Monomer, polymer, film, device, preparation method and application
By designing new monomers and preparing electrochromic/electrocontrolled fluorescent polymers by oxidation polymerization, the problem of insufficient fluorescence contrast and stability of existing materials is solved, and electrochromic/electrocontrolled with high contrast and stability is achieved Fluorescent materials, suitable for sensors and 3D coded information storage fields.
Patent Information
- Application Number
- CN202410949909.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-08
AI Technical Summary
The existing electrochromic/electrocontrolled fluorescence dual-function polymers have insufficient performance in fluorescence contrast and stability, limiting their application performance in high-resolution display and complex environmental monitoring.
A new monomer was designed to prepare electrochromic/electrocontrolled fluorescent polymers with high fluorescence contrast by oxidative polymerization. The fluorescence performance of the material is enhanced by aggregation-induced luminescence effect, and prepared by solution processing to form a film. Thin film, suitable for sensors and 3D coded information storage fields.
It significantly improves the fluorescence contrast and stability of the polymer, ensures the reliability and high contrast display performance of the material in a variety of application environments, overcomes the fluorescence quenching problem of traditional fluorescent materials, and has potential application value.
Smart Images

Figure CN118908855A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of organic polymer chemistry, and specifically relates to a monomer for preparing an electrochromic / electro-controlled fluorescent bifunctional polymer, an electrochromic / electro-controlled fluorescent bifunctional polymer and a preparation method and application thereof, as well as a film and a device prepared using the bifunctional polymer. Background Art
[0002] Electrochromic / electrofluorochromic (EC / EFC) is a reversible redox reaction of a material due to the injection and removal of charges under the action of an external electric field, accompanied by the doping and dedoping of electrolyte ions. This phenomenon leads to a stable and reversible change in the optical properties of the material, usually manifested as a change in the color and fluorescence properties of the material.
[0003] According to the differences in material structure, electrochromic / electrofluorescent materials are mainly divided into two categories: small molecule electrochromic / electrofluorescent materials and polymer electrochromic / electrofluorescent materials. The core advantage of polymer electrochromic / electrofluorescent materials lies in their band gap tunability, which means that through sophisticated chemical design, the absorption and emission wavelengths of the material can be precisely controlled, thereby achieving precise control of the luminescent color. In addition to their superior optical and electrical properties, polymer electrochromic / electrofluorescent materials also have excellent mechanical robustness and physical stability, which greatly enhances the durability and service life of the material. In addition, the excellent processability of polymer electrochromic / electrofluorescent materials allows for large-scale production through simple methods, which is particularly suitable for the manufacture of large-area flexible films, providing a broad space for innovation in application areas such as smart windows.
[0004] At present, although electrochromic / electrofluorescent bifunctional polymers show great potential in the field of smart materials, there are still several challenges in converting them into practical applications, especially in the preparation of electrochromic / electrofluorescent devices. Among them, the lack of fluorescence contrast and stability is the main technical obstacle that currently limits the application of bifunctional polymers. Fluorescence contrast, that is, the degree of difference in fluorescence intensity of the material under different electrochemical states, is crucial for achieving high-definition visual feedback and fine information display. Ideally, bifunctional polymers should exhibit significant changes in fluorescence intensity between the oxidized and reduced states to ensure a high-contrast display effect. However, most of the existing bifunctional polymer materials perform poorly in this regard, which directly affects the application performance of the materials in fields such as high-resolution display, fine information transmission, and complex environmental monitoring. Summary of the invention
[0005] In order to solve the above technical problems, the present application mainly provides a monomer for preparing an electrochromic / electrically controlled fluorescent bifunctional polymer, and an electrochromic / electrically controlled fluorescent bifunctional polymer with high fluorescence contrast and stability prepared using the monomer. This is achieved specifically through the following technical solutions:
[0006] A monomer, the structural formula of the monomer is as follows:
[0007] Wherein, R is selected from naphthalene, anthracene, and pyrene.
[0008] A polymer, wherein the structural formula of the polymer repeating unit is as follows:
[0009] Wherein, n is 20 to 1000, and R is selected from naphthalene, anthracene, and pyrene.
[0010] A method for preparing the above polymer, wherein the polymer is formed by polymerizing the monomer of formula (I) in an organic solvent.
[0011] The above polymers are used in the fields of optical display, sensor and 3D coded information storage.
[0012] A film comprises a substrate and an electrochromic layer formed on the surface of the substrate by solution processing; the electrochromic layer adopts the above polymer material. The solution processing film means dissolving the polymer in a solvent to obtain a solution, coating the solution on the substrate, and drying to obtain a film.
[0013] Preferably, the solvent used in the solution processing into film is any one of dichloromethane, chloroform, tetrahydrofuran, toluene and dimethylformamide.
[0014] Preferably, the substrate is selected from any one of indium tin oxide conductive glass, fluorine tin oxide conductive glass and polyethylene terephthalate conductive substrate.
[0015] A device comprises the film described in any one of the above items.
[0016] Compared with the prior art, this application has the following beneficial effects:
[0017] The core of the present invention application lies in an innovative monomer design, which cleverly combines the two functions of electrochromic and electro-controlled fluorescence. By integrating the aggregation-induced emission unit, the fluorescence contrast in the polymer system is significantly improved, thereby enhancing the high-contrast display performance of the material. The aggregation-induced emission effect enables the polymer to emit strong fluorescence in an aggregated state. Compared with traditional fluorescent materials, this property effectively overcomes the problem of fluorescence quenching caused by aggregation, thereby ensuring the stability and reliability of the material in a variety of application environments. This application adopts a simple oxidative polymerization method to prepare an electrochromic / electro-controlled fluorescent polymer material with high fluorescence contrast using the above-mentioned monomers. The polymer material is used to prepare an electrochromic / electro-controlled fluorescent film by spin coating or spray coating, which has potential application value in the fields of sensors and 3D coded information storage. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] In order to clearly illustrate the embodiments, the following is a brief introduction to the accompanying drawings:
[0019] Figure 1 The cyclic voltammetry curve of the film of this application;
[0020] Figure 2 The UV-visible absorption spectra of the film of this application at different voltages;
[0021] Figure 3 , 4 This is the transmittance variation curve of the film in the present application at 505nm band under different voltages;
[0022] Figure 5 , 6 This is the fluorescence intensity change curve of the film of this application in the 566nm band under different voltages;
[0023] Figure 7 It is the preparation reaction formula of monomers I, II and III. DETAILED DESCRIPTION
[0024] The present application will be further described below in the form of specific embodiments. Those of ordinary skill in the art will be able to implement the present application based on these descriptions. In addition, the embodiments of the present application involved in the following description are generally only embodiments of a part of the present application, rather than all embodiments. Therefore, based on the embodiments in the present application, all other embodiments obtained by those of ordinary skill in the art without making creative work should fall within the scope of protection of the present application.
[0025] Example 1: Preparation of Monomer I
[0026] Preparation of compound I. In a 250mL round-bottom flask, add 0.9371g (6mmol) of 1-naphthaldehyde, 1.1956g (6.1mmol) of 4-bromobenzeneacetonitrile and 30mL of ethanol solution, stir at 40°C for 15min to fully dissolve, then add 16 drops of tetrabutylammonium hydroxide solution, and heat and stir for 4h. After the reaction is completed, collect the blue-green solid product and wash it with a large amount of ethanol solution until the solution is clear and transparent. Then put the obtained blue-green solid into a vacuum oven and dry it at 60°C for 3h for standby use to obtain 1.9385g (5.8mmol) of blue-green solid with a yield of 96.7%.
[0027] Pre-preparation of catalyst: Under nitrogen atmosphere, tris(dibenzylideneacetone)dipalladium(0) (24 mg, 0.026 mmol) and tri-tert-butylphosphine (5.5 mg, 0.026 mmol) were dissolved in anhydrous toluene (12 mL) and stirred at room temperature for 10 min to obtain a pre-prepared catalyst.
[0028] Preparation of Monomer I. In a nitrogen atmosphere, add diphenylamine (0.3553 g, 2.1 mmol), 2-(4-bromophenyl)-3-(naphthalene-1-yl) acrylonitrile (0.8356 g, 2.5 mmol) and sodium tert-butoxide (0.3015 g, 3.14 mmol), anhydrous toluene solution (25 mL) and preformed catalyst in sequence. The reaction mixture was heated to reflux at 90 ° C for 24 h and then cooled to room temperature. After the reaction was completed, it was extracted three times with saturated brine and dichloromethane. The organic phase extract was collected, concentrated in vacuo, dehydrated with anhydrous sodium sulfate, and purified by silica gel column chromatography. The mobile phase was dichloromethane and petroleum ether in a ratio of 4:1. The eluent containing the target compound was collected by thin layer chromatography, the solvent was evaporated, and dried to obtain 0.7211 g of a yellow-green solid product compound with a yield of 81.3%.
[0029] Example 2: Preparation of Monomer II
[0030] Preparation of compound II. In a 250mL round-bottom flask, add 0.9540g (6mmol) of 1-anthracenecarboxaldehyde, 1.1956g (6.1mmol) of 4-bromobenzeneacetonitrile and 30mL of ethanol solution, stir at 40°C for 15min to fully dissolve, then add 16 drops of tetrabutylammonium hydroxide solution, heat and stir for 4h. After the reaction is completed, collect the yellow solid product and wash it with a large amount of ethanol solution until the solution is clear and transparent. Then put the obtained yellow solid into a vacuum oven and dry it at 60°C for 3h for standby use to obtain 2.0313g (5.29mmol) of yellow solid with a yield of 88.1%.
[0031] Pre-preparation of catalyst: Under nitrogen atmosphere, tris(dibenzylideneacetone)dipalladium(0) (24 mg, 0.026 mmol) and tri-tert-butylphosphine (5.5 mg, 0.026 mmol) were dissolved in anhydrous toluene (12 mL) and stirred at room temperature for 10 min to obtain a pre-prepared catalyst.
[0032] Preparation of Monomer II. In a nitrogen atmosphere, add diphenylamine (0.3553 g, 2.1 mmol), 2-(4-bromophenyl)-3-(anthracen-9-yl) acrylonitrile (0.9607 g, 2.5 mmol), sodium tert-butoxide (0.3015 g, 3.14 mmol), anhydrous toluene solution (25 mL) and preformed catalyst in sequence. The reaction mixture was heated to reflux at 90 ° C for 24 h and then cooled to room temperature. After the reaction was completed, it was extracted three times with saturated brine and dichloromethane. The organic phase extract was collected, concentrated in vacuo, and dehydrated with anhydrous sodium sulfate, and purified by silica gel column chromatography. The mobile phase was a ratio of dichloromethane to petroleum ether of 3:1. The eluent containing the target compound was collected by thin layer chromatography, the solvent was evaporated, and dried to obtain 0.7844 g of a yellow-green solid product compound with a yield of 79.1%.
[0033] Example 3: Preparation of Monomer III
[0034] Preparation of compound III. In a 250mL round-bottom flask, add 1.3816g (6mmol) of 1-anthracenecarboxaldehyde, 1.1956g (6.1mmol) of 4-bromobenzeneacetonitrile and 30mL of ethanol solution, stir at 40°C for 15min to fully dissolve, then add 16 drops of tetrabutylammonium hydroxide solution, heat and stir for 6h. After the reaction is completed, collect the yellow solid product and wash it with a large amount of ethanol solution until the solution is clear and transparent. Then put the obtained bright yellow solid into a vacuum oven and dry it at 60°C for 3h for standby use to obtain 1.9967g (4.89mmol) of orange solid with a yield of 81.5%.
[0035] Pre-preparation of catalyst: Under nitrogen atmosphere, tris(dibenzylideneacetone)dipalladium(0) (24 mg, 0.026 mmol) and tri-tert-butylphosphine (5.5 mg, 0.026 mmol) were dissolved in anhydrous toluene (12 mL) and stirred at room temperature for 10 min to obtain a pre-prepared catalyst.
[0036] Preparation of monomer III. In a nitrogen atmosphere, add diphenylamine (0.3553g, 2.1mmol), 2-(4-bromophenyl)-3-(pyrene-1-yl) acrylonitrile (1.0208g, 2.5mmol) and sodium tert-butoxide (0.3015g, 3.14mmol), anhydrous toluene solution (25mL) and preformed catalyst in sequence. The reaction mixture was heated to reflux at 90°C for 24h and then cooled to room temperature. After the reaction, it was extracted three times with saturated brine and dichloromethane. The organic phase extract was collected, concentrated in vacuo, and dehydrated with anhydrous sodium sulfate, and purified by silica gel column chromatography. The mobile phase was a ratio of dichloromethane to petroleum ether of 4:1. The eluent containing the target compound was collected by thin layer chromatography, the solvent was evaporated, and dried to obtain 0.8274g of a yellow-green solid product compound with a yield of 79.4%.
[0037] Example 4: Preparation of polymer and film
[0038] Preparation of electrochromic / electrofluorescent polymer. 1 mmol of monomer I was dissolved in 20 mL of chloroform, and ferric chloride (FeCl3·6H2O, 3.3 mmol) was gradually added. The solution was stirred at 40 ° C for 24 h under a nitrogen atmosphere. After the polymerization reaction was completed, the mixture was poured into a methanol solution to extract the product, and then the product was separated by filtration and washed with methanol several times to obtain a yellow-brown powder. In order to further purify the product, the crude product was Soxhlet extracted in the order of methanol, petroleum ether, acetone, and chloroform, and the washing liquid of the chloroform stage was retained and spin-dried to obtain an electrochromic / electrofluorescent polymer.
[0039] The prepared electrochromic / electrofluorescent polymer was dissolved in chloroform to prepare a 2 mg / mL solution for later use. Indium tin oxide conductive glass was used as the substrate and placed on a heating plate at a temperature of 100°C. The above solution was evenly sprayed on the surface of the substrate using a spray gun for 10 times. After spraying, it was placed in a 65°C oven for drying to obtain an electrochromic / electrofluorescent PDNPC polymer film.
[0040] Example 5: Preparation of polymer and film
[0041] Preparation of electrochromic / electrofluorescent polymer. 1 mmol of monomer II was dissolved in 20 mL of chloroform, and ferric chloride (FeCl3·6H2O, 3.3 mmol) was gradually added. The solution was stirred at 40 ° C for 24 h under a nitrogen atmosphere. After the polymerization reaction was completed, the mixture was poured into a methanol solution to extract the product, and then the product was separated by filtration and washed with methanol several times to obtain a yellow-brown powder. In order to further purify the product, the crude product was Soxhlet extracted in the order of methanol, petroleum ether, acetone, and chloroform, and the washing liquid of the chloroform stage was retained and spin-dried to obtain an electrochromic / electrofluorescent polymer.
[0042] The prepared electrochromic / electrofluorescent polymer was dissolved in dichloromethane to prepare a 3 mg / mL solution for use. Use tin oxide conductive glass as the substrate and place it on a heating plate at 90°C. Use a spray gun to evenly spray the solution on the surface of the substrate for 5 times. After spraying, place it in a 50°C oven to dry to obtain an electrochromic / electrofluorescent PDNPC polymer film.
[0043] Example 6: Preparation of polymer and film
[0044] Preparation of electrochromic / electrofluorescent polymer. 1 mmol of monomer III was dissolved in 20 mL of chloroform, and ferric chloride (FeCl3·6H2O, 3.3 mmol) was gradually added. The solution was stirred at 40 ° C for 24 h under a nitrogen atmosphere. After the polymerization reaction was completed, the mixture was poured into a methanol solution to extract the product, and then the product was separated by filtration and washed with methanol several times to obtain a yellow-brown powder. In order to further purify the product, the crude product was Soxhlet extracted in the order of methanol, petroleum ether, acetone, and chloroform, and the washing liquid of the chloroform stage was retained and spin-dried to obtain an electrochromic / electrofluorescent polymer.
[0045] The prepared electrochromic / electrofluorescent polymer was dissolved in tetrahydrofuran to prepare a 1.5 mg / mL solution for use. A polyethylene terephthalate conductive substrate was used as the substrate and placed on a heating plate at a temperature of 95°C. The solution was evenly sprayed on the surface of the substrate using a spray gun for 8 times. After spraying, it was placed in a 55°C oven for drying to obtain an electrochromic / electrofluorescent PDNPC polymer film.
[0046] Example 7: Electrochromic / Electro-controlled Fluorescent Device
[0047] This embodiment discloses an electrochromic / electrically controlled fluorescent device, which includes the film disclosed in Example 4 and an electrolyte layer, an ion storage layer and a transparent conductive layer sequentially arranged on the surface of the electrochromic / electrically controlled fluorescent polymer; the transparent conductive layer is selected from indium tin oxide conductive glass.
[0048] Example 8: Electrochromic / Electro-controlled Fluorescent Device
[0049] This embodiment discloses an electrochromic / electro-controlled fluorescent device, which includes the film disclosed in Example 5 and an electrolyte layer, an ion storage layer and a transparent conductive layer sequentially arranged on the surface of the electrochromic / electro-controlled fluorescent polymer; the transparent conductive layer is selected from tin fluoride conductive glass.
[0050] Example 9: Electrochromic / Electro-controlled Fluorescent Device
[0051] This embodiment discloses an electrochromic / electro-controlled fluorescent device, which includes the film disclosed in Example 6 and an electrolyte layer, an ion storage layer and a transparent conductive layer sequentially arranged on the surface of the electrochromic / electro-controlled fluorescent polymer; the transparent conductive layer is selected from a polyethylene terephthalate conductive substrate.
[0052] Performance Testing
[0053] 0.106g of lithium perchlorate was added to a 10mL volumetric flask and fixed to volume with acetonitrile (ACN) to obtain a 0.1mol / L solution, which was used as a blank supporting electrolyte solution. The electrochromic / electrofluorescent PDNPC polymer film prepared in Example 4 was used as a working electrode, a Pt wire as a counter electrode, and Ag / AgCl as a reference electrode to form a three-electrode system. The electrochemical, electrochromic, and electrofluorescent properties of the film were tested as follows.
[0054] The cyclic voltammetric performance of the electrochromic / electrofluorescent PDNPC polymer film at 0-1.3V was tested. The test results are as follows Figure 1 As shown. Figure 1 It can be seen that the prepared electrochromic / electrofluorescent PDNPC polymer film shows obvious redox peaks, which indicates that the polymer has good redox activity and the redox behavior is reversible.
[0055] The UV-visible absorption spectrum of the electrochromic / electrically controlled fluorescent PDNPC polymer film at a wavelength of 350-1100 nm is tested. The test results are as follows: Figure 2 Further, by testing the absorption change curve of the PDNPC polymer film at the maximum absorption wavelength of 505nm under a step voltage of 0 to 1.1V (as shown in Figure 3 The calculated optical contrast of the film is 53.8%. The coloring time is 3.3s and the fading time is 1.5s. Further, the cyclic stability of the film at 505nm was tested (as shown in Figure 4 As shown in FIG. 2 , after 250 cycles, the optical contrast of the PDNPC polymer film maintained 66.4% of the original contrast, which indicates that the prepared electrochromic / electrically controlled fluorescent film has good electrochromic properties.
[0056] The spectral performance of electrochromic / electrically controlled fluorescent PDNPC polymer film at a wavelength of 566nm was tested. The test results are as follows Figure 5 As shown in Figure 2, the calculated fluorescence switching contrast of the film is 137. The coloring time is 4.3s and the fading time is 4.4s. The fluorescence cycle stability of the film at 566nm was further tested. Figure 6As shown, after 30 cycles, the maximum fluorescence switching contrast of the PDNPC film maintained 66.8% of the original contrast, which indicates that the prepared electrochromic / electro-controlled fluorescent film has good electro-controlled fluorescent properties.
[0057] In summary, the polymer film of the present application has fast response speed, good stability, and high fluorescence contrast, and is expected to be used in the fields of sensors and 3D coded information storage.
Claims
1. A monomer, characterized in that The structural formula of the monomer is shown below: Wherein, R is selected from naphthalene, anthracene, and pyrene.
2. A polymer, characterized in that The structural formula of the repeating unit of the polymer is as follows: Wherein, n is 20 to 1000, and R is selected from naphthalene, anthracene, and pyrene.
3. A method for preparing the polymer according to claim 3, characterized in that: The polymer is formed by polymerizing the monomer of formula (I) in an organic solvent.
4. Application of the polymer according to claim 3 in the fields of optical display, sensor and 3D coded information storage.
5. A film, characterized in that: It comprises a substrate, and an electrochromic layer formed on the surface of the substrate by film processing from a solution; the electrochromic layer adopts the polymer material of claim 3.
6. A film according to claim 6, characterized in that: The solvent used in the film-forming process of the solution is any one of dichloromethane, chloroform, tetrahydrofuran, toluene and dimethylformamide.
7. A film according to claim 6, characterized in that: The substrate is selected from any one of indium tin oxide conductive glass, fluorine tin oxide conductive glass and polyethylene terephthalate conductive substrate.
8. A device, characterized in that A film comprising the film according to any one of claims 6 to 8.