Impermeable phase change interface material and preparation method thereof

By using components such as high-purity silicone oil and paraffin in phase change interface materials, combined with ceramic thermal powder and thermal fillers, the problems of poor dimensional stability and limited application range of traditional phase change interface materials are solved, and a higher level of Thermal conductivity and mechanical strength are suitable for a variety of application scenarios and prevent leakage through barrier membranes.

CN118909440APending Publication Date: 2024-11-08NANTONG HONGCHUANG BIOTECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410952219.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Traditional phase transition interface materials have poor dimensional stability during the phase transition process, are easily affected by the external environment, and are difficult to adjust the phase transition temperature, resulting in limited application range and difficult maintenance.

Method used

Anti-permeable phase change interface material composed of substrates, organic hydrocarbons, phase change materials, ceramic thermal powders, thermal fillers, thickeners, antioxidants and crosslinkers, and ensures the material through strict formula ratios and process flow. Stability and reliability, including the use of high-purity silicone oils, polyisobutylene and paraffin, as well as the addition of ceramic thermal powders and thermal fillers, improve thermal conductivity and mechanical strength.

Benefits of technology

It achieves the improvement of the dimensional stability and thermal conductivity of the material, extends the service life, is suitable for a wider range of application scenarios, and effectively prevents leakage through TPU film and PE barrier film, ensuring the material under temperature circulation and humidity changes. Stable performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004947537370000121
    Figure BDA0004947537370000121
  • Figure BDA0004947537370000131
    Figure BDA0004947537370000131
Patent Text Reader

Abstract

The invention relates to a phase change interface material, in particular to an anti-permeation phase change interface material and a preparation method thereof, the material is prepared by curing a TPU (thermoplastic polyurethane) material formed by a base material, organic hydrocarbon, a phase change material, ceramic heat conduction powder, heat conduction filler, a thickening agent, an antioxidant and a cross-linking agent through a three-layer coating process, according to the technical scheme, the material is prepared from, by mass, 30-40 parts of a base material, 10-15 parts of organic hydrocarbon, 15-20 parts of a phase change material, 15-25 parts of ceramic heat conduction powder, 4-10 parts of heat conduction filler, 4-8 parts of a thickening agent, 1-2 parts of an antioxidant and 1-3 parts of a cross-linking agent, all the components in the process and the formula are prepared according to the strict mass proportion, and it is ensured that the material has stable performance and reliable working effect; the material is used for manufacturing PCM series products, can effectively solve the problems of sweating and permeability of the products, and further comprises a TPU film with the thickness of about 25 microns and a PE barrier film with the thickness of 5-6 microns, so that material leakage can be effectively prevented.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of phase change interface materials, in particular to an anti-penetration phase change interface material and a preparation method thereof. Background Art

[0002] Phase change interface material is a composite material with specific functions, usually composed of a substrate and a composite layer with phase change material added. Phase change material can undergo a phase change process within a specific temperature range, thereby absorbing or releasing a large amount of heat to regulate the ambient temperature. During the phase change process, the material changes from solid to liquid or liquid to solid, and its temperature remains relatively stable, so that the temperature of the environment in which it is located also remains relatively stable. Phase change interface materials provide additional functions or performance by integrating this phase change material into the substrate.

[0003] Anti-permeability is crucial for phase change interface materials, especially in applications such as construction, automobiles or electronic equipment. Phase change materials are usually wrapped in waterproof materials or protected by other means to prevent them from getting wet or damaged, which would affect their performance and service life. Effective anti-permeability can ensure that the phase change material can work stably for a long time during use and is not affected by the external environment.

[0004] Generally, traditional phase change interface materials have poor dimensional stability and may experience volume changes during the phase change process, making it difficult to precisely control the size and shape of the material in some applications. Some phase change materials may experience performance degradation after multiple phase change processes, especially under frequent temperature cycles, and are prone to fatigue and damage. In addition, the general phase change temperature is usually fixed, making it difficult to adjust or expand its application range according to specific needs. At the same time, they are highly sensitive to environmental humidity and other external factors, requiring special protection and packaging measures to ensure long-term stable performance, and are difficult to maintain.

[0005] In summary, it is necessary to propose an anti-permeability phase change interface material and a preparation method thereof to solve the above problems. Summary of the invention

[0006] The object of the present invention is to provide an anti-permeability phase change interface material and a preparation method thereof to solve the problems raised in the above background technology.

[0007] To achieve the above object, the present invention provides the following technical solutions:

[0008] A permeation-proof phase-change interface material, which is composed of a substrate, organic hydrocarbons, a phase-change material, ceramic thermally conductive powder, a thermally conductive filler, a thickener, an antioxidant and a cross-linking agent, wherein, by mass ratio, the substrate accounts for 30-40 parts, the organic hydrocarbons account for 10-15 parts, the phase-change material accounts for 15-20 parts, the ceramic thermally conductive powder accounts for 15-25 parts, the thermally conductive filler accounts for 4-10 parts, the thickener accounts for 4-8 parts, the antioxidant accounts for 1-2 parts, and the cross-linking agent accounts for 1-3 parts.

[0009] Preferably, the substrate is specifically prepared by reacting chlorosilane and water to generate cyclic or linear siloxane, and in the presence of an acidic or alkaline catalyst, the cyclic or linear siloxane is subjected to a ring-opening polymerization reaction to form high molecular weight polydimethylsiloxane, and low molecular weight components and impurities are removed by distillation and filtration to obtain high-purity silicone oil with a purity of more than 99%.

[0010] Preferably, the organic hydrocarbon is specifically isobutylene separated from cracking gas, liquefied by condensation, anionic polymerization of isobutylene is carried out at -100°C to -70°C using BF3 as a catalyst, and finally the catalyst and unreacted monomers are removed by solvent extraction, evaporation and drying to obtain high-purity polyisobutylene with a purity of more than 95%.

[0011] Preferably, the phase change material is a lubricating oil fraction separated from crude oil by a distillation process, the lubricating oil fraction is cooled, acetone-toluene is added and solid paraffin is separated by filtration, and finally the paraffin is refined by a decolorization, deodorization and impurity removal process with a purity of more than 98%.

[0012] Preferably, the ceramic thermally conductive powder is composed of 10-15 parts of boron nitride and 5-10 parts of aluminum oxide;

[0013] The boron nitride is prepared by mixing boric acid and ammonium nitride, pre-treating the mixture in a dryer, calcining the mixture at 900-1400° C. in a nitrogen atmosphere to generate boron nitride, and removing impurities by pickling and heat treatment, with a purity of more than 99%;

[0014] The alumina is obtained by crushing bauxite, leaching it with sodium hydroxide solution to obtain sodium aluminate solution, decomposing the sodium aluminate solution by carbonation or seed crystal method to obtain aluminum hydroxide precipitation, and calcining the aluminum hydroxide in a high-temperature furnace at 1000-1200° C., with a purity of more than 99%.

[0015] Preferably, the thermal conductive filler is composed of 2-5 parts of silver powder and 2-5 parts of copper powder;

[0016] The silver powder is produced by electrolyzing a silver nitrate solution in an electrolytic cell with pure silver as an anode and stainless steel as a cathode, removing impurities in the electrolyte by washing and centrifugal separation, drying the silver powder, and further purifying it by screening and heat treatment, with a purity of more than 99.9%;

[0017] The copper powder is produced by electrolyzing a copper sulfate solution in an electrolytic cell with pure copper as an anode and an iron plate as a cathode, removing impurities in the electrolyte by washing and centrifugal separation, drying the copper powder, and further purifying it by screening and heat treatment, with a purity of more than 99%.

[0018] Preferably, the thickener is composed of 3-5 parts of silicon dioxide and 1-3 parts of bentonite;

[0019] The silicon dioxide is obtained by reacting a sodium silicate solution with sulfuric acid or hydrochloric acid to generate a silicic acid precipitate, then removing the reaction byproducts and dissolved salts by filtering and washing with water, and finally drying and calcining the silicic acid precipitate, with a purity of more than 99%;

[0020] The bentonite is obtained by mechanically crushing and grinding natural bentonite ore to obtain bentonite powder, which is then removed from impurities through water washing, sedimentation and drying processes, and has a purity of more than 95%.

[0021] Preferably, the antioxidant is composed of 0.5-1 part of butylated hydroxyanisole and 0.5-1 part of butylated hydroxytoluene;

[0022] The butylated hydroxyanisole is prepared by alkylating p-methoxyphenol with tert-butyl alcohol under the action of an acid catalyst, controlling the reaction temperature and time to ensure complete reaction, and finally removing unreacted raw materials and by-products by distillation or crystallization, with a purity of more than 99%;

[0023] The butylated hydroxytoluene is prepared by alkylating p-cresol with isobutylene under the action of an acid catalyst, controlling the reaction temperature and time to ensure complete reaction, and removing unreacted raw materials and by-products by distillation or crystallization, with a purity of more than 99%.

[0024] Preferably, the crosslinking agent is prepared by reacting alkyl halosilane with alcohol under anhydrous conditions to generate alkoxysilane, hydrolyzing the alkoxysilane in water to generate silanol, and removing unreacted raw materials and by-products through distillation and filtration after condensation reaction to obtain polysiloxane with a purity of more than 98%.

[0025] Based on the above formula, the present invention also proposes a method for preparing an anti-permeability phase change interface material, comprising the following steps:

[0026] S1. Prepare the components according to the formula ratio: substrate, organic hydrocarbon, phase change material, ceramic thermal conductive powder, thermal conductive filler, thickener, antioxidant, cross-linking agent, add the substrate first, and gradually add organic hydrocarbon and phase change material under stirring to ensure preliminary uniform mixing. Under continued stirring, add ceramic thermal conductive powder, thermal conductive filler, thickener in turn, and control the stirring speed at 300-400rpm. Finally, add antioxidant and cross-linking agent, and increase the stirring speed to 500-600rpm to ensure that all components are fully dispersed. The total mixing time is controlled at 60-90 minutes to ensure that all components are evenly mixed. Keep the temperature of the mixing kettle at 40-60℃ to prevent excessive temperature from causing component degradation or incomplete reaction;

[0027] S2. Inject the mixed TPU material into the pre-prepared mold. The mold can be designed according to the required material shape and size. Slightly vibrate the mold to ensure that the material is evenly filled and avoid bubbles and gaps. Use a coater or coating equipment to evenly coat or apply the material on the substrate surface. Control the thickness and uniformity. The coating speed and thickness are adjusted according to the material performance requirements. The coating thickness is 0.5-2mm, and the cycle is repeated three times;

[0028] S3. Place the formed TPU material into a curing furnace, and ensure that a 25-micron thick TPU film and a 5-6-micron thick PE barrier film are set between every two layers of the composite structure. The temperature is controlled at 80-120°C. Depending on the different components of the material, the curing time is 2-4 hours. After the curing is completed, the temperature is gradually lowered to room temperature to prevent rapid cooling from causing material stress concentration and performance degradation;

[0029] S4. Use a thermal conductivity meter to measure the thermal conductivity of the material to ensure that it meets the design requirements. Use an anti-permeability tester to test the anti-permeability performance of the material to ensure that it can be effectively anti-seepage in practical applications. Use a mechanical properties tester to test the tensile strength and compressive strength of the material to ensure the stability and reliability of the material during use.

[0030] Compared with the prior art, the beneficial effects of the present invention are as follows: the components in the process and formula of the present invention are formulated in strict mass proportions to ensure that the material has stable performance and reliable working results; the stability and durability of the material are ensured by high-purity silicone oil, polyisobutylene, and phase change materials; the thermal conductivity and mechanical strength of the material are improved by adding ceramic thermal conductive powder and thermal conductive filler, making it suitable for a wider range of application scenarios; it also includes strict mixing, stirring, curing and testing processes to ensure the controllability of each step and the consistency of the material; it has strong applicability and wide versatility; therefore, the present invention is used to make PCM series products, which can effectively solve the problems of sweating and permeability of the products; it also includes a TPU film of about 25 microns thick and a PE barrier film of 5-6 microns thick, which can effectively prevent material leakage. DETAILED DESCRIPTION

[0031] The present invention provides a technical solution:

[0032] A permeation-proof phase-change interface material, which is composed of a substrate, organic hydrocarbons, a phase-change material, ceramic thermally conductive powder, a thermally conductive filler, a thickener, an antioxidant and a cross-linking agent, wherein, by mass ratio, the substrate accounts for 30-40 parts, the organic hydrocarbons account for 10-15 parts, the phase-change material accounts for 15-20 parts, the ceramic thermally conductive powder accounts for 15-25 parts, the thermally conductive filler accounts for 4-10 parts, the thickener accounts for 4-8 parts, the antioxidant accounts for 1-2 parts, and the cross-linking agent accounts for 1-3 parts.

[0033] It should also be noted that the substrate of the present invention is specifically prepared by reacting chlorosilane and water to generate cyclic or linear siloxane, and in the presence of an acidic or alkaline catalyst, the cyclic or linear siloxane is subjected to a ring-opening polymerization reaction to form high molecular weight polydimethylsiloxane, and low molecular weight components and impurities are removed by distillation and filtration to obtain a high-purity silicone oil with a purity of more than 99%.

[0034] It should also be noted that the organic hydrocarbon of the present invention is specifically separated from isobutylene from the cracking gas, liquefied by condensation, anionic polymerization of isobutylene is carried out at -100°C to -70°C using BF3 as a catalyst, and finally the catalyst and unreacted monomers are removed by solvent extraction, evaporation and drying to obtain high-purity polyisobutylene with a purity of more than 95%.

[0035] It should also be noted that the phase change material of the present invention is obtained by separating the lubricating oil fraction from crude oil through a distillation process, cooling the lubricating oil fraction, adding acetone-toluene and filtering to separate the solid paraffin, and finally refining the paraffin through a decolorization, deodorization and impurity removal process, with a purity of more than 98%.

[0036] It should also be noted that the ceramic thermally conductive powder of the present invention is composed of 10-15 parts of boron nitride and 5-10 parts of aluminum oxide;

[0037] The boron nitride is prepared by mixing boric acid and ammonium nitride, pre-treating the mixture in a dryer, calcining the mixture at 900-1400° C. in a nitrogen atmosphere to generate boron nitride, and removing impurities by pickling and heat treatment, with a purity of more than 99%;

[0038] The alumina is obtained by crushing bauxite, leaching it with sodium hydroxide solution to obtain sodium aluminate solution, decomposing the sodium aluminate solution by carbonation or seed crystal method to obtain aluminum hydroxide precipitation, and calcining the aluminum hydroxide in a high-temperature furnace at 1000-1200° C., with a purity of more than 99%.

[0039] It should also be noted that the thermal conductive filler of the present invention is composed of 2-5 parts of silver powder and 2-5 parts of copper powder;

[0040] The silver powder is produced by electrolyzing a silver nitrate solution in an electrolytic cell with pure silver as an anode and stainless steel as a cathode, removing impurities in the electrolyte by washing and centrifugal separation, drying the silver powder, and further purifying it by screening and heat treatment, with a purity of more than 99.9%;

[0041] The copper powder is produced by electrolyzing a copper sulfate solution in an electrolytic cell with pure copper as an anode and an iron plate as a cathode, removing impurities in the electrolyte by washing and centrifugal separation, drying the copper powder, and further purifying it by screening and heat treatment, with a purity of more than 99%.

[0042] It should also be noted that the thickener of the present invention is composed of 3-5 parts of silicon dioxide and 1-3 parts of bentonite;

[0043] The silicon dioxide is obtained by reacting a sodium silicate solution with sulfuric acid or hydrochloric acid to generate a silicic acid precipitate, then removing the reaction byproducts and dissolved salts by filtering and washing with water, and finally drying and calcining the silicic acid precipitate, with a purity of more than 99%;

[0044] The bentonite is obtained by mechanically crushing and grinding natural bentonite ore to obtain bentonite powder, which is then removed from impurities through processes such as water washing, sedimentation and drying, and has a purity of more than 95%.

[0045] It should also be noted that the antioxidant of the present invention is composed of 0.5-1 part of butylated hydroxyanisole and 0.5-1 part of butylated hydroxytoluene;

[0046] The butylated hydroxyanisole is prepared by alkylating p-methoxyphenol with tert-butyl alcohol under the action of an acid catalyst, controlling the reaction temperature and time to ensure complete reaction, and finally removing unreacted raw materials and by-products by distillation or crystallization, with a purity of more than 99%;

[0047] The butylated hydroxytoluene is prepared by alkylating p-cresol with isobutylene under the action of an acid catalyst, controlling the reaction temperature and time to ensure complete reaction, and removing unreacted raw materials and by-products by distillation or crystallization, with a purity of more than 99%.

[0048] It should also be noted that the crosslinking agent of the present invention is specifically prepared by reacting an alkyl halosilane with an alcohol under anhydrous conditions to generate an alkoxysilane, which is hydrolyzed in water to generate a silanol, and then the unreacted raw materials and by-products are removed by distillation and filtration after the condensation reaction to obtain a polysiloxane with a purity of more than 98%.

[0049] Example 1

[0050] Based on the above formula, this embodiment also proposes a method for preparing an anti-permeability phase change interface material, comprising the following steps:

[0051] S1. Prepare the following components according to the formula ratio: 35 parts of substrate, 12.5 parts of organic hydrocarbon, 17.5 parts of phase change material, 20 parts of ceramic thermal conductive powder, 7 parts of thermal conductive filler, 6 parts of thickener, 1.5 parts of antioxidant, and 2 parts of cross-linking agent;

[0052] First add the substrate, then gradually add the organic hydrocarbon and phase change material under stirring to ensure the initial uniform mixing. Under continued stirring, add the ceramic thermal conductive powder, thermal conductive filler, and thickener in turn, with the stirring speed controlled at 400rpm. Finally, add the antioxidant and cross-linking agent, and increase the stirring speed to 600rpm to ensure that all components are fully dispersed. The total mixing time is controlled at 90 minutes to ensure that all components are evenly mixed. Keep the mixing kettle temperature at 60℃ to prevent excessive temperature from causing component degradation or incomplete reaction;

[0053] S2. Inject the mixed TPU material into the pre-prepared mold. The mold can be designed according to the required material shape and size. Slightly vibrate the mold to ensure that the material is evenly filled and avoid bubbles and gaps. Use a coater or coating equipment to evenly coat or apply the material on the substrate surface. Control the thickness and uniformity. The coating speed and thickness are adjusted according to the material performance requirements. The coating thickness is 2mm;

[0054] S3. Place the formed TPU material into a curing furnace, and ensure that a 25-micron-thick TPU film and a 5-6-micron-thick PE barrier film are set between every two layers of the composite structure. The temperature is controlled at 120°C. Depending on the different components of the material, the curing time is 4 hours. After the curing is completed, the temperature is gradually lowered to room temperature to prevent rapid cooling from causing material stress concentration and performance degradation;

[0055] S4. Use a thermal conductivity meter to measure the thermal conductivity of the material to ensure that it meets the design requirements. Use an anti-permeability tester to test the anti-permeability performance of the material to ensure that it can be effectively anti-seepage in practical applications. Use a mechanical properties tester to test the tensile strength, compressive strength and other mechanical properties of the material to ensure the stability and reliability of the material during use.

[0056] Example 2

[0057] In this embodiment, a method for preparing an anti-permeability phase change interface material comprises the following steps:

[0058] S1. Prepare the following components according to the formula ratio: 35 parts of substrate, 12.5 parts of organic hydrocarbon, 17.5 parts of phase change material, 25 parts of ceramic thermal conductive powder, 7 parts of thermal conductive filler, 6 parts of thickener, 1.5 parts of antioxidant, and 2 parts of cross-linking agent;

[0059] First add the substrate, then gradually add the organic hydrocarbon and phase change material under stirring to ensure the initial uniform mixing. Under continued stirring, add the ceramic thermal conductive powder, thermal conductive filler, and thickener in turn, with the stirring speed controlled at 400rpm. Finally, add the antioxidant and cross-linking agent, and increase the stirring speed to 600rpm to ensure that all components are fully dispersed. The total mixing time is controlled at 90 minutes to ensure that all components are evenly mixed. Keep the mixing kettle temperature at 60℃ to prevent excessive temperature from causing component degradation or incomplete reaction;

[0060] S2. Inject the mixed TPU material into the pre-prepared mold. The mold can be designed according to the required material shape and size. Slightly vibrate the mold to ensure that the material is evenly filled and avoid bubbles and gaps. Use a coater or coating equipment to evenly coat or apply the material on the substrate surface. Control the thickness and uniformity. The coating speed and thickness are adjusted according to the material performance requirements. The coating thickness is 2mm;

[0061] S3. Place the formed TPU material into a curing furnace, and ensure that a 25-micron-thick TPU film and a 5-6-micron-thick PE barrier film are set between every two layers of the composite structure. The temperature is controlled at 120°C. Depending on the different components of the material, the curing time is 4 hours. After the curing is completed, the temperature is gradually lowered to room temperature to prevent rapid cooling from causing material stress concentration and performance degradation;

[0062] S4. Use a thermal conductivity meter to measure the thermal conductivity of the material to ensure that it meets the design requirements. Use an anti-permeability tester to test the anti-permeability performance of the material to ensure that it can be effectively anti-seepage in practical applications. Use a mechanical properties tester to test the tensile strength, compressive strength and other mechanical properties of the material to ensure the stability and reliability of the material during use.

[0063] Example 3

[0064] A method for preparing an anti-permeability phase change interface material comprises the following steps:

[0065] S1. Prepare the following components according to the formula ratio: 35 parts of substrate, 12.5 parts of organic hydrocarbon, 17.5 parts of phase change material, 12.5 parts of ceramic thermal conductive powder, 7 parts of thermal conductive filler, 6 parts of thickener, 1.5 parts of antioxidant, and 2 parts of cross-linking agent;

[0066] First add the substrate, then gradually add the organic hydrocarbon and phase change material under stirring to ensure the initial uniform mixing. Under continued stirring, add the ceramic thermal conductive powder, thermal conductive filler, and thickener in turn, with the stirring speed controlled at 400rpm. Finally, add the antioxidant and cross-linking agent, and increase the stirring speed to 600rpm to ensure that all components are fully dispersed. The total mixing time is controlled at 90 minutes to ensure that all components are evenly mixed. Keep the mixing kettle temperature at 60℃ to prevent excessive temperature from causing component degradation or incomplete reaction;

[0067] S2. Inject the mixed TPU material into the pre-prepared mold. The mold can be designed according to the required material shape and size. Slightly vibrate the mold to ensure that the material is evenly filled and avoid bubbles and gaps. Use a coater or coating equipment to evenly coat or apply the material on the substrate surface. Control the thickness and uniformity. The coating speed and thickness are adjusted according to the material performance requirements. The coating thickness is 2mm;

[0068] S3. Place the formed TPU material into a curing furnace, and ensure that a 25-micron-thick TPU film and a 5-6-micron-thick PE barrier film are set between every two layers of the composite structure. The temperature is controlled at 120°C. Depending on the different components of the material, the curing time is 4 hours. After the curing is completed, the temperature is gradually lowered to room temperature to prevent rapid cooling from causing material stress concentration and performance degradation;

[0069] S4. Use a thermal conductivity meter to measure the thermal conductivity of the material to ensure that it meets the design requirements. Use an anti-permeability tester to test the anti-permeability performance of the material to ensure that it can be effectively anti-seepage in practical applications. Use a mechanical properties tester to test the tensile strength, compressive strength and other mechanical properties of the material to ensure the stability and reliability of the material during use.

[0070] Example 4

[0071] A method for preparing an anti-permeability phase change interface material comprises the following steps:

[0072] S1. Prepare the following components according to the formula ratio: 35 parts of substrate, 15 parts of organic hydrocarbon, 15 parts of phase change material, 20 parts of ceramic thermal conductive powder, 7 parts of thermal conductive filler, 6 parts of thickener, 1.5 parts of antioxidant, and 2 parts of cross-linking agent;

[0073] First add the substrate, then gradually add the organic hydrocarbon and phase change material under stirring to ensure the initial uniform mixing. Under continued stirring, add the ceramic thermal conductive powder, thermal conductive filler, and thickener in turn, with the stirring speed controlled at 400rpm. Finally, add the antioxidant and cross-linking agent, and increase the stirring speed to 600rpm to ensure that all components are fully dispersed. The total mixing time is controlled at 90 minutes to ensure that all components are evenly mixed. Keep the mixing kettle temperature at 60℃ to prevent excessive temperature from causing component degradation or incomplete reaction;

[0074] S2. Inject the mixed TPU material into the pre-prepared mold. The mold can be designed according to the required material shape and size. Slightly vibrate the mold to ensure that the material is evenly filled and avoid bubbles and gaps. Use a coater or coating equipment to evenly coat or apply the material on the substrate surface. Control the thickness and uniformity. The coating speed and thickness are adjusted according to the material performance requirements. The coating thickness is 2mm;

[0075] S3. Place the formed TPU material into a curing furnace, and ensure that a 25-micron-thick TPU film and a 5-6-micron-thick PE barrier film are set between every two layers of the composite structure. The temperature is controlled at 120°C. Depending on the different components of the material, the curing time is 4 hours. After the curing is completed, the temperature is gradually lowered to room temperature to prevent rapid cooling from causing material stress concentration and performance degradation;

[0076] S4. Use a thermal conductivity meter to measure the thermal conductivity of the material to ensure that it meets the design requirements. Use an anti-permeability tester to test the anti-permeability performance of the material to ensure that it can be effectively anti-seepage in practical applications. Use a mechanical properties tester to test the tensile strength, compressive strength and other mechanical properties of the material to ensure the stability and reliability of the material during use.

[0077] Example 5

[0078] A method for preparing an anti-permeability phase change interface material comprises the following steps:

[0079] S1. Prepare the following components according to the formula ratio: 35 parts of substrate, 12.5 parts of organic hydrocarbon, 17.5 parts of phase change material, 15 parts of ceramic thermal conductive powder, 7 parts of thermal conductive filler, 6 parts of thickener, 1.5 parts of antioxidant, and 2 parts of cross-linking agent;

[0080] First add the substrate, then gradually add the organic hydrocarbon and phase change material under stirring to ensure the initial uniform mixing. Under continued stirring, add the ceramic thermal conductive powder, thermal conductive filler, and thickener in turn, with the stirring speed controlled at 400rpm. Finally, add the antioxidant and cross-linking agent, and increase the stirring speed to 600rpm to ensure that all components are fully dispersed. The total mixing time is controlled at 90 minutes to ensure that all components are evenly mixed. Keep the mixing kettle temperature at 60℃ to prevent excessive temperature from causing component degradation or incomplete reaction;

[0081] S2. Inject the mixed TPU material into the pre-prepared mold. The mold can be designed according to the required material shape and size. Slightly vibrate the mold to ensure that the material is evenly filled and avoid bubbles and gaps. Use a coater or coating equipment to evenly coat or apply the material on the substrate surface. Control the thickness and uniformity. The coating speed and thickness are adjusted according to the material performance requirements. The coating thickness is 2mm;

[0082] S3. Place the formed TPU material into a curing furnace, and ensure that a 25-micron-thick TPU film and a 5-6-micron-thick PE barrier film are set between every two layers of the composite structure. The temperature is controlled at 120°C. Depending on the different components of the material, the curing time is 4 hours. After the curing is completed, the temperature is gradually lowered to room temperature to prevent rapid cooling from causing material stress concentration and performance degradation;

[0083] S4. Use a thermal conductivity meter to measure the thermal conductivity of the material to ensure that it meets the design requirements. Use an anti-permeability tester to test the anti-permeability performance of the material to ensure that it can be effectively anti-seepage in practical applications. Use a mechanical properties tester to test the tensile strength, compressive strength and other mechanical properties of the material to ensure the stability and reliability of the material during use.

[0084] Example 6

[0085] A method for preparing an anti-permeability phase change interface material comprises the following steps:

[0086] S1. Prepare the following components according to the formula ratio: 35 parts of substrate, 15 parts of organic hydrocarbon, 17.5 parts of phase change material, 20 parts of ceramic thermal conductive powder, 7 parts of thermal conductive filler, 6 parts of thickener, 1.5 parts of antioxidant, and 2 parts of cross-linking agent;

[0087] First add the substrate, then gradually add the organic hydrocarbon and phase change material under stirring to ensure the initial uniform mixing. Under continued stirring, add the ceramic thermal conductive powder, thermal conductive filler, and thickener in turn, with the stirring speed controlled at 400rpm. Finally, add the antioxidant and cross-linking agent, and increase the stirring speed to 600rpm to ensure that all components are fully dispersed. The total mixing time is controlled at 90 minutes to ensure that all components are evenly mixed. Keep the mixing kettle temperature at 60℃ to prevent excessive temperature from causing component degradation or incomplete reaction;

[0088] S2. Inject the mixed TPU material into the pre-prepared mold. The mold can be designed according to the required material shape and size. Slightly vibrate the mold to ensure that the material is evenly filled and avoid bubbles and gaps. Use a coater or coating equipment to evenly coat or apply the material on the substrate surface. Control the thickness and uniformity. The coating speed and thickness are adjusted according to the material performance requirements. The coating thickness is 2mm;

[0089] S3. Place the formed TPU material into a curing furnace, and ensure that a 25-micron-thick TPU film and a 5-6-micron-thick PE barrier film are set between every two layers of the composite structure. The temperature is controlled at 120°C. Depending on the different components of the material, the curing time is 4 hours. After the curing is completed, the temperature is gradually lowered to room temperature to prevent rapid cooling from causing material stress concentration and performance degradation;

[0090] S4. Use a thermal conductivity meter to measure the thermal conductivity of the material to ensure that it meets the design requirements. Use an anti-permeability tester to test the anti-permeability performance of the material to ensure that it can be effectively anti-seepage in practical applications. Use a mechanical properties tester to test the tensile strength, compressive strength and other mechanical properties of the material to ensure the stability and reliability of the material during use.

[0091] Experimental verification

[0092] The specific formula ratios in the above-mentioned Examples 1 to 6 are made into phase change materials, and their performance is tested, wherein the material components are shown in Table 1:

[0093] Table 1 Material components of Examples 1 to 6

[0094]

[0095]

[0096] Design of the experiment:

[0097] Experiment 1. Thermal conductivity test: Use a thermal conductivity meter to measure the thermal conductivity of the material to ensure that it meets the design requirements;

[0098] Experiment 2. Anti-penetration test: Use an anti-penetration tester to test the anti-penetration performance of the material to ensure that it can effectively prevent penetration in practical applications;

[0099] Experiment 3. Mechanical strength test: Use a mechanical properties tester to test the tensile strength, compression strength and other mechanical properties of the material to ensure the stability and reliability of the material during use;

[0100] Performance parameters are shown in Table 2;

[0101] Table 2 Phase change material properties of Examples 1 to 6

[0102] Performance Indicators Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Thermal conductivity (W / mK) 1.8 2.1 1.6 1.9 2.0 2.2 Permeation resistance 98% 97% 96% 95% 99% 99% Tensile strength(MPa) 5.5 5.7 5.2 5.4 5.6 5.8 Compression strength(MPa) 12.1 12.5 11.8 12.0 12.3 12.6

[0103] Conclusion: Through performance comparison, Example 6 performs well in thermal conductivity, anti-permeability and mechanical strength, and is selected as the best example.

[0104] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. An anti-permeability phase change interface material, It is characterized in that The material is made by curing a TPU material composed of a substrate, organic hydrocarbons, phase change materials, ceramic thermal conductive powder, thermal conductive fillers, thickeners, antioxidants and crosslinking agents through a three-layer coating process, wherein the substrate accounts for 30-40 parts, the organic hydrocarbons account for 10-15 parts, the phase change materials account for 15-20 parts, the ceramic thermal conductive powder accounts for 15-25 parts, the thermal conductive fillers account for 4-10 parts, the thickeners account for 4-8 parts, the antioxidants account for 1-2 parts, and the crosslinking agents account for 1-3 parts.

2. The anti-permeability phase change interface material according to claim 1, Features: The substrate is specifically prepared by reacting chlorosilane and water to generate cyclic or linear siloxane, and in the presence of an acidic or alkaline catalyst, the cyclic or linear siloxane is subjected to a ring-opening polymerization reaction to form high molecular weight polydimethylsiloxane, and low molecular weight components and impurities are removed by distillation and filtration to obtain high-purity silicone oil with a purity of more than 99%.

3. The anti-permeability phase change interface material according to claim 2, Features: The organic hydrocarbon is specifically obtained by separating isobutylene from cracking gas, liquefying it by condensation, carrying out anionic polymerization of isobutylene at -100°C to -70°C using BF3 as a catalyst, and finally removing the catalyst and unreacted monomers by solvent extraction, evaporation and drying to obtain high-purity polyisobutylene with a purity of more than 95%.

4. The anti-permeability phase change interface material according to claim 3, Features: The phase change material is obtained by separating lubricating oil fraction from crude oil through distillation process, cooling the lubricating oil fraction, adding acetone-toluene and filtering to separate solid paraffin, and finally refining the paraffin through decolorization, deodorization and impurity removal process, with a purity of more than 98%.

5. The anti-permeability phase change interface material according to claim 4, Features: The ceramic thermally conductive powder is composed of 10-15 parts of boron nitride and 5-10 parts of aluminum oxide; The boron nitride is prepared by mixing boric acid and ammonium nitride, pre-treating the mixture in a dryer, calcining the mixture at 900-1400° C. in a nitrogen atmosphere to generate boron nitride, and removing impurities by pickling and heat treatment, with a purity of more than 99%; The alumina is obtained by crushing bauxite, leaching it with sodium hydroxide solution to obtain sodium aluminate solution, decomposing the sodium aluminate solution by carbonation or seed crystal method to obtain aluminum hydroxide precipitation, and calcining the aluminum hydroxide in a high-temperature furnace at 1000-1200° C., with a purity of more than 99%.

6. The anti-permeability phase change interface material according to claim 5, Features: The thermal conductive filler is composed of 2-5 parts of silver powder and 2-5 parts of copper powder; The silver powder is produced by electrolyzing a silver nitrate solution in an electrolytic cell with pure silver as an anode and stainless steel as a cathode, removing impurities in the electrolyte by washing and centrifugal separation, drying the silver powder, and further purifying it by screening and heat treatment, with a purity of more than 99.9%; The copper powder is produced by electrolyzing a copper sulfate solution in an electrolytic cell with pure copper as an anode and an iron plate as a cathode, removing impurities in the electrolyte by washing and centrifugal separation, drying the copper powder, and further purifying it by screening and heat treatment, with a purity of more than 99%.

7. The anti-permeability phase change interface material according to claim 6, Features: The thickener is composed of 3-5 parts of silicon dioxide and 1-3 parts of bentonite; The silicon dioxide is obtained by reacting a sodium silicate solution with sulfuric acid or hydrochloric acid to generate a silicic acid precipitate, then removing the reaction byproducts and dissolved salts by filtering and washing with water, and finally drying and calcining the silicic acid precipitate, with a purity of more than 99%; The bentonite is obtained by mechanically crushing and grinding natural bentonite ore to obtain bentonite powder, which is then removed from impurities through water washing, sedimentation and drying processes, and has a purity of more than 95%.

8. The anti-permeability phase change interface material according to claim 7, Features: The antioxidant is composed of 0.5-1 part of butylated hydroxyanisole and 0.5-1 part of butylated hydroxytoluene; The butylated hydroxyanisole is prepared by alkylating p-methoxyphenol with tert-butyl alcohol under the action of an acid catalyst, controlling the reaction temperature and time to ensure complete reaction, and finally removing unreacted raw materials and by-products by distillation or crystallization, with a purity of more than 99%; The butylated hydroxytoluene is prepared by alkylating p-cresol with isobutylene under the action of an acid catalyst, controlling the reaction temperature and time to ensure complete reaction, and removing unreacted raw materials and by-products by distillation or crystallization, with a purity of more than 99%.

9. The anti-permeability phase change interface material according to claim 8, Features: The crosslinking agent is specifically prepared by reacting alkyl halogen silane with alcohol under anhydrous conditions to generate alkoxy silane, hydrolyzing the alkoxy silane in water to generate silanol, and removing unreacted raw materials and by-products through distillation and filtration after condensation reaction to obtain polysiloxane with a purity of more than 98%.

10. A method for preparing an anti-permeability phase change interface material according to any one of claims 1 to 9, It is characterized in that The following steps are involved: S1. Prepare the components according to the formula ratio: substrate, organic hydrocarbon, phase change material, ceramic thermal conductive powder, thermal conductive filler, thickener, antioxidant, cross-linking agent, add the substrate first, and gradually add the organic hydrocarbon and phase change material under stirring to ensure preliminary uniform mixing. Under continued stirring, add the ceramic thermal conductive powder, thermal conductive filler, thickener in turn, and control the stirring speed at 300-400rpm. Finally, add the antioxidant and cross-linking agent, and increase the stirring speed to 500-600rpm to ensure that all components are fully dispersed. The total mixing time is controlled at 60-90 minutes to ensure that the components are evenly mixed, and keep the temperature of the mixing kettle at 40-60℃; S2. Inject the mixed TPU material into the pre-prepared mold. The mold can be designed according to the required material shape and size. Slightly vibrate the mold to ensure that the material is evenly filled and avoid bubbles and gaps. Use a coater or coating equipment to evenly coat or apply the material on the substrate surface. Control the thickness and uniformity. The coating speed and thickness are adjusted according to the material performance requirements. The coating thickness is 0.5-2mm, and the cycle is repeated three times; S3. Place the formed TPU material into a curing oven, and ensure that a 25-micron-thick TPU film and a 5-6-micron-thick PE barrier film are set between each two layers of the composite structure. The temperature is controlled at 80-120°C. Depending on the different components of the material, the curing time is 2-4 hours. After the curing is completed, the temperature is gradually lowered to room temperature. S4. Use a thermal conductivity meter to measure the thermal conductivity of the material to ensure that it meets the design requirements. Use an anti-permeability tester to test the anti-permeability performance of the material to ensure that it can be effectively waterproof in practical applications. Use a mechanical properties tester to test the mechanical properties of the tensile strength and compressive strength of the material.