Smelting and rolling production method of low-temperature-resistant and corrosion-resistant composite functional steel bar
Through the smelting and rolling method of iron desulfurization-converter-LF refining-VD vacuum treatment-continuous casting-rolling, the problem of insufficient low temperature and corrosion resistance in buildings in extremely cold areas is solved, and the high yield strength of the steel bars is achieved , the improvement of tensile strength and low-temperature impact performance ensures the safety of the building structure under extreme conditions.
Patent Information
- Application Number
- CN202410978906.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-08
AI Technical Summary
The existing steel bars have insufficient low temperature resistance and corrosion resistance in buildings in extremely cold areas, resulting in an increase in the probability of brittle damage to the structure under extreme conditions and poses safety hazards.
The smelting and rolling production method is adopted for desulfurization of molten iron-converter-LF refining-VD vacuum treatment-continuous casting-rolling, through KR method, top-bottom reblowing decarbonization, LF furnace refining, constant pull speed continuous casting and high-pressure water Descaling and rolling processes such as controlling the chemical composition and rolling temperature of the steel bars, and improving their yield strength, tensile strength and low-temperature impact performance.
The yield strength of the steel bar Rp0.2≥425MPa, the tensile strength Rm≥560MPa, the elongation A≥20%, the uniform elongation Agt≥10%, the strong yield ratio Rm0/ReL0≥1.25, the flexion ratio ReL0/ReL≤1.30, -50℃ low-temperature impact performance Akv≥34J, meeting the composite functional requirements of low temperature and corrosion resistance.
Smart Images

Figure CN118910502A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of smelting and rolling processes, and in particular relates to a smelting and rolling production method for low-temperature-resistant and corrosion-resistant composite functional steel bars. Background Art
[0002] Reinforced concrete structures are often used in extreme conditions. Their working conditions are not only low temperature and corrosive environment, but also dynamic loads and caused by natural or technical reasons. Lower temperature and corrosive environment increase the probability of brittle failure of reinforced structures, causing accidents in building structures. Russian National Standard 5781, grade As-II steel bars are made of 10GT steel to improve product reliability. At present, grade A-1I1 (A400) steel bars made of 25G2S steel are used for cold-resistant materials. Under the condition of dynamic loads, unwelded (bound into frames and grids) steel bars can be used in an environment of not less than -50°C, and steel bars with welds can be used in an environment of not less than -40°C.
[0003] In China, Ma Steel and Nanjing Steel have mainly studied and applied steel bars for -165℃ storage tanks. Low-temperature steel bars are mainly used in various reinforced concrete structures of low-temperature storage tanks to support and reinforce the tanks. They also protect the tanks when low-temperature liquid leaks. They are not in direct contact with low-temperature liquids. The concept is completely different from that of general low-temperature steel (steel plates for low-temperature containers), and the performance requirements are also inconsistent. Low-temperature steel bars are mainly required to have higher strength and better toughness at low temperatures, especially higher defect sensitivity at low temperatures.
[0004] Domestic plates, H-shaped steel, rails and other materials are developing in the direction of high strength, low temperature resistance, corrosion resistance and other research directions, and requirements for low temperature resistance have also been put forward. However, domestic steel bars only have -165℃ storage tank steel bars. There is little research and development of steel bars for construction in extremely cold regions in China, and there is no application, which poses a great hidden danger to buildings in extremely cold regions. It is urgent to propose a smelting and rolling production method for low temperature resistant and corrosion resistant composite functional steel bars. Summary of the invention
[0005] The purpose of the present invention is to provide a smelting and rolling production method of low-temperature resistant and corrosion-resistant composite functional steel bars, solve the corrosion and low-temperature sensitivity problems of steel bars in concrete, realize the production of composite functional steel bars for concrete, and cope with extremely complex environments of steel bars.
[0006] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0007] The present invention discloses a smelting and rolling production method for low temperature resistant and corrosion resistant composite functional steel bars, the main preparation process of which is: hot metal desulfurization - converter - LF refining - VD vacuum treatment - continuous casting - rolling; wherein:
[0008] Hot metal desulfurization: before desulfurization, blast furnace slag is removed to improve desulfurization efficiency; iron ore is melted into hot metal, and the hot metal is desulfurized by KR method, that is, the hot metal is stirred by a stirring paddle at a speed of 85-95r / min, stirred for 2 minutes, and then a desulfurizer is added, stirred for reaction, and allowed to stand; after the hot metal is desulfurized and allowed to stand, the desulfurization slag is removed to stabilize the desulfurization effect, prevent the desulfurization slag from entering the converter and causing the converter to return to sulfur, and ensure that the sulfur content in the steel is controlled below 0.01%;
[0009] Converter: top and bottom combined blowing is used for decarburization and dephosphorization. Steel is tapped at 1650°C until the carbon content in the molten steel is less than 0.05% and the phosphorus content is less than 0.01%. During the tapping process, protective gas is used to stir the molten steel at a pressure of 0.5MPa. When the tapping is 1 / 4, ferrosilicon and silicon-manganese alloy are added for deoxidation, and carbon enhancer, coke and slag-making materials are added. A large amount of slag is prevented during tapping. At the same time, the protective gas pressure gradually decreases with the amount of steel tapped;
[0010] Refining: LF refining is adopted, deoxidation is carried out at 1575℃ until the oxygen content in the molten steel is 0.002%, and ferromanganese, nickel plate, ferrochrome, vanadium nitrogen alloy, ferroniobium alloy and copper plate are added. After refining, calcium iron alloy wire is fed, and the soft blowing time is ensured to be not less than 15 minutes;
[0011] Continuous casting: Try to ensure constant drawing speed for steel drawing, the drawing speed is controlled at 1.8-2.0m / min, and the slag protection uses a protective slag with a basicity of 1.2-1.4;
[0012] Rolling: heat the continuous casting billet to 1250±50℃, measure the temperature of the billet after it leaves the furnace at 1160±30℃, and then roll it after descaling with high-pressure water at a temperature of 1030±20℃. After rough rolling and intermediate rolling, control the final rolling temperature at 890±20℃. During the rolling process, the steel bars cannot be penetrated by water. Then, the billet is put on the cooling bed and enters the finishing and bundling process.
[0013] The chemical composition of the steel bar by mass percentage is: C: 0.09-0.12%, Si: 0.20-0.30%, Mn: 1.10-1.35%, P: ≤0.015%, S: ≤0.010%, Cu: 0.30-0.35%, Cr: 0.20-0.30%, Ni: 0.40-0.50%, V: 0.03-0.05%, Nb: 0.03-0.05%, La or Ce: 0.0010-0.0050%, and the balance is Fe and unavoidable impurity elements.
[0014] Furthermore, the properties of the steel bars after rolling meet the following requirements:p0.2 ≥425MPa, tensile strength R m ≥560MPa, elongation A≥20%, uniform elongation A gt ≥10%, strength-to-yield ratio R m 0 / R eL 0 ≥1.25, flexural ratio R eL 0 / R eL ≤1.30, -50℃ low temperature impact performance A kv ≥34J.
[0015] Furthermore, the desulfurizer is a mixture of lime powder and fluorite in a mass ratio of 9:1.
[0016] Furthermore, the cross-section of the ingot is 150 mm×150 mm, and the length of the ingot is 11.5 m.
[0017] Furthermore, the chemical composition of the steel bar by mass percentage is: C: 0.011%, Si: 0.25%, Mn: 1.25%, P: 0.012%, S: 0.003%, Cu: 0.32%, Cr: 0.24%, Ni: 0.43%, V: 0.036%, Nb: 0.034%, La or Ce: 0.0019%, and the remainder is Fe and unavoidable impurity elements.
[0018] Furthermore, the chemical composition of the steel bar by mass percentage is: C: 0.009%, Si: 0.29%, Mn: 1.27%, P: 0.010%, S: 0.005%, Cu: 0.33%, Cr: 0.27%, Ni: 0.47%, V: 0.039%, Nb: 0.038%, La or Ce: 0.0038%, and the remainder is Fe and unavoidable impurity elements.
[0019] Compared with the prior art, the beneficial technical effects of the present invention are:
[0020] After rolling, the steel bar meets the following requirements: yield strength R p0.2 ≥425MPa, tensile strength R m ≥560MPa, elongation A≥20%, uniform elongation A gt ≥10%, strength-to-yield ratio R m 0 / R eL 0 ≥1.25, flexural ratio R eL 0 / R eL ≤1.30, -50℃ low temperature impact performance A kv (-50℃)≥34J. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a metallographic structure photograph of a 400MPa grade low-temperature resistant and corrosion resistant composite functional steel bar. DETAILED DESCRIPTION
[0022] The present invention will be further described below in conjunction with the embodiments.
[0023] The chemical composition of the 400MPa grade low temperature resistant and corrosion resistant composite functional steel bar in this example is shown in Table 1. The main preparation process of the steel bar is: molten iron desulfurization - converter - LF refining - VD vacuum treatment - continuous casting - rolling. Molten iron desulfurization: remove blast furnace slag before desulfurization to improve desulfurization efficiency; take iron ore molten into molten iron, and the molten iron is desulfurized by the KR method, that is, the molten iron is stirred with a stirring paddle at a speed of 90r / min, and after stirring for 2 minutes, a desulfurizer is added. The desulfurizer is a mixture of lime powder and fluorite in a mass ratio of 9:1, and the reaction is stirred for 10 minutes and allowed to stand for 5 minutes. After the molten iron is desulfurized and allowed to stand, the desulfurization slag is removed to stabilize the desulfurization effect, prevent the desulfurization slag from entering the converter and causing the converter to return to sulfur, and ensure that the sulfur content in the steel is controlled below 0.01%. Converter: Use top and bottom combined blowing for decarburization and dephosphorization, smelt at 1650℃ until the carbon content in the molten steel is less than 0.05% and the phosphorus content is less than 0.01% before tapping. Use protective gas to stir the molten steel at a pressure of 0.5MPa during tapping. Add ferrosilicon and silicon-manganese alloy for deoxidation when the tapping is 1 / 4, add carburizer, coke and slag-making materials, prevent a large amount of slag during tapping, and the pressure of the protective gas gradually decreases with the amount of tapping. Refining: Use LF furnace refining, deoxidize at 1575℃ until the oxygen content in the molten steel is 0.002%, add ferromanganese, nickel plate, ferrochrome, vanadium-nitrogen alloy, ferroniobium alloy, and copper plate, feed calcium-iron alloy wire after refining, and ensure that the soft blowing time is not less than 15min. Continuous casting: Try to ensure constant pulling speed for steel drawing, the pulling speed is controlled at 1.9m / min, the cross section of the ingot is 150mm×150mm, the ingot length is 11.5m, and the protective slag uses a special protective slag for peritectic steel with a basicity of 1.2-1.4. Rolling: The specific rolling process is shown in Table 2. The continuous casting ingot is heated to 1250±50℃, the temperature is measured at 1160±30℃ after it is taken out of the furnace, and it is rolled after descaling with high-pressure water. The rolling temperature is 1030±20℃. After rough rolling and intermediate rolling, the final rolling temperature is controlled at 890±20℃. The steel bars cannot be penetrated by water during the rolling process, and then they are put on the cooling bed and enter the finishing and bundling process.
[0024] After the steel bar is offline, the mechanical properties are tested. The mechanical properties results are shown in Table 3. The test method is as follows:
[0025] The test was carried out in accordance with GB1499.2-2018 Steel for reinforced concrete Part 2: Hot-rolled ribbed steel bars. The test was carried out in accordance with the bending and reverse bending test methods in the national standard GB / T33953-2017 Corrosion-resistant steel bars for reinforced concrete. After the steel bars were bent 180° in the forward bending, no obvious cracks visible to the naked eye were found on the surface of the steel bars. The reverse bending was to bend the steel bars forward 90°, then keep them in a heating furnace at 100±20℃ for 30 minutes, conduct a reverse bending test after natural cooling, and then bend them in the reverse direction 20°. After the test, the steel bar surface was observed, and no obvious cracks visible to the naked eye were found.
[0026] Corrosion resistance test: The cyclic immersion corrosion test was carried out in accordance with YB / T 4368-2014 "Corrosion test method for steel bars in industrial atmospheric environment". The specimen was a 18mm×50mm cylinder, and the test solution was a sodium bisulfite solution with an initial concentration of (0.34±0.009) mol / L (mass fraction of 2.0%±0.05%). The specific test conditions were: temperature: 45℃±2℃; humidity: 70%±10%RH; test time: 72h; each cycle: 60min±2min; immersion time: 12min±2min; the highest surface temperature of the sample after baking: 70℃±10℃. The corrosion resistance test results are shown in Table 4.
[0027] Table 1 Chemical composition of 400MPa grade low temperature resistant and corrosion resistant composite functional steel bars
[0028]
[0029] Table 2 Rolling process of 400MPa grade low temperature resistant and corrosion resistant composite functional steel bars
[0030]
[0031] Table 3 Mechanical properties of 400MPa grade low temperature resistant and corrosion resistant composite functional steel bars
[0032] Specific Examples <![CDATA[R p0.2 / MPa]]> <![CDATA[R m / MPa]]> A% <![CDATA[A gt / %]]> <![CDATA[R m 0 / R eL 0 ]]> <![CDATA[R eL 0 / R eL ]]> Specific Example 1 481 689 25.0 14 1.43 1.20 Specific Example 2 467 697 27.0 16 1.49 1.17 Specific Example 3 434 674 26.0 18 1.55 1.09 Specific Example 4 439 635 25.0 17 1.45 1.10 Specific Example 5 472 682 23.0 16 1.44 1.18
[0033] Table 4 Corrosion test results of 400MPa grade low temperature resistant and corrosion resistant composite functional steel bars
[0034]
[0035] Table 5 Low temperature impact performance of 400MPa grade low temperature resistant and corrosion resistant composite functional steel bars
[0036]
[0037] The embodiments described above are only descriptions of the preferred embodiments of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A smelting and rolling production method for low temperature resistant and corrosion resistant composite functional steel bars, characterized in that: The main preparation process is: hot metal desulfurization - converter - LF refining - VD vacuum treatment - continuous casting - rolling; among which: Hot metal desulfurization: before desulfurization, blast furnace slag is removed to improve desulfurization efficiency; iron ore is melted into hot metal, and the hot metal is desulfurized by KR method, that is, the hot metal is stirred by a stirring paddle at a speed of 85-95r / min, stirred for 2 minutes, and then a desulfurizer is added, stirred for reaction, and allowed to stand; after the hot metal is desulfurized and allowed to stand, the desulfurization slag is removed to stabilize the desulfurization effect, prevent the desulfurization slag from entering the converter and causing the converter to return to sulfur, and ensure that the sulfur content in the steel is controlled below 0.01%; Converter: top and bottom combined blowing is used for decarburization and dephosphorization. Steel is tapped at 1650°C until the carbon content in the molten steel is less than 0.05% and the phosphorus content is less than 0.01%. During the tapping process, protective gas is used to stir the molten steel at a pressure of 0.5MPa. When the tapping is 1 / 4, ferrosilicon and silicon-manganese alloy are added for deoxidation, and carbon enhancer, coke and slag-making materials are added. A large amount of slag is prevented during tapping. At the same time, the protective gas pressure gradually decreases with the amount of steel tapped; Refining: LF refining is adopted, deoxidation is carried out at 1575℃ until the oxygen content in the molten steel is 0.002%, and ferromanganese, nickel plate, ferrochrome, vanadium nitrogen alloy, ferroniobium alloy and copper plate are added. After refining, calcium iron alloy wire is fed, and the soft blowing time is ensured to be not less than 15 minutes; Continuous casting: Try to ensure constant drawing speed for steel drawing, the drawing speed is controlled at 1.8-2.0m / min, and the slag protection uses a protective slag with a basicity of 1.2-1.4; Rolling: heat the continuous casting billet to 1250±50℃, measure the temperature of the billet after it leaves the furnace at 1160±30℃, and then roll it after descaling with high-pressure water at a temperature of 1030±20℃. After rough rolling and intermediate rolling, control the final rolling temperature at 890±20℃. During the rolling process, the steel bars cannot be penetrated by water. Then, the billet is put on the cooling bed and enters the finishing and bundling process. The chemical composition of the steel bar by mass percentage is: C: 0.09-0.12%, Si: 0.20-0.30%, Mn: 1.10-1.35%, P: ≤0.015%, S: ≤0.010%, Cu: 0.30-0.35%, Cr: 0.20-0.30%, Ni: 0.40-0.50%, V: 0.03-0.05%, Nb: 0.03-0.05%, La or Ce: 0.0010-0.0050%, and the balance is Fe and unavoidable impurity elements.
2. The smelting and rolling production method of low temperature resistant and corrosion resistant composite functional steel bars according to claim 1 is characterized in that: The properties of the steel bars after rolling meet the following requirements: yield strength R p0.2 ≥425MPa, tensile strength R m ≥560MPa, elongation A≥20%, uniform elongation A gt ≥10%, strength-to-yield ratio R m 0 / R eL 0 ≥1.25, flexural ratio R eL 0 / R eL ≤1.30, -50℃ low temperature impact performance A kv ≥34J.
3. The smelting and rolling production method of low temperature resistant and corrosion resistant composite functional steel bar according to claim 1 is characterized in that: The desulfurizer is lime powder and fluorite mixed in a mass ratio of 9:
1.
4. The smelting and rolling production method of low temperature resistant and corrosion resistant composite functional steel bars according to claim 1 is characterized in that: The cross section of the ingot is 150mm×150mm and the length of the ingot is 11.5m.
5. The smelting and rolling production method of low temperature resistant and corrosion resistant composite functional steel bar according to claim 1 is characterized in that: The chemical composition of the steel bar by mass percentage is: C: 0.011%, Si: 0.25%, Mn: 1.25%, P: 0.012%, S: 0.003%, Cu: 0.32%, Cr: 0.24%, Ni: 0.43%, V: 0.036%, Nb: 0.034%, La or Ce: 0.0019%, and the remainder is Fe and inevitable impurity elements.
6. The smelting and rolling production method of low temperature resistant and corrosion resistant composite functional steel bar according to claim 2 is characterized in that: The chemical composition of the steel bar by mass percentage is: C: 0.009%, Si: 0.29%, Mn: 1.27%, P: 0.010%, S: 0.005%, Cu: 0.33%, Cr: 0.27%, Ni: 0.47%, V: 0.039%, Nb: 0.038%, La or Ce: 0.0038%, and the remainder is Fe and unavoidable impurity elements.
Citation Information
Cited By
400MPa-grade low-temperature corrosion-resistant steel bar for frozen soil engineering and preparation method of low-temperature corrosion-resistant steel bar
CN121718804A