High-Tg lead-free copper-clad plate and preparation method thereof

By combining phosphorus-containing epoxy resin and modified filler in copper clad plate, the problems of high Df and Dk values ​​and poor heat resistance in traditional copper clad plates are solved, and the high heat resistance of high Tg lead-free copper clad plates are achieved and Good dispersion, meets the flame retardant requirements of UL94V-0 level, and ensures the reliability and trust of the product.

CN118909399AInactive Publication Date: 2024-11-08GUANGDE LONGTAI ELECTRONICS SCI TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410992618.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Traditional epoxy resin-based copper clad plates have problems with high Df and Dk values, heat resistance and poor dimensional stability in high Tg lead-free plates, and the addition of inorganic fillers can easily lead to interfacial incompatibility and uneven dispersion problems. .

Method used

Using phosphorus-containing epoxy resin combined with modified fillers, the use of inorganic flame retardant is reduced, the flame retardant and mechanical properties of the material are improved, and the specific process steps are used. Ensure uniform dispersion of the filler to form high Tg lead-free copper clad plate.

Benefits of technology

The high heat resistance, low thermal expansion coefficient and flame retardant grade of the material are achieved, ensuring the reliability and trust of the terminal products, and avoiding the problems of secondary agglomeration and uneven dispersion of fillers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004959269570000081
    Figure BDA0004959269570000081
Patent Text Reader

Abstract

The invention discloses a high-Tg lead-free copper-clad plate and a preparation method thereof, and belongs to the technical field of copper-clad plate processing, the high-Tg lead-free copper-clad plate comprises glass fiber cloth, a glue solution and a copper foil, the glue solution comprises the following components in parts by weight: 160-165 parts of phosphorus-containing epoxy resin, 40-60 parts of a modified filler, 10-12 parts of an inorganic flame retardant, 2-3 parts of a curing agent and 2-3 parts of an organic solvent, the modified filler is amino-terminated hyperbranched polymer modified carboxylated filler. After the modified filler is treated, the agglomeration problem is improved, the introduced hyperbranched polymer is high in branching degree, molecular chains are not prone to entanglement, and secondary agglomeration of the filler after conventional dispersion treatment is avoided. Based on the addition of the modified filler, the high-Tg lead-free copper-clad plate is obtained, has high heat resistance, low CTE and UL94V-0 heat resistance grade, has a wide development prospect, and ensures that a terminal product has good reliability and reliability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of copper clad laminate processing, and in particular relates to a high Tg lead-free copper clad laminate and a preparation method thereof. Background Art

[0002] With the demand for electronic products to be light, thin, short, small and digital, miniaturization, multi-function, high performance and high reliability have become the mainstream development direction, causing PCB to move towards fine graphics, high density and high multi-layer. The requirements for line width, line spacing, aperture, hole wall and other processes in the production of PCB industry are also gradually developing towards high integration, high density and high multi-layer. For example, the mainstream high-density interconnection laminate requires that the micro-via aperture is less than 6mil, the micro-via ring diameter is more than 0.35mm, and the wiring width is 117in / m 2 Above, the line width * line spacing is below 0.1mm / 0.1mm, while high-level HDI (more than twelve layers) needs to withstand special processes such as high-level multiple hot pressing and more precise and detailed process requirements. With the development of high-density installation technology, especially the full implementation of lead-free and the rapid development of surface mounting technology, in PCB processing and whole machine accessories installation, the number of times and temperatures that materials are repeatedly subjected to thermal shock are higher than the traditional requirements in the past. All of this ultimately translates into a huge challenge to the reliability of high-performance copper clad laminates.

[0003] Copper clad laminate is a composite material that is a composite of reinforcing material and resin, formed by hot pressing and covered with copper foil on one or both sides; copper clad laminates mainly include glass fiber cloth-based copper clad laminates, non-woven cloth-based copper clad laminates, composite-based copper clad laminates and synthetic fiber cloth-based copper clad laminates. Epoxy resin is widely used in high-frequency copper clad laminates. Epoxy resin has the characteristics of small curing shrinkage, high viscosity of the cured product, good chemical corrosion resistance and excellent electrical properties. However, with the upgrading of electronic products, traditional epoxy resin-based copper clad laminates are difficult to meet the requirements of heat resistance and flame retardancy of high Tg lead-free board materials.

[0004] In order to improve the defects of the resin in the copper clad laminate, inorganic fillers can be added to the original resin matrix to improve the flame retardancy and heat resistance of the resin or reduce the content of polar groups per unit volume in the resin matrix. For example, patent CN110239164A discloses a high heat-resistant medium Tg copper clad laminate and a preparation method thereof. The expansion coefficient is changed by adjusting the type of filler. However, there are disadvantages such as interface incompatibility between the inorganic filler and the resin, and the copper clad laminate doped with hollow glass microspheres will have a lot of dust when cutting and the hollow glass microspheres are not easy to disperse evenly. Summary of the invention

[0005] The object of the present invention is to provide a high Tg lead-free copper clad laminate and a preparation method thereof.

[0006] This is to solve the problem that when epoxy resin is directly used in copper clad laminates, there are high Df and Dk, poor heat resistance and dimensional stability.

[0007] The purpose of the present invention can be achieved through the following technical solutions:

[0008] A high Tg lead-free copper clad laminate comprises glass fiber cloth, glue and copper foil. The glue comprises, by weight, 160-165 parts of phosphorus-containing epoxy resin, 40-60 parts of modified filler, 10-12 parts of inorganic flame retardant, 2-3 parts of curing agent and 2-3 parts of organic solvent. The phosphorus-containing epoxy resin contains phosphorus element and can generate phosphoric acid, polyphosphoric acid and water vapor during combustion. The inorganic flame retardant is added as a flame retardant raw material to improve the flame retardant performance of the material. However, excessive addition of the inorganic flame retardant will lead to a decrease in the mechanical properties of the material. In the present invention, the content of the inorganic flame retardant is reduced (generally 20% needs to be added to meet the flame retardant requirements), and the phosphorus-containing epoxy resin and the modified filler are combined to make the material meet the flame retardant level of UL94V-0.

[0009] Furthermore, the modified filler is prepared by the following steps:

[0010] Mix 4'amino-4-biphenol and triethylamine, add butanone, stir and dissolve, slowly add dimethyldichlorosilane while stirring at 60°C, heat and reflux for 12 hours, filter, wash with water to remove salt, dissolve and recrystallize to obtain an amino-terminated siloxane intermediate; the molar ratio of 4'amino-4-biphenol to dimethyldichlorosilane is 2:1;

[0011] Under nitrogen protection, the amino-terminated siloxane intermediate and glacial acetic acid are mixed, and then excess methyl acrylate is added, and the reaction is carried out at 80°C in the dark for 2 hours. After the reaction liquid is completed, the methyl acrylate is removed by vacuum concentration to obtain an intermediate product. The intermediate product and ethylenediamine are mixed, and the reaction is carried out at a temperature of 100°C for 2 hours. N, N-dimethylacetamide is added and the temperature is raised to 120°C for reaction for 2 hours, and the temperature is further raised to 140°C for reaction for 6 hours. The obtained reactant is precipitated with ether and petroleum ether to obtain an amino-terminated hyperbranched polymer. The mass ratio of the intermediate product to ethylenediamine is 2:1.

[0012] The carboxylated filler was added to acetone, and then the amino-terminated hyperbranched polymer and p-toluenesulfonic acid were added, and the mixture was heated under reflux for reaction for 40-50 minutes. After the reaction was completed, the mixture was dried at 40° C. to a constant weight to obtain a modified filler.

[0013] Furthermore, the added amount of the amino-terminated hyperbranched polymer is 12-16% of the mass of the carboxylated filler, and the added amount of p-toluenesulfonic acid is 0.3% of the mass of the carboxylated filler.

[0014] Furthermore, the carboxylated filler is prepared by the following steps:

[0015] After adding the filler into water and ultrasonically dispersing it, the system is adjusted to be weakly acidic, and then vinyl triethoxysilane is added. At 80-85°C, the reaction is stirred for 2-3 hours. Then, acrylic acid, ammonium persulfate and sodium bisulfite are added, and the reaction is continued with stirring for 3-4 hours. After the reaction is completed, the mixture is cooled, washed and freeze-dried to obtain a carboxylated filler.

[0016] Furthermore, the filler is one of nano-silicon dioxide and hexagonal boron nitride nanosheets.

[0017] Furthermore, the weakly acidic pH value is 6-6.5.

[0018] Furthermore, the mass fraction of phosphorus in the phosphorus-containing epoxy resin is 2.5-3%.

[0019] Furthermore, the inorganic flame retardant is one of aluminum hydroxide and magnesium hydroxide, or a mixture of the two in any proportion.

[0020] A method for preparing a high Tg lead-free copper clad laminate comprises the following steps:

[0021] The first step is to mix the phosphorus-containing epoxy resin, the curing agent and the organic solvent, stir for 30-40 minutes, add the modified filler and the inorganic flame retardant and continue to stir for 30-40 minutes to obtain a glue solution;

[0022] The second step is to apply glue on the surface of the glass fiber cloth, bake and cure at 100℃-250℃ to obtain a prepreg, and the curing time is 80-100min;

[0023] The third step is to stack the prepregs in groups of 8 to 16 sheets with copper foil and press them to obtain a high Tg lead-free copper clad laminate.

[0024] Furthermore, the mass ratio of glass fiber cloth to adhesive is 10:5-6;

[0025] Furthermore, the pressing parameters include: pressure 100-200Psi, temperature 100-150°C, vacuum degree 0.03-0.1MPa, and pressing time 150-200min.

[0026] Beneficial effects of the present invention:

[0027] The glue used in the copper clad laminate of the present invention adds a self-made modified filler, which is obtained by sequentially treating the filler with a coupling agent, carboxylating, and grafting a hyperbranched polymer. The filler improves the problem of easy agglomeration after treatment, and the introduced hyperbranched polymer has a high degree of branching, and it is not easy for molecular chains to be entangled, thereby avoiding the problem of easy secondary agglomeration of the filler after conventional dispersion treatment. Based on the addition of the modified filler, a high Tg lead-free copper clad laminate is obtained, which has high heat resistance, low CTE, and UL94V-0 heat resistance grade, has broad development prospects, and ensures that the terminal product has good reliability and trustworthiness.

[0028] In the present invention, an amino-terminated hyperbranched polymer is prepared using an amino-terminated siloxane intermediate as a raw material, and the filler is subjected to a secondary treatment. The formed branched polymer chains form a "loose structure" on the surface of the filler, thereby avoiding secondary agglomeration. More importantly, the biphenyl group introduced into the structure of the amino-terminated siloxane intermediate is beneficial to improving the glass transition temperature of the copper clad laminate material, and the siloxane group can effectively reduce the thermal expansion coefficient of the material.

[0029] The terminal amino group of the hyperbranched structure in the grafted hyperbranched polymer used in the modified filler of the present invention can participate in the curing reaction of the resin, and a covalent bond is formed between the terminal amino group in the grafted hyperbranched polymer and the epoxy group of the epoxy resin. No additional curing accelerator is needed, and the curing reaction is further promoted, thereby increasing the network crosslinking density of the glue resin system, thereby increasing the Tg of the copper clad laminate material and reducing the thermal expansion coefficient of the copper clad laminate material. DETAILED DESCRIPTION

[0030] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] Example 1

[0032] The modified filler is prepared by the following steps:

[0033] Mix 1 mol 4'amino-4-biphenol and 1 mol triethylamine, add 250 mL butanone, stir to dissolve, slowly add 0.5 mol dimethyldichlorosilane while stirring at 60°C, heat to reflux for 12 hours, filter, wash with water to remove salt, dissolve and recrystallize to obtain an amino-terminated siloxane intermediate;

[0034] Under nitrogen protection, the amino-terminated siloxane intermediate and glacial acetic acid are mixed, and then excess methyl acrylate is added, and the reaction is carried out at 80° C. in the dark for 2 hours. After the reaction liquid is completed, the methyl acrylate is removed by vacuum concentration to obtain an intermediate product. 2 g of the intermediate product and 1 g of ethylenediamine are mixed, and the reaction is carried out at a temperature of 100° C. for 2 hours. 6 mL of N, N-dimethylacetamide is added and the temperature is raised to 120° C. for reaction for 2 hours, and the temperature is further raised to 140° C. for reaction for 6 hours. The obtained reactant is precipitated with ether and petroleum ether to obtain an amino-terminated hyperbranched polymer.

[0035] 2 g of filler was added to 100 mL of water for ultrasonic dispersion, and the pH value of the system was adjusted to 6. Then, 50 mg of unsaturated silane coupling agent was added. The mixture was stirred and reacted at 80° C. for 2 h. Then, 2 g of acrylic acid, 30 mg of ammonium persulfate and 30 mg of sodium bisulfite were added. The mixture was stirred and reacted for 3 h. After the reaction was completed, the mixture was cooled, washed and freeze-dried to obtain a carboxylated filler.

[0036] The carboxylated filler is added to acetone, and then the amino-terminated hyperbranched polymer and p-toluenesulfonic acid are added, and the mixture is heated under reflux for reaction for 40 minutes. After the reaction is completed, the mixture is dried at 40° C. to a constant weight to obtain a modified filler; the amount of the amino-terminated hyperbranched polymer added is 12% of the mass of the carboxylated filler, and the amount of the p-toluenesulfonic acid added is 0.3% of the mass of the carboxylated filler.

[0037] Example 2

[0038] The modified filler is prepared by the following steps:

[0039] 3 g of filler was added to 100 mL of water for ultrasonic dispersion, and the pH value of the system was adjusted to 6.5. Then, 50 mg of unsaturated silane coupling agent was added. The mixture was stirred and reacted at 85° C. for 3 h. Then, 3 g of acrylic acid, 30 mg of ammonium persulfate and 30 mg of sodium bisulfite were added. The mixture was stirred and reacted for 4 h. After the reaction was completed, the mixture was cooled, washed and freeze-dried to obtain a carboxylated filler.

[0040] The carboxylated filler was added to acetone, and then an amino-terminated hyperbranched polymer (the preparation process of the amino-terminated hyperbranched polymer is the same as that in Example 1) and p-toluenesulfonic acid were added, and the mixture was heated to reflux for reaction for 50 minutes. After the reaction was completed, the mixture was dried at 40° C. to constant weight to obtain a modified filler; the amount of the amino-terminated hyperbranched polymer added was 12% of the mass of the carboxylated filler, and the amount of the p-toluenesulfonic acid added was 0.3% of the mass of the carboxylated filler.

[0041] Example 3

[0042] Compared with Example 2, the added amount of the amino hyperbranched polymer in this example is 13% of the mass of the carboxylated filler.

[0043] Example 4

[0044] Compared with Example 2, the added amount of the amino hyperbranched polymer in this example is 15% of the mass of the carboxylated filler.

[0045] Example 5

[0046] A method for preparing a high Tg lead-free copper clad laminate comprises the following steps:

[0047] The first step is to mix 160 parts of phosphorus-containing epoxy resin (epoxy resin with a phosphorus mass fraction of 2.5% (E2145): Wuxi Akeli Chemical Co., Ltd.), 2 parts of dicyandiamide and 2 parts of acetone according to parts by weight, stir for 30 minutes, add 40 parts of modified filler prepared according to the proportion of Example 1 and 10 parts of aluminum hydroxide, and continue stirring for 30 minutes to obtain a glue solution;

[0048] Step 2: Apply glue on the surface of glass fiber cloth, bake and cure at 100℃ to obtain a prepreg, the curing time is 80min; the mass ratio of glass fiber cloth to glue is 10:5;

[0049] The third step is to stack the semi-cured sheets with copper foil in groups of 8 sheets and press them to obtain a high Tg lead-free copper clad laminate; the pressing parameters include: pressure 200Psi, temperature 100°C, vacuum degree 0.03-0.1MPa, and pressing time 150min.

[0050] Example 6

[0051] A method for preparing a high Tg lead-free copper clad laminate comprises the following steps:

[0052] The first step is to mix 165 parts of phosphorus-containing epoxy resin (epoxy resin with a phosphorus mass fraction of 3.0% (KEG-H5138): Kolon Suzhou Chemical Co., Ltd.), 3 parts of dicyandiamide and 3 parts of acetone according to parts by weight, stir for 40 minutes, add 60 parts of modified filler prepared according to the proportion in Example 2 and 12 parts of aluminum hydroxide, and continue stirring for 40 minutes to obtain a glue solution;

[0053] Step 2: Apply glue on the surface of glass fiber cloth, bake and cure at 1250℃ to obtain a prepreg, and the curing time is 100min; the mass ratio of glass fiber cloth to glue is 10:6;

[0054] The third step is to stack the semi-cured sheets with copper foil in groups of 8 sheets and press them to obtain a high Tg lead-free copper clad laminate; the pressing parameters include: pressure 100Psi, temperature 150°C, vacuum degree 0.03-0.1MPa, and pressing time 200min.

[0055] Example 7

[0056] Compared with Example 6, the modified filler in this example is replaced with a modified filler prepared according to the proportion in Example 3, and the other raw materials and preparation process remain the same as those in Example 6.

[0057] Example 8

[0058] Compared with Example 6, the modified filler in this example is replaced with a modified filler prepared according to the proportion in Example 4, and the other raw materials and preparation process remain the same as those in Example 6.

[0059] Example 9

[0060] Compared with Example 8, the addition amount of the modified filler in this example is adjusted to 50 parts, and the other raw materials and preparation process remain the same as those in Example 8.

[0061] Comparative Example 1

[0062] Compared with Example 5, the filler prepared in this comparative example is nano-silicon dioxide treated with γ-aminopropyltriethoxysilane. The other raw materials and preparation process are the same as those in Example 5.

[0063] The samples prepared in Examples 5-9 and Comparative Example 1 were tested, and the results are shown in Table 1:

[0064] Glass transition temperature Tg (DSC): tested using a DMA instrument and measured in accordance with the DMA test method specified in IPC-TM-6502.4.24.4.

[0065] Heat resistance T288: Tested using TMA instrument and determined according to the test method specified in IPC-TM-6502.4.24.1.

[0066] Copper foil peel strength PS: tested using Shimadzu tensile testing machine, measured according to the test method specified in IPC-TM-6502.4.8.

[0067] Coefficient of thermal expansion CTE: Tested using a TMA instrument and measured according to the TMA test method specified in IPC-TM-6502.4.24.

[0068] Dielectric constant (Dk) and dielectric loss factor (Df): The dielectric constant and dielectric loss factor test methods are determined in accordance with the test methods specified in IPC-TM-6502.5.5.9.

[0069] Flame retardant grade test: carried out in accordance with UL94 standard.

[0070] Table 1

[0071]

[0072] In summary, the samples prepared in the present invention have the following performance parameters:

[0073] 1. Glass transition temperature (DSC) Tg>180℃.

[0074] 2. Heat resistance T288>30min.

[0075] 3. Copper foil peel strength PS>8.01b / in(1oz).

[0076] 4. Thermal weight loss Td (5% wt)>350℃.

[0077] 5. Coefficient of thermal expansion CTE (50℃-60℃, Z axis) ≤2.3%.

[0078] 6. Dielectric constant Dk≤4.3@2GHz-10GHz, dielectric loss Df≤0.013@10GHz.

[0079] 7. The combustion performance reaches UL94V-0 level.

[0080] Furthermore, the samples prepared in Examples 5-9 all passed the CAF·100V·85°C / 85%·1000h test.

[0081] In Comparative Example 1, a commonly used silane coupling agent is used as a modifier to treat the filler. Silane coupling agent is often used as a modifier for treating fillers, but silane coupling agent is also a small molecule material and has limited modification effect on the filler. When the treated filler is added in too large an amount, secondary aggregation is prone to occur, resulting in poor dispersion effect. In Examples 5-9, amino-terminated hyperbranched polymers are prepared using amino-terminated siloxane intermediates as raw materials, and the fillers are subjected to secondary treatment. The formed branched polymer chains form a "loose structure" on the surface of the filler, avoiding secondary aggregation. More importantly, the biphenyl group introduced into the structure of the amino-terminated siloxane intermediate is beneficial to increasing the glass transition temperature of the material, and the siloxane group can effectively reduce the thermal expansion coefficient of the material.

[0082] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0083] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A high Tg lead-free copper clad laminate, characterized in that: The invention comprises glass fiber cloth, adhesive and copper foil. The adhesive comprises 160-165 parts of phosphorus-containing epoxy resin, 40-60 parts of modified filler, 10-12 parts of inorganic flame retardant, 2-3 parts of curing agent and 2-3 parts of organic solvent by weight. The modified filler is a carboxylated filler modified by a terminal amino hyperbranched polymer.

2. A high Tg lead-free copper clad laminate according to claim 1, characterized in that: The modified filler is prepared by the following steps: The carboxylated filler was added to acetone, and then the amino-terminated hyperbranched polymer and p-toluenesulfonic acid were added, and the mixture was heated under reflux for reaction for 40-50 minutes. After the reaction was completed, the mixture was dried at 40° C. to a constant weight to obtain a modified filler.

3. A high Tg lead-free copper clad laminate according to claim 2, characterized in that: The amino-terminated hyperbranched polymer is prepared by the following steps: Mix 4'amino-4-biphenol and triethylamine, add butanone, stir and dissolve, slowly add dimethyldichlorosilane while stirring at 60°C, heat and reflux for 12 hours, filter, wash with water to remove salt, dissolve and recrystallize to obtain an amino-terminated siloxane intermediate; the molar ratio of 4'amino-4-biphenol to dimethyldichlorosilane is 2:1; Under nitrogen protection, the amino-terminated siloxane intermediate and glacial acetic acid are mixed, and then excess methyl acrylate is added, and the reaction is carried out at 80°C in the dark for 2 hours. After the reaction liquid is completed, the methyl acrylate is removed by vacuum concentration to obtain an intermediate product. The intermediate product and ethylenediamine are mixed, and the reaction is carried out at a temperature of 100°C for 2 hours. N, N-dimethylacetamide is added and the temperature is raised to 120°C for reaction for 2 hours, and the temperature is further raised to 140°C for reaction for 6 hours. The obtained reactant is precipitated with ether and petroleum ether to obtain an amino-terminated hyperbranched polymer. The mass ratio of the intermediate product to ethylenediamine is 2:

1.

4. A high Tg lead-free copper clad laminate according to claim 2, characterized in that: The added amount of the amino-terminated hyperbranched polymer is 12-16% of the mass of the carboxylated filler, and the added amount of p-toluenesulfonic acid is 0.3% of the mass of the carboxylated filler.

5. The high Tg lead-free copper clad laminate according to claim 2, characterized in that: The carboxylated filler is prepared by the following steps: After adding the filler into water and ultrasonically dispersing it, the system is adjusted to be weakly acidic, and then vinyl triethoxysilane is added. At 80-85°C, the reaction is stirred for 2-3 hours. Then, acrylic acid, ammonium persulfate and sodium bisulfite are added, and the reaction is continued with stirring for 3-4 hours. After the reaction is completed, the mixture is cooled, washed and freeze-dried to obtain a carboxylated filler.

6. The high Tg lead-free copper clad laminate according to claim 1, characterized in that: The filler is one of nano silicon dioxide and hexagonal boron nitride nanosheets.

7. The high Tg lead-free copper clad laminate according to claim 1, characterized in that: The mass fraction of phosphorus in the phosphorus-containing epoxy resin is 2.5-3%.

8. The high Tg lead-free copper clad laminate according to claim 1, characterized in that: The inorganic flame retardant is one of aluminum hydroxide and magnesium hydroxide or a mixture of the two in any proportion.

9. The method for preparing a high Tg lead-free copper clad laminate according to claim 1, characterized in that: The steps include: The first step is to mix the phosphorus-containing epoxy resin, the curing agent and the organic solvent, stir for 30-40 minutes, add the modified filler and the inorganic flame retardant and continue to stir for 30-40 minutes to obtain a glue solution; The second step is to apply glue on the surface of the glass fiber cloth, bake and cure at 100℃-250℃ to obtain a prepreg, and the curing time is 80-100min; The third step is to stack the prepregs in groups of 8 to 16 sheets with copper foil and press them to obtain a high Tg lead-free copper clad laminate.

10. The method for preparing a high Tg lead-free copper clad laminate according to claim 9, characterized in that: The mass ratio of glass fiber cloth to adhesive is 10:5-6; The pressing parameters include: pressure 100-200Psi, temperature 100-150°C, vacuum degree 0.03-0.1MPa, and pressing time 150-200min.