underground engineering governance, achieving efficient environmental governance and resource recycling.

CN118908647APending Publication Date: 2024-11-08QINGDAO METRO LINE 6 CO LTD +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410953241.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In water-rich and corrosive environments, traditional cement slurries have problems such as poor durability, long settling time and low water retention rate, which cannot meet the needs of tunnel and underground engineering management. At the same time, the utilization rate of bulk solid waste is low, resulting in Severe environmental pollution.

Method used

Use low-calcium solid waste fly ash, coal gasification slag and coal gangue as matrix materials, combine cement, alkaline substances and salt substances as composite excitants, and use water reducing agents, flocculants, premature strength agents and other admixtures. Prepare high-strength and strong permeability green gelling material, which is suitable for grouting and filling projects.

Benefits of technology

It has achieved efficient management of underground engineering disasters in a water-rich and corrosive environment, improved the utilization rate of solid waste resources, reduced costs, and significantly improved the corrosion resistance and stability of materials, solving the durability and retention of traditional cement slurry Rate issue.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004947814310000081
    Figure BDA0004947814310000081
  • Figure BDA0004947814310000091
    Figure BDA0004947814310000091
  • Figure BDA0004947814310000092
    Figure BDA0004947814310000092
Patent Text Reader

Abstract

The invention discloses a green cementing material as well as a preparation method and application thereof, and the green cementing material is prepared from the following components in parts by mass: 80-100 parts of slag, 120-180 parts of fly ash, 120-300 parts of coal gasification slag, 80-120 parts of coal gangue, 80-90 parts of a composite activator and 20-30 parts of an additive, the composite exciting agent comprises the following components in parts by weight: 6-10 parts of sodium hydroxide, 20-30 parts of water glass, 10-30 parts of calcium chloride and 60-80 parts of cement; and the additive comprises the following components in parts by weight: 7-10 parts of a water reducing agent, 8-15 parts of a flocculating agent and 3-5 parts of an early strength agent. The green cementing material has the properties of high strength, high forming speed, good stability and the like, is beneficial to realizing efficient treatment of underground engineering disasters and resource utilization of a large amount of solid wastes, and can further improve the stability of underground engineering backfill and reduce settlement deformation and cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of comprehensive utilization of solid waste and preparation of engineering materials, and mainly relates to a green gelling material and a preparation method and application thereof. Background Art

[0002] The statements herein merely provide background information related to the present invention and do not necessarily constitute prior art.

[0003] In the construction of tunnels and underground projects, due to the existence of unfavorable geological conditions such as fault fracture zones and karst fissures, disasters such as sudden water and mud are often encountered, causing serious property losses, project delays and casualties. Grouting technology has been widely used due to its excellent treatment effect. However, in water-rich and corrosive environments, traditional cement slurries have problems such as poor durability, long setting time, and low dynamic water retention rate, which cannot meet the needs of engineering treatment.

[0004] At present, the output of bulk solid waste is large and the utilization rate is low. Its large-scale stacking seriously pollutes the environment and urgently needs to be recycled. Statistics show that the accumulated stockpile of bulk solid waste in a certain country is about 60 billion tons, and the annual increase in stockpile is nearly 3 billion tons. It is urgent to develop high value-added application technologies to realize the transformation of industrial solid waste into treasure. Summary of the invention

[0005] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a green cementitious material and its preparation method and application. The green cementitious material has the properties of high strength, fast molding, good stability, etc., which is conducive to the efficient management of underground engineering disasters and the resource utilization of large amounts of solid waste, and can further improve the stability of underground engineering backfill, reduce settlement deformation and reduce costs.

[0006] In order to achieve the above object, the present invention is implemented through the following technical solutions:

[0007] In a first aspect, the present invention provides a green cementitious material, which is composed of the following components by weight: 80-100 parts of slag, 120-180 parts of fly ash, 120-300 parts of coal gasification slag, 80-120 parts of coal gangue, 80-90 parts of composite activator, and 20-30 parts of admixture;

[0008] The composite activator is composed of: 6-10 parts of sodium hydroxide, 20-30 parts of water glass, 10-30 parts of calcium chloride, and 60-80 parts of cement;

[0009] The composition of the admixture is: 7-10 parts of water reducing agent, 8-15 parts of flocculant, and 3-5 parts of early strength agent.

[0010] Fly ash is the fine ash in the flue gas of coal-fired power plants, with a silicon-alumina mineral component of about 85%, a D50 of 15.46μm, and a loss on ignition of ≤10%.

[0011] Coal gasification slag is the fine slag produced in the coal gasification production process, with a silicon and aluminum content of up to 70%, a loss on ignition ≤ 20%, and a particle size of ≤ 100μm after grinding and screening.

[0012] Coal gangue is the associated waste rock in the process of coal mining and coal washing. Its main mineral components are quartz and illite, and the silicon-aluminum content can reach 73%.

[0013] The slag is S95 blast furnace slag.

[0014] The green inorganic cementitious material provided by the present invention uses low-calcium solid waste fly ash, coal gasification slag and coal gangue with extremely low cementing activity as matrix materials, cement, alkaline substances and salt substances as composite activators, and admixtures such as water reducers, flocculants and early strength agents to achieve precise control of the working performance of the material.

[0015] The composite activator includes sodium hydroxide, water glass, cement and calcium chloride. Solid waste materials such as slag, fly ash, coal gasification slag, coal gangue, etc. have low activity and slow hydration reaction in natural state. Cement, sodium hydroxide and water glass in the composite activator provide alkaline environment at the same time, which accelerates the dissolution of silicon-aluminum raw materials and the breaking and recombination of their chemical bonds, and promotes the formation of -Si-O-Al- network structure.

[0016] Slag is a by-product of the blast furnace ironmaking process. It contains a large amount of silica, calcium oxide and other mineral components with potential gelling activity. In the alkaline environment provided by sodium hydroxide, water glass and cement hydration, the oxides in the slag react with alkali metal ions to produce a large amount of CSH and CASH gel.

[0017] Fly ash is the main solid waste discharged from coal-fired power plants. It contains a large amount of chemical components such as silicon dioxide, aluminum oxide and calcium oxide. It can continuously react in an alkaline environment to produce a large amount of amorphous gels such as hydrated sodium aluminosilicate, hydrated sodium silicate and hydrated sodium aluminate, which cement the unhydrated particles and form a dense structure. At the same time, fly ash contains a large number of glass beads, which are evenly distributed in the slurry, which can improve the workability of the material.

[0018] Coal gasification slag is the main solid waste in the coal gasification production process. It contains a large amount of silicon dioxide and aluminum oxide. The main mineral phase is amorphous aluminosilicate, which can be well dissolved and form gel in an alkaline environment. Compared with fly ash, coal gasification slag has higher hardness and density. It can play the role of micro-aggregate in the whole system, combining with the gel produced by slag, fly ash, cement, etc. to form a high-strength gelled structure.

[0019] Coal gasification slag is a kind of solid waste produced during coal mining. Its silicon and aluminum content can reach more than 70%. Its main mineral components are quartz and illite. It can undergo depolymerization and polycondensation in an alkaline environment to form hydrated sodium aluminosilicate gel. The utilization of coal gangue can reduce the cost of materials and reduce the environmental pollution caused by coal gangue accumulation.

[0020] Cement hydration not only provides an alkaline environment, but also provides good early strength during the depolymerization-polycondensation process of solid waste materials.

[0021] In some embodiments, the cement is ordinary Portland cement.

[0022] Preferably, the modulus of the water glass is 3.2 and the mass concentration is 40-50%.

[0023] The modulus of water glass refers to the ratio of the molar number of silicon dioxide to the number of alkali metal oxides.

[0024] In some embodiments, the water reducer is a polycarboxylic acid high-efficiency water reducer or a naphthalene-based water reducer.

[0025] In some embodiments, the flocculant is cellulose ether or polyacrylamide.

[0026] The function of flocculants is to improve the anti-dispersion of materials in a dynamic water environment. Its working principle is to change the intermolecular forces and link the gelling molecules through bridging. Therefore, the selection of flocculants should be based on the molecular characteristics of the gelling system, and the amount of flocculants needs to be adjusted through experiments. Too little flocculant will not achieve the expected anti-dispersion effect, and too much will cause the flocculant to gel, and the gelling molecules will not be able to gel, resulting in a reduction in the flocculation effect.

[0027] In some embodiments, the early strength agent is triethanolamine, potassium aluminum sulfate or triisopropylamine.

[0028] In a second aspect, the present invention provides a method for preparing the green cementitious material, comprising the following steps: grinding coal gangue and coal gasification slag;

[0029] Then, slag, fly ash, coal gasification slag, coal gangue, composite activator and admixture are weighed in proportion and mixed evenly to obtain the product.

[0030] In some embodiments, when preparing the gelling slurry, the obtained green gelling material is mixed with water evenly to obtain the slurry.

[0031] Preferably, in the cementitious slurry, the water-cement ratio is 0.5-0.7.

[0032] In a third aspect, the present invention provides the use of the green cementitious material in grouting and filling projects in a water-rich and corrosive environment.

[0033] The beneficial effects achieved by one or more embodiments of the present invention are as follows:

[0034] The present invention uses high-calcium solid waste mineral powder and low-calcium solid waste fly ash, coal gasification slag, and coal gangue to replace cement materials, and uses alkali-salt-cement as a composite activator to give full play to the potential activity of solid waste materials; a variety of functional admixtures are used to modify the comprehensive performance of cementitious materials. The final prepared material has many advantages such as strong impermeability, high volume stability, good adhesion, strong corrosion resistance, controllable and adjustable gelling time, strong anti-dynamic water dispersibility, green and low carbon, low cost, etc. It is suitable for grouting and filling projects in water-rich corrosive environments, and solves the problems of traditional cement slurry being difficult to retain, large shrinkage, easy to deteriorate, and high cost, and has high ecological and economic value.

[0035] The cementitious material of the present invention has a high content of solid waste, which can well absorb the stockpiles of coal gasification slag and coal gangue, and effectively improve the utilization rate of solid waste materials. DETAILED DESCRIPTION

[0036] It should be noted that the following detailed descriptions are illustrative and intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used in the present invention have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.

[0037] The present invention will be further described in detail below in conjunction with specific embodiments. It should be noted that the specific embodiments are intended to explain the present invention rather than to limit it.

[0038] Example 1

[0039] A green cementitious material is prepared by using the following raw materials in parts by weight: 80 parts of slag, 180 parts of fly ash, 120 parts of coal gasification slag, 120 parts of coal gangue, 80 parts of composite activator and 20 parts of admixture.

[0040] The composition of the composite activator is: 10 parts of sodium hydroxide, 30 parts of water glass, and 60 parts of ordinary Portland cement.

[0041] The composition of the admixture is: 8 parts of polycarboxylic acid water reducer, 10 parts of polyacrylamide, and 6 parts of triethanolamine.

[0042] Preparation method: Weigh the raw materials according to the mass ratio and mix them evenly, stir with water and mix them evenly, the water-cement ratio is 0.6.

[0043] Example 2

[0044] A green cementitious material is prepared from the following raw materials in parts by weight: 100 parts of slag, 120 parts of fly ash, 180 parts of coal gasification slag, 80 parts of coal gangue, 90 parts of composite activator and 20 parts of admixture.

[0045] The composition of the composite activator is: 10 parts of sodium hydroxide, 30 parts of calcium chloride, and 80 parts of ordinary Portland cement.

[0046] The composition of the admixture is: 8 parts of naphthalene-based water reducer, 10 parts of cellulose ether, and 5 parts of potassium aluminum sulfate.

[0047] Preparation method: Weigh the raw materials according to the mass ratio and mix them evenly, stir with water and mix them evenly, the water-cement ratio is 0.6.

[0048] Example 3

[0049] A green cementitious material is prepared from the following raw materials in parts by weight: 80 parts of slag, 120 parts of fly ash, 180 parts of coal gasification slag, 120 parts of coal gangue, 80 parts of composite activator, and 30 parts of admixture.

[0050] The composition of the composite activator is: 20 parts of water glass, 10 parts of calcium chloride and 80 parts of ordinary Portland cement.

[0051] The composition of the admixture is: 12 parts of polycarboxylate water reducer, 10 parts of sodium alginate, and 7 parts of triisopropylamine.

[0052] Preparation method: Weigh the raw materials according to the mass ratio and mix them evenly, stir with water and mix them evenly, the water-cement ratio is 0.6.

[0053] Example 4

[0054] A green cementitious material is prepared from the following raw materials in parts by weight: 100 parts of slag, 180 parts of fly ash, 120 parts of coal gasification slag, 80 parts of coal gangue, 90 parts of composite activator, and 30 parts of admixture.

[0055] The composition of the composite activator is: 8 parts of sodium hydroxide, 20 parts of water glass, 20 parts of calcium chloride, and 60 parts of ordinary Portland cement.

[0056] The composition of the admixture is: 10 parts of polycarboxylic acid water reducer, 8 parts of polyacrylamide, and 5 parts of triethanolamine.

[0057] Preparation method: Weigh the raw materials according to the mass ratio and mix them evenly, stir with water and mix them evenly, the water-cement ratio is 0.6.

[0058] Comparative Example 1

[0059] The difference from Example 4 is that the activator is 8 parts of sodium hydroxide, 20 parts of water glass, and 20 parts of calcium chloride, and ordinary Portland cement is omitted.

[0060] Comparative Example 2

[0061] The difference from Example 4 is that the admixture composition is 8 parts of polycarboxylic acid water-reducing agent, 16 parts of cellulose ether, and 8 parts of triethanolamine.

[0062] Comparative Example 3

[0063] The difference from Example 4 is that the fly ash is replaced by coal gasification slag, and the total amount of coal gasification slag is 300 parts.

[0064] Comparative Example 4

[0065] The difference from Example 4 is that the activator is 90 parts of ordinary Portland cement, without sodium hydroxide, water glass and calcium chloride.

[0066] The fluidity and setting time of the freshly mixed slurries of Examples 1-4 and Comparative Examples 1-4 were measured, and the results are shown in Table 1;

[0067] The stirred material was placed in 0.8 m / s flowing water for retention test. 4×4×16 test blocks were cast and placed in 95% humidity and 20°C environment for standard curing for 28 days. A sulfate erosion control group was also set up. The consolidation rate, compressive strength (standard curing / sulfate erosion) and impermeability pressure were tested. The results are shown in Table 1.

[0068] Table 1

[0069]

[0070]

[0071] However, the retention rate of conventional cement slurry at a water velocity of 0.8 m / s is less than 10%, and the cement stone body will experience severe cracking in a sulfate corrosion environment, with a strength reduction of up to 30%. The material in the embodiment has much better performance than cement slurry under the same conditions, has a higher retention rate and durability, and responds to the national call for green construction.

[0072] The dynamic water retention rate test is carried out using a dynamic water flushing instrument, which can provide a continuous circulating water flow with an adjustable flow rate of 0-4m / s. Weigh a fresh slurry with a mass of m0 and place it in the flushing instrument. After flushing with dynamic water at a flow rate of 0.8m / s for one minute, collect the remaining slurry after flushing and weigh its mass m1. The dynamic water retention rate R of the slurry is calculated according to formula 1. The larger the value, the stronger the ability to resist dynamic water flushing.

[0073]

[0074] Sulfate erosion test: Using a Na2SO4 solution with a mass fraction of 10, the test blocks were placed in deionized water and Na2SO4 solution respectively, and cured at 20°C and 95% humidity. When cured to 120 days old, the compressive strength C0 and C1 of the test blocks in deionized water and Na2SO4 solution were tested respectively. Formula 2 is used to calculate the material's anti-corrosion ability C. The smaller the value, the stronger the anti-corrosion ability.

[0075]

[0076] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A green gelling material, characterized by: The composition is composed of the following components by weight: 80-100 parts of slag, 120-180 parts of fly ash, 120-300 parts of coal gasification slag, 80-120 parts of coal gangue, 80-90 parts of composite activator, and 20-30 parts of admixture; The composite activator is composed of: 6-10 parts of sodium hydroxide, 20-30 parts of water glass, 10-30 parts of calcium chloride, and 60-80 parts of cement; The composition of the admixture is: 7-10 parts of water reducing agent, 8-15 parts of flocculant, and 3-5 parts of early strength agent.

2. The green gelling material according to claim 1, characterized in that: The cement is ordinary Portland cement.

3. The green gelling material according to claim 1, characterized in that: The modulus of the water glass is 3.2, and the mass concentration is 40-50%.

4. The green gelling material according to claim 1, characterized in that: The water reducer is a polycarboxylic acid high-efficiency water reducer or a naphthalene-based water reducer.

5. The green gelling material according to claim 1, characterized in that: The flocculant is cellulose ether or polyacrylamide.

6. The green gelling material according to claim 1, characterized in that: The early strength agent is triethanolamine, potassium aluminum sulfate or triisopropylamine.

7. The method for preparing the green gelling material according to any one of claims 1 to 6, characterized in that: The method comprises the following steps: grinding coal gangue and coal gasification slag; Then, slag, fly ash, coal gasification slag, coal gangue, composite activator and admixture are weighed in proportion and mixed evenly to obtain the product.

8. The method for preparing the green gelling material according to claim 7, characterized in that: When preparing the gelling slurry, the obtained green gelling material is mixed with water evenly.

9. The method for preparing the green gelling material according to claim 8, characterized in that: In cementitious slurry, the water-cement ratio is 0.5-0.

7.

10. Use of the green cementitious material according to any one of claims 1 to 6 in grouting and filling projects in water-rich and corrosive environments.

Citation Information

Patent Citations

  • Multi-source solid waste-based grouting cementing material as well as preparation method and application thereof

    CN111689752A

  • Method for preparing filling material from multi-source coal-based solid waste

    CN113045282A

  • Green cementing material for underground engineering backfill and preparation method of green cementing material

    CN114315205A

  • Low-carbon inorganic gelling grouting filling material as well as preparation method and application thereof

    CN115196932A

  • Cementing material based on multi-source road domain substances as well as preparation method and application of cementing material

    CN116621508A