Polyvinyl butyral resin and preparation method thereof

By adding a hydrogen bond disruptor diol to a polyvinyl alcohol solution and controlling the reaction conditions, the solubility and crosslinking problems of polyvinyl butyral resin were solved, achieving rapid dissolution and uniform particle size, improving the dispersibility and adhesion of ceramic slurry, and increasing production efficiency.

CN118909167AActive Publication Date: 2024-11-08ANHUI WANWEI ADVANCED FUNCTIONAL MEMBRANE MATERIALS RESEARCH INSTITUTE CO LTD +1

Patent Information

Application Number
CN202411153348.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-08
Estimated Expiration
2044-08-21

AI Technical Summary

Technical Problem

In the existing technology, polyvinyl butyral resin has a slow reaction rate and high production energy consumption at low temperatures, resulting in poor solubility and easy formation of intermolecular cross-linking reactions, which affects the uniformity of ceramic green bodies and product quality.

Method used

By adding hydrogen bond disrupting diols, such as propylene glycol or butanediol, to a polyvinyl alcohol solution and controlling the reaction temperature and feeding rate, a ternary system of polyvinyl alcohol-diol-water is formed, which weakens the hydrogen bond forces and regulates the uniformity and particle size distribution of the acetalization reaction.

Benefits of technology

This method enables the rapid dissolution of polyvinyl butyral resin in ethanol solution, resulting in uniform particle size distribution, improved dispersibility and adhesion of ceramic slurry, and enhanced production efficiency and product quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005004220890000091
    Figure BDA0005004220890000091
  • Figure BDA0005004220890000101
    Figure BDA0005004220890000101
Patent Text Reader

Abstract

The invention discloses polyvinyl butyral resin and a preparation method thereof, and belongs to the technical field of high polymer materials, the polyvinyl butyral resin is prepared into 10.0 wt% ethanol solution to be dissolved within 30 min; the viscosity change rate of the 10.0 wt% ethanol solution prepared from the polyvinyl butyral resin is less than 1.5 after the solution is placed for 24 hours; the particle size of the polyvinyl butyral resin ranges from 1.20 to 2.00; the viscosity change is small under the high solid content, the polyvinyl butyral resin is prepared into 10wt% and 20wt% ethanol solutions, and the rotary viscosity V20wt% / V10wt% lt is tested; 20. According to the preparation method provided by the invention, the hydrogen bond breaker is added into the polyvinyl alcohol-water system, so that the hydrogen bond acting force is effectively reduced, and the ceramic slurry has relatively good dispersity and dissolvability when being prepared, and has good market competitiveness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer materials, and particularly relates to a polyvinyl butyral resin and a preparation method thereof. Background Art

[0002] Polyvinyl butyral (PVB) is often used for bonding and assembly of electronic instrument components, bonding of metals and porous materials, and electronic ceramics because of its good bonding properties. There are vinyl alcohol groups (VA units), vinyl butyral (VB units), and vinyl acetate (VAc units) in the PVB molecular chain, and the existence of the above groups in the molecular chain affects the solubility and bonding properties of polyvinyl butyral resin. In the application of electronic ceramics, polyvinyl butyral resin is generally used as a binder to increase the strength of ceramics after bonding. First, the polyvinyl butyral polymer needs to be dissolved in an organic solvent to form a solution with a certain adhesion effect; then, the ceramic powder is added to the above solution, and the ceramic powder is uniformly dispersed in the organic solution by continuous stirring, and adheres to each other; finally, it is dried to form a cast green body with a certain strength and plasticity. Among them, the dissolution rate of polyvinyl acetal resin in organic solvents is very important. Fast dissolution rate and small viscosity change are conducive to better preparation of slurry compositions and improved production efficiency.

[0003] In the engineering production of PVB resin adhesives for electronic ceramics, in order to ensure the stability of the reaction system and prevent problems such as agglomeration during resin synthesis, it is necessary to carry out a long-term stable reaction at a low temperature of 0 to 5.0°C. However, this causes problems such as slow acetalization reaction speed, high production energy consumption, and low production efficiency, which is not conducive to efficient production in engineering. In addition, at a lower condensation reaction temperature, the hydrogen bond force in the polyvinyl alcohol-water system used in the conventional process is strong, and strong interchain interactions are easily formed. Due to the strong hydrogen bond interactions between and within the polyvinyl alcohol-water molecular chains, intermolecular cross-linking reactions are prone to occur during the acetalization reaction. As the reaction continues, the cross-linking situation intensifies, and butyraldehyde is difficult to react with the PVA molecular chains wrapped inside, resulting in uneven acetalization reaction, which ultimately leads to the generated PVB resin showing low solubility in the solution, and even problems such as insolubility. If the PVB resin cannot be dissolved evenly and quickly in the alcohol solvent, the ceramic powder cannot be fully dispersed when mixed with the ceramic powder. Ultimately, during the preparation of the ceramic green body, the surface of the green body will become uneven, seriously affecting the product quality.

[0004] The key to improving the solubility of PVB resin products lies in controlling the uniformity of the acetalization reaction of PVB resin and reducing the degree of cross-linking between PVB molecules. The key to controlling the uniformity of the acetalization reaction of PVB resin lies in reducing the hydrogen bond interaction of the reaction system.

[0005] In addition, it is also necessary to regulate the resin size particles, with a wide particle size distribution, good dispersibility in the solvent, and the solvent can penetrate into the particle size, further accelerating the dissolution rate. Some patents report methods for regulating hydrogen bond interactions. For example, the patent application with publication number CN115677886A discloses the inhibition of interchain crosslinking reactions by using inorganic salts. By introducing ions that can destroy the strong interaction of hydrogen bonds in the PVA stock solution, the crosslinking reaction can be prevented to a certain extent. However, the use of a large amount of inorganic salts causes water washing difficulties, and the residual trace ions have an adverse effect on the weather resistance and aging resistance of the product. Or, as disclosed in the patent application with publication number CN103124748A, the use of modified polyvinyl alcohol is improved by changing the polarity of the molecular end, solubility in water, and surface activity effect, thereby producing a polyvinyl alcohol acetal resin with excellent solubility performance. However, this process is complicated, has high requirements for the production process of PVA raw materials, and the change of the molecular end group needs to be confirmed by nuclear magnetic resonance, which is not conducive to industrial production. Summary of the invention

[0006] The object of the present invention is to provide a polyvinyl butyral resin and a preparation method thereof, so as to solve the problem of poor solubility of the polyvinyl butyral resin.

[0007] The purpose of the present invention can be achieved by the following technical solutions:

[0008] A polyvinyl butyral resin, wherein the polyvinyl butyral resin is configured to be dissolved in a 10.0 wt% ethanol solution within 30 minutes;

[0009] The viscosity of the polyvinyl butyral resin prepared into a 10.0 wt% ethanol solution is placed for 24 hours and the viscosity change rate is less than 1.5, that is, V 10wt%,24h / V 10wt% <1.5;

[0010] The particle size distribution of the polyvinyl butyral resin is in the range of 1.20 to 2.00;

[0011] The polyvinyl butyral resin was prepared into 10wt% and 20wt% ethanol solutions, and the rotational viscosity was tested. The ratio between the two (viscosity change rate) was less than 20, that is, V 20wt% / V 10wt% <20.

[0012] Furthermore, the polyvinyl butyral resin is used as an adhesive for ink, an adhesive for coatings, or an adhesive for ceramic molding.

[0013] A method for preparing polyvinyl butyral resin comprises adding a hydrogen bond breaker in the process of preparing a polyvinyl alcohol solution, wherein the hydrogen bond breaker is a diol.

[0014] Furthermore, the amount of the hydrogen bond destroyer added is 5%-10% of the mass of the polyvinyl alcohol;

[0015] The diol is one of propylene glycol and butylene glycol.

[0016] Butanediol is one of 1,2-butanediol, 1,3-butanediol and 1,4-butanediol;

[0017] Propylene glycol is one of 1,2-propylene glycol and 1,3-propylene glycol.

[0018] Preferably, the butanediol is 1,4-butanediol, and the propylene glycol is 1,3-propylene glycol.

[0019] A method for preparing polyvinyl butyral resin comprises the following steps:

[0020] Step a, dissolving polyvinyl alcohol in water, and then adding a hydrogen bond breaker to obtain a polyvinyl alcohol solution;

[0021] Step b, controlling the temperature of the reaction system to 20-60° C., adding part of butyraldehyde and part of the acid catalyst to the mixed solution and mixing them evenly, and controlling the temperature of the system to 30-50° C. for insulation;

[0022] Step c, controlling the system temperature to 20-30° C., and adding the remaining butyraldehyde and the remaining acid catalyst dropwise; in the present invention, the hydrogen bonding effect is further reduced by reacting at 20-30° C., and at this temperature, the amount of butyraldehyde and hydrochloric acid added and the time used for adding the materials form a certain degree of acetalization.

[0023] Step d, after the remaining butyraldehyde and the remaining acid catalyst are added dropwise, the system temperature is controlled to be 20-30° C., the reaction is continued with low temperature stirring, and then the system temperature is controlled to be gradually increased to 40-60° C., and the temperature is kept for aging;

[0024] Step e, cooling the matured system to below 60° C., adding alkali solution into the system, stirring, filtering, and washing and drying the solid resin product obtained after filtering to obtain polyvinyl butyral resin.

[0025] Furthermore, the mass fraction of polyvinyl alcohol in the polyvinyl alcohol solution is 5%-15%;

[0026] The degree of polymerization of the polyvinyl alcohol is 200-2500.

[0027] Furthermore, the acidic catalyst is one of hydrochloric acid, sulfuric acid and phosphoric acid.

[0028] Furthermore, the total amount of butyraldehyde is 50%-60% of the mass of polyvinyl alcohol;

[0029] The mass fraction of the acid catalyst is 31%, and the total amount of the acid catalyst is 30%-50% of the mass of the polyvinyl alcohol;

[0030] In step b, the portion of butyraldehyde is 5% to 60% of the total amount of butyraldehyde;

[0031] In step b, the portion of the acidic catalyst is 50%-100% of the total amount of the acidic catalyst.

[0032] Furthermore, the insulation time in step b is 0.5-2h;

[0033] The time of low temperature stirring reaction in step d is 30-120min;

[0034] The gradient heating time in step d is 60-240 min;

[0035] The heat preservation and aging time in step d is 60-240 minutes;

[0036] The stirring time of adding the alkali solution in step e is 5-30 minutes.

[0037] Beneficial effects of the present invention:

[0038] 1. In the present invention, the polyvinyl alcohol-water system is changed to a polyvinyl alcohol-diol-water ternary system, and the hydrogen bond force between the polyvinyl alcohol molecular chains is weakened by adding a hydrogen bond breaker, thereby reducing the degree of crosslinking between molecules. A hydrogen bond breaker that can destroy the hydrogen bond interaction is introduced into the reaction system, and the thermodynamic conditions of the acetalization reaction are controlled, thereby achieving the purpose of controlling the crosslinking reaction in the synthesis process of the PVB resin and regulating the uniformity of the acetalization reaction, thereby achieving the purpose of regulating the solubility performance of the product.

[0039] 2. Since PVA molecules contain a large number of hydroxyl groups, strong hydrogen bond interactions are easily formed between molecules and within molecules, which intensifies the degree of crosslinking between PVA molecules. In the subsequent acetalization reaction with an acidic catalyst and an aldehyde through a temperature increase reaction, a PVB with a high degree of intramolecular crosslinking is formed, which is not conducive to dissolution in a solvent. The present invention introduces a hydrogen bond breaker into the PVA system. When heated, the hydrogen bonds in the polyvinyl alcohol aqueous solution are reorganized, and the hydrogen bonds between the PVA molecular chains and the chains are replaced by hydrogen bonds between the PVA molecular chains and the aqueous solvent and the co-solvent, which weakens the hydrogen bond force and reduces the degree of crosslinking between PVA molecules in the homogeneous phase. In addition, by regulating the synthesis process, the degree of crosslinking between PVB molecular chains is reduced, thereby achieving the purpose of improving the solubility performance of the PVB resin. The hydrogen bonding force can be weakened by increasing the reaction temperature and diluting the concentration, i.e. reducing the solid content, reducing the cross-linking between molecules, and adding some butyraldehyde and hydrochloric acid, which makes it easier to form a certain degree of acetalization in the system, but not to the extent that PVB can be precipitated. At the same time, at high temperatures, a small amount of PVB molecular chains are cross-linked and the stretching degree between the chains is high, which is more conducive to the further reaction of butyraldehyde with the PVB with a lower degree of acetalization wrapped inside, promoting the acetalization reaction, and making the acetalization in the whole system more uniform. When the reaction temperature is reduced to a low temperature, since a certain degree of acetalization has been formed in the system at high temperature, the remaining butyraldehyde and hydrochloric acid are added at this time, and the PVB resin is precipitated faster and the particle size is more uniform.

[0040] 3. In the preparation method of the present invention, when the phase transition critical point is reached, the feeding is stopped, and the acetalization degree is further increased by keeping the temperature at high temperature for a period of time. A small amount of crystals have been precipitated in the system, and the system is turbid in the macroscopic manifestation. At this time, the remaining butyraldehyde and acid are added simultaneously, and the acetalization reaction is further carried out on the precipitated small amount of crystals to form a PVB resin with a wide particle size distribution. The PVB resin with a wide particle size distribution is better dispersed in the solvent, and the solubility is improved.

[0041] 4. The process of the present invention is simple and the cost is low. Compared with the existing production process, the present invention does not need to add other catalysts or emulsifiers that may affect the product performance, and the added hydrogen bond destroyer does not participate in the reaction. After the reaction is completed, it is washed away by water without any residue. At the same time, the process conditions of the present invention are simple, and the solubility of the resin can be regulated without changing the existing production equipment, so that it has better dispersibility, solubility and adhesion when making ceramic slurry, and has good market competitiveness.

[0042] 5. According to the present invention, a polyvinyl acetal resin can be provided. When the resin of the present invention is used as an ink or coating binder, it has good dispersibility in the ink when used at a high concentration.

[0043] 6. According to the present invention, a polyvinyl alcohol acetal resin can be provided. When the resin of the present invention is used as an electronic ceramic adhesive, it dissolves quickly in an organic solvent and has no undissolved colloids. It has good adhesion to inorganic materials when preparing ceramic slurry, and the composite system has good uniformity and stability. It can greatly optimize cracking and other phenomena during high-temperature sintering, and can produce laminated ceramic capacitors with excellent reliability, which greatly improves production efficiency. DETAILED DESCRIPTION

[0044] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0045] Example 1

[0046] This embodiment provides a polyvinyl butyral resin, which is prepared by the following steps:

[0047] Step a, dissolving 100 g of polyvinyl alcohol with an average degree of polymerization of 500 (alcoholysis degree of 99.05 wt%) in 1150.0 g of pure water, and stirring at 95° C. for 3 h to fully dissolve it, to obtain a polyvinyl alcohol stock solution with a solid content of 8.0 wt%; adding 10.0 g of butanediol to the prepared stock solution to obtain a polyvinyl alcohol solution;

[0048] Step b, cool the polyvinyl alcohol solution prepared above to 30°C, add 6.05g of butyraldehyde to the system, mix thoroughly, then uniformly add 23.59g of hydrochloric acid with a mass concentration of 36% to 38% to the system within 30min, and keep warm for 0.5h.

[0049] Step c, cool the system to 20.0°C, and simultaneously dropwise add the remaining 54.45g of butyraldehyde and 23.59g of hydrochloric acid at a uniform rate within 60min.

[0050] Step d: After all the butyraldehyde and hydrochloric acid are added, the reaction is continued to be stirred at this temperature for 30 minutes; then the reaction system is heated to 40° C. at a rate of 5° C. / h, and the reaction is stirred at this temperature for 2 hours.

[0051] Step e: After stirring at 40° C. for 2 h, 80 mL of 15 wt % sodium hydroxide was added to the reaction solution, and the mixture was stirred for 30 min. The mixture was centrifuged for dehydration and dried to obtain a solid product.

[0052] Example 2

[0053] This example is prepared by the same method and conditions as Example 1, except that butanediol is replaced by propylene glycol in step a.

[0054] Example 3

[0055] This example was prepared by the same method and conditions as Example 1, except that the content of butanediol in step a was changed from 10.0 g to 5.0 g.

[0056] Example 4

[0057] This example was prepared by the same method and conditions as in Example 1, except that the addition stage of butanediol in step a was changed to that after phase change and precipitation in step c;

[0058] Example 5

[0059] This embodiment is prepared by the same method and conditions as Example 1, except that the mass ratio of polyvinyl alcohol to pure water in step a is 1:12; the amount of butyraldehyde added in the first step in step b is changed from 6.05 g to 12.10 g, and the amount of butyraldehyde added in the second step in step c is changed from 54.45 g to 48.40 g.

[0060] Example 6

[0061] This embodiment is prepared by the same method and conditions as Example 1, except that: the mass ratio of polyvinyl alcohol to pure water in step a is 1:14; the amount of butyraldehyde added in the first step in step b is changed from 6.05 g to 18.15 g, and the amount of acid added in the first step is changed from 47.17 g to 33.02 g; the amount of butyraldehyde added in the second step in step c is changed from 54.45 g to 42.35 g; and the amount of acid added in the second step is changed from 0 g to 14.15 g.

[0062] Example 7

[0063] This example was prepared by the same method and conditions as in Example 1, except that: in step a, the PVA with an average degree of polymerization of 500 was replaced with a PVA with an average degree of polymerization of 800;

[0064] Example 8

[0065] This example was prepared by the same method and conditions as in Example 1, except that: in step a, the PVA with an average degree of polymerization of 500 was replaced with PVA with an average degree of polymerization of 1700;

[0066] Comparative Example 1

[0067] This example was prepared by the same method and conditions as Example 1, except that the amount of butanediol added in step a was changed from 10.0 g to 0 g.

[0068] Comparative Example 2

[0069] This example was prepared by the same method and conditions as Example 1, except that the amount of butanediol added in step a was changed from 10.0 g to 20.0 g.

[0070] Comparative Example 3

[0071] This example was prepared by the same method and conditions as in Example 1, except that the addition stage of butanediol in step a was changed to step d;

[0072] Comparative Example 4

[0073] This example is prepared by the same method and conditions as Example 1, except that the temperature in steps b and c is reduced from 30.0°C and 20°C to 5.0°C instead.

[0074] Comparative Example 5

[0075] This example was prepared by the same method and conditions as Example 1, with the only difference being that in step a, the PVA with an average degree of polymerization of 500 was replaced by the PVA with an average degree of polymerization of 800; and the amount of butanediol added was changed from 10.0 g to 0 g.

[0076] Comparative Example 6

[0077] This comparative example was prepared by the same method and conditions as Example 1, except that the butanediol in step a was replaced by methanol.

[0078] Comparative Example 7

[0079] This example was prepared by the same method and conditions as Example 1, with the only difference being that the PVA with an average degree of polymerization of 500 in step a was replaced by the PVA with an average degree of polymerization of 1700; and the amount of butanediol added was changed from 10.0 g to 0 g.

[0080] <Evaluation method>:

[0081] 1. High solid viscosity ratio: PVB resin was dissolved in ethanol to prepare 10.0wt% and 20wt% solutions, and the rotational viscosity was tested at 20.0℃ to calculate different solid viscosity ratios.

[0082] 2. Uniformity: PVB resin was dissolved in ethanol at 60° C. to prepare a 10.0 wt % solution, and the transmittance of the solution at a wavelength of 660 nm was tested using an ultraviolet spectrophotometer.

[0083] 3. Solubility:

[0084] (1) Dissolution time: PVB resin was dissolved in ethanol solvent to prepare a 10.0 wt% solution, placed in a 20.0° C. water bath and stirred at 500 r / min, and the time when it was completely dissolved was recorded.

[0085] (2) Viscosity change after standing: PVB resin was dissolved in ethanol to prepare a 10.0 wt% solution and then left for 24 hours to measure the viscosity change:

[0086] Excellent solubility: V 10wt%,24h / V 10wt% <1.5;

[0087] General solubility: 1.5 <V 10wt%,24h / V 10wt% <1.7

[0088] Poor solubility: V 10wt%,24h / V 10wt% >1.7;

[0089] (3) Dissolution status after 30 min.

[0090] 4. Particle size distribution (discreteness): Use a laser particle size analyzer to test and obtain the particle size and discreteness.

[0091] The test results corresponding to Examples 1 to 7 and Comparative Examples 1 to 6 are shown in Tables 1 and 2 below:

[0092] Table 1

[0093]

[0094] Table 2

[0095]

[0096] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0097] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A polyvinyl butyral resin, characterized in that The polyvinyl butyral resin is configured to be dissolved in a 10.0 wt % ethanol solution within 30 minutes; The viscosity of the polyvinyl butyral resin in a 10.0 wt% ethanol solution is set aside for 24 hours and the viscosity change rate is less than 1.5; The particle size distribution of the polyvinyl butyral resin is in the range of 1.20 to 2.00; Polyvinyl butyral resin was prepared into 10wt%, 20wt% ethanol solution, and the rotational viscosity and viscosity change rate V were tested. 20wt% / V 10wt% <20.

2. The polyvinyl butyral resin according to claim 1, characterized in that The polyvinyl butyral resin is used as an adhesive for ink, an adhesive for coating or an adhesive for ceramic molding.

3. A method for preparing a polyvinyl butyral resin, characterized in that: For preparing the polyvinyl butyral resin as claimed in claim 1, a hydrogen bond breaker is added during the preparation of the polyvinyl alcohol solution, and the hydrogen bond breaker is a diol.

4. The method for preparing a polyvinyl butyral resin according to claim 3, characterized in that: The amount of the hydrogen bond destroyer added is 5%-10% of the mass of the polyvinyl alcohol; The diol is one of propylene glycol and butylene glycol.

5. The method for preparing a polyvinyl butyral resin according to claim 3, characterized in that: The steps include: Step a, dissolving polyvinyl alcohol in water, and then adding a hydrogen bond breaker to obtain a polyvinyl alcohol solution; Step b, controlling the temperature of the reaction system to 20-60° C., adding part of butyraldehyde and part of the acid catalyst to the mixed solution and mixing them evenly, and controlling the temperature of the system to 30-50° C. for insulation; Step c, controlling the system temperature to 20-30° C., and adding the remaining butyraldehyde and the remaining acid catalyst dropwise; Step d, after the remaining butyraldehyde and the remaining acid catalyst are added dropwise, the system temperature is controlled to 20-30° C., the reaction is continued with low temperature stirring, and then the system temperature is controlled to 40-60° C., and the temperature is kept for aging; Step e, cooling the matured system to below 60° C., adding alkali solution into the system, stirring, filtering, and washing and drying the solid resin product obtained after filtering to obtain polyvinyl butyral resin.

6. The method for preparing a polyvinyl butyral resin according to claim 5, characterized in that: The mass fraction of polyvinyl alcohol in the polyvinyl alcohol solution is 5%-15%; The degree of polymerization of the polyvinyl alcohol is 200-2500.

7. The method for preparing a polyvinyl butyral resin according to claim 5, characterized in that: The acidic catalyst is one of hydrochloric acid, sulfuric acid and phosphoric acid.

8. The method for preparing a polyvinyl butyral resin according to claim 5, characterized in that: The total amount of butyraldehyde is 50%-60% of the mass of polyvinyl alcohol; The mass fraction of the acid catalyst is 31%, and the total amount of the acid catalyst is 30%-50% of the mass of the polyvinyl alcohol; In step b, the portion of butyraldehyde is 5% to 60% of the total amount of butyraldehyde; In step b, the portion of the acidic catalyst is 50%-100% of the total amount of the acidic catalyst.

9. The method for preparing a polyvinyl butyral resin according to claim 5, characterized in that: The insulation time in step b is 0.5-2h; The time of low temperature stirring reaction in step d is 30-120min; The heat preservation and aging time in step d is 60-240 minutes; The stirring time of adding the alkali solution in step e is 5-30 minutes.

Citation Information

Patent Citations

  • Modified polyvinyl alcohol, modified polyvinyl acetal and ceramic slurry composition

    CN103124748A

  • Method for preparing high-acetalization-rate polyvinyl butyral without adding surfactant

    CN115677886A

  • High acetalization degree polyvinyl butyral resin and preparation method thereof

    CN108299578A

  • Heat-resistant PVB resin and preparation method thereof

    CN113461841A

  • Water-based PVB (polyvinyl butyral) emulsion and preparation method thereof

    CN114456283A

Cited By

  • Whitening type temperature indicator based on polyvinyl acetal polymer

    CN122149675A