Modified ceramic coating, preparation method thereof, modified layer and cup

By modifying the polymer, polymethylsiloxane and silica in ceramic coatings, the hydrogen bond donor is reduced, and the residual taste problem of ceramic cladding water cup is solved, improving the improvement of the odor of the ceramic coating. The user experience and the stability and ease of cleaning are provided.

CN118909464AActive Publication Date: 2024-11-08WUHAN SUPOR COOKWARE
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410867960.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-11-08
Estimated Expiration
2044-06-28

AI Technical Summary

Technical Problem

The existing ceramic clad water cups have obvious coffee flavor after use and lasts for a long time, which affects the consumption experience.

Method used

Modified ceramic coating is used to marinate the mixed slurry of dimethylsiloxane and silica polymer, polymethylsiloxane and silicic acid to form a coating, reduce hydrogen bond donor, and reduce beverage odor substances and The probability of bonding on the coating surface to avoid odor residue.

Benefits of technology

It significantly reduces flavor residue, improves consumer experience, and improves the cup's ease of cleaning and stability through the non-stickness and durability of the modified coating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004921669470000161
    Figure BDA0004921669470000161
Patent Text Reader

Abstract

The invention provides a modified ceramic coating, a preparation method thereof, a modified layer and a cup. Wherein the modified ceramic coating is formed by curing a mixed slurry containing a polymer of dimethyl siloxane and silicon dioxide, 3-5 parts by weight of polymethylsiloxane and 20-35 parts by weight of silicic acid, and the modified ceramic coating is prepared from the following components in parts by weight: 1-5 parts by weight of polymethylsiloxane, 1-5 parts by weight of silicon dioxide, 1-5 parts by weight of silicon dioxide and 1-5 parts by weight of silicon dioxide. The weight part of the polymer of the dimethyl siloxane and the silicon dioxide is 20 to 35 parts. According to the modified ceramic coating provided by the embodiment of the invention, compared with an existing ceramic coating, a coating formed by the modified ceramic coating obtained by mixing the raw materials can provide a relatively small number of hydrogen bond donors, so that when the modified ceramic coating is used, the number of the hydrogen bond donors is relatively small; and the probability that odorous substances in drinks (such as odorous substances in coffee) are combined with the surface of the coating is reduced, so that taste residues can be avoided to a great extent, and the use experience of consumers is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of coating technology, and in particular to a modified ceramic coating and a preparation method thereof, a modified layer and a cup. Background Art

[0002] There are currently water cups on the market that are sprayed with ceramic coatings and then sintered (called "ceramic coated water cups"). It is often found that when such water cups are used to soak some beverages with their own odor (for example, coffee), even if the cup is cleaned after use, a relatively obvious coffee smell will still remain, and the residual smell usually takes a long time (usually more than half a month) to gradually dissipate. These residual smells are obvious and "linger for a long time", seriously affecting the consumer's experience. Summary of the invention

[0003] The present application aims to at least solve the problem in the above-mentioned prior art or related art that the residual smell of the water cup after use is obvious and "lingers for a long time", which seriously affects the consumer's experience of use.

[0004] To achieve the above-mentioned purpose, the first aspect embodiment of the present application provides a modified ceramic coating, wherein the modified ceramic coating is formed by ripening a mixed slurry including a polymer of dimethylsiloxane and silicon dioxide, polymethylsiloxane and silicic acid, wherein, in parts by weight, the weight of the polymethylsiloxane is 3 parts to 5 parts, the weight of the silicic acid is 20 parts to 35 parts, and the weight of the polymer of dimethylsiloxane and silicon dioxide is 20 parts to 35 parts.

[0005] According to the modified ceramic coating of the embodiment of the present application, compared with the existing ceramic coating, the modified ceramic coating obtained by ripening the above raw materials can provide a relatively small number of hydrogen bond donors in the coating. Therefore, when in use, due to the small number of hydrogen bond donors, the probability of odor substances in beverages (such as odor substances in coffee) combining with the coating surface is reduced, thereby being able to avoid taste residue to a large extent and improving the consumer's usage experience.

[0006] In some embodiments, the modified ceramic coating includes a reaction product of dimethylsiloxane in combination with a polymer of silicon dioxide, polymethylsiloxane, and silicic acid.

[0007] In these embodiments, the modified ceramic coating includes a polymer of dimethylsiloxane and silicon dioxide, and a reaction product of polymethylsiloxane and silicic acid. When the modified ceramic coating is sprayed to form a modified layer, as the solvent and the like evaporate, a reaction product of a polymer of dimethylsiloxane and silicon dioxide, and polymethylsiloxane and silicic acid can be formed as a coating for the cup. The number of hydrogen bond donors therein is less than that of conventional ceramic coatings, thereby ensuring that the cup is not prone to residual taste during use, further enhancing the consumer experience.

[0008] In some embodiments, based on 100% of the total weight of the modified ceramic coating, the weight of the reaction product in the modified ceramic coating accounts for 2.5%-8% of the total weight of the modified ceramic coating.

[0009] In these embodiments, the modified ceramic coating contains 2.5%-8% by weight of the reaction product, which can ensure that the cup is non-stick and further enhance the consumer's experience.

[0010] In some embodiments, the mixed slurry further comprises titanium dioxide, pigment brown and a solvent, wherein, in parts by weight, the weight of the titanium dioxide is 10-20 parts, the weight of the pigment brown is 1-2 parts, and the weight of the solvent is 10-30 parts.

[0011] In these embodiments, titanium dioxide is usually white, and pigment brown is usually black. By setting the two to have a suitable weight ratio, a modified ceramic coating with a desired color can be obtained, thereby obtaining a coating of a cup with a desired color. The ceramic coating (modified ceramic coating) after aging of the multi-component mixed slurry has a suitable viscosity, which can avoid sagging when spraying to form a coating, thereby ensuring the quality of the coating. In addition, the stability and uniformity of the formed modified ceramic coating can also be ensured.

[0012] In some embodiments, the modified ceramic coating includes zinc oxide, and the weight ratio of the zinc oxide to the mixed slurry is (0.5-3): 100. In this way, the stability of the modified ceramic coating can be ensured to avoid deterioration while improving the antibacterial property.

[0013] According to a second aspect of the present application, a method for preparing a modified ceramic coating is provided, wherein the method comprises: forming a mixed slurry comprising a polymer of dimethylsiloxane and silicon dioxide, polymethylsiloxane and silicic acid, wherein, in parts by weight, the weight of the polymethylsiloxane is 3 to 5 parts, the weight of the silicic acid is 20 to 35 parts, and the weight of the polymer of dimethylsiloxane and silicon dioxide is 20 to 35 parts; stirring and mixing the mixed slurry to obtain a matured ceramic coating, thereby obtaining the modified ceramic coating.

[0014] According to the method for preparing a modified ceramic coating provided in an embodiment of the present application, the modified ceramic coating is obtained by mixing and ripening a mixed slurry including a polymer of dimethylsiloxane and silicon dioxide, polymethylsiloxane and silicic acid. Compared with the existing ceramic coating, the modified ceramic coating formed by the mixed and ripened raw materials can provide a relatively small number of hydrogen bond donors. Thus, when in use, due to the small number of hydrogen bond donors, the probability of odor substances in beverages (such as odor substances in coffee) combining with the coating surface is reduced, thereby being able to avoid taste residue to a large extent and improving the consumer's usage experience.

[0015] In some embodiments, the forming of a mixed slurry comprising a polymer of dimethylsiloxane and silicon dioxide, polymethylsiloxane and silicic acid comprises: mixing the polymer of dimethylsiloxane and silicon dioxide and silicic acid, and then adding the polymethylsiloxane to form a mixed slurry comprising a polymer of dimethylsiloxane and silicon dioxide, polymethylsiloxane and silicic acid.

[0016] In these embodiments, first, the polymer of dimethylsiloxane and silica and silicic acid are mixed evenly to ensure that the two components are evenly distributed in the system. Silicic acid can act as a crosslinking agent here, and can react with the hydroxyl groups in the polymer of dimethylsiloxane and silica to form a preliminary crosslinked network. Next, when polymethylsiloxane is added, since its reactivity with silicic acid is higher than that with the polymer of dimethylsiloxane and silica, polymethylsiloxane will preferentially react with silicic acid to further expand and reinforce the crosslinked network. This reaction may involve condensation between the methyl in polymethylsiloxane and the hydroxyl in silicic acid to form a more stable silicon-oxygen-silicon bond. Through this step-by-step mixing and reaction method, a more uniform and dense crosslinked network can be formed, thereby improving the strength, durability and other physical properties of the coating. In addition, this method also helps to control the reaction rate and reduce the generation of by-products, for example, it can reduce the possibility of most polymethylsiloxane and silicic acid directly forming methylsiloxane polymers, thereby optimizing the overall performance of the product.

[0017] In some embodiments, in the step of stirring the mixed slurry, the mixing temperature is controlled to be 20° C.-30° C., and the stirring time is 8 h-12 h. Under these conditions, the formation of the matured ceramic coating can be promoted.

[0018] In some embodiments, the mixed slurry further comprises titanium dioxide, pigment brown and a solvent, wherein, in parts by weight, the weight of the titanium dioxide is 10-20 parts, the weight of the pigment brown is 1-2 parts, and the weight of the solvent is 10-30 parts.

[0019] In these embodiments, titanium dioxide is usually white, and pigment brown is usually black. By setting the two to have a suitable weight ratio, a modified ceramic coating of a desired color can be formed, thereby obtaining a coating of a cup with a desired color. The matured ceramic coating formed by the mixed slurry of the above multiple components can ensure that the ceramic coating has a suitable viscosity, avoid sagging when spraying to form the coating, and ensure the quality of the coating. In addition, the stability and uniformity of the formed modified ceramic coating can also be ensured.

[0020] In some embodiments, the method further comprises: adding zinc oxide powder to the cured ceramic coating, so that the zinc oxide powder is dispersed in the cured ceramic coating, thereby forming the modified ceramic coating.

[0021] In these embodiments, the modified ceramic coating is obtained by mixing zinc oxide powder and the cured ceramic coating, and the antibacterial properties of the modified ceramic coating can be improved. In addition, after the mixed slurry is stirred and mixed to obtain the cured ceramic coating, the zinc oxide powder is added, which can avoid the influence of the properties of zinc oxide itself (for example, activity, acidity and alkalinity, etc.) on the pH value and stability of the curing process (for example, it can avoid unnecessary reactions of zinc oxide with other components during the curing process), thereby ensuring the stability of the curing process. In addition, the added zinc oxide powder can interfere with the viscosity of the modified ceramic coating due to the absence of the influence of the solvent, avoid the sagging phenomenon when spraying to form the coating, and ensure the quality of the modified layer formed by the modified ceramic coating.

[0022] In some embodiments, the weight ratio of the zinc oxide to the aged ceramic coating is (0.5-3): 100. In this way, the stability of the modified ceramic coating can be ensured and deterioration can be avoided while improving the antibacterial property.

[0023] According to a third aspect of the present application, a modified layer is provided, wherein the modified layer is formed by spraying the modified ceramic coating described above.

[0024] In these embodiments, a relatively small number of hydrogen bond donors can be provided in the modified layer. Thus, when in use, due to the small number of hydrogen bond donors, the probability of odor substances in the beverage (such as odor substances in coffee) binding to the coating surface is reduced, thereby being able to avoid odor residue to a large extent and improving the consumer's experience. In addition, the polymer of dimethylsiloxane and silicon dioxide in the modified ceramic coating can reduce the brittleness of the formed coating and can improve the bonding strength with the cup body. In addition, according to the modified ceramic coating of the present application, when zinc oxide is added, the anti-odor performance can be optimized to a certain extent.

[0025] In some embodiments, the thickness of the modified layer is 10 μm-30 μm, so that the life of the modified layer can be guaranteed.

[0026] In some embodiments, the main component of the modified layer is a reaction product of dimethylsiloxane, a polymer of silicon dioxide, polymethylsiloxane and silicic acid.

[0027] In these embodiments, the reaction product of dimethylsiloxane and a polymer of silicon dioxide, polymethylsiloxane and silicic acid can provide a relatively small number of hydrogen bond donors. Thus, when used, due to the small number of hydrogen bond donors, the probability of odor substances in the beverage (such as odor substances in coffee) binding to the coating surface is reduced, thereby being able to avoid flavor residue to a large extent and improving the consumer's experience.

[0028] According to a fourth aspect of the present application, a cup is provided, wherein the cup comprises a cup body and a modified layer formed on an inner wall surface of the cup body, wherein the modified layer is the modified layer described above. DETAILED DESCRIPTION

[0029] The following specific embodiments are provided to help the reader obtain a comprehensive understanding of the methods, devices and / or systems described herein. However, after understanding the disclosure of the present application, various changes, modifications and equivalents of the methods, devices and / or systems described herein will be clear. For example, the order of operations described herein is only an example and is not limited to those orders set forth herein, but can be changed as will be clear after understanding the disclosure of the present application, except for operations that must occur in a specific order. In addition, for greater clarity and simplicity, the description of features known in the art may be omitted.

[0030] The existing ceramic coating is a liquid coating with the reaction product (methylsiloxane polymer) formed by polymethylsiloxane and silicic acid as the main non-stick component, which is mainly used in cookware. With the gradual improvement of living standards, people have certain requirements for the easy cleanability of cups. To this end, the applicant applied the existing ceramic coating for cookware to cups. After use, it was found that when the water cup was soaked in some drinks with its own odor (for example, coffee), even if the cup was cleaned after use, a relatively obvious coffee smell would still remain, and the residual smell usually needs to be left for a long time (generally more than half a month) before it will gradually dissipate. These residual smells are obvious and "long-lasting", which seriously affects the consumer's experience.

[0031] To this end, the applicant discovered that after the existing ceramic coating is air-sprayed and sintered, the surface groups in the coating formed have a large number of hydroxyl groups that can serve as hydrogen bond donors, and the carbonyl and amino groups in the odorous substances in coffee substances (such as ketones, esters, aldehydes, and pyridine nitrogen-containing compounds) are good hydrogen bond acceptors. When the coating formed by the coating comes into contact with beverages containing a large number of hydrogen bond donors, the coating formed by the coating is easy to adsorb the odorous substances in these beverages (for example, odorous substances in coffee substances), that is, beverages containing hydrogen bond acceptors (such as certain ingredients in coffee) form hydrogen bonds with the surface of the coating, resulting in the ceramic coated water cup easily retaining the coffee smell even after cleaning.

[0032] In this regard, the applicant wants to obtain the modified ceramic coating of the present application by blocking the formation of hydrogen bond donor groups (hydroxyl groups) during the formation of the ceramic coating, so as to reduce the number of hydrogen bond donors in the formed coating as much as possible, thereby ensuring that the cups are not easily adsorbed by coffee-like odor substances due to hydrogen bonding during use, avoiding odor residue, and improving the consumer's experience.

[0033] Specifically, the applicant found that the modified ceramic coating is formed by mixing a polymer of dimethylsiloxane and silicon dioxide and polymethylsiloxane and silicic acid. Due to the low temperature and the low content of polymethylsiloxane and silicic acid that are easy to react, a small part of the three components of dimethylsiloxane and silicon dioxide polymer and polymethylsiloxane and silicic acid in the modified ceramic coating will interact with each other. When the modified ceramic coating is sprayed on the cup substrate to form a modified layer, most of the three components of dimethylsiloxane and silicon dioxide polymer and polymethylsiloxane and silicic acid in the modified layer will interact (cross-link with each other) under the temperature of the sintering stage, forming a modified layer according to the present application that is not easy to form hydrogen bonds with other substances.

[0034] According to the first aspect of the present application, a modified ceramic coating is provided for cups, wherein the modified ceramic coating is formed by ripening a mixed slurry including a polymer of dimethylsiloxane and silicon dioxide, polymethylsiloxane and silicic acid, wherein, in parts by weight, the weight of polymethylsiloxane is 3 parts to 5 parts, the weight of silicic acid is 20 parts to 35 parts, and the weight of the polymer of dimethylsiloxane and silicon dioxide is 20 parts to 35 parts.

[0035] According to the modified ceramic coating of the embodiment of the present application, compared with the existing ceramic coating, the modified ceramic coating obtained by ripening the above raw materials can provide a relatively small number of hydrogen bond donors in the coating. Therefore, when in use, due to the small number of hydrogen bond donors, the probability of odor substances in beverages (such as odor substances in coffee) combining with the coating surface is reduced, thereby being able to avoid taste residue to a large extent and improving the consumer's usage experience.

[0036] According to the present application, ceramic coatings are coatings that are formed by mixing various components when they are needed. Specifically, before aging, each component needs to be stored separately. For example, the polymer of dimethylsiloxane and silicon dioxide, polymethylsiloxane and silicic acid can be diluted in corresponding solvents and stored separately to be used as the raw material part of the modified ceramic coating. As an example, the solvent can be isopropanol, purified water, alcohol, etc., which can be more convenient to form a mixed slurry with uniform mixing. When aging is required, the diluted substances are mixed to form a modified ceramic coating. In this way, the uniformity and stability of the coating can be ensured, and the risk of unevenness, instability and other problems in the coating can be reduced. It should be noted that according to the present application, after aging, the modified ceramic coating can maximize the performance and advantages of the ceramic coating within a certain period of time to ensure the quality and stability of the coating. As an example, the storage time of the ceramic coating after aging does not exceed 72h.

[0037] In some embodiments, the modified ceramic coating is a coating comprising a reaction product of a polymer of dimethylsiloxane and silicon dioxide, a polymethylsiloxane and a silicic acid. As an example, in the modified ceramic coating, the reaction product may include a bonding product of polymethylsiloxane and silicic acid, a bonding product of dimethylsiloxane and a polymer of silicon dioxide and silicic acid, a bonding product of dimethylsiloxane and a polymer of silicon dioxide and polymethylsiloxane, and a bonding product of polymethylsiloxane, silicic acid, and a polymer of dimethylsiloxane and silicon dioxide. According to the present application, different bonding product combinations can provide different properties and characteristics for the coating, so that it can adapt to a wider range of application scenarios and more stringent use requirements. As an example, the bonding product of polymethylsiloxane and silicic acid can provide a certain degree of non-stickiness, so that the cups with the modified layer have easy-to-clean properties. The bonding product of dimethylsiloxane, a polymer of silicon dioxide and silicic acid has wear resistance, so that the cups with the modified layer have good stability and durability.

[0038] In these embodiments, the modified ceramic coating includes a polymer of dimethylsiloxane and silicon dioxide, and a reaction product of polymethylsiloxane and silicic acid. When the modified ceramic coating is sprayed to form a modified layer, as the solvent and the like evaporate, a reaction product of a polymer of dimethylsiloxane and silicon dioxide, and polymethylsiloxane and silicic acid can be formed as a coating for the cup. The number of hydrogen bond donors therein is less than that of conventional ceramic coatings, thereby ensuring that the cup is not prone to residual taste during use, further enhancing the consumer experience.

[0039] In some embodiments, based on the total weight of the modified ceramic coating being 100%, the weight of the reaction product in the modified ceramic coating accounts for 2.5% to 8% of the total weight of the modified ceramic coating.

[0040] In these embodiments, the modified ceramic coating contains 2.5%-8% by weight of the reaction product, which can ensure that the cup is non-stick and further enhance the consumer's experience.

[0041] In some embodiments, the mixed slurry further comprises titanium dioxide, pigment brown and a solvent, wherein, in parts by weight, the weight of titanium dioxide is 10-20 parts, the weight of pigment brown is 1-2 parts, and the weight of the solvent is 10-30 parts.

[0042] In these embodiments, titanium dioxide is usually white, and pigment brown is usually black. By setting the two to have a suitable weight ratio, a modified ceramic coating with a desired color can be obtained, thereby obtaining a coating of a cup with a desired color. The ceramic coating (modified ceramic coating) after aging of the multi-component mixed slurry has a suitable viscosity, which can avoid sagging when spraying to form a coating, thereby ensuring the quality of the coating. In addition, the stability and uniformity of the formed modified ceramic coating can also be ensured.

[0043] In some embodiments, the modified ceramic coating includes zinc oxide, and the weight ratio of zinc oxide to the mixed slurry is (0.5-3): 100. In this way, the stability of the modified ceramic coating can be ensured to avoid deterioration while improving the antibacterial property.

[0044] According to a second aspect of the present application, a method for preparing a modified ceramic coating is provided, wherein the method for preparing the modified ceramic coating comprises:

[0045] Step S101, forming a mixed slurry including a polymer of dimethylsiloxane and silicon dioxide, polymethylsiloxane and silicic acid, in which, in parts by weight, the weight of polymethylsiloxane is 3 parts to 5 parts, the weight of silicic acid is 20 parts to 35 parts, and the weight of the polymer of dimethylsiloxane and silicon dioxide is 20 parts to 35 parts.

[0046] Step S102, stirring and mixing the mixed slurry to obtain a matured ceramic coating, thereby forming a modified ceramic coating.

[0047] According to the method for preparing a modified ceramic coating provided in an embodiment of the present application, the modified ceramic coating is obtained by mixing and ripening a mixed slurry including a polymer of dimethylsiloxane and silicon dioxide, polymethylsiloxane and silicic acid. Compared with the existing ceramic coating, the modified ceramic coating formed by the mixed and ripened raw materials can provide a relatively small number of hydrogen bond donors. Thus, when in use, due to the small number of hydrogen bond donors, the probability of odor substances in beverages (such as odor substances in coffee) combining with the coating surface is reduced, thereby being able to avoid taste residue to a large extent and improving the consumer's usage experience.

[0048] Hereinafter, the method for preparing the modified ceramic coating according to the present application will be described in combination with specific steps.

[0049] Forming mixed slurry

[0050] According to the present application, polymethylsiloxane can be obtained commercially. In some embodiments, the viscosity of polymethylsiloxane is within the range of 6 seconds to 12 seconds when tested with Iwata No. 2 cup. In the modified layer, most of the polymethylsiloxane will hydrolyze to form a network structure. In the coating formed by the coating with polymethylsiloxane, polymethylsiloxane improves the non-stickiness (methyl group provided) on the one hand, and on the other hand, the network structure formed makes it easy for the silicon dioxide molecules generated by silicic acid to be filled into the network structure and combined, playing the role of fixing silicon dioxide and strengthening the function of the coating. In addition, the weight of the raw material polymethylsiloxane in the modified ceramic coating is 3 parts to 5 parts, which should not be too much or too little. If the weight of the raw material polymethylsiloxane in the modified ceramic coating is too much, there will be more hydroxyl groups in the formed coating, which can serve as hydrogen bond donors. In this case, it will be detrimental to the purpose of reducing the hydrogen bond donors of the coating in the present application. If the weight of the raw material polymethylsiloxane in the modified ceramic coating is too little, it will affect the performance of the formed coating, for example, water resistance, weather resistance, hardness and other properties will decrease.

[0051] According to the present application, the raw materials for forming the modified ceramic coating include silicic acid, which is in liquid form and can be obtained commercially. Silicic acid can decompose to form silicon dioxide under heating conditions, as shown in the reaction equation: H2SiO3→SiO2+H2O. The silicon dioxide therein is a floc formed by the agglomeration of silicon dioxide molecules. The SiO2 generated by the heating and decomposition of silicic acid (H2SiO3) has a small particle size and a high specific surface area, which can significantly improve the adhesion and dispersibility of the coating, so that the SiO2 generated by the heating and decomposition of silicic acid (H2SiO3) is suitable for the needs of ceramic coatings in terms of particle size and structure, so it is different from the silicon dioxide powder in the prior art. In addition, the SiO2 generated by the heating and decomposition of silicic acid (H2SiO3) has better compatibility and reactivity, and can better participate in the chemical reaction in the coating, thereby improving the performance of the ceramic coating. The silicic acid in the modified ceramic coating plays a reinforcing function in the final coating, similar to the stone in concrete.

[0052] According to the present application, the reaction product of dimethyl (siloxane and polysiloxane) and silicon dioxide, also known as the polymer of dimethyl siloxane and silicon dioxide, CAS: 67762-90-7, has hydrophobicity, chemical stability and mechanical strength, and can embed silane functional groups on the surface of silicon dioxide formed by silicic acid, thereby generating a layer of stable chemically bonded silane product.

[0053] According to the present application, the polymer of dimethylsiloxane and silicon dioxide can be obtained from the market or prepared by the following preparation method. As an example, dimethylsiloxane and chlorosilane (such as trichlorosilane, trichloromethylsilane, etc.) are hydrolyzed under the catalysis of hydrochloric acid to obtain a polymer of dimethylsiloxane and silicon dioxide.

[0054] According to the present application, the polymer of dimethylsiloxane and silicon dioxide, on the one hand, provides non-stickiness (provided by the methyl group), and on the other hand, can react with silicic acid to hydrolyze to form SiO2, thereby ensuring the integrity of the modified ceramic coating, and does not introduce hydrogen bond donors itself. At the same time, it can reduce the brittleness of the formed modified layer to improve the strength, and has good bonding with the cup body, thereby improving the overall strength of the modified layer.

[0055] It should be noted that the mixed slurry may also include raw materials such as solvents. The solvent is used to adjust the viscosity of the modified ceramic coating so that the coating can be better applied and coated on the surface of the cup base. The filler is used to adjust the appearance of the final coating product. As an example, the solvent can be isopropyl alcohol, purified water, alcohol, etc.

[0056] According to the present application, after preparing the various raw materials, they are mixed. Specifically, a mixed slurry comprising a polymer of dimethylsiloxane and silicon dioxide, polymethylsiloxane and silicic acid is formed, which comprises mixing a polymer of dimethylsiloxane and silicon dioxide and silicic acid, and then adding polymethylsiloxane to form a mixed slurry comprising a polymer of dimethylsiloxane and silicon dioxide, polymethylsiloxane and silicic acid.

[0057] In these embodiments, first, the polymer of dimethylsiloxane and silica and silicic acid are mixed evenly to ensure that the two components are evenly distributed in the system. Silicic acid can act as a crosslinking agent here, and can react with the hydroxyl groups in the polymer of dimethylsiloxane and silica to form a preliminary crosslinked network. Next, when polymethylsiloxane is added, since its reactivity with silicic acid is higher than that with the polymer of dimethylsiloxane and silica, polymethylsiloxane will preferentially react with silicic acid to further expand and reinforce the crosslinked network. This reaction may involve condensation between the methyl group in polymethylsiloxane and the hydroxyl group in silicic acid to form a more stable silicon-oxygen-silicon bond. Through this step-by-step mixing and reaction method, a more uniform and dense crosslinked network can be formed, thereby improving the strength, durability and other physical properties of the coating. In addition, this method also helps to control the reaction rate and reduce the generation of by-products, thereby optimizing the overall performance of the product.

[0058] According to the present application, during the mixing process, the pH value of the mixed slurry system is maintained in the range of 5-7 and the temperature is 20° C.-30° C. Under these conditions, the formation of the matured ceramic coating can be promoted.

[0059] According to the present application, in the step of stirring and mixing, the temperature in the mixing step is controlled to be 20°C-30°C, and the mixing time is 8h-12h. Specifically, the mixed slurry is added to the mixing device, and the temperature of the mixing device and the stirring device of the mixing device are controlled so that the mixing of the mixed slurry is also mixed and stirred at 20°C-30°C for 8h-12h to ensure that the components in the coating are fully mixed. During the mixing process, a small part of the three dimethylsiloxane and the polymer of silicon dioxide, polymethylsiloxane and silicic acid interact with each other, and most of them will be cross-linked with each other in the subsequent sintering stage after the coating is formed to form a modified layer according to the present application that is not easy to form hydrogen bonds with other substances. Specifically, during the sintering stage, a large number of cross-linking reactions will occur between dimethylsiloxane, the polymer of silicon dioxide, polymethylsiloxane and silicic acid. These reactions combine the various components tightly together to form a modified layer with excellent performance. This modified layer not only has excellent anti-odor performance, but also has excellent physical properties such as strength, hardness and wear resistance.

[0060] According to the present application, the mixed slurry includes a polymer of dimethylsiloxane and silicon dioxide, polymethylsiloxane and silicic acid, wherein, in parts by weight, the weight of polymethylsiloxane is 3 parts to 5 parts, the weight of silicic acid is 20 parts to 35 parts, and the weight of the polymer of dimethylsiloxane and silicon dioxide is 20 parts to 35 parts. In some embodiments, the mixed slurry also includes titanium dioxide, pigment brown and a solvent, wherein the weight of titanium dioxide is 10 parts to 20 parts, the weight of pigment brown is 1 parts to 2 parts, and the weight of the solvent is 10 parts to 30 parts.

[0061] In these embodiments, titanium dioxide is usually white, and pigment brown is usually black. By setting the two to have a suitable weight ratio, a modified ceramic coating of a desired color can be formed, thereby obtaining a coating of a cup with a desired color. The matured ceramic coating formed by the mixed slurry of the above multiple components can ensure that the ceramic coating has a suitable viscosity, avoid sagging when spraying to form the coating, and ensure the quality of the coating. In addition, the stability and uniformity of the formed modified ceramic coating can also be ensured.

[0062] Curing is a key step in the preparation of ceramic coatings, which involves chemical reactions and physical changes of various components in the coating to form a stable coating system. In this process, pH value and stability are two very important parameters, which directly affect the quality and performance of the coating.

[0063] According to the present application, the method for preparing the modified ceramic coating further comprises the step of adding zinc oxide powder to the aged ceramic coating, so that the zinc oxide powder is dispersed in the aged ceramic coating, thereby forming the modified ceramic coating.

[0064] In these embodiments, the modified ceramic coating is obtained by mixing zinc oxide powder and the cured ceramic coating, and the antibacterial properties of the modified ceramic coating can be improved. In addition, after the mixed slurry is stirred and mixed to obtain the cured ceramic coating, the zinc oxide powder is added, which can avoid the influence of the properties of zinc oxide itself (for example, activity, acidity and alkalinity, etc.) on the pH value and stability of the curing process (for example, it can avoid unnecessary reactions of zinc oxide with other components during the curing process), thereby ensuring the stability of the curing process. In addition, the added zinc oxide powder can interfere with the viscosity of the modified ceramic coating due to the absence of the influence of the solvent, avoid the sagging phenomenon when spraying to form the coating, and ensure the quality of the modified layer formed by the modified ceramic coating.

[0065] In some embodiments, the weight ratio of zinc oxide to the mixed slurry is (0.5-3):100, so that the anti-odor performance can be optimized while minimizing the impact on strength, ensuring the stability of the modified ceramic coating and avoiding deterioration.

[0066] In some embodiments, the zinc oxide powder and the aged ceramic coating may be mixed for 0.5 h to 1 h. Under the mixing effect of the above time, the zinc oxide powder can be dispersed in the aged ceramic coating.

[0067] According to the present application, a modified layer is provided, which is at least used for cups, wherein the modified layer is formed by spraying the modified ceramic coating provided according to the above embodiment.

[0068] According to the modified layer of the present application, a relatively small number of hydrogen bond donors can be provided in the modified layer. Thus, when in use, due to the small number of hydrogen bond donors, the probability of odor substances in the beverage (such as odor substances in coffee) combining with the coating surface is reduced, thereby being able to avoid taste residue to a large extent and improving the consumer's usage experience.

[0069] According to the present application, the modified layer has a suitable thickness. In some embodiments, the thickness of the modified layer is 10 μm-30 μm, so that the life of the modified layer can be guaranteed.

[0070] According to the present application, the preparation method of the modified layer includes spraying the modified ceramic coating to form the modified layer, wherein the spraying can be air spraying, as an example, the spray gun caliber: 1.4mm-1.6mm, the parameters of air spraying include: spraying distance is 140mm-180mm; air pressure is 0.2MPa-0.4MPa; flow rate is 5L / min-10L / min; the movement speed of the spray gun is 30cm / second-60cm / second; the angle between the gun nozzle and the sprayed object is 80°-100°; the movement speed of the spray gun is 30cm / second-60cm / second; the spray gun caliber is 1.4mm-1.6mm. In the process of forming the modified layer, because the modified ceramic coating is a liquid coating, it can be evenly distributed on the surface of the substrate and is easy to apply.

[0071] According to the present application, after spraying, the method for preparing the modified layer also includes a step of curing the air-sprayed modified layer. As an example, the coating can be cured by sintering. Specifically, the sintering temperature is 200°C-300°C and the sintering time is 8-15 minutes to improve the overall quality of the modified layer.

[0072] Under the influence of sintering temperature, the solvent in the modified layer sprayed by air is volatilized. When the solvent is reduced, most of the dimethylsiloxane and silicon dioxide polymer, polymethylsiloxane and silicic acid in the modified ceramic coating interact with each other at this stage to form a modified layer with the main components of the reaction product of dimethylsiloxane and silicon dioxide polymer, polymethylsiloxane and silicic acid. In this way, the anti-odor performance of the cup with the modified layer can be further optimized.

[0073] Specifically, the molecular formula of silicate can be written as Si(OH)4, -OH, which can also be called hydroxyl group. During the sintering process, silicate will decompose into SiO2, polymethylsiloxane and silicon dioxide will react to form a silicon dioxide polymer with methyl group, and when the polymer of dimethylsiloxane and silicon dioxide and silicon dioxide are mixed and reacted under the action of temperature, the hydroxyl group on the surface of silicate will react chemically with the methyl group on the molecular chain of the polymer of dimethylsiloxane and silicon dioxide to form a binary cross-linked structure. That is, after sintering, a modified layer with the reaction product of the polymer of dimethylsiloxane and silicon dioxide, polymethylsiloxane and silica as the main component can be formed.

[0074] According to a fourth aspect of the present application, a cup is provided, wherein the cup comprises a cup body and a modified layer formed on the inner wall surface of the cup body, wherein the modified layer is the modified layer provided according to the above embodiment.

[0075] In some embodiments, the cup body can be a stainless steel body, specifically 304 stainless steel or 316 stainless steel.

[0076] Hereinafter, the beneficial effects of the inventive concept will be described in conjunction with specific examples.

[0077] Example 1

[0078] The modified ceramic coating is formed by the following method.

[0079] S10, forming a mixed slurry including a polymer of dimethylsiloxane and silicon dioxide, polymethylsiloxane and silicic acid, wherein the mixed slurry comprises, by weight, 4 parts of polymethylsiloxane, 25 parts of silicic acid, 25 parts of the polymer of dimethylsiloxane and silicon dioxide, 15 parts of titanium dioxide, 1.5 parts of pigment brown and 20 parts of solvent.

[0080] S20, stirring and mixing the mixed slurry at a temperature of 25°C for 10 hours to obtain a matured ceramic coating, thereby forming a modified ceramic coating.

[0081] The modified ceramic coating is used to manufacture deodorizing cups by the following method.

[0082] S30: Providing a cup body.

[0083] S40: Preheating: Clean the cup body and preheat it to 60°C.

[0084] S50: Spraying. The modified ceramic coating is sprayed on the inner surface of the cup body by air spraying to form a modified layer with a film thickness of 20 microns. The spray gun caliber is 1.0 mm, and the air spraying parameters are as follows: the spraying distance is 160 mm; the air pressure is 0.3 MPa, the flow rate is 7 L / min; the moving speed of the spray gun is 40 cm / second; and the angle between the gun nozzle and the sprayed object is 90°.

[0085] S60: Sintering. Curing at 280°C for 10 minutes.

[0086] Through the above method, the deodorizing cup of Example 1 is obtained.

[0087] Example 2

[0088] The deodorizing cups of Example 2 were manufactured in the same manner as in Example 1, except that in step S10, different weight portions of raw materials were used to form the modified ceramic coating (wherein, in weight portions, the weight portions of polymethylsiloxane were 3 parts, the weight portions of silicic acid were 25 parts, the weight portions of the polymer of dimethylsiloxane and silicon dioxide were 25 parts, the weight portions of titanium dioxide were 15 parts, the weight portions of pigment brown were 1.5 parts, and the weight portions of the solvent were 20 parts).

[0089] Example 3

[0090] The deodorizing cups of Example 3 were manufactured in the same manner as in Example 1, except that in step S10, different weight portions of raw materials were used to form the modified ceramic coating (wherein, in weight portions, the weight portion of polymethylsiloxane was 5 parts, the weight portion of silicic acid was 25 parts, the weight portion of the polymer of dimethylsiloxane and silicon dioxide was 25 parts, the weight portion of titanium dioxide was 15 parts, the weight portion of pigment brown was 1.5 parts, and the weight portion of the solvent was 20 parts).

[0091] Example 4

[0092] The deodorizing cups of Example 4 were manufactured in the same manner as in Example 1, except that in step S10, different weight portions of raw materials were used to form the modified ceramic coating (wherein, in weight portions, the weight portion of polymethylsiloxane was 4 parts, the weight portion of silicic acid was 20 parts, the weight portion of the polymer of dimethylsiloxane and silicon dioxide was 25 parts, the weight portion of titanium dioxide was 15 parts, the weight portion of pigment brown was 1.5 parts, and the weight portion of the solvent was 20 parts).

[0093] Example 5

[0094] The deodorizing cups of Example 5 were manufactured in the same manner as in Example 1, except that in step S10, different weight portions of raw materials were used to form the modified ceramic coating (wherein, in weight portions, the weight portion of polymethylsiloxane was 4 parts, the weight portion of silicic acid was 35 parts, the weight portion of the polymer of dimethylsiloxane and silicon dioxide was 25 parts, the weight portion of titanium dioxide was 15 parts, the weight portion of pigment brown was 1.5 parts, and the weight portion of the solvent was 20 parts).

[0095] Example 6

[0096] The deodorizing cups of Example 6 were manufactured in the same manner as in Example 1, except that in step S10, different weight portions of raw materials were used to form the modified ceramic coating (wherein, in weight portions, the weight portion of polymethylsiloxane was 4 parts, the weight portion of silicic acid was 25 parts, the weight portion of the polymer of dimethylsiloxane and silicon dioxide was 20 parts, the weight portion of titanium dioxide was 15 parts, the weight portion of pigment brown was 1.5 parts, and the weight portion of the solvent was 20 parts).

[0097] Example 7

[0098] The deodorizing cups of Example 7 were manufactured in the same manner as in Example 1, except that in step S10, different weight portions of raw materials were used to form the modified ceramic coating (wherein, in weight portions, the weight portion of polymethylsiloxane was 4 parts, the weight portion of silicic acid was 25 parts, the weight portion of the polymer of dimethylsiloxane and silicon dioxide was 35 parts, the weight portion of titanium dioxide was 15 parts, the weight portion of pigment brown was 1.5 parts, and the weight portion of the solvent was 20 parts).

[0099] Example 8

[0100] The deodorizing cup of Example 8 was manufactured in the same manner as in Example 1, except that in step S20, zinc oxide powder was mixed with the matured ceramic coating in a weight ratio of 0.5:100 so that the zinc oxide powder was dispersed in the matured ceramic coating to form a modified ceramic coating.

[0101] Example 9

[0102] The deodorizing cups of Example 9 were manufactured in the same manner as in Example 1, except that in step S20, zinc oxide powder was mixed with the mixed and matured ceramic coating in a weight ratio of 3:100 so that the zinc oxide powder was dispersed in the matured ceramic coating to form a modified ceramic coating.

[0103] Example 10

[0104] The deodorizing cups of Example 10 were manufactured in the same manner as in Example 1, except that in step S20, zinc oxide powder was mixed with the matured ceramic coating in a weight ratio of 1:100 so that the zinc oxide powder was dispersed in the matured ceramic coating to form a modified ceramic coating.

[0105] Comparative Example 1

[0106] The deodorizing cups of Comparative Example 1 were manufactured in the same manner as in Example 1, except that in step S10, different ceramic coatings were used instead of the modified ceramic coatings (wherein the ceramic coating of Comparative Example 1 was a ceramic coating after polymethylsiloxane, silicic acid, titanium dioxide, pigment brown and solvent were matured, and in the ceramic coating, the weight parts of polymethylsiloxane were 4 parts, the weight parts of silicic acid were 30 parts, the weight parts of titanium dioxide were 15 parts, the weight parts of pigment brown were 1.5 parts, and the weight parts of solvent were 20 parts).

[0107] Comparative Example 2

[0108] The deodorizing cups of Comparative Example 2 were manufactured in the same manner as in Example 1, except that in step S10, a different ceramic coating was used instead of the modified ceramic coating (wherein the ceramic coating of Comparative Example 1 is a ceramic coating after polymethylsiloxane, silicic acid, titanium dioxide, pigment brown and solvent ripening, in which the weight parts of polymethylsiloxane are 4 parts, the weight parts of silicic acid are 40 parts, the weight parts of titanium dioxide are 15 parts, the weight parts of pigment brown are 1.5 parts, and the weight parts of solvent are 20 parts).

[0109] The non-stick properties of the deodorizing cups of the above-mentioned Examples 1-10 and Comparative Examples 1-2 were tested, and the test results are shown in Table 1 below.

[0110] Performance index test

[0111] The above-obtained deodorizing cups were subjected to performance tests, and the specific performance test methods are as follows:

[0112] (1) Odor test method:

[0113] 1. Brew coffee (15g coffee + 150ml water), pour out the coffee after soaking for a period of time, wash and smell it, and then continue soaking.

[0114] 2. Evaluation: Grade A (no odor); Grade B (slight odor, acceptable); Grade C (obvious odor, unacceptable);

[0115] 3. Test the odor every 1 hour and record the time it takes for the cup to reach Class C. The longer the time, the better the anti-odor effect.

[0116] (2) Cleanability test method:

[0117] 1. Wash the cups in the dishwasher for 5 consecutive times (each time for 1.5 hours).

[0118] 2. Spread the ketchup evenly on the bottom of the cup and leave it for 2 hours.

[0119] 3. Rinse with tap water and check for stains and stains that are difficult to clean.

[0120] 4. Evaluation method: Grade A (no difficult-to-clean stains and stains after rinsing); Grade B (there are difficult-to-clean stains, but no stains); Grade C (there are stains remaining).

[0121] 5. The above is one cycle. Record the number of cycles to reach Class C. The greater the number of cycles, the better the cleanability.

[0122] (3) Impact resistance test method: Use a 50g steel ball to drop freely from a certain height to hit the bottom of a water cup coated with a ceramic coating, and record the height at which the collapse occurs. The higher the height, the higher the coating strength.

[0123] Table 1 Test result record

[0124]

[0125] By comparing and analyzing the embodiments 1-10 and comparative examples 1-2 of the present invention, it can be known that compared with the cups with ceramic coatings formed by conventional ceramic coatings, the cups formed by the modified ceramic coatings including polymers of dimethylsiloxane and silicon dioxide, polymethylsiloxane and silicic acid according to the present application can be used for a long time without odor, and the user experience is good. In addition, the polymer of dimethylsiloxane and silicon dioxide in the modified ceramic coating can reduce the brittleness of the formed coating and can improve the bonding strength with the cup body, so that the overall strength of the cup is better. In addition, according to the modified ceramic coating of the present application, when zinc oxide is added, the anti-odor performance can be optimized while affecting the strength as little as possible.

[0126] Although the embodiments of the present application have been described in detail above, those skilled in the art may make various modifications and variations to the embodiments of the present application without departing from the spirit and scope of the present application. However, it should be understood that, in the opinion of those skilled in the art, these modifications and variations will still fall within the spirit and scope of the embodiments of the present application defined by the claims.

Claims

1. A modified ceramic coating, characterized in that: The modified ceramic coating is formed by ripening a mixed slurry including a polymer of dimethylsiloxane and silicon dioxide, polymethylsiloxane and silicic acid, wherein, in parts by weight, the weight of the polymethylsiloxane is 3 parts to 5 parts, the weight of the silicic acid is 20 parts to 35 parts, and the weight of the polymer of dimethylsiloxane and silicon dioxide is 20 parts to 35 parts.

2. The modified ceramic coating according to claim 1, characterized in that: The modified ceramic coating comprises a reaction product of dimethylsiloxane combined with a silicon dioxide polymer, polymethylsiloxane and silicic acid.

3. The modified ceramic coating according to claim 2, characterized in that: Based on the total weight of the modified ceramic coating being 100%, the weight of the reaction product in the modified ceramic coating accounts for 2.5%-8% of the total weight of the modified ceramic coating.

4. The modified ceramic coating according to claim 1, characterized in that: The mixed slurry also includes titanium dioxide, pigment brown and solvent, wherein, in parts by weight, the weight of the titanium dioxide is 10-20 parts, the weight of the pigment brown is 1-2 parts, and the weight of the solvent is 10-30 parts.

5. The modified ceramic coating according to any one of claims 1 to 4, characterized in that: The modified ceramic coating includes zinc oxide, and the weight ratio of the zinc oxide to the mixed slurry is (0.5-3):

100.

6. A method for preparing a modified ceramic coating, characterized in that: The method comprises: Forming a mixed slurry comprising a polymer of dimethylsiloxane and silicon dioxide, polymethylsiloxane and silicic acid, wherein in the mixed slurry, the weight portion of the polymethylsiloxane is 3 parts to 5 parts, the weight portion of the silicic acid is 20 parts to 35 parts, and the weight portion of the polymer of dimethylsiloxane and silicon dioxide is 20 parts to 35 parts; The mixed slurry is stirred and mixed to obtain a matured ceramic coating, thereby obtaining the modified ceramic coating.

7. The method according to claim 6, characterized in that The forming of a mixed slurry comprising a polymer of dimethylsiloxane and silicon dioxide, polymethylsiloxane and silicic acid comprises: The dimethylsiloxane and the polymer of silicon dioxide and silicic acid are mixed, and then the polymethylsiloxane is added to form a mixed slurry including the dimethylsiloxane and the polymer of silicon dioxide, polymethylsiloxane and silicic acid.

8. The method according to claim 6, characterized in that In the step of stirring and mixing the mixed slurry, the mixing temperature is controlled to be 20° C.-30° C., and the stirring and mixing time is 8 h-12 h.

9. The method according to claim 6, characterized in that The mixed slurry also includes titanium dioxide, pigment brown and solvent, wherein, in parts by weight, the weight of the titanium dioxide is 10-20 parts, the weight of the pigment brown is 1-2 parts, and the weight of the solvent is 10-30 parts.

10. The method according to any one of claims 6 to 9, characterized in that The method further comprises: Zinc oxide powder is added to the aged ceramic coating so that the zinc oxide powder is dispersed in the aged ceramic coating, thereby forming the modified ceramic coating.

11. The method according to claim 10, characterized in that The weight ratio of the zinc oxide powder to the aged ceramic coating is (0.5-3):

100.

12. A modified layer, characterized in that: The modified layer is formed by spraying the modified ceramic coating according to any one of claims 1 to 5, or by spraying the modified ceramic coating prepared by the method for preparing a modified ceramic coating according to any one of claims 6 to 11.

13. The modified layer according to claim 12, characterized in that: The thickness of the modified layer is 10 μm-30 μm, and / or the main component of the modified layer is a reaction product of a polymer of dimethylsiloxane and silicon dioxide, polymethylsiloxane and silicic acid.

14. A cup, characterized in that: The cup comprises a cup body and a modified layer formed on the inner wall surface of the cup body, wherein the modified layer is the modified layer according to claim 12 or 13.

Citation Information

Patent Citations

  • Coating solution for forming transparent silica coating film and method for producing transparent silica coating

    CA2402678A1

  • Ceramic coating with scratch resistance and thermal conduction properties

    CN103785601A

  • Preparation method of high temperature-resistant and fireproof waterborne nanocoating

    CN108441116A

  • Modified ceramic coating, composite coating, preparation methods of modified ceramic coating and composite coating, and cooker

    CN116082956A

  • Light glass ceramic anticorrosive paint for flue gas equipment as well as preparation method and application of light glass ceramic anticorrosive paint

    CN116731544A