Method for cooperatively controlling inclusion of sulfide and oxide in steel

By controlling the calcium line feeding amount, feeding speed, soft blowing flow rate and ladle side blowing during steelmaking, combined with alloying treatment and slag deoxidation treatment, the control problem of sulfide and oxide in steel is solved. Effective management of quantity and size has been achieved, and the quality of steel has been improved.

CN118910362AActive Publication Date: 2024-11-08SHOUGANG GROUP CO LTD +2
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202410819738.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-24
Publication Date
2024-11-08
Estimated Expiration
2044-06-24

AI Technical Summary

Technical Problem

The prior art is difficult to effectively coordinate the quantity and size of sulfide and oxide inclusions in steel, resulting in poor quality of steel.

Method used

Through the control of the calcium line feeding amount, feeding speed, soft blowing flow and ladle side blowing parameters during desulfurization pretreatment, converter smelting, LF refining, RH refining and casting, combined with alloying treatment and slag deoxidation treatment, we ensure that Generation and removal of MnS inclusion modification and Ca-Al-O inclusions.

Benefits of technology

The coordinated control of the inclusion of sulfide and oxide in steel is achieved, and the quantity density and size are within the controllable range, which improves the quality of the steel.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910362A_ABST
    Figure CN118910362A_ABST
Patent Text Reader

Abstract

The invention provides a method for cooperatively controlling inclusion of sulfide and oxide in steel, and belongs to the field of smelting. The method comprises the following steps: carrying out desulfurization pretreatment and slagging-off on molten iron to obtain desulfurized molten iron; the desulfurized molten iron is subjected to converter smelting, and converter molten steel is obtained; the converter molten steel is subjected to LF refining, alloying treatment and slag deoxidation treatment are conducted in the LF refining process, and first refined molten steel is obtained; the first refined molten steel is subjected to RH refining, the following parameters of RH refining are controlled: the calcium line feeding amount, the calcium line feeding speed, the soft blowing flow and the soft blowing time, and second refined molten steel is obtained; and the second refined molten steel is cast, steel ladle side blowing is conducted in the casting process, and a casting blank is obtained. The alloying operation is moved to LF refining, parameters of the RH refining process are controlled, and inert gas is laterally blown to a steel ladle in the later period of casting, so that the number and the size of sulfide and oxide inclusions in steel are cooperatively controlled.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of steelmaking, and in particular to a method for collaboratively controlling sulfide and oxide inclusions in steel. Background Art

[0002] The control of inclusions in steel has always been a key research topic in the field of iron and steel metallurgy, especially the control of non-metallic inclusions. In recent years, with the increasing requirements for high-quality steel production, inclusion control has become increasingly critical. According to the composition, inclusions are generally divided into sulfide inclusions (type A), alumina inclusions (type B), silicate inclusions (type C), spherical oxide inclusions (type D) and single-particle spherical inclusions (type Ds). Each type of inclusion has an adverse effect on the quality of steel, such as easily causing stress concentration in steel and causing fracture.

[0003] For most steel grades, sulfide inclusions and oxide inclusions have always been difficult to control. For the control of sulfide inclusions in steel, in addition to controlling the S content in raw materials and auxiliary materials, performing KR pretreatment and LF desulfurization, calcium treatment (calcium wire feeding) is usually used to modify the sulfides, mainly to convert the more harmful MnS inclusions into CaS inclusions. For the control of oxide inclusions in steel, Al-based or Si-Mn-based deoxidizers are mainly used for deoxidation; in addition, for hot-drying steel grades, calcium treatment is generally used to convert the high-melting-point Al 2 O 3 The inclusions are modified into low melting point Ca-Al-O inclusions to prevent nozzle blockage. Calcium treatment in the refining process is a common method to control sulfide and oxide inclusions. The practice of most steel mills shows that when the calcium feeding amount is small, MnS inclusions cannot be effectively controlled, while when the calcium feeding amount is large, Al 2 O 3 After inclusion modification, large-sized Ca-Al-O inclusions (>20μm) are often generated, which is not conducive to improving steel quality. To solve this problem, some steel mills have developed precise calcium treatment models, but the application effect is poor. Therefore, it is urgent to develop a method that can synergistically control sulfide and oxide inclusions in steel. Summary of the invention

[0004] The present application provides a method for collaboratively controlling sulfide and oxide inclusions in steel to solve the following technical problem: how to collaboratively control the number and size of sulfide and oxide inclusions in steel.

[0005] The present application provides a method for collaboratively controlling sulfide and oxide inclusions in steel, the method comprising:

[0006] The molten iron is subjected to desulfurization pretreatment and slag removal to obtain desulfurized molten iron;

[0007] The desulfurized molten iron is subjected to converter smelting to obtain converter molten steel;

[0008] The converter molten steel is subjected to LF refining, and alloying treatment and slag deoxidation treatment are performed during the LF refining process to obtain a first refined molten steel;

[0009] The first refined molten steel is subjected to RH refining, and the following parameters of the RH refining are controlled: calcium wire feeding amount, calcium wire feeding speed, soft blowing flow rate and soft blowing time, to obtain a second refined molten steel;

[0010] The second refined molten steel is cast, and during the casting process, the ladle is side-blown to obtain a cast billet.

[0011] Optionally, the value of the calcium wire feeding speed satisfies the following relationship:

[0012] V=2+(d 实测 -d min ) / (d max -d min )

[0013] Wherein, V represents the value of the calcium wire feeding speed, in m / s; d 实测 d max d min They respectively represent the actual thickness value, maximum thickness value and minimum thickness value in the ladle top slag thickness detection, both in mm.

[0014] Optionally, the soft blowing time is 6 minutes to 8 minutes, and the value of the soft blowing flow rate satisfies the following relationship:

[0015] L=0.5+(d 实测 -d min ) / 100

[0016] Wherein, L represents the value of the soft blowing flow rate, and the unit is NL / (min·t steel); d 实测 d min They respectively represent the actual thickness value and the minimum thickness value in the ladle top slag thickness detection, both in mm.

[0017] Optionally, the actual thickness value in the ladle top slag thickness detection is 50 mm to 120 mm.

[0018] Optionally, the ladle side blowing is performed during the casting process, including:

[0019] In the later stage of casting, the ladle is side-blown when the ladle is poured to 1 / 4. After the ladle slag detection system alarms, the ladle side-blowing is stopped. The ladle side-blowing uses inert gas, and the flow rate of the inert gas is 1.5NL / (min·t steel) ~ 2.0NL / (min·t steel).

[0020] Optionally, the raw material for the slag deoxidation treatment is aluminum particles, the amount of the aluminum particles added is 0.6kg / t·steel to 0.7kg / t·steel, and the aluminum particles are added in batches of 2 to 3 batches.

[0021] Optionally, the number of times of slag removal is ≥2 times, the total time of slag removal is ≤10 minutes, and the bright surface area of ​​the slag removal is ≥95%.

[0022] Optionally, the temperature of the molten iron is greater than 1330° C., and the [S] content in the molten iron is ≤0.06% by mass fraction; and the oxygen activity of the converter molten steel is ≤0.045%.

[0023] Optionally, the ladle containing the molten iron is an online turnover ladle with a ladle age ≥5 years.

[0024] Optionally, the number density of MnS inclusions and Ca-Al-O inclusions in the ingot is ≤ 0.30 / mm 2 , the size of the MnS inclusion is ≤6μm, and the size of the Ca-Al-O inclusion is ≤20μm.

[0025] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:

[0026] The present application provides a method for collaboratively controlling sulfide and oxide inclusions in steel, comprising: subjecting molten iron to desulfurization pretreatment and slag removal to obtain desulfurized molten iron; subjecting the desulfurized molten iron to converter smelting to obtain converter molten steel; subjecting the converter molten steel to LF refining, and performing alloying treatment and slag deoxidation treatment during the LF refining process to obtain a first refined molten steel; subjecting the first refined molten steel to RH refining, and controlling the following parameters of the RH refining: calcium wire feeding amount, calcium wire feeding speed, soft blowing flow rate and soft blowing time to obtain a second refined molten steel; casting the second refined molten steel, and performing ladle side blowing during the casting process to obtain a cast ingot. By moving alloying operations such as Ti adjustment to LF refining, the problem of alloy sulfur increase can be solved; by controlling the calcium wire feeding amount, feeding speed and soft blowing flow rate in the RH refining process, while ensuring the full modification of MnS inclusions, the generation and removal of large-sized Ca-Al-O inclusions can be controlled; by blowing inert gas from the ladle side in the late casting stage, the formation of vortexes can be controlled to solve the problem of excessive inclusions in steel caused by slag rolls. Thus, the number and size of sulfide and oxide inclusions in steel can be controlled in a coordinated manner. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.

[0028] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.

[0029] Figure 1 A schematic flow chart of a method for collaboratively controlling sulfide and oxide inclusions in steel provided in an embodiment of the present application;

[0030] Figure 2 A front view of a ladle side blowing structure provided in an embodiment of the present application;

[0031] Figure 3 A top view of a ladle side blowing structure provided in an embodiment of the present application. DETAILED DESCRIPTION

[0032] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.

[0033] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values ​​within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.

[0034] In addition, in the description of the specification of the present application, the terms "including", "comprising", etc. mean "including but not limited to". In this article, relational terms such as "first" and "second", etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. In this article, "and / or" describes the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. Wherein A and B can be singular or plural. In this article, "at least one" means one or more, and "plurality" means two or more. "At least one", "the following at least one item (items)" or similar expressions refer to any combination of these items, including any combination of single items (items) or plural items (items). For example, "at least one of a, b, or c", or "at least one of a, b and c", can both mean: a, b, c, ab (i.e. a and b), ac, bc or abc, where a, b, c can be single or plural, respectively.

[0035] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.

[0036] Figure 1 A schematic flow chart of a method for collaboratively controlling sulfide and oxide inclusions in steel provided in an embodiment of the present application.

[0037] See also Figure 1 The present application provides a method for collaboratively controlling sulfide and oxide inclusions in steel, the method comprising:

[0038] S1, pre-treating the molten iron for desulfurization and slagging to obtain desulfurized molten iron;

[0039] In some embodiments, the temperature of the molten iron is greater than 1330° C., and the [S] content in the molten iron is ≤0.06% by mass.

[0040] The positive effect of controlling the temperature of molten iron to be greater than 1330°C and the [S] content to be less than or equal to 0.06% is as follows: The thermodynamics of molten iron desulfurization shows that the higher the temperature, the higher the desulfurization rate. The molten iron temperature is controlled to be greater than 1330°C, thereby ensuring the desulfurization effect, controlling the lower [S] content of the molten iron entering the furnace after KR pretreatment, and reducing the desulfurization load of the converter and refining. Exemplarily, the temperature of the molten iron can be 1330°C, 1335°C, 1340°C, 1345°C, 1350°C, etc., and the [S] content can be 0.01%, 0.02%, 0.03%, 0.04%, 0.05%, 0.06%, etc.

[0041] In some embodiments, the number of times of slag removal is ≥ 2 times, the total time of slag removal is ≤ 10 min, and the bright surface area of ​​the slag removal is ≥ 95%.

[0042] The positive effects of controlling the number of slag removal to be ≥2 times, the total time of slag removal to be ≤10min, and the bright area of ​​slag removal to be ≥95% are as follows: controlling the number of slag removal after KR pretreatment can achieve the purpose of lowering the [S] content of the molten iron entering the furnace after KR pretreatment, and reduce the desulfurization load of the converter and refining. The purpose of controlling the slag removal time is to ensure the efficient connection between the KR pretreatment process and the converter process, and to avoid excessive temperature loss of the molten iron; controlling the bright area of ​​slag removal to be ≥95% can effectively reduce the amount of desulfurization slag entering the converter and reduce the subsequent desulfurization load. Exemplarily, the total time of slag removal can be 5min, 6min, 7min, 8min, 9min, 10min, etc., and the bright area of ​​slag removal can be 95%, 96%, 97%, 98%, etc.

[0043] In some embodiments, the number of times of skimming is 2 times.

[0044] In some embodiments, the ladle containing the molten iron is an online turnover ladle with a ladle age of ≥5 years.

[0045] It should be noted that ladle age refers to the number of online turnovers of the ladle between two adjacent maintenance periods. It can be understood that after the ladle is put online after maintenance, when it has been turned over 5 times, the ladle age is 5. The positive effect of controlling the ladle to be an online turnover ladle with a ladle age ≥ 5: the refractory materials of the ladle wall and the bottom of the new ladle with a ladle age < 5 generally have not reached the heat storage saturation. The use of such a ladle to hold the molten iron will cause a large temperature drop in the molten iron, which is not conducive to desulfurization; at the same time, the non-online turnover ladle with a ladle age ≥ 5 also has the above-mentioned problem. Exemplarily, the ladle of the molten iron can be an online turnover ladle with a ladle age of 5, 6, 7, 8, etc.

[0046] S2, subjecting the desulfurized molten iron to converter smelting to obtain converter molten steel;

[0047] In some embodiments, the oxygen activity of the converter molten steel is ≤0.045%.

[0048] The positive effect of controlling the oxygen activity of the converter steel liquid to ≤ 0.045% is that the oxygen content in the steel liquid is controlled at a lower level, which is conducive to controlling the generation of oxidized inclusions. For example, the oxygen activity of the converter steel liquid can be 0.020%, 0.025%, 0.030%, 0.035%, 0.040%, 0.045%, etc.

[0049] S3, subjecting the converter molten steel to LF refining, and performing alloying treatment and slag deoxidation treatment during the LF refining process to obtain a first refined molten steel;

[0050] In some embodiments, the raw material for the slag deoxidation treatment is aluminum particles, the amount of the aluminum particles added is 0.6kg / t·steel to 0.7kg / t·steel, and the aluminum particles are added in batches of 2 to 3 batches.

[0051] According to the steel grade composition requirements, alloying agents need to be added during the refining process, and the alloy usually contains a certain amount of S elements. If alloying is performed during the RH refining process, the S elements brought into the alloy are difficult to remove and are inherited into the ingot. The alloying operation is moved to LF refining. The desulfurization function of LF refining can effectively remove the S brought in. At the same time, LF refining produces reducing slag, which does not affect the yield of alloying elements. The same is true for the use of aluminum particles for deoxidation in LF refining. Exemplarily, the amount of aluminum particles added can be 0.6kg / t·steel, 0.62kg / t·steel, 0.64kg / t·steel, 0.66kg / t·steel, 0.68kg / t·steel, 0.7kg / t·steel, etc. The aluminum particles can be added to the slag surface in 2 or 3 batches.

[0052] S4, subjecting the first refined molten steel to RH refining, and controlling the following parameters of the RH refining: calcium wire feeding amount, calcium wire feeding speed, soft blowing flow rate and soft blowing time, to obtain a second refined molten steel;

[0053] In some embodiments, the calcium wire feeding amount in the RH refining process mainly depends on the composition of the molten steel. The calcium wire feeding amount is adjusted according to the [Mn] and [S] content in the molten steel. The higher the [Mn] and [S] content in the molten steel, the more calcium wire is fed.

[0054] In some embodiments, the value of the calcium wire feeding speed satisfies the following relationship:

[0055] V=2+(d 实测 -d min ) / (d max -d min )

[0056] Wherein, V represents the value of the calcium wire feeding speed, in m / s; d 实测 d max d min They respectively represent the actual thickness value, maximum thickness value and minimum thickness value in the ladle top slag thickness detection, both in mm.

[0057] In some embodiments, the value of the calcium wire feeding speed is rounded to one decimal place.

[0058] The calcium wire feeding process will inevitably cause liquid level fluctuations. The faster the feeding speed, the greater the liquid level fluctuations. When the ladle top slag is thicker, liquid level fluctuations are not likely to cause molten steel to be exposed. At this time, a faster feeding speed can be used; when the ladle top slag is thinner, liquid level fluctuations are likely to cause molten steel to be exposed. At this time, the feeding speed needs to be controlled at a lower level. By dynamically regulating the calcium wire feeding speed through the ladle top slag thickness, the secondary oxidation problem caused by the exposure of molten steel under liquid level fluctuations can be avoided, while taking into account the calcium feeding efficiency. It should be noted that the actual thickness value in the ladle top slag thickness detection is within the range of the minimum thickness and the maximum thickness. For example, the actual thickness value is 80mm, the minimum thickness and the maximum thickness are 50mm and 120mm respectively, then substituting into the above relationship, the calcium wire feeding speed is calculated to be 2.4m / s.

[0059] In some embodiments, the soft blowing time is 6 minutes to 8 minutes, and the value of the soft blowing flow rate satisfies the following relationship:

[0060] L=0.5+(d 实测 -d min ) / 100

[0061] Wherein, L represents the value of the soft blowing flow rate, and the unit is NL / (min·t steel); d 实测 d min They respectively represent the actual thickness value and the minimum thickness value in the ladle top slag thickness detection, both in mm.

[0062] Soft blowing after the calcium feeding line is completed can increase the diffusion rate of Ca element in molten steel and accelerate the floating removal of inclusions; usually the soft blowing time is controlled at 6min~8min, which can achieve the above effect without affecting the efficient connection between the refining process and the continuous casting process. When the ladle top slag is thin, even if the soft blowing flow rate is low, it can cause the liquid surface to be exposed, resulting in secondary oxidation; when the ladle top slag is thick, soft blowing is not easy to cause the liquid surface to be exposed, and the soft blowing flow rate can be appropriately increased to play its role in promoting the diffusion of Ca elements and accelerating the floating removal of inclusions. Therefore, it is of practical significance to dynamically control the soft blowing flow rate according to the ladle top slag thickness. It should be noted that the actual thickness value in the ladle top slag thickness detection is ≥ the minimum thickness value. For example, the soft blowing time can be 6min, 6.5min, 7min, 7.5min, 8min, etc. For example, the actual thickness value is 80mm and the minimum thickness value is 50mm. Substituting the above relationship, the soft blowing flow rate is calculated to be 0.8NL / (min·t steel).

[0063] In some embodiments, the actual thickness value in the ladle top slag thickness detection is 50 mm to 120 mm.

[0064] When the ladle top slag is thin, even if the calcium wire feeding speed is low, it can cause the liquid surface to be exposed, affecting the calcium feeding efficiency; when the ladle top slag is thick, the slag has a greater impact on the quality of the molten steel. Therefore, it is necessary to control the thickness of the ladle top slag. It should be noted that the actual thickness value is controlled in the range of 50mm to 120mm, that is, the maximum thickness can be 120mm, and the minimum thickness can be 50mm. Exemplarily, the actual thickness value can be 50mm, 60mm, 70mm, 80mm, 90mm, 100mm, 110mm, 120mm, etc.

[0065] S5. Casting the second refined molten steel, and performing side blowing of the ladle during the casting process to obtain a cast billet.

[0066] In some embodiments, the ladle side blowing is performed during the casting process, comprising:

[0067] In the later stage of casting, the ladle is side-blown when the ladle is poured to 1 / 4. After the ladle slag detection system alarms, the ladle side-blowing is stopped. The ladle side-blowing uses inert gas, and the flow rate of the inert gas is 1.5NL / (min·t steel) ~ 2.0NL / (min·t steel).

[0068] Figure 2 A front view of a ladle side blowing structure provided in an embodiment of the present application;

[0069] Figure 3 A top view of a ladle side blowing structure provided in an embodiment of the present application.

[0070] See the schematic diagram of the ladle side blowing structure for Figure 2 and 3 . In the later stage of casting, the vortex phenomenon of the molten steel in the ladle is obvious, which is easy to cause slag rolling. In order to prevent the problem of excessive inclusions caused by the vortex slag rolling in the later stage of casting, the ladle steel retention operation is usually adopted to control it, but it reduces the metal recovery rate and is not conducive to cost reduction and efficiency improvement. In the present application, when the ladle is poured to 1 / 4 in the later stage of casting, the side blowing of inert gas can effectively control the generation of vortex and control the side blowing flow rate. The generated side blowing airflow can interfere with the generation of vortex, thereby avoiding the problem of excessive inclusions in the steel caused by vortex slag rolling. Exemplarily, the flow rate of inert gas can be 1.5NL / (min·t steel), 1.6NL / (min·t steel), 1.7NL / (min·t steel), 1.8NL / (min·t steel), 1.9NL / (min·t steel), 2.0NL / (min·t steel), etc.

[0071] In some embodiments, the number density of MnS inclusions and Ca-Al-O inclusions in the ingot is ≤ 0.30 / mm 2, the size of the MnS inclusion is ≤6μm, and the size of the Ca-Al-O inclusion is ≤20μm.

[0072] This application reduces the subsequent refining and desulfurization load by controlling the molten iron [S] content, molten iron temperature, and degree of slag removal after KR desulfurization; moves alloying operations such as Ti adjustment to LF refining to solve the problem of alloy sulfur increase; controls the calcium wire feed amount, feed speed, and soft blowing flow rate during the RH refining process to ensure that the MnS inclusions are fully modified while controlling the generation and removal of large-sized Ca-Al-O inclusions; and blows inert gas from the ladle side in the later stage of casting to control the formation of vortices and solve the problem of excessive inclusions in the steel caused by slag rolling. Exemplarily, the number density of MnS inclusions and Ca-Al-O inclusions in the ingot can be 0.25 pcs / mm 2 , 0.26 pieces / mm 2 , 0.27 pieces / mm 2 , 0.28 / mm 2 , 0.30pcs / mm 2 The size of the MnS inclusions can be 4.00μm, 4.50μm, 5.00μm, 5.50μm, 6.00μm, etc., and the size of the Ca-Al-O inclusions can be 13.00μm, 14.00μm, 15.00μm, 16.00μm, 18.00μm, 20.00μm, etc.

[0073] It should be noted that the inclusion control method provided in this application is mainly applicable to medium and high carbon steels with a C content ≥ 0.25%.

[0074] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to industry standards. If there is no corresponding industry standard, then the conditions recommended by the manufacturer are followed.

[0075] The present application provides a method for collaboratively controlling sulfide and oxide inclusions in steel, comprising the following steps:

[0076] S11, performing desulfurization pretreatment and slag removal on the molten iron to obtain desulfurized molten iron; wherein the slag removal is performed twice;

[0077] S12, subjecting the desulfurized molten iron to converter smelting to obtain converter molten steel;

[0078] S13, subjecting the converter molten steel to LF refining, and performing alloying treatment and slag deoxidation treatment during the LF refining process to obtain a first refined molten steel; the raw material for the slag deoxidation treatment is aluminum particles, which are added to the slag surface in 2 to 3 batches;

[0079] S14, subjecting the first refined molten steel to RH refining, and controlling the following parameters of the RH refining: calcium wire feeding amount, calcium wire feeding speed, soft blowing flow rate and soft blowing time, to obtain second refined molten steel; the maximum thickness of the ladle top slag and the minimum thickness of the ladle top slag are controlled to be 120 mm and 50 mm respectively, and the thickness of the ladle top slag is ≥50 mm and ≤120 mm;

[0080] S15. Casting the second refined molten steel, and performing ladle side blowing during the casting process to obtain a cast ingot. The process parameters of the method for collaboratively controlling sulfide and oxide inclusions in steel are shown in Table 1.

[0081] Table 1 Process parameters of the method for collaboratively controlling sulfide and oxide inclusions in steel

[0082]

[0083] The application effect of the method of the present invention is characterized by the number density and size of MnS and Ca-Al-O inclusions in the ingot. The results of the embodiment and the comparative example are shown in Table 2.

[0084] Table 2 Comparison of the number density and size of MnS and Ca-Al-O inclusions in the ingots of the embodiments and comparative examples

[0085]

[0086]

[0087] It can be seen from Table 2 that the number density of MnS inclusions and Ca-Al-O inclusions in the ingot of the embodiment of the present application is controlled at 0.30 / mm 2 Within, meeting the quality control requirements, the maximum sizes of MnS inclusions and Ca-Al-O inclusions are controlled within 6μm and 20μm, respectively, meeting the quality control requirements. In Comparative Example 1, no side blowing was performed, resulting in the number density and maximum size of Ca-Al-O inclusions not meeting the quality control requirements. In Comparative Example 2, the calcium wire feed amount was small and the feeding speed was fast, resulting in the number density of MnS and Ca-Al-O inclusions and the maximum size of MnS inclusions not meeting the quality control requirements. In Comparative Example 3, the soft blowing flow rate was large, resulting in the number density and maximum size of Ca-Al-O inclusions not meeting the quality control requirements. In Comparative Example 4, the composition and temperature of the molten iron before KR pretreatment, the area of ​​the bright surface area after slagging, and the oxygen activity at the end of the converter were not controlled according to the method, and the number density of Ca-Al-O inclusions and the maximum size of MnS inclusions did not meet the quality control requirements.

[0088] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.

Claims

1. A method for collaboratively controlling sulfide and oxide inclusions in steel, characterized in that: The method comprises: The molten iron is subjected to desulfurization pretreatment and slag removal to obtain desulfurized molten iron; The desulfurized molten iron is subjected to converter smelting to obtain converter molten steel; The converter molten steel is subjected to LF refining, and alloying treatment and slag deoxidation treatment are performed during the LF refining process to obtain a first refined molten steel; The first refined molten steel is subjected to RH refining, and the following parameters of the RH refining are controlled: calcium wire feeding amount, calcium wire feeding speed, soft blowing flow rate and soft blowing time, to obtain a second refined molten steel; The second refined molten steel is cast, and during the casting process, the ladle is side-blown to obtain a cast billet.

2. The method according to claim 1, characterized in that The value of the calcium wire feeding speed satisfies the following relationship: V=2+(d 实测 -d min ) / (d max -d min ) Wherein, V represents the value of the calcium wire feeding speed, in m / s; d 实测 d max d min They respectively represent the actual thickness value, maximum thickness value and minimum thickness value in the ladle top slag thickness detection, both in mm.

3. The method according to claim 1, characterized in that The soft blowing time is 6 minutes to 8 minutes, and the value of the soft blowing flow rate satisfies the following relationship: L=0.5+(d 实测 -d min ) / 100 Wherein, L represents the value of the soft blowing flow rate, and the unit is NL / (min·t steel); d 实测 d min They respectively represent the actual thickness value and the minimum thickness value in the ladle top slag thickness detection, both in mm.

4. The method according to claim 2 or 3, characterized in that: The actual thickness value in the ladle top slag thickness detection is 50 mm to 120 mm.

5. The method according to claim 1, characterized in that The ladle side blowing is performed during the casting process, comprising: In the later stage of casting, the ladle is side-blown when the ladle is poured to 1 / 4. After the ladle slag detection system alarms, the ladle side-blowing is stopped. The ladle side-blowing uses inert gas, and the flow rate of the inert gas is 1.5NL / (min·t steel) ~ 2.0NL / (min·t steel).

6. The method according to claim 1, characterized in that The raw material for the slag deoxidation treatment is aluminum particles, the addition amount of the aluminum particles is 0.6kg / t·steel to 0.7kg / t·steel, and the aluminum particles are added in batches of 2 to 3 batches.

7. The method according to claim 1, characterized in that The number of scraping is ≥2 times, the total time of scraping is ≤10min, and the bright surface area of ​​the scraping is ≥95%.

8. The method according to claim 1, characterized in that The temperature of the molten iron is greater than 1330° C., and the [S] content in the molten iron is ≤0.06% by mass fraction; and the oxygen activity of the converter molten steel is ≤0.045%.

9. The method according to claim 1, characterized in that: The ladle for holding the molten iron is an online turnover ladle with a ladle age of ≥5 years.

10. The method according to claim 1, characterized in that The number density of MnS inclusions and Ca-Al-O inclusions in the ingot is ≤0.30 / mm 2 , the size of the MnS inclusion is ≤6μm, and the size of the Ca-Al-O inclusion is ≤20μm.

Citation Information

Patent Citations

  • Continuous casting production process for improving quality of free cutting steel casting blank

    CN102303108A

  • Calcium treatment method under special steelmaking process

    CN103614513A

  • Calcium treatment method for pipeline steel

    CN105506221A

  • Control technology for B-class inclusions of low-carbon low-sulfur pipeline steel

    CN106011377A

  • Magnesium adding process method for magnesium containing free-cutting steel

    CN110117694A