Surface-modified hexagonal boron nitride and polyimide composite heat-conducting film as well as preparation method and application thereof

Hexagonal boron nitride is surface treated by small molecule coupling agent and polymer modifier, which improves its compatibility with polyimide, and solves the dispersion and interface of hexagonal boron nitride in the polyimide matrix. The problem of insufficient compatibility achieves excellent thermal conductivity and mechanical properties of the polyimide composite thermal conductivity film, and is low in cost.

CN118909309APending Publication Date: 2024-11-08NINGBO BOYA POLY ADVANCED MATERIALS CO LTD

Patent Information

Application Number
CN202411136417.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the prior art, the poor dispersion and insufficient interfacial compatibility of hexagonal boron nitride in the polyimide matrix lead to poor thermal conductivity and mechanical properties of the composite film, and the existing surface modification methods are expensive and difficult to commercially .

Method used

Small-molecular coupling agent and polymer modifier are used to surface treatment of hexagonal boron nitride, introducing a large number of hydrophilic groups, improving its compatibility with polyimide, reducing the probability of interfacial voids, and forming low structural defects. Polyimide composite thermal conductive film with high order orientation.

Benefits of technology

The excellent thermal conductivity and mechanical properties of the polyimide composite thermal conductivity film are achieved, with low cost and significant modification effect, and both high thermal conductivity and high mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005001061430000081
    Figure BDA0005001061430000081
  • Figure BDA0005001061430000082
    Figure BDA0005001061430000082
  • Figure BDA0005001061430000141
    Figure BDA0005001061430000141
Patent Text Reader

Abstract

The invention provides a surface-modified hexagonal boron nitride and polyimide composite heat-conducting film as well as a preparation method and application thereof. The surface-modified hexagonal boron nitride is obtained by sequentially carrying out surface treatment on unmodified hexagonal boron nitride through a micromolecular coupling agent and a macromolecular modifier; a small-molecule coupling agent and a high-molecular modifier are matched to serve as a modifier, a large number of hydrophilic groups are successfully introduced to the surface of hexagonal boron nitride, and then the compatibility of the obtained surface-modified hexagonal boron nitride and polyimide is effectively improved; the interior of the polyimide composite heat-conducting film prepared by compounding the two has low structural defects and high-order structural orientation, so that the polyimide composite heat-conducting film has excellent heat-conducting property and mechanical property.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of thin films, and in particular relates to a surface-modified hexagonal boron nitride and polyimide composite thermally conductive film and a preparation method and application thereof. Background Art

[0002] At present, most heat dissipation components in electronic devices are made of metal materials such as copper or aluminum alloy. Although the thermal conductivity of pure copper and pure aluminum can be as high as 402W / (m·K) and 237W / (m·K) respectively, metal thermal conductive materials have disadvantages such as poor flexibility, high density, easy oxidation and no insulation. Therefore, the development of organic thermal conductive materials with good flexibility, low density, chemical stability and good insulation has become a hot research direction.

[0003] Polyimides (PI) are a class of organic polymer compounds containing imide rings and aromatic ring structures on the main chain. This special molecular structure gives it excellent mechanical properties, high and low temperature resistance, low dielectric properties and chemical stability, so it is widely used as an electronic packaging material; however, the thermal conductivity of the PI film itself is low (generally around 0.2W / (m·K)), which cannot meet the heat dissipation requirements of microelectronic devices; therefore, in order to improve the thermal conductivity of the PI film, it is usually necessary to introduce high thermal conductivity filler particles so that heat is more transmitted along the thermal conduction path formed by the filler particles, which significantly improves the thermal conductivity of the PI film; due to the poor interface compatibility between the inorganic thermal conductive filler particles and the PI matrix, gaps are easily formed at the interface between the two phases, which not only leads to a significant decrease in the mechanical properties of the composite film, but also seriously affects the thermal conductivity of the composite film. The easy agglomeration of the inorganic thermal conductive filler particles also makes it difficult to form a continuous thermal conduction path in the PI matrix when the filler content is low, which seriously affects the thermal conductivity of the PI composite film; therefore, it is necessary to surface modify the inorganic thermal conductive filler.

[0004] Hexagonal boron nitride (h-BN) is one of the most commonly used inorganic thermal conductive fillers. Due to its surface hydrophobic properties, the unsurface-modified h-BN has poor dispersibility in the polymer matrix, and it is easy for the filler particles to agglomerate, resulting in serious phonon scattering, which affects the orderly transfer of heat. Moreover, the unsurface-modified h-BN has poor interface compatibility with polymer matrices such as PI, and it is very easy to form voids at the interface between the two phases during processing such as thermoforming, which seriously affects the mechanical properties and thermal conductivity of the composite film.

[0005] At present, the reported h-BN surface modification methods usually use small molecule modifiers such as titanate coupling agents, siloxane coupling agents, and 2,4-diisocyanatotoluene. However, since there are few groups available for modification on the h-BN surface, the amount of small molecule modifiers that can be grafted on its surface is also very small, which has a very limited effect on improving the interfacial compatibility between filler particles and polymer matrices. In addition, CN116061525A discloses a polydopamine-modified boron nitride nanosheet / polyimide composite fiber thermal conductive film and its preparation method and application. The polydopamine-modified boron nitride nanosheet is added to a polyamic acid solution and stirred to obtain a polydopamine-modified boron nitride nanosheet / polyamic acid mixed solution; a composite fiber felt is prepared by using the polydopamine-modified boron nitride nanosheet / polyamic acid mixed solution through an electrospinning method, and the composite fiber felt is subjected to thermal imidization treatment to obtain a polydopamine-modified nitride film. Boron nanosheet / polyimide composite fiber felt; several layers of polydopamine modified boron nitride nanosheet / polyimide composite fiber felt are compression molded to obtain the polydopamine modified boron nitride nanosheet / polyimide composite fiber thermal conductive film, the method combines low-temperature polycondensation, electrospinning and compression molding to achieve zigzag directional arrangement of PI fibers, so that the mechanical properties and thermal conductivity of the PI fiber film are significantly improved; however, the high price of dopamine means that this modification method cannot be commercially applied.

[0006] Therefore, in view of the above technical problems, it is urgent to develop a surface-modified hexagonal boron nitride with low cost and excellent modification effect. Summary of the invention

[0007] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a surface-modified hexagonal boron nitride and polyimide composite thermally conductive film and a preparation method and application thereof. By selecting a small molecule coupling agent and a polymer modifier as modifiers to sequentially treat the surface of hexagonal boron nitride, a large number of hydrophilic groups are successfully introduced on the surface of hexagonal boron nitride, thereby effectively improving the compatibility of the surface-modified hexagonal boron nitride and polyimide, so that the polyimide composite thermally conductive film composited by the two can have both excellent thermal conductivity and mechanical properties.

[0008] To achieve this object, the present invention adopts the following technical solutions:

[0009] In a first aspect, the present invention provides a surface-modified hexagonal boron nitride, wherein the surface-modified hexagonal boron nitride is obtained by sequentially surface-treating unmodified hexagonal boron nitride with a small molecule coupling agent and a polymer modifier.

[0010] The surface-modified hexagonal boron nitride provided by the present invention is obtained by sequentially surface-treating unmodified hexagonal boron nitride with a small molecule coupling agent and a polymer modifier. The small molecule coupling agent and the polymer modifier are used together as modifiers, which not only has low cost, but also can successfully introduce a large number of hydrophilic groups on the surface of the hexagonal boron nitride by combining the two, effectively improving the dispersibility of the hexagonal boron nitride in the polyamic acid solution and the compatibility with polyimide, greatly reducing the probability of generating voids at the interface between the two phases during the casting and baking process, so that the finally obtained polyimide composite thermally conductive film has low structural defects and a highly ordered orientation structure inside, thereby having both excellent thermal conductivity and mechanical properties.

[0011] Preferably, the mass ratio of the unmodified hexagonal boron nitride, the small molecule coupling agent and the polymer modifier is 10:(2-6):(2-4), for example, 10:2:2, 10:3:2.2, 10:4:2.5, 10:4:3, 10:5:6.5 or 10:6:4, etc.

[0012] Preferably, the unmodified hexagonal boron nitride has a thickness of 2 to 100 nm, for example, 2 nm, 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm or 100 nm.

[0013] Preferably, the radial length of the unmodified hexagonal boron nitride is 0.1-100 μm, for example, 0.15 μm, 10 μm, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm or 100 μm.

[0014] Preferably, the small molecule coupling agent includes any one of an isocyanate small molecule coupling agent, a titanate small molecule coupling agent or a silane small molecule coupling agent, or a combination of at least two of them.

[0015] Preferably, the isocyanate small molecule coupling agent includes any one of p-phenylene diisocyanate, bis(4-isocyanatephenyl)methane, toluene-2,4-diisocyanate or 4,4'-diisocyanate dicyclohexylmethane, or a combination of at least two thereof.

[0016] Preferably, the titanate small molecule coupling agent includes any one or a combination of at least two of tetraethyl titanate, tetra-tert-butyl titanate, tetraisooctyl titanate, isopropyl dioleyl (dioctyl phosphate) titanate, isopropyl tris(dioctyl phosphate) titanate, isopropyl trioleyl titanate, diisopropyl ethyl acetoacetate titanate, triisostearate titanate isopropyl, bis(dioctyl pyrophosphate) ethylene titanate, di(triethanolamine) titanate diisopropyl, isopropyl tris(dioctyl pyrophosphate) titanate, di(triethylamine) titanate diisopropyl or tetraisopropyl di(dioctyl phosphite) titanate.

[0017] Preferably, the silane-based small molecule coupling agent includes γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, γ-aminopropylmethyldiethoxysilane, γ-aminopropylmethyldimethoxysilane, N-phenyl-γ-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane, N,N-diethyl-3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, γ-diethylenetriaminopropyltrimethoxysilane, γ-diethylaminomethyltriethoxysilane, N-phenylaminomethyltriethoxysilane, bis-(γ-trimethoxysilylpropyl) Amine, bis(3-triethoxysilylpropyl)amine, 4-amino-3,3-dimethylbutyltrimethoxysilane, 3-(2-aminoethyl)-aminopropyltriethoxysilane, 3-(N,N-dimethylaminopropyl)-aminopropylmethyldimethoxysilane, (N,N-dimethyl-3-aminopropyl)trimethoxysilane, N-(n-butyl)-γ-aminopropyltrimethoxysilane, vinylbenzylaminoethylaminopropyltrimethoxysilane, N-cyclohexyl-γ-aminopropylmethyldimethoxysilane, 3-ureidopropyltrimethoxysilane, 3-ureidopropyltriethoxysilane, γ-piperazinylpropylmethyldimethoxysilane, γ-glycidyl Oleyloxypropyl trimethoxysilane, γ-glycidyloxypropyl triethoxysilane, 3-(2,3-epoxypropyloxy)propyl methyldimethoxysilane, β-(3,4-epoxycyclohexyl)-ethyltriethoxysilane, β-(3,4-epoxycyclohexyl)-ethyltrimethoxysilane, 3-(2,3-epoxypropyloxy)propylmethyldiethoxysilane, γ-methacryloxypropyl trimethoxysilane, γ-methacryloxypropyl triisopropoxysilane, γ-methacryloxypropyl methyldimethoxysilane, γ-methacryloxypropyl tri(trimethylsiloxy)silane, 3-methacryloxypropyl tri Any one of ethoxysilane, 3-(methacryloyloxy)propylmethyldiethoxysilane, 3-acetoxypropyltrimethoxysilane, 3-(acryloyloxy)propyltrimethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, vinyltriisopropoxysilane, vinyltri(2-methoxyethoxy)silane, vinyltriacetoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, methylphenyldimethoxysilane, methylphenyldiethoxysilane, γ-mercaptopropyltrimethoxysilane, γ-mercaptopropyltriethoxysilane, methyltrimethoxysilane or tetraethoxysilane, or a combination of at least two thereof.

[0018] Preferably, the polymer modifier includes any one of polyethyleneimine (PEI), polyethylene glycol 400 (PEG-400), polyethylene glycol 600 (PEG-600), polyethylene glycol 800 (PEG-800), polyethylene glycol 1000 (PEG-1000), polyethylene glycol 2000 (PEG-2000), polyvinyl alcohol (PVA), branched polyethyleneimine-block-polyethylene glycol (branched PEI-g-PEG) or polyacrylic acid (PAA) or a combination of at least two thereof.

[0019] In a second aspect, the present invention provides a method for preparing the surface-modified hexagonal boron nitride as described in the first aspect, the preparation method comprising the following steps:

[0020] (1) reacting unmodified hexagonal boron nitride and a small molecule coupling agent in solvent A, filtering, and obtaining hexagonal boron nitride modified with a small molecule coupling agent;

[0021] (2) reacting the hexagonal boron nitride modified with the small molecule coupling agent obtained in step (1) with a polymer modifier in solvent B, filtering, and obtaining the surface-modified hexagonal boron nitride.

[0022] Preferably, the mass ratio of the unmodified hexagonal boron nitride, the small molecule coupling agent and the polymer modifier is 10:(2-6):(2-4), for example, 10:2:2, 10:3:2.2, 10:4:2.5, 10:4:3, 10:5:6.5 or 10:6:4, etc.

[0023] Preferably, the solvent A and the solvent B each independently include any one of water, methanol, ethanol, isopropanol, tert-butanol, toluene, p-xylene, n-hexane, tetrahydrofuran, N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc) or N-methylpyrrolidone (NMP) or a combination of at least two thereof.

[0024] Preferably, based on the mass of the unmodified hexagonal boron nitride as 1 g, the amount of the solvent A is 10 to 20 mL (e.g., 10 mL, 12 mL, 14 mL, 16 mL, 18 mL or 20 mL, etc.), and the amount of the solvent B is 10 to 15 mL (e.g., 10 mL, 11 mL, 12 mL, 13 mL, 14 mL or 15 mL, etc.).

[0025] Preferably, the reaction temperature in step (1) is 30-100°C, for example, 30°C, 40°C, 50°C, 60°C, 70°C, 80°C, 90°C or 100°C, more preferably 50-100°C, further preferably 50-70°C.

[0026] Preferably, the reaction time of step (1) is 20 to 30 h, for example, 20 h, 22 h, 24 h, 26 h, 28 h or 30 h.

[0027] Preferably, the filtration in step (1) is reduced pressure filtration.

[0028] Preferably, after the filtration in step (1) is completed, a washing step is further included to remove the incompletely reacted small molecule coupling agent.

[0029] Preferably, the washing agent used in the washing comprises solvent A.

[0030] Preferably, the reaction temperature in step (2) is 30-100°C, such as 30°C, 40°C, 50°C, 60°C, 70°C, 80°C, 90°C or 100°C, more preferably 30-70°C.

[0031] Preferably, the reaction time of step (2) is 10 to 15 h, for example, 10 h, 11 h, 12 h, 13 h, 14 h or 15 h.

[0032] Preferably, the filtration in step (2) is reduced pressure filtration.

[0033] Preferably, after the filtration in step (2), washing and drying steps are also included.

[0034] As a preferred technical solution, the preparation method comprises the following steps:

[0035] (1) reacting unmodified hexagonal boron nitride and a small molecule coupling agent in solvent A at a temperature of 30 to 100° C. for 20 to 30 hours, filtering and washing under reduced pressure to obtain hexagonal boron nitride modified with a small molecule coupling agent;

[0036] (2) reacting the hexagonal boron nitride modified with the small molecule coupling agent obtained in step (1) with a polymer modifier in solvent B at a temperature of 30 to 100° C. for 10 to 15 hours, filtering under reduced pressure, washing and drying to obtain the surface-modified hexagonal boron nitride.

[0037] In a third aspect, the present invention provides a polyimide composite thermally conductive film, wherein the material of the polyimide composite thermally conductive film comprises polyimide and the surface-modified hexagonal boron nitride as described in the first aspect.

[0038] Preferably, the mass ratio of the polyimide to the surface-modified hexagonal boron nitride is (3-5):1, for example, 3:1, 3.2:1, 3.4:1, 3.5:1, 3.6:1, 3.8:1, 4:1, 4.2:1, 4.4:1, 4.6:1, 4.8:1 or 5:1, etc.

[0039] In a fourth aspect, the present invention provides a method for preparing the polyimide composite thermally conductive film as described in the third aspect, the preparation method comprising: mixing the surface-modified hexagonal boron nitride and polyamic acid solution as described in the first aspect, and obtaining the polyimide composite thermally conductive film by casting and heat treatment.

[0040] Preferably, the polyamic acid solution is obtained by reacting a diamine monomer and a dianhydride monomer in an organic solvent.

[0041] Preferably, the reaction temperature is 0-50°C, such as 0°C, 5°C, 10°C, 20°C, 30°C, 40°C or 50°C.

[0042] Preferably, the reaction time is 5 to 12 h, for example, 5 h, 6 h, 7 h, 8 h, 9 h, 10 h, 11 h or 12 h.

[0043] Preferably, the dianhydride monomer comprises any one or a combination of at least two of the following compounds:

[0044]

[0045] Preferably, the diamine monomer includes any one or a combination of at least two of the following compounds:

[0046]

[0047] Preferably, the organic solvent includes any one of N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone or m-cresol, or a combination of at least two thereof.

[0048] Preferably, the solid content of the polyamic acid solution is 1-35%, for example 1%, 5%, 10%, 15%, 20%, 25%, 30% or 35%, more preferably 10-35%, further preferably 20-35%.

[0049] Preferably, the viscosity of the polyamic acid solution is 10000-160000 cP / 25°C, for example, 10000 cP / 25°C, 120000 cP / 25°C, 140000 cP / 25°C or 160000, more preferably 50000-160000 cP / 25°C, further preferably 100000-160000 cP / 25°C.

[0050] Preferably, after the mixing is completed, the step of filtering with a filter membrane having a pore size of 30 to 50 μm (eg, 30 μm, 35 μm, 40 μm, 45 μm or 50 μm, etc.) is further included.

[0051] Preferably, the heat treatment is carried out under the condition of staged heating, and the staged heating method includes: first heating to 75-85°C (for example, 75°C, 77°C, 79°C, 81°C, 83°C or 85°C, etc.), first heat preservation for 20-40min (for example, 20min, 23min, 26min, 29min, 32min, 35min, 38min or 40min, etc.), second heating to 95-105°C (for example, 95°C, 99°C, 101°C, 1 03℃ or 105℃, etc.), the second heat preservation is 20-40min (for example, 20min, 23min, 26min, 29min, 32min, 35min, 38min or 40min, etc.), the third temperature is raised to 115-125℃ (for example, 115℃, 118℃, 121℃, 123℃ or 125℃, etc.), the third heat preservation is 20-40min (for example, 20min, 23min, 26min, 29min, 32min, 35min, 38min or 40min, etc.), the temperature is raised to 115-125℃ (for example, 115℃, 118℃, 121℃, 123℃ or 125℃, etc.), the third heat preservation is 20-40min (for example, 20min, 23min, 26min, 29min, 32min, 35min, The fourth time is heated to 155-165°C (for example, 155°C, 157°C, 159°C, 161°C, 163°C or 165°C), the fourth time is kept warm for 20-40min (for example, 20min, 23min, 26min, 29min, 32min, 35min, 38min or 40min), the fifth time is heated to 290-310°C (for example, 290°C, 293°C, 296°C, 299°C, 302°C, 30 5℃, 308℃ or 310℃, etc.), the fifth heat preservation is 10-20min (for example, 10min, 12min, 14min, 16min, 18min or 20min, etc.), the sixth temperature rises to 340-360℃ (for example, 340℃, 345℃, 350℃, 355℃ or 360℃, etc.), the fifth heat preservation is 5-15min (for example, 5min, 7min, 9min, 11min, 13min or 15min, etc.), completing the staged heating.

[0052] Preferably, the heating rates of the first heating, the second heating, the third heating, the fourth heating and the fifth heating are each independently 4 to 6°C / min, for example, 4°C / min, 4.5°C / min, 5°C / min, 5.5°C / min or 6°C / min.

[0053] In a fourth aspect, the present invention provides the use of the surface-modified hexagonal boron nitride as described in the first aspect, or the polyimide composite thermally conductive film as described in the third aspect in the preparation of electronic device packaging materials, new energy products or aerospace products.

[0054] Compared with the prior art, the present invention has the following beneficial effects:

[0055] The surface-modified hexagonal boron nitride provided by the present invention is obtained by sequentially surface-treating unmodified hexagonal boron nitride with a small molecule coupling agent and a polymer modifier; by selecting a combination of a small molecule coupling agent and a polymer modifier as a modifier, a large number of hydrophilic groups are successfully introduced onto the surface of the hexagonal boron nitride, thereby effectively improving the compatibility of the obtained surface-modified hexagonal boron nitride with polyimide, so that the polyimide composite thermal conductive film composited with the two has low structural defects and highly ordered structural orientation inside, thereby being able to have both excellent heat resistance and mechanical properties. DETAILED DESCRIPTION

[0056] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0057] Unless otherwise specified, the raw materials involved in the following examples and comparative examples are conventional materials in the art.

[0058] Preparation Example 1

[0059] A polyamic acid solution has a solid content of 30% and a viscosity of 160000 cP / 25°C. The preparation method comprises: adding 0.10 mol (20.02 g) of 4,4'-diaminodiphenyl ether (ODA) monomer to 168 g of N,N-dimethylacetamide (DMAc) and stirring until the monomer is completely dissolved, then adding 0.10 mol (21.82 g) of pyromellitic dianhydride (PMDA) in batches, continuing to stir and react at room temperature for 12 hours after the addition is complete, and refrigerating the obtained polyamic acid solution for standby use.

[0060] Example 1

[0061] A surface-modified hexagonal boron nitride, the preparation method of which comprises the following steps:

[0062] (1) 10 g of unmodified hexagonal boron nitride (average thickness of 25 nm, average radial length of 4 μm) was added to 200 mL of dry toluene, and ultrasonicated for 0.5 h. 4.5 g of p-phenylene diisocyanate was added thereto under a nitrogen atmosphere, and the temperature was raised to 60° C. and stirred for reaction for 24 h. After the reaction was completed, the mixture was cooled to room temperature, and the mixture was rapidly filtered under reduced pressure. The filter cake was washed with dry toluene for 3 to 4 times to obtain p-phenylene diisocyanate-modified hexagonal boron nitride;

[0063] (2) The p-phenylene diisocyanate-modified hexagonal boron nitride obtained in step (1) was dispersed again in 150 mL of dry toluene, and 3 g of polyethyleneimine (number average molecular weight of 2000, purchased from Sigma-Aldrich) was added thereto under a nitrogen atmosphere. The temperature was raised to 60° C. and stirred for reaction for 12 h. After the reaction was completed, the mixture was cooled to room temperature and filtered under reduced pressure. The filter cake was washed three times with toluene and dried in vacuo to obtain the surface-modified hexagonal boron nitride.

[0064] Example 2

[0065] A surface-modified hexagonal boron nitride, the preparation method of which comprises the following steps:

[0066] (1) 10 g of unmodified hexagonal boron nitride (average thickness of 25 nm, average radial length of 4 μm) was added to 200 mL of dry toluene, and ultrasonicated for 0.5 h. 3 g of tetra-tert-butyl titanate was added thereto under a nitrogen atmosphere, and the temperature was raised to 50° C. and stirred for reaction for 24 h. After the reaction was completed, the mixture was cooled to room temperature, and the mixture was rapidly filtered under reduced pressure. The filter cake was washed 3 to 4 times with dry toluene to obtain tetra-tert-butyl titanate-modified hexagonal boron nitride.

[0067] (2) The tetra-tert-butyl titanate-modified hexagonal boron nitride obtained in step (1) was dispersed again in 150 mL of dry toluene, and 3 g of polyacrylic acid (number average molecular weight 45,000, purchased from Sigma-Aldrich) was added thereto under a nitrogen atmosphere. The temperature was raised to 50° C. and stirred for reaction for 15 h. After the reaction was completed, the mixture was cooled to room temperature and filtered under reduced pressure. The filter cake was washed three times with toluene and dried in vacuo to obtain the surface-modified hexagonal boron nitride.

[0068] Example 3

[0069] A surface-modified hexagonal boron nitride, the preparation method of which comprises the following steps:

[0070] (1) 10 g of unmodified hexagonal boron nitride (average thickness of 25 nm, average radial length of 4 μm) was added to 200 mL of dry toluene, and ultrasonicated for 0.5 h. 5 g of γ-aminopropyltrimethoxysilane was added thereto under a nitrogen atmosphere, and the temperature was raised to 80° C. and stirred for reaction for 20 h. After the reaction was completed, the mixture was cooled to room temperature, and the mixture was rapidly filtered under reduced pressure. The filter cake was washed 3 to 4 times with dry toluene to obtain hexagonal boron nitride modified with tetra-tert-butyl titanate;

[0071] (2) The tetra-tert-butyl titanate-modified hexagonal boron nitride obtained in step (1) was dispersed again in 150 mL of dry toluene, and 3 g of polyacrylic acid (number average molecular weight 45,000, purchased from Sigma-Aldrich) was added thereto under a nitrogen atmosphere. The temperature was raised to 55° C. and stirred for reaction for 14 h. After the reaction was completed, the mixture was cooled to room temperature and filtered under reduced pressure. The filter cake was washed three times with toluene and dried in vacuo to obtain the surface-modified hexagonal boron nitride.

[0072] Embodiment 4-5

[0073] A surface-modified hexagonal boron nitride, which differs from Example 1 only in that the amounts of p-phenylene diisocyanate used are 1 g (Example 4) and 8 g (Example 5), respectively, and other substances, amounts used and preparation methods are the same as those in Example 1.

[0074] Embodiment 6-7

[0075] A surface-modified hexagonal boron nitride, which differs from Example 1 only in that the amounts of polyethyleneimine used are 1 g (Example 6) and 5 g (Example 7), respectively, and other substances, amounts used and preparation methods are the same as those in Example 1.

[0076] Embodiments 8 to 11

[0077] A surface-modified hexagonal boron nitride, which differs from Example 1 only in that the stirring reaction temperatures in step (1) are 70°C (Example 8), 80°C (Example 9), 30°C (Example 10) and 20°C (Example 11), respectively, and other substances, amounts and preparation methods are the same as those in Example 1.

[0078] Embodiments 12 to 15

[0079] A surface-modified hexagonal boron nitride, which differs from Example 1 only in that the stirring reaction temperatures in step (2) are 70°C (Example 12), 80°C (Example 13), 30°C (Example 14) and 20°C (Example 15), respectively, and other substances, amounts and preparation methods are the same as those in Example 1.

[0080] Comparative Example 1

[0081] An unmodified hexagonal boron nitride with an average thickness of 25nm and an average radial length of 4μm.

[0082] Comparative Example 2

[0083] A surface-modified hexagonal boron nitride, the preparation method of which comprises: adding 10g of unmodified hexagonal boron nitride (average thickness of 25nm, average radial length of 4μm) into 200mL of dry toluene, ultrasonicating for 0.5h, adding 4.5g of p-phenylene diisocyanate thereto under a nitrogen atmosphere, heating to 60°C and stirring for reaction for 24h, cooling to room temperature after the reaction, rapidly filtering under reduced pressure, washing the filter cake with dry toluene for 3-4 times, and obtaining the surface-modified hexagonal boron nitride.

[0084] Comparative Example 3

[0085] A surface-modified hexagonal boron nitride, the preparation method of which comprises: dispersing 10g of unmodified hexagonal boron nitride (average thickness of 25nm, average radial length of 4μm) in 150mL of dry toluene, adding 3g of polyethyleneimine (number average molecular weight of 2000, purchased from Sigma-Aldrich) thereto under a nitrogen atmosphere, heating to 60°C and stirring for reaction for 12h, cooling to room temperature after the reaction is completed, filtering under reduced pressure, washing the filter cake with toluene for 3 times, and vacuum drying to obtain the surface-modified hexagonal boron nitride.

[0086] Application Example 1

[0087] A polyimide composite thermally conductive film, the preparation method of which comprises: adding surface modified hexagonal boron nitride (Example 1) to a polyamic acid solution (Preparation Example 1) (the mass ratio of the surface modified hexagonal boron nitride to the solute in the polyamic acid solution is 1:3.5), mechanically stirring and dispersing at 1000 rpm for 3 hours, casting the obtained mixed solution, and subjecting the wet film to a stepwise heating heat treatment at 80°C×30min, 100°C×30min, 120°C×30min, 160°C×30min, 300°C×15min, and 350°C×10min, with the heating rate being 5°C / min, to obtain the polyimide composite thermally conductive film.

[0088] Application Examples 2 to 15

[0089] A polyimide composite thermally conductive film is different from Application Example 1 in that the surface modified hexagonal boron nitride provided in Examples 2 to 15 is used to replace the surface modified hexagonal boron nitride provided in Example 1, and other substances, amounts and preparation methods are the same as those in Example 1.

[0090] Application Examples 16-19

[0091] A polyimide composite thermally conductive film, which differs from Application Example 1 in that the mass ratios of surface modified hexagonal boron nitride to the solute in the polyamide solution are 1:2 (Application Example 16), 1:3 (Application Example 17), 1:5 (Application Example 18) and 1:8 (Application Example 19), respectively, and other substances, amounts and preparation methods are the same as those in Example 1.

[0092] Comparative Application Examples 1 to 3

[0093] A polyimide composite thermally conductive film is disclosed, which differs from Application Example 1 in that the surface-modified hexagonal boron nitride provided in Example 1 is replaced by the hexagonal boron nitride provided in Comparative Examples 1 to 3, and other substances, dosages and preparation methods are the same as those in Example 1.

[0094] Comparative Application Example 4

[0095] A polyimide film, which differs from Application Example 1 in that the surface-modified hexagonal boron nitride provided in Example 1 is not added, and other substances, amounts and preparation methods are the same as those in Application Example 1.

[0096] Performance Testing:

[0097] (1) Thermal conductivity: The test is carried out using the transient plane heat source method, and the test method refers to ISO 22007-2;

[0098] (2) Tensile strength, elongation at break and modulus: Tested according to the method provided in GB13022-91.

[0099] According to the above test method, the polyimide composite thermal conductive film provided by Examples 1 to 19 and Comparative Application Examples 1 to 4 was tested, and the test results are shown in Table 1:

[0100] Table 1

[0101]

[0102]

[0103] From the data in Table 1, we can see that:

[0104] (1) The polyimide composite thermally conductive film provided in Application Examples 1 to 3 has a thermal conductivity of 0.6314 to 0.7321 W / (m·K), a tensile strength of 119 to 132 MPa, an elongation at break of 47 to 52%, and a modulus of 3.56 to 3.62 GPa, and has both excellent thermal conductivity and mechanical properties.

[0105] (2) By comparing the data of Application Example 1 and Application Examples 4-5, it can be seen that when preparing surface-modified hexagonal boron nitride, the optimal amount of the small molecule coupling agent used in the first step is about 4.5 g. An amount lower than this will result in a significant decrease in the thermal conductivity of the resulting composite thermally conductive film, while an amount higher than this will not significantly increase the thermal conductivity of the resulting composite thermally conductive film.

[0106] (3) By comparing the data of Application Example 1 and Application Examples 6-7, it can be found that when preparing the surface-modified hexagonal boron nitride, the optimal amount of the polymer modifier used is about 3 g, but reducing the amount to 1 g will cause the thermal conductivity of the resulting composite thermally conductive film to decrease slightly, and increasing the amount to 5 g will also cause the thermal conductivity of the resulting composite thermally conductive film to decrease slightly.

[0107] (4) By comparing the data of Application Example 1 and Application Examples 8 to 11, it can be seen that when preparing surface-modified hexagonal boron nitride, the optimal reaction temperature for surface modification of hexagonal boron nitride using a small molecule coupling agent is 50 to 70°C. Too high or too low a reaction temperature will affect the modification efficiency, thereby causing the thermal conductivity of the final composite thermally conductive film to decrease and the thermal conductivity performance to deteriorate.

[0108] (5) By comparing the data of Application Example 1 and Application Examples 12 to 15, it can be seen that when preparing surface-modified hexagonal boron nitride, the reaction temperature for surface modification using a polymer modifier is preferably between 30 and 70°C. Too high or too low a temperature will lead to a decrease in the thermal conductivity of the final composite thermally conductive film, resulting in poor thermal conductivity.

[0109] (6) By comparing the data of Application Example 1 and Application Examples 16 to 19, it can be seen that increasing the doping amount of surface-modified hexagonal boron nitride in the polyimide composite thermally conductive film can improve the thermal conductivity of the composite thermally conductive film, but too high a doping amount will lead to a significant decrease in the mechanical properties of the composite thermally conductive film.

[0110] (7) Finally, by comparing the data of Application Example 1 and Comparative Application Examples 1 to 4, it can be seen that, at the same doping amount, the thermal conductivity of the composite film is significantly reduced by adding hexagonal boron nitride without surface modification, hexagonal boron nitride modified only with a small molecule coupling agent, hexagonal boron nitride modified only with a polymer modifier, and no hexagonal boron nitride added.

[0111] The applicant declares that the present invention uses the above-mentioned embodiments to illustrate a surface-modified hexagonal boron nitride and polyimide composite thermal conductive film and its preparation method and application, but the present invention is not limited to the above-mentioned embodiments, that is, it does not mean that the present invention must rely on the above-mentioned embodiments to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the scope of protection and disclosure of the present invention.

Claims

1. A surface-modified hexagonal boron nitride, characterized in that: The surface-modified hexagonal boron nitride is obtained by sequentially treating the surface of unmodified hexagonal boron nitride with a small molecule coupling agent and a polymer modifier.

2. The surface-modified hexagonal boron nitride according to claim 1, characterized in that: The mass ratio of the unmodified hexagonal boron nitride, the small molecule coupling agent and the polymer modifier is 10:(2-6):(2-4).

3. The surface-modified hexagonal boron nitride according to claim 1 or 2, characterized in that: The unmodified hexagonal boron nitride has a thickness of 2 to 100 nm and a radial length of 0.1 to 100 μm; Preferably, the small molecule coupling agent includes any one of an isocyanate small molecule coupling agent, a titanate small molecule coupling agent or a silane small molecule coupling agent, or a combination of at least two thereof; Preferably, the isocyanate small molecule coupling agent includes any one or a combination of at least two of p-phenylene diisocyanate, bis(4-isocyanatephenyl)methane, toluene-2,4-diisocyanate or 4,4'-diisocyanate dicyclohexylmethane; Preferably, the titanate-based small molecule coupling agent includes any one of tetraethyl titanate, tetra-tert-butyl titanate, tetraisooctyl titanate, isopropyl dioleyl (dioctyl phosphate) titanate, isopropyl tris(dioctyl phosphate) titanate, isopropyl trioleyl titanate, diisopropyl bisacetoacetate titanate, isopropyl triisostearate titanate, bis(dioctyl pyrophosphate) ethylene titanate, di(triethanolamine) titanate diisopropyl, isopropyl tris(dioctyl pyrophosphate) titanate, di(triethylamine) titanate diisopropyl or tetraisopropyl di(dioctyl phosphite) titanate, or a combination of at least two thereof; Preferably, the silane-based small molecule coupling agent includes γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, γ-aminopropylmethyldiethoxysilane, γ-aminopropylmethyldimethoxysilane, N-phenyl-γ-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane, N,N-diethyl-3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, γ-diethylenetriaminopropyltrimethoxysilane, γ-diethylaminomethyltriethoxysilane, N-phenylaminomethyltriethoxysilane, bis-(γ-trimethoxysilylpropyl) Amine, bis(3-triethoxysilylpropyl)amine, 4-amino-3,3-dimethylbutyltrimethoxysilane, 3-(2-aminoethyl)-aminopropyltriethoxysilane, 3-(N,N-dimethylaminopropyl)-aminopropylmethyldimethoxysilane, (N,N-dimethyl-3-aminopropyl)trimethoxysilane, N-(n-butyl)-γ-aminopropyltrimethoxysilane, vinylbenzylaminoethylaminopropyltrimethoxysilane, N-cyclohexyl-γ-aminopropylmethyldimethoxysilane, 3-ureidopropyltrimethoxysilane, 3-ureidopropyltriethoxysilane, γ-piperazinylpropylmethyldimethoxysilane, γ-glycidyl Oleyloxypropyl trimethoxysilane, γ-glycidyloxypropyl triethoxysilane, 3-(2,3-epoxypropyloxy)propyl methyldimethoxysilane, β-(3,4-epoxycyclohexyl)-ethyltriethoxysilane, β-(3,4-epoxycyclohexyl)-ethyltrimethoxysilane, 3-(2,3-epoxypropyloxy)propylmethyldiethoxysilane, γ-methacryloxypropyl trimethoxysilane, γ-methacryloxypropyl triisopropoxysilane, γ-methacryloxypropyl methyldimethoxysilane, γ-methacryloxypropyl tri(trimethylsiloxy)silane, 3-methacryloxypropyl tri Any one of ethoxysilane, 3-(methacryloyloxy)propylmethyldiethoxysilane, 3-acetoxypropyltrimethoxysilane, 3-(acryloyloxy)propyltrimethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, vinyltriisopropoxysilane, vinyltri(2-methoxyethoxy)silane, vinyltriacetoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, methylphenyldimethoxysilane, methylphenyldiethoxysilane, γ-mercaptopropyltrimethoxysilane, γ-mercaptopropyltriethoxysilane, methyltrimethoxysilane or tetraethoxysilane, or a combination of at least two thereof; Preferably, the polymer modifier includes any one or a combination of at least two of polyethylene imine, polyethylene glycol 400, polyethylene glycol 600, polyethylene glycol 800, polyethylene glycol 1000, polyethylene glycol 2000, polyvinyl alcohol, branched polyethylene imine-block-polyethylene glycol or polyacrylic acid.

4. A method for preparing surface-modified hexagonal boron nitride according to any one of claims 1 to 3, characterized in that: The preparation method comprises the following steps: (1) reacting unmodified hexagonal boron nitride and a small molecule coupling agent in solvent A, filtering, and obtaining hexagonal boron nitride modified with a small molecule coupling agent; (2) reacting the hexagonal boron nitride modified with the small molecule coupling agent obtained in step (1) with a polymer modifier in solvent B, filtering, and obtaining the surface-modified hexagonal boron nitride.

5. The preparation method according to claim 4, wherein the solvent A and the solvent B independently include any one of water, methanol, ethanol, isopropanol, tert-butyl alcohol, toluene, p-xylene, n-hexane, tetrahydrofuran, N,N-dimethylformamide, N,N-dimethylacetamide or N-methylpyrrolidone, or a combination of at least two thereof; Preferably, the reaction temperature in step (1) is 30 to 100° C., more preferably 50 to 100° C., and further preferably 50 to 70° C.; Preferably, the reaction time in step (1) is 20 to 30 hours; Preferably, the filtration in step (1) is reduced pressure filtration; Preferably, after the filtration in step (1) is completed, a washing step is also included; Preferably, the reaction temperature in step (2) is 30 to 100° C., more preferably 30 to 70° C.; Preferably, the reaction time in step (2) is 10 to 15 hours; Preferably, the filtration in step (2) is reduced pressure filtration; Preferably, after the filtration in step (2), washing and drying steps are also included.

6. A polyimide composite thermally conductive film, characterized in that: The material of the polyimide composite thermal conductive film comprises polyimide and the surface-modified hexagonal boron nitride as claimed in any one of claims 1 to 3.

7. The polyimide composite thermally conductive film according to claim 6, characterized in that: The mass ratio of the polyimide to the surface-modified hexagonal boron nitride is (3-5):

1.

8. A method for preparing the polyimide composite thermally conductive film as claimed in claim 6 or 7, characterized in that: The preparation method comprises: mixing the surface-modified hexagonal boron nitride according to any one of claims 1 to 3 with a polyamic acid solution, and performing casting and heat treatment to obtain the polyimide composite thermal conductive film.

9. The preparation method according to claim 8, characterized in that: The polyamic acid solution is obtained by reacting a diamine monomer and a dianhydride monomer in an organic solvent; Preferably, the reaction temperature is 0 to 50°C and the reaction time is 5 to 12 hours; Preferably, the dianhydride monomer comprises any one or a combination of at least two of the following compounds: Preferably, the diamine monomer includes any one or a combination of at least two of the following compounds: Preferably, the organic solvent comprises any one of N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone or m-cresol, or a combination of at least two thereof; Preferably, the solid content of the polyamic acid solution is 1 to 35%, more preferably 10 to 35%, and further preferably 20 to 35%; Preferably, the viscosity of the polyamic acid solution is 10000 to 160000 cP / 25°C, more preferably 50000 to 160000 cP / 25°C, and further preferably 100000 to 160000 cP / 25°C; Preferably, after the mixing is completed, the step of filtering with a filter membrane having a pore size of 30 to 50 μm is also included; Preferably, the heat treatment is carried out under the condition of staged heating, and the staged heating method includes: heating to 75-85°C for the first time, keeping warm for 20-40 minutes for the first time, heating to 95-105°C for the second time, keeping warm for 20-40 minutes for the second time, heating to 115-125°C for the third time, keeping warm for 20-40 minutes for the third time, heating to 155-165°C for the fourth time, keeping warm for 20-40 minutes for the fourth time, heating to 290-310°C for the fifth time, keeping warm for 10-20 minutes for the fifth time, heating to 340-360°C for the sixth time, keeping warm for 5-15 minutes for the fifth time, and completing the staged heating; Preferably, the heating rates of the first heating, the second heating, the third heating, the fourth heating and the fifth heating are each independently 4-6° C. / min.

10. Use of the surface-modified hexagonal boron nitride according to any one of claims 1 to 3, or the polyimide composite thermally conductive film according to claim 6 or 7 in the preparation of electronic device packaging materials, new energy products or aerospace products.

Citation Information

Patent Citations

  • Polydopamine modified boron nitride nanosheet / polyimide composite fiber heat-conducting film as well as preparation method and application thereof

    CN116061525A

Cited By

  • Preparation method of aramid nanofiber-based composite film with high thermal conductivity and breakdown resistance

    CN121064510A

  • Preparation method of aramid nanofiber-based composite film with high thermal conductivity and high breakdown resistance

    CN121064510B