A kind of high curing strength soft soil curing agent and preparation method thereof

By using a combination of modified glass fiber and composite silica aerogel in the soft soil curing agent, a cross-linking network and porous structure with high curing strength is formed, and the problem of insufficient strength of soft soil curing agent in the prior art is solved. Significantly improves compressive strength and water absorption.

CN118908686BActive Publication Date: 2024-12-06YANTAI ANDA ENVIRONMENTAL PROTECTION TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411404323.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-10-10
Publication Date
2024-12-06
Estimated Expiration
2044-10-10

AI Technical Summary

Technical Problem

It is difficult for existing soft soil curing agents to effectively improve the curing strength of soft soil at room temperature, especially because cement cannot fill the pores in the inner holes in the soil pellets, which limits the increase in the cured soil strength.

Method used

Modified glass by using a high curing strength soft soil curing agent that includes cementing components of modified glass fiber and silicate cement, as well as expanded components of composite silica aerogel, sulfur aluminate cement and gypsum powder. The fiber reacts with the epoxy resin to form a crosslinking network, and the composite silica aerogel forms hydrogen bonds with water molecules and fills the pores in the soil particles to enhance the curing strength.

Benefits of technology

The compressive strength of the soft soil is significantly improved, especially under high water content, forming a through curing network and porous structure, which significantly improves the curing strength and water absorption.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a high-curing strength soft soil curing agent and a preparation method thereof, and relates to the technical field of building materials. The high-curing strength soft soil curing agent in the present invention includes a bonding component and an expansion component, the bonding component includes modified glass fiber and silicate cement, the expansion component includes composite silica aerogel, sulphoaluminate cement and gypsum powder, the modified glass fiber is prepared by coating the surface of hydroxyl glass fiber with carboxyl-terminated polyurethane and then reacting with epoxy resin, so that the soft soil curing agent with the bonding component forms a through curing network during the curing process, and the curing strength is enhanced; the composite silica aerogel is prepared by reacting polyhydroxy polyurethane, tetrapod-shaped zinc oxide and amino-modified silica aerogel, and the polyhydroxy polyurethane is prepared by reacting isocyanate with β-cyclodextrin, which can enhance water absorption, accelerate the combination with water in soft soil, and fill the pores in the aggregate by extrusion, thereby improving the strength of the cured soil.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building materials, in particular to a high-curing strength soft soil curing agent and a preparation method thereof. Background Art

[0002] Soft soil generally refers to fine-grained soil with a gray appearance, a natural porosity greater than or equal to 1.0, and a natural water content greater than the liquid limit. It has the characteristics of high natural water content, large natural porosity, high compressibility, low shear strength, small consolidation coefficient, long consolidation time, high sensitivity, high disturbance, and poor permeability. Soft soil has a high water content, and most of the water exists between soil particles in the form of free water, which keeps the friction between soil particles at a low level. Therefore, the engineering performance of soft soil is very poor. Soft soil solidifier can react with free water in soft soil at room temperature to convert part of the free water in soft soil into chemically bound water. At the same time, the hydration product can directly bond the surface of soil particles in soft soil, condensing the soil particles into an integral, solid, stable, and lasting plate structure, greatly increasing the bearing capacity of soft soil. However, due to the high water content of soft soil, soft soil solidifier needs to be added in a very high amount to bond the soil and meet the solidification requirements.

[0003] Commonly used soft soil curing agents are mainly cement, which has a poor effect on curing soft soil. Clay particles in soft clay usually exist in the form of soil aggregates containing inner pores, and cement that only produces cementitious hydrates cannot fill the inner pores in the soil aggregates, limiting the further improvement of the solidified soil strength. Therefore, the present invention studies and prepares a high-curing strength soft soil curing agent with both cementitious and expansive properties. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a soft soil curing agent prepared by using a high curing strength soft soil curing agent, which has high curing strength for soft soil.

[0005] The present invention proposes a technical solution to solve the above technical problems: a high curing strength soft soil curing agent, comprising a bonding component and an expansion component; the bonding component comprises modified glass fiber and silicate cement; the expansion component comprises composite silica aerogel, sulphoaluminate cement and gypsum powder.

[0006] Preferably, the modified glass fiber is prepared by coating the surface of the hydroxyl glass fiber with carboxyl-terminated polyurethane and then reacting with epoxy resin.

[0007] Preferably, the epoxy resin is 4,4'-methylenebis(N,N-dicyclopropyloxyaniline).

[0008] Preferably, the composite silica aerogel is prepared by reacting polyhydroxy polyurethane, tetrapod-shaped zinc oxide and amino-modified silica aerogel.

[0009] Preferably, the polyol polyurethane is prepared by reacting isocyanate with β-cyclodextrin.

[0010] Preferably, the preparation method of the high curing strength soft soil curing agent comprises the following specific steps:

[0011] S1. TEOS, ethanol, N,N-dimethylformamide and deionized water were mixed in a volume ratio of 10-11:8:0.4:1, stirred evenly, and then the pH was adjusted to 1-2 with hydrochloric acid, and 0.2-0.4 times the mass of tetrapod-shaped zinc oxide of TEOS was added, the temperature was raised to 43-45°C, and the reaction was carried out for 80-90 minutes. The pH was adjusted to 7-8 with aqueous ammonia to obtain a wet gel; the wet gel was placed in a mixed solution of 10-12 times the volume of n-hexane and trimethoxychlorosilane, and the volume ratio of n-hexane to trimethoxychlorosilane in the mixed solution of n-hexane and trimethoxychlorosilane was 1:8-10. After surface modification for 24 hours, the mixture was transferred to a n-hexane solution and immersed for 24 hours. After being fished out, the mixture was calcined at 500-600°C for 2-4 hours to obtain a silica aerogel;

[0012] S2. Toluene and 3-aminopropyltriethoxysilane were mixed in a volume ratio of 10:1~2, 0.08~0.12 times the mass of toluene was added to the silica aerogel, the temperature was raised to 78~82°C, refluxed for 16~20h, and then 0.1~0.2 times the mass of toluene was added to the polyhydroxy polyurethane, the temperature was raised to 190~220°C, the reaction was carried out for 2~4h, and the composite silica aerogel was obtained by washing with n-hexane and toluene for 3~5 times in sequence, and finally dried at 120~140°C;

[0013] S3. Mix the hydroxyl glass fiber and the carboxyl-terminated polyurethane in a mass ratio of 0.8-1.2:5, raise the temperature to 100-120°C, react for 2-4 hours, add 4,4'-methylenebis(N,N-dicyclopropyloxyaniline) in an amount 10-12 times that of the hydroxyl glass fiber, continue to react for 2-4 hours, filter and wash with N,N-dimethylformamide for 3-5 times, and then dry in a vacuum drying oven at 100-120°C to obtain a modified glass fiber;

[0014] S4. The modified glass fiber and silicate cement were mixed in a mass ratio of 1:20 to 40, stirred evenly, and a cementing component was obtained; the composite silica aerogel, sulphoaluminate cement and gypsum powder were mixed in a mass ratio of 1 to 3:20:9 to 13, and stirred evenly to obtain an expansion component;

[0015] S5. Mix the cementitious component and the expansive component in equal amounts to prepare a high-curing strength soft soil solidifying agent.

[0016] Preferably, in the above step S1, the preparation method of tetrapod-shaped zinc oxide is as follows: immersing zinc powder in a hydrogen peroxide solution with a mass fraction of 0.1-0.2%, grinding at a rate of 60-80 rpm for 30-50 min, filtering and placing at room temperature for 24 h, and then drying at 150-180 ° C to obtain aged zinc powder, mixing the aged zinc powder with white carbon black in a mass ratio of 1:10-20, placing in a muffle furnace at 900-1000 ° C, compressing air at a rate of 10-30 m / s, and finally obtaining tetrapod-shaped zinc oxide on the upper layer of white carbon black.

[0017] Preferably, in the above step S2, the preparation method of the polyhydroxy polyurethane is: under a nitrogen atmosphere, β-cyclodextrin and N,N'-dimethylacetamide are mixed in a mass ratio of 3-3.4:10, the temperature is raised to 68-72°C, p-phenylene diisocyanate and N,N'-dimethylacetamide are mixed in a mass ratio of 0.8-1.2:20, and the mixture is stirred to obtain a mixed solution, and the mixed solution with a mass of 10-12 times of β-cyclodextrin is added dropwise at a rate of 1-3 ml / min. After reacting for 24 hours, the mixture is washed with acetone and deionized water for 3-5 times in sequence and vacuum dried, and the mixture is ground to obtain the polyhydroxy polyurethane.

[0018] Preferably, in the above step S3, the preparation method of hydroxyl glass fiber is: silane coupling agent KH550, ethanol and deionized water are mixed in a mass ratio of 0.8~1:4:20, hydrolyzed for 30~50 minutes, and then 5~7 times the mass of glass fiber of silane coupling agent KH550 is added, the temperature is raised to 75~85°C, reacted for 6~8h, filtered and dried in a vacuum drying oven at 100~120°C to obtain hydroxyl glass fiber.

[0019] Preferably, in the above step S3, the preparation method of the carboxyl-terminated polyurethane is: heating the polytetrahydrofuran diol to 48-52° C., adding 0.8-1.2 times the mass of the polytetrahydrofuran diol toluene-2,4-diisocyanate and 0.02-0.04 times the mass of the polytetrahydrofuran diol as accelerator dibutyltin dilaurate under stirring at 200-400 rpm, reacting for 8-12 hours, adding 2-4 times the mass of the polytetrahydrofuran diol N,N-dimethylformamide, heating to 100-120° C., and continuing the reaction for 3-6 hours to obtain the carboxyl-terminated polyurethane.

[0020] Compared with the prior art, the beneficial effects achieved by the present invention are:

[0021] The high-curing strength soft soil curing agent of the present invention comprises a bonding component and an expansion component, wherein the bonding component comprises modified glass fiber and silicate cement, and the expansion component comprises composite silica aerogel, sulphoaluminate cement and gypsum powder;

[0022] The modified glass fiber is prepared by coating the surface of the hydroxyl glass fiber with carboxyl-terminated polyurethane and then reacting with epoxy resin. After the carboxyl-terminated polyurethane is coated on the surface of the hydroxyl glass fiber, it reacts with epoxy resin 4,4´-methylenebis(N,N-dicyclopropyloxyaniline) to form a cross-linked network structure with high curing strength on the surface of the glass fiber, so that the soft soil curing agent with a bonding component forms a through curing network during the curing process, thereby enhancing the curing strength.

[0023] The composite silica aerogel is prepared by the reaction of polyhydroxy polyurethane, tetrapod-shaped zinc oxide and amino-modified silica aerogel. The polyhydroxy polyurethane is prepared by the reaction of isocyanate and β-cyclodextrin. Ethyl orthosilicate is used as a silicon source to react with 3-aminopropyltriethoxysilane, and tetrapod-shaped zinc oxide is added to form porous silica aerogel on the surface of the tetrapod-shaped zinc oxide. The surface is then coated with polyurethane having a polyhydroxy structure. While enhancing the curing strength, the composite silica aerogel can form hydrogen bonds with water molecules, thereby enhancing water absorption, accelerating the combination with water in soft soil, and filling the pores in the aggregates by extrusion to improve the strength of the cured soil. DETAILED DESCRIPTION

[0024] The present invention is described in detail below by way of examples. It is necessary to point out that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Those skilled in the art can make some non-essential improvements and adjustments to the present invention based on the above content of the present invention. Unless otherwise defined, all professional and scientific terms used herein have the same meanings as those familiar to those skilled in the art.

[0025] In order to more clearly illustrate the method provided by the present invention, the following examples are used to describe in detail the various index testing methods of the high curing strength soft soil curing agent prepared in the examples and comparative examples as follows:

[0026] Compressive strength test: The same amount of the high curing strength soft soil curing agent prepared in the embodiment and the comparative example was used to perform compressive strength tests on sludge with a water content of 60% and 100%, respectively.

[0027] Example 1

[0028] The preparation method of the high curing strength soft soil curing agent in this embodiment is:

[0029] S1. Immerse zinc powder in a hydrogen peroxide solution with a mass fraction of 0.1%, grind at a speed of 60 rpm for 30 minutes, filter and place at room temperature for 24 hours, and then dry at 150°C to obtain aged zinc powder, mix the aged zinc powder with white carbon black in a mass ratio of 1:10, place it in a muffle furnace at 900°C, compress air at a rate of 10m / s, and finally obtain four-needle zinc oxide on the upper layer of white carbon black; mix ethyl orthosilicate, ethanol, N,N-dimethylformamide and deionized water in a volume ratio of 10:8:0.4:1, After stirring evenly, adjust the pH to 1 with hydrochloric acid, add tetrapod-shaped zinc oxide with a mass of 0.2 times that of ethyl orthosilicate, heat to 43°C, react for 80 minutes, adjust the pH to 7 with ammonia water, and obtain wet gel; place the wet gel in a mixture of 10 times the volume of n-hexane and trimethoxychlorosilane, the volume ratio of n-hexane to trimethoxychlorosilane in the mixture is 1:8, after surface modification for 24 hours, transfer to n-hexane solution and soak for 24 hours, remove and calcine at 500°C for 2 hours, and obtain silica aerogel;

[0030] S2. In a nitrogen atmosphere, β-cyclodextrin and N,N'-dimethylacetamide were mixed in a mass ratio of 3:10, heated to 68°C, paraphenylene diisocyanate and N,N'-dimethylacetamide were mixed in a mass ratio of 0.8:20, stirred evenly to obtain a mixed solution, and the mixed solution 10 times the mass of β-cyclodextrin was added dropwise at a rate of 1 ml / min. After reacting for 24 hours, the mixture was washed with acetone and deionized water three times in sequence and vacuum dried, and ground to obtain polyhydroxy polyurethane; toluene and 3-aminopropyltriethoxysilane were mixed in a volume ratio of 10:1, 0.08 times the mass of toluene silica aerogel was added, the temperature was raised to 78°C, refluxed for 16 hours, and then 0.1 times the mass of toluene polyhydroxy polyurethane was added, the temperature was raised to 190°C, reacted for 2 hours, washed with n-hexane and toluene three times in sequence, and finally dried at 120°C to obtain a composite silica aerogel;

[0031] S3. Silane coupling agent KH550, ethanol and deionized water were mixed in a mass ratio of 0.8:4:20, and after hydrolysis for 30 minutes, 5 times the mass of glass fiber of silane coupling agent KH550 was added, the temperature was raised to 75°C, reacted for 6 hours, filtered and dried in a vacuum drying oven at 100°C to obtain hydroxy glass fiber; polytetrahydrofuran diol was heated to 48°C, and 0.8 times the mass of toluene-2,4-diisocyanate of polytetrahydrofuran diol and 0.02 times the mass of accelerator dilauryl were added under stirring at 200rpm. dibutyltin ether, after reacting for 8 hours, add N,N-dimethylformamide twice the mass of polytetrahydrofuran diol, heat to 100°C, continue to react for 3 hours, and obtain terminal carboxyl polyurethane; hydroxy glass fiber and terminal carboxyl polyurethane are mixed at a mass ratio of 0.8:5, heat to 100°C, react for 2 hours, add 4,4´-methylenebis(N,N-dicyclopropyloxyaniline) 10 times the mass of hydroxy glass fiber, continue to react for 2 hours, filter and wash with N,N-dimethylformamide 3 times, and then dry in a vacuum drying oven at 100°C to obtain modified glass fiber;

[0032] S4. The modified glass fiber and silicate cement were mixed in a mass ratio of 1:20 and stirred to obtain a cementing component; the composite silica aerogel, sulphoaluminate cement and gypsum powder were mixed in a mass ratio of 1:20:9 and stirred to obtain an expansion component;

[0033] S5. Mix the cementitious component and the expansive component in equal amounts to prepare a high-curing strength soft soil solidifying agent.

[0034] Example 2

[0035] The preparation method of the high curing strength soft soil curing agent in this embodiment is:

[0036] S1. Immerse zinc powder in a hydrogen peroxide solution with a mass fraction of 0.15%, grind at a speed of 70 rpm for 40 min, filter and place at room temperature for 24 h, and then dry at 165 ° C to obtain aged zinc powder, mix the aged zinc powder with white carbon black in a mass ratio of 1:15, place it in a muffle furnace at 950 ° C, compress air at a rate of 20 m / s, and finally obtain four-needle zinc oxide on the upper layer of white carbon black; mix ethyl orthosilicate, ethanol, N, N-dimethylformamide and deionized water in a volume ratio of 10.5:8:0.4:1, stir After mixing evenly, adjust the pH to 1.5 with hydrochloric acid, add tetrapod-shaped zinc oxide with a mass of 0.3 times that of ethyl orthosilicate, heat to 44°C, react for 85 minutes, adjust the pH to 7.5 with ammonia water, and obtain wet gel; place the wet gel in a mixed solution of 11 times the volume of n-hexane and trimethoxychlorosilane, the volume ratio of n-hexane to trimethoxychlorosilane in the mixed solution of n-hexane and trimethoxychlorosilane is 1:9, after surface modification for 24 hours, transfer to n-hexane solution and soak for 24 hours, remove and calcine at 550°C for 3 hours to obtain silica aerogel;

[0037] S2. In a nitrogen atmosphere, β-cyclodextrin and N,N'-dimethylacetamide were mixed in a mass ratio of 3.2:10, heated to 70°C, paraphenylene diisocyanate and N,N'-dimethylacetamide were mixed in a mass ratio of 1.0:20, stirred evenly to obtain a mixed solution, and the mixed solution 11 times the mass of β-cyclodextrin was added dropwise at a rate of 2 ml / min. After reacting for 24 hours, the mixture was washed with acetone and deionized water four times in sequence and vacuum dried, and ground to obtain polyhydroxy polyurethane; toluene and 3-aminopropyltriethoxysilane were mixed in a volume ratio of 10:1.5, 0.1 times the mass of toluene silica aerogel was added, the temperature was raised to 50°C, refluxed for 18 hours, and then 0.15 times the mass of toluene polyhydroxy polyurethane was added, the temperature was raised to 205°C, reacted for 3 hours, washed with n-hexane and toluene four times in sequence, and finally dried at 130°C to obtain a composite silica aerogel;

[0038] S3. Silane coupling agent KH550, ethanol and deionized water were mixed in a mass ratio of 0.9:4:20, and after hydrolysis for 40 minutes, glass fiber with a mass of 6 times that of silane coupling agent KH550 was added, the temperature was raised to 80°C, the reaction was carried out for 7 hours, and the mixture was filtered and dried in a vacuum drying oven at 110°C to obtain hydroxyl glass fiber; polytetrahydrofuran diol was heated to 50°C, and toluene-2,4-diisocyanate with a mass of 1.0 times that of polytetrahydrofuran diol and accelerator dilaurate with a mass of 0.03 times that of polytetrahydrofuran diol were added under stirring at 300 rpm. Butyl tin, after reacting for 10 hours, add N,N-dimethylformamide 3 times the mass of polytetrahydrofuran diol, heat to 110°C, continue to react for 5 hours, and obtain terminal carboxyl polyurethane; mix hydroxy glass fiber and terminal carboxyl polyurethane in a mass ratio of 0.9.2:5, heat to 110°C, react for 3 hours, add 4,4´-methylenebis(N,N-dicyclopropyloxyaniline) 11 times the mass of hydroxy glass fiber, continue to react for 3 hours, filter and wash with N,N-dimethylformamide 4 times, and then dry in a vacuum drying oven at 110°C to obtain modified glass fiber;

[0039] S4. The modified glass fiber and silicate cement were mixed in a mass ratio of 1:30 and stirred to obtain a cementing component; the composite silica aerogel, sulphoaluminate cement and gypsum powder were mixed in a mass ratio of 2:20:11 and stirred to obtain an expansion component;

[0040] S5. Mix the cementitious component and the expansive component in equal amounts to prepare a high-curing strength soft soil solidifying agent.

[0041] Example 3

[0042] The preparation method of the high curing strength soft soil curing agent in this embodiment is:

[0043] S1. Immerse zinc powder in a hydrogen peroxide solution with a mass fraction of 0.2%, grind at a speed of 80 rpm for 50 min, filter and place at room temperature for 24 h, and then dry at 180°C to obtain aged zinc powder, mix the aged zinc powder with white carbon black in a mass ratio of 1:20, place in a muffle furnace at 1000°C, compress air at a rate of 30 m / s, and finally obtain tetrapod-shaped zinc oxide on the upper layer of white carbon black; mix ethyl orthosilicate, ethanol, N,N-dimethylformamide and deionized water in a volume ratio of 11:8:0.4:1, After stirring evenly, adjust the pH to 2 with hydrochloric acid, add tetrapod-shaped zinc oxide with a mass of 0.4 times that of ethyl orthosilicate, heat to 45°C, react for 90 minutes, adjust the pH to 8 with ammonia water, and obtain wet gel; place the wet gel in a mixed solution of 12 times the volume of n-hexane and trimethoxychlorosilane, the volume ratio of n-hexane to trimethoxychlorosilane in the mixed solution of n-hexane and trimethoxychlorosilane is 1:10, and after surface modification for 24 hours, transfer to a n-hexane solution and soak for 24 hours, remove and calcine at 600°C for 4 hours to obtain silica aerogel;

[0044] S2. In a nitrogen atmosphere, β-cyclodextrin and N,N'-dimethylacetamide were mixed in a mass ratio of 3.4:10, heated to 72°C, paraphenylene diisocyanate and N,N'-dimethylacetamide were mixed in a mass ratio of 1.2:20, stirred evenly to obtain a mixed solution, and the mixed solution of 12 times the mass of β-cyclodextrin was added dropwise at a rate of 3 ml / min. After reacting for 24 hours, the mixture was washed with acetone and deionized water for 5 times in sequence and vacuum dried, and multi-hydroxy polyurethane was obtained by grinding; toluene and 3-aminopropyltriethoxysilane were mixed in a volume ratio of 10:2, 0.12 times the mass of toluene silica aerogel was added, the temperature was raised to 82°C, refluxed for 20 hours, and then 0.2 times the mass of toluene polyhydroxy polyurethane was added, the temperature was raised to 220°C, reacted for 4 hours, washed with n-hexane and toluene for 5 times in sequence, and finally dried at 140°C to obtain a composite silica aerogel;

[0045] S3. Silane coupling agent KH550, ethanol and deionized water were mixed in a mass ratio of 1:4:20, and after hydrolysis for 50 minutes, glass fiber with a mass of 7 times that of silane coupling agent KH550 was added, the temperature was raised to 85°C, the reaction was carried out for 8 hours, the mixture was filtered and dried in a vacuum drying oven at 120°C to obtain hydroxyl glass fiber; polytetrahydrofuran diol was heated to 52°C, and toluene-2,4-diisocyanate with a mass of 1.2 times that of polytetrahydrofuran diol and accelerator dilaurate with a mass of 0.04 times that of polytetrahydrofuran diol were added under stirring at 400 rpm. Butyl tin, after reacting for 12 hours, add N,N-dimethylformamide 4 times the mass of polytetrahydrofuran diol, heat to 120°C, continue to react for 6 hours, and obtain terminal carboxyl polyurethane; hydroxy glass fiber and terminal carboxyl polyurethane are mixed at a mass ratio of 1.2:5, heat to 120°C, react for 4 hours, add 4,4´-methylenebis(N,N-dicyclopropyloxyaniline) 12 times the mass of hydroxy glass fiber, continue to react for 4 hours, filter and wash with N,N-dimethylformamide 5 times, and then dry in a vacuum drying oven at 120°C to obtain modified glass fiber;

[0046] S4. The modified glass fiber and silicate cement were mixed in a mass ratio of 1:40 and stirred to obtain a cementing component; the composite silica aerogel, sulphoaluminate cement and gypsum powder were mixed in a mass ratio of 3:20:13 and stirred to obtain an expansion component;

[0047] S5. Mix the cementitious component and the expansive component in equal amounts to prepare a high-curing strength soft soil solidifying agent.

[0048] Comparative Example 1

[0049] The preparation method of comparative example 1 is the same as that of example 2. The difference between the high curing strength soft soil curing agent and example 2 is that the modified glass fiber is prepared by coating the surface of the hydroxyl glass fiber with carboxyl-terminated polyurethane.

[0050] Comparative Example 2

[0051] The preparation method of Comparative Example 2 is the same as that of Example 2. The difference between the high curing strength soft soil curing agent and Example 2 is that the modified glass fiber is only hydroxyl glass fiber.

[0052] Comparative Example 3

[0053] The preparation method of Comparative Example 3 is the same as that of Example 2. The difference between the high curing strength soft soil curing agent and Example 2 is that the composite silica aerogel is prepared by reacting tetrapod-shaped zinc oxide and amino-modified silica aerogel.

[0054] Comparative Example 4

[0055] The preparation method of Comparative Example 4 is the same as that of Example 2. The difference between the high curing strength soft soil curing agent and Example 2 is that the composite silica aerogel is prepared by reacting polyhydroxy polyurethane and amino-modified silica aerogel.

[0056] Comparative Example 5

[0057] The preparation method of Comparative Example 5 is the same as that of Example 2. The difference between the high curing strength soft soil curing agent and Example 2 is that the composite silica aerogel is only amino-modified silica aerogel.

[0058] Comparative Example 6

[0059] The preparation method of Comparative Example 6 is the same as that of Example 2. The difference between the high curing strength soft soil curing agent and Example 2 is that the bonding component is only silicate cement, and the expansion component is only sulphoaluminate cement and gypsum powder.

[0060] Effect example

[0061] Table 1 below shows the performance analysis results of the high curing strength soft soil curing agents prepared using Examples 1 to 3 of the present invention and Comparative Examples 1 to 6:

[0062] Table 1: Performance test data of soft soil stabilizer

[0063] Compressive strength of sludge with 60% water content (MPa) Compressive strength of sludge with 100% water content (MPa) Example 1 2.98 1.39 Example 2 3.64 1.46 Example 3 3.08 1.40 Comparative Example 1 2.57 1.11 Comparative Example 2 2.37 1.04 Comparative Example 3 2.31 0.89 Comparative Example 4 2.09 0.83 Comparative Example 5 1.67 0.65 Comparative Example 6 0.46 0.24

[0064] By comparing the experimental data of the examples and the comparative examples in Table 1, it can be clearly found that the high curing strength soft soil curing agent prepared by using Examples 1, 2 and 3 has excellent curing strength for soft soil with high water content.

[0065] From the comparison of the experimental data of Example 1, Example 2, Example 3 and Comparative Example 1, Comparative Example 2, Comparative Example 6, it can be found that after the end carboxyl polyurethane is coated on the surface of the hydroxyl glass fiber, it is reacted with the epoxy resin 4,4´-methylenebis(N,N-dicyclopropyloxyaniline) to form a cross-linked network structure with high curing strength on the surface of the glass fiber, so that the soft soil curing agent with a bonding component forms a through curing network during the curing process, thereby enhancing the curing strength.

[0066] From the comparison of the experimental data of Example 1, Example 2, Example 3 and Comparative Example 3, Comparative Example 4, Comparative Example 5, and Comparative Example 6, it can be found that by reacting ethyl orthosilicate with 3-aminopropyltriethoxysilane as a silicon source and adding tetrapod-shaped zinc oxide, a porous silica aerogel is formed on the surface of the tetrapod-shaped zinc oxide, and then the surface is coated with a polyurethane having a polyhydroxy structure. While enhancing the curing strength, the composite silica aerogel can form hydrogen bonds with water molecules, thereby enhancing water absorption, accelerating the combination with water in soft soil, and filling the pores in the agglomerates by extrusion, thereby improving the strength of the cured soil.

[0067] Obviously, the above embodiments are merely examples for clearly illustrating the embodiments of the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. However, these obvious changes or modifications derived from the spirit of the present invention are still within the scope of protection of the present invention.

Claims

1. A high curing strength soft soil curing agent, characterized in that: It comprises a bonding component and an expansion component; the bonding component comprises modified glass fiber and silicate cement; the expansion component comprises composite silica aerogel, sulphoaluminate cement and gypsum powder; the modified glass fiber is prepared by coating the surface of hydroxyl glass fiber with carboxyl-terminated polyurethane and then reacting with epoxy resin; The preparation steps of the composite silica aerogel are: S1. TEOS, ethanol, N,N-dimethylformamide and deionized water were mixed in a volume ratio of 10-11:8:0.4:1, stirred evenly, and then the pH was adjusted to 1-2 with hydrochloric acid, and 0.2-0.4 times the mass of tetrapod-shaped zinc oxide of TEOS was added, the temperature was raised to 43-45°C, and the reaction was carried out for 80-90 minutes. The pH was adjusted to 7-8 with aqueous ammonia to obtain a wet gel; the wet gel was placed in a mixed solution of 10-12 times the volume of n-hexane and trimethoxychlorosilane, and the volume ratio of n-hexane to trimethoxychlorosilane in the mixed solution of n-hexane and trimethoxychlorosilane was 1:8-10. After surface modification for 24 hours, the mixture was transferred to a n-hexane solution and immersed for 24 hours. After being fished out, the mixture was calcined at 500-600°C for 2-4 hours to obtain a silica aerogel; S2. Mix toluene and 3-aminopropyltriethoxysilane in a volume ratio of 10:1~2, add 0.08~0.12 times the mass of toluene into silica aerogel, heat to 78~82°C, reflux for 16~20h, then add 0.1~0.2 times the mass of toluene into polyhydroxy polyurethane, heat to 190~220°C, react for 2~4h, wash with n-hexane and toluene for 3~5 times in turn, and finally dry at 120~140°C to obtain composite silica aerogel.

2. A high curing strength soft soil curing agent according to claim 1, characterized in that: The epoxy resin is 4,4'-methylenebis(N,N-dicyclopropyloxyaniline).

3. The high curing strength soft soil curing agent according to claim 1, characterized in that: The polyhydroxy polyurethane is prepared by the reaction of isocyanate and beta-cyclodextrin.

4. A method for preparing a high curing strength soft soil curing agent as claimed in claim 1, characterized in that: The specific steps include: S1. TEOS, ethanol, N,N-dimethylformamide and deionized water were mixed in a volume ratio of 10-11:8:0.4:1, stirred evenly, and then the pH was adjusted to 1-2 with hydrochloric acid, and 0.2-0.4 times the mass of tetrapod-shaped zinc oxide of TEOS was added, the temperature was raised to 43-45°C, and the reaction was carried out for 80-90 minutes. The pH was adjusted to 7-8 with aqueous ammonia to obtain a wet gel; the wet gel was placed in a mixed solution of 10-12 times the volume of n-hexane and trimethoxychlorosilane, and the volume ratio of n-hexane to trimethoxychlorosilane in the mixed solution of n-hexane and trimethoxychlorosilane was 1:8-10. After surface modification for 24 hours, the mixture was transferred to a n-hexane solution and immersed for 24 hours. After being fished out, the mixture was calcined at 500-600°C for 2-4 hours to obtain a silica aerogel; S2. Toluene and 3-aminopropyltriethoxysilane were mixed in a volume ratio of 10:1~2, 0.08~0.12 times the mass of toluene was added to the silica aerogel, the temperature was raised to 78~82°C, refluxed for 16~20h, and then 0.1~0.2 times the mass of toluene was added to the polyhydroxy polyurethane, the temperature was raised to 190~220°C, the reaction was carried out for 2~4h, and the composite silica aerogel was obtained by washing with n-hexane and toluene for 3~5 times in sequence, and finally dried at 120~140°C; S3. Mix the hydroxyl glass fiber and the carboxyl-terminated polyurethane in a mass ratio of 0.8-1.2:5, raise the temperature to 100-120°C, react for 2-4 hours, add 4,4'-methylenebis(N,N-dicyclopropyloxyaniline) in an amount 10-12 times that of the hydroxyl glass fiber, continue to react for 2-4 hours, filter and wash with N,N-dimethylformamide for 3-5 times, and then dry in a vacuum drying oven at 100-120°C to obtain a modified glass fiber; S4. The modified glass fiber and silicate cement were mixed in a mass ratio of 1:20 to 40, stirred evenly, and a cementing component was obtained; the composite silica aerogel, sulphoaluminate cement and gypsum powder were mixed in a mass ratio of 1 to 3:20:9 to 13, and stirred evenly to obtain an expansion component; S5. Mix the cementitious component and the expansive component in equal amounts to prepare a high-curing strength soft soil solidifying agent.

5. The method for preparing a high curing strength soft soil curing agent according to claim 4, characterized in that: In the above step S1, the preparation method of tetrapod-shaped zinc oxide is as follows: immersing zinc powder in a hydrogen peroxide solution with a mass fraction of 0.1-0.2%, grinding at a rate of 60-80 rpm for 30-50 min, filtering and placing at room temperature for 24 h, and then drying at 150-180 ° C to obtain aged zinc powder, mixing the aged zinc powder with white carbon black in a mass ratio of 1:10-20, placing it in a muffle furnace at 900-1000 ° C, compressing air at a rate of 10-30 m / s, and finally obtaining tetrapod-shaped zinc oxide on the upper layer of white carbon black.

6. The method for preparing a high curing strength soft soil curing agent according to claim 4, characterized in that: In the above step S2, the preparation method of the polyhydroxy polyurethane is: under a nitrogen atmosphere, β-cyclodextrin and N,N'-dimethylacetamide are mixed in a mass ratio of 3-3.4:10, the temperature is raised to 68-72°C, p-phenylene diisocyanate and N,N'-dimethylacetamide are mixed in a mass ratio of 0.8-1.2:20, and stirred to obtain a mixed solution, and the mixed solution with a mass of 10-12 times of β-cyclodextrin is added dropwise at a rate of 1-3 ml / min. After reacting for 24 hours, the mixture is washed with acetone and deionized water for 3-5 times in sequence and vacuum dried, and ground to obtain the polyhydroxy polyurethane.

7. The method for preparing a high curing strength soft soil curing agent according to claim 4, characterized in that: In the above step S3, the preparation method of hydroxyl glass fiber is: silane coupling agent KH550, ethanol and deionized water are mixed in a mass ratio of 0.8~1:4:20, hydrolyzed for 30~50 minutes, and then 5~7 times the mass of glass fiber of silane coupling agent KH550 is added, the temperature is raised to 75~85°C, reacted for 6~8h, filtered and dried in a vacuum drying oven at 100~120°C to obtain hydroxyl glass fiber.

8. The method for preparing a high curing strength soft soil curing agent according to claim 4, characterized in that: In the above step S3, the preparation method of the carboxyl-terminated polyurethane is as follows: the polytetrahydrofuran diol is heated to 48-52° C., and under stirring at 200-400 rpm, 0.8-1.2 times the mass of the polytetrahydrofuran diol of toluene-2,4-diisocyanate and 0.02-0.04 times the mass of the polytetrahydrofuran diol of accelerator dibutyltin dilaurate are added, and after reacting for 8-12 hours, 2-4 times the mass of the polytetrahydrofuran diol of N,N-dimethylformamide are added, the temperature is raised to 100-120° C., and the reaction is continued for 3-6 hours to obtain the carboxyl-terminated polyurethane.