Passivator for solar cell, application of passivator and TopCon solar cell passivation method
By coating the passivating agent of polytetrafluoroethylene dispersion and metal oxide nanoparticles on the cutting surface of TopCon solar cells, the problems of edge damage and leakage current after laser cutting are solved, and the efficiency improvement and cost reduction are achieved.
Patent Information
- Application Number
- CN202410951459.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-15
AI Technical Summary
TopCon solar cells have severe cutting edge damage during laser cutting, resulting in large leakage current, the existing passivation technology is costly and complex, and cannot meet the requirements of cleanliness and efficiency.
The passivating agent is used for polytetrafluoroethylene dispersion and metal oxide nanoparticles (alumina and magnesium oxide). After laser cutting, the passivating agent is applied on the cutting surface. The passivation effect is used to reduce cutting damage and Leakage current to improve battery efficiency.
The leakage current at the cutting edge is reduced, the efficiency of the solar cell is improved, and the process is low, the process is simplified, and the operation is simple, avoiding the impact of high temperature on the battery efficiency.
Smart Images

Figure BDA0004948326910000121 
Figure BDA0004948326910000131
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of solar cells, in particular to a passivating agent for solar cells and application thereof and a TopCon solar cell passivation method. Background Art
[0002] TopCon solar cells need to be cut by laser during the preparation process of modules. Then the cut cell strips are connected to the positive and negative electrodes through welding strips to form a cell string. After processing the cell string, the cell module is finally formed. The laser cutting process will cause a certain degree of damage to the cell, resulting in a decrease in the efficiency of the cell.
[0003] In the existing passivation technology, the TopCon solar cells cut by laser lossless cutting generally use ALD technology to deposit aluminum oxide film on their cut surfaces, but the ALD equipment has high cost and maintenance costs, and it cannot provide special gas at the component end and cannot meet its cleanliness requirements. In addition, the ALD process takes a long time, and the high temperature during operation will also affect the efficiency of the cells to varying degrees. Therefore, the existing TopCon solar cells have cutting damage on the cutting edges after laser lossless cutting, and the leakage current of the cells at the cutting edges is large, affecting the efficiency of the cells. The existing passivation technology is costly and the process is complicated.
[0004] In view of this, the present invention is proposed. Summary of the invention
[0005] One of the purposes of the present invention is to provide a passivator for solar cells, the passivator for solar cells comprising the following components: polytetrafluoroethylene dispersion and metal oxide nanoparticles; wherein the metal oxide nanoparticles include at least one of aluminum oxide nanoparticles and magnesium oxide nanoparticles. Polytetrafluoroethylene has a good passivation effect, aluminum oxide nanoparticles have excellent thermal stability, and nano magnesium oxide has strong antioxidant and corrosion inhibition capabilities. The passivator for solar cells provided by the present invention is formed by adding metal oxide nanoparticles to the polytetrafluoroethylene dispersion, and has a good passivation effect, can reduce edge leakage current and improve battery efficiency.
[0006] The second object of the present invention is to provide an application of the solar cell passivator in passivating solar cells.
[0007] The third object of the present invention is to provide a TopCon solar cell passivation method. The TopCon solar cell passivation method comprises the following steps: applying the solar cell passivator to the cut surface of the cell strip after cutting to passivate the cell strip. The cell strip passivated with the passivator can passivate the exposed dangling bonds, reduce cutting damage, thereby reducing edge leakage current and improving cell efficiency.
[0008] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:
[0009] In a first aspect, the present invention provides a passivator for a solar cell, wherein the passivator for a solar cell comprises the following components:
[0010] polytetrafluoroethylene dispersion and metal oxide nanoparticles;
[0011] Wherein, the metal oxide nanoparticles include at least one of aluminum oxide nanoparticles and magnesium oxide nanoparticles.
[0012] In the present invention, the passivation agent component adopts polytetrafluoroethylene dispersion. The large binding energy of CF bond in polytetrafluoroethylene makes it have good heat resistance, and the physical and chemical properties of the passivation liquid components can be maintained in the subsequent drying process. In addition, the fluorine atoms are negatively charged, which effectively shields the positive charge of the main chain carbon atoms. At the same time, the negative charge they carry can form a negative electric field on the surface of the cutting surface, preventing electrons from flowing out of the cutting edge of the battery, increasing the parallel resistance and reducing the leakage current, and playing a good passivation role. In addition, the fluorine atoms are large in size and repel each other with the same charge, so that the molecular chain cannot be in a plane zigzag shape but in a spiral twisted shape. The complex molecular chain shape can protect the cutting surface of the battery. On the one hand, the complex molecular chain shape can also better wrap the aluminum oxide nanoparticles and magnesium oxide nanoparticles to prevent the agglomeration of the nanoparticles and maintain the stability of the passivation solution; nano-alumina has excellent thermal stability, outstanding chemical inertness and excellent electrical insulation properties. While maintaining the stability of the passivation organization, it can avoid the reduction of parallel resistance caused by the component manufacturing process and maintain the battery efficiency; nano-magnesium oxide has strong antioxidant and corrosion inhibition capabilities, which can protect the passivation solution from being oxidized during the drying process. At the same time, its excellent stability can avoid damage to the passivation organization during the component manufacturing process.
[0013] Preferably, the weight ratio of polytetrafluoroethylene to metal oxide nanoparticles is (2:1)-(1:1). In the present invention, the weight ratio of solute polytetrafluoroethylene to metal oxide nanoparticles in the dispersion can be, for example, 2:1, 1.5:1, 1:1, etc.
[0014] Preferably, the concentration of the polytetrafluoroethylene dispersion is 10%-30%, for example, it can be 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30%, etc.
[0015] Preferably, the polytetrafluoroethylene dispersion is synthesized by low-pressure dispersion polymerization.
[0016] In the present invention, a low-pressure dispersion polymerization method is adopted to prepare a polytetrafluoroethylene dispersion liquid. The prepared dispersion liquid has high film-forming property and good crack resistance, and has good repairing and passivation effects on cutting edges.
[0017] Preferably, the weight ratio of the aluminum oxide nanoparticles to the magnesium oxide nanoparticles is (1:1)-(3:1), for example, 1:1, 2:1, 3:1, etc.
[0018] Preferably, the particle size of the aluminum oxide nanoparticles is 10 nm to 30 nm, for example, 10 nm, 11 nm, 12 nm, 13 nm, 14 nm, 15 nm, 16 nm, 17 nm, 18 nm, 19 nm, 20 nm, 21 nm, 22 nm, 23 nm, 24 nm, 25 nm, 26 nm, 27 nm, 28 nm, 29 nm, 30 nm, etc.
[0019] Preferably, the particle size of the magnesium oxide nanoparticles is 10 nm to 30 nm, for example, 10 nm, 11 nm, 12 nm, 13 nm, 14 nm, 15 nm, 16 nm, 17 nm, 18 nm, 19 nm, 20 nm, 21 nm, 22 nm, 23 nm, 24 nm, 25 nm, 26 nm, 27 nm, 28 nm, 29 nm, 30 nm, etc.;
[0020] Preferably, the solid content of the passivator for solar cells is 20% to 40%, for example, it can be 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30%, 31%, 32%, 33%, 34%, 35%, 36%, 37%, 38%, 39%, or 40%.
[0021] In a second aspect, the present invention provides a use of the solar cell passivator in passivating a solar cell.
[0022] In a third aspect, the present invention provides a TopCon solar cell passivation method, the TopCon solar cell passivation method comprising the following steps:
[0023] The solar cell passivator is applied to the cut surface of the cut cell strip to passivate the cell strip.
[0024] In the present invention, a passivating agent is applied to the cut surface of the laminated battery strip to passivate the exposed dangling bonds and reduce cutting damage, thereby reducing edge leakage current and improving battery efficiency.
[0025] Preferably, the coating thickness of the passivator for solar cells is 0.05-0.2 mm, for example, it can be 0.05 mm, 0.06 mm, 0.07 mm, 0.08 mm, 0.09 mm, 0.1 mm, 0.11 mm, 0.12 mm, 0.13 mm, 0.14 mm, 0.15 mm, 0.16 mm, 0.17 mm, 0.18 mm, 0.19 mm, 0.2 mm, etc.
[0026] Preferably, the battery sheet is cut by laser to obtain a plurality of battery strips;
[0027] Preferably, a non-destructive laser process is used to cut the battery cells;
[0028] Preferably, the temperature of the cutting process is 150-250°C, for example, it can be 150°C, 160°C, 170°C, 180°C, 190°C, 200°C, 210°C, 220°C, 230°C, 240°C, 250°C, etc., and the power range is 5-50W, for example, it can be 5W, 10W, 15W, 20W, 25W, 30W, 35W, 40W, 45W, 50W, etc.;
[0029] Preferably, two ends of the battery cell are grooved relative to each other, and the groove length is 0-3 mm, for example, it can be 0 mm, 0.5 mm, 1 mm, 1.5 mm, 2 mm, 2.5 mm, 3 mm, etc.
[0030] In the present invention, a laser non-destructive cutting process is used to cut the battery cell, and grooves are formed at both ends of the battery cell along the thickness direction of the battery cell. The grooves at both ends are arranged opposite to each other, and laser heating is used between the two grooves, and then water is sprayed for cooling. The battery cell is split to form a battery strip. The present invention uses a laser non-destructive cutting method to cut the entire battery cell. The non-destructive cutting can cut a flat cutting surface, which can ensure the uniformity of subsequent liquid phase passivation liquid coating.
[0031] Preferably, the TopCon solar cell passivation method further comprises the following steps: before applying the passivating agent to the cell strips, laminating and pressing the cut cell strips;
[0032] In the present invention, the cut battery strips are laminated and pressurized before the passivation agent is coated, which can improve the coating efficiency and prevent the passivation liquid from penetrating into the front and back sides of the battery strips to affect the battery grid lines.
[0033] Preferably, during the lamination pressurization process, the applied pressure is greater than or equal to 200N, for example, it can be 200N, 250N, 300N, etc.;
[0034] Preferably, during the lamination and pressurization process, the number of battery strips is greater than or equal to 2, for example, it can be 2, 10, 50, 100, 150, 200, etc.
[0035] Preferably, the TopCon solar cell passivation method further comprises the following steps: drying the cell strip after the passivation agent is applied to obtain the passivated cell strip;
[0036] Preferably, the battery strip after applying the passivating agent is dried in a nitrogen atmosphere;
[0037] Preferably, the flow rate of the nitrogen is 10-15 L / min, for example, it can be 10 L / min, 11 L / min, 12 L / min, 13 L / min, 14 L / min, 15 L / min, etc.;
[0038] Preferably, the drying temperature is 80-100°C, for example, 80°C, 85°C, 90°C, 95°C, 100°C, etc.;
[0039] Preferably, the drying time is 1-3 min, for example, it can be 1 min, 1.5 min, 2 min, 2.5 min, 3 min, etc.
[0040] In the present invention, the battery strip coated with the passivator is dried at a certain temperature so as to be processed at the component end.
[0041] Furthermore, the TopCon solar cell passivation method comprises the following steps:
[0042] (1) Using laser non-destructive cutting to cut the entire cell to obtain a smooth cutting edge;
[0043] Among them, the temperature of laser non-destructive cutting process is 150-250℃, the power is 5-50W, and the length of the slots at both ends of laser non-destructive cutting is 0-3mm;
[0044] (2) Laminating and pressurizing the cut battery strips;
[0045] The number of battery strips in the lamination pressurization process is greater than or equal to 2, and the applied pressure is greater than or equal to 200N;
[0046] (3) applying a passivating agent to the cut surface of the laminated battery strip to passivate edge defects;
[0047] The components of the passivator are polytetrafluoroethylene dispersion and metal oxide nanoparticles, the metal oxide nanoparticles include at least one of aluminum oxide nanoparticles and magnesium oxide nanoparticles; the weight ratio of polytetrafluoroethylene to metal oxide nanoparticles is (2:1)-(1:1); the synthesis method of the polytetrafluoroethylene dispersion is low-pressure dispersion polymerization, and the concentration of the dispersion is 10%-30%; the particle size of the aluminum oxide nanoparticles and the magnesium oxide nanoparticles is 10nm-30nm, and the weight ratio of the two is (1:1)-(3:1); the solid content of the passivator is 20%-40%; the coating thickness of the passivation solution is 0.05-0.2mm;
[0048] (4) drying the battery strip coated with the passivating agent in a nitrogen atmosphere to obtain a repaired battery strip;
[0049] Among them, the nitrogen flow rate is 10-15L / min; the drying temperature is 80-100℃; and the drying time is 1-3min.
[0050] Compared with the prior art, the present invention has the following beneficial effects:
[0051] In the solar cell passivator provided by the present invention, polytetrafluoroethylene has good passivation effect, aluminum oxide nanoparticles have excellent thermal stability, and nano magnesium oxide has strong antioxidant and corrosion inhibition capabilities. The passivator is formed by adding metal oxide nanoparticles into a polytetrafluoroethylene dispersion, has strong passivation performance, can reduce edge leakage current, and improve battery efficiency.
[0052] The TopCon solar cell passivation method provided by the present invention adopts a method of directly coating a liquid phase passivation liquid on the cut surface of the TopCon solar cell to reduce cutting damage on the cut edge of the cell. In addition, the present invention does not require the addition of large-scale coating equipment, has low cost, simple operation, short process time, high production efficiency, and is not affected by high temperature during operation, so the passivation effect is better. DETAILED DESCRIPTION
[0053] Unless otherwise defined herein, scientific and technical terms used in conjunction with the present invention shall have the meanings commonly understood by those of ordinary skill in the art. The meaning and scope of the terms should be clear, however, in the case of any potential ambiguity, the definitions provided herein take precedence over any dictionary or external definitions. In this application, unless otherwise stated, the use of "or" means "and / or". In addition, the use of the term "including" and other forms is non-limiting.
[0054] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0055] The present invention is further described below by way of examples. Unless otherwise specified, the materials in the examples are prepared according to existing methods or directly purchased from the market.
[0056] Example 1
[0057] This embodiment provides a passivator for solar cells, whose components include polytetrafluoroethylene dispersion and aluminum oxide nanoparticles in a weight ratio of 2:1, the concentration of the polytetrafluoroethylene dispersion is 10%, and the synthesis method of the polytetrafluoroethylene dispersion is a low-pressure dispersion polymerization method; the particle size of the aluminum oxide nanoparticles is 10nm; and the solid content of the passivator for solar cells is 40%.
[0058] Example 2
[0059] The present embodiment provides a passivator for solar cells, the components of which include a polytetrafluoroethylene dispersion and magnesium oxide nanoparticles in a weight ratio of 1:1, the concentration of the polytetrafluoroethylene dispersion is 30%, and the synthesis method of the polytetrafluoroethylene dispersion is a low-pressure dispersion polymerization method; the particle size of the magnesium oxide nanoparticles is 30nm; and the solid content of the passivator for solar cells is 20%.
[0060] Example 3
[0061] The present embodiment provides a passivator for solar cells, the components of which include a polytetrafluoroethylene dispersion and metal oxide nanoparticles in a weight ratio of 1.5:1, wherein the metal oxide nanoparticles include aluminum oxide nanoparticles and magnesium oxide nanoparticles in a weight ratio of 1:1, the concentration of the polytetrafluoroethylene dispersion is 20%, and the synthesis method of the polytetrafluoroethylene dispersion is a low-pressure dispersion polymerization method; the particle size of the aluminum oxide nanoparticles and the magnesium oxide nanoparticles is 20nm; and the solid content of the passivator for solar cells is 30%.
[0062] Example 4
[0063] This embodiment provides a passivator for solar cells. The difference between this embodiment and embodiment 3 is that the metal oxide nanoparticles include aluminum oxide nanoparticles and magnesium oxide nanoparticles in a weight ratio of 3:1, and the rest is consistent with embodiment 3.
[0064] Example 5
[0065] This embodiment provides a passivator for solar cells. The difference between this embodiment and embodiment 3 is that the metal oxide nanoparticles include aluminum oxide nanoparticles and magnesium oxide nanoparticles in a weight ratio of 2:1, and the rest is consistent with embodiment 3.
[0066] Example 6
[0067] This embodiment provides a passivator for solar cells. The difference between this embodiment and embodiment 5 is that the weight ratio of polytetrafluoroethylene to metal oxide nanoparticles is 3:1, and the rest is consistent with embodiment 5.
[0068] Example 7
[0069] This embodiment provides a passivator for solar cells. The difference between this embodiment and embodiment 5 is that the weight ratio of polytetrafluoroethylene to metal oxide nanoparticles is 0.5:1, and the rest is consistent with embodiment 5.
[0070] Example 8
[0071] This embodiment provides a passivating agent for solar cells. The difference between this embodiment and embodiment 5 is that the concentration of the polytetrafluoroethylene dispersion is 35%, and the rest is the same as embodiment 5.
[0072] Example 9
[0073] This embodiment provides a passivating agent for solar cells. The difference between this embodiment and embodiment 5 is that the concentration of the polytetrafluoroethylene dispersion is 5%, and the rest is the same as embodiment 5.
[0074] Example 10
[0075] This embodiment provides a passivating agent for solar cells. The difference between this embodiment and embodiment 5 is that the particle sizes of aluminum oxide nanoparticles and magnesium oxide nanoparticles are both 50 nm, and the rest is consistent with embodiment 5.
[0076] Embodiment 11
[0077] This embodiment provides a passivating agent for solar cells. The difference between this embodiment and embodiment 5 is that the particle sizes of aluminum oxide nanoparticles and magnesium oxide nanoparticles are both 5 nm, and the rest is consistent with embodiment 5.
[0078] Example 12
[0079] This embodiment provides a passivating agent for solar cells. The difference between this embodiment and embodiment 5 is that the weight ratio of aluminum oxide nanoparticles to magnesium oxide nanoparticles is 1:2, and the rest is consistent with embodiment 5.
[0080] Example 13
[0081] This embodiment provides a passivator for a solar cell. The difference between this embodiment and embodiment 5 is that the solid content of the passivator for a solar cell is 45%, and the rest is the same as embodiment 5.
[0082] Embodiment 14
[0083] This embodiment provides a passivator for a solar cell. The difference between this embodiment and embodiment 5 is that the solid content of the passivator for a solar cell is 10%, and the rest is the same as embodiment 5.
[0084] Embodiment 15
[0085] This embodiment provides a passivator for solar cells. The difference between this embodiment and embodiment 5 is that the coating thickness of the passivation solution is 0.5 mm, and the rest is consistent with embodiment 5.
[0086] Example 16
[0087] This embodiment provides a passivator for solar cells. The difference between this embodiment and embodiment 5 is that the coating thickness of the passivation solution is 0.01 mm, and the rest is consistent with embodiment 5.
[0088] Embodiment 17
[0089] This embodiment provides a TopCon solar cell passivation method, comprising the following steps:
[0090] (1) Using laser non-destructive cutting to cut the entire cell to obtain a smooth cutting edge;
[0091] The laser non-destructive cutting process temperature is 150°C and the power is 50W. The laser non-destructively cuts the position of the battery to be cut to cut the battery sheet into battery strips.
[0092] (2) Laminating and pressurizing the cut battery strips;
[0093] Among them, the number of battery strips in the stacking pressurization process is 200, and the applied pressure is equal to 200N;
[0094] (3) applying the passivating agent in Example 5 to the cut surface of the laminated battery strip to passivate the edge defects;
[0095] Among them, the coating thickness of the passivating agent is 0.05mm;
[0096] (4) drying the battery strip coated with the passivating agent in a nitrogen atmosphere to obtain a repaired battery strip;
[0097] Among them, the nitrogen flow rate is 10L / min; the drying temperature is 100°C; and the drying time is 1min.
[0098] Embodiment 18
[0099] This embodiment provides a TopCon solar cell passivation method, comprising the following steps:
[0100] (1) Using laser non-destructive cutting to cut the entire cell to obtain a smooth cutting edge;
[0101] Among them, the temperature of the laser non-destructive cutting process is 250℃, the power is 5W, and the length of the slots at both ends of the laser non-destructive cutting is 3mm;
[0102] (2) Laminating and pressurizing the cut battery strips;
[0103] Among them, the number of battery strips in the stacking pressurization process is 250, and the applied pressure is equal to 250N;
[0104] (3) applying the passivating agent in Example 5 to the cut surface of the laminated battery strip to passivate the edge defects;
[0105] Among them, the coating thickness of the passivating agent is 0.2mm;
[0106] (4) drying the battery strip coated with the passivating agent in a nitrogen atmosphere to obtain a repaired battery strip;
[0107] Among them, the nitrogen flow rate is 15L / min; the drying temperature is 80°C; and the drying time is 3min.
[0108] Examples 19-34
[0109] This embodiment provides a TopCon solar cell passivation method, comprising the following steps:
[0110] (1) Using laser non-destructive cutting to cut the entire cell to obtain a smooth cutting edge;
[0111] Among them, the laser non-destructive cutting process temperature is 200℃, the power is 20W, and the length of the slots at both ends of the laser non-destructive cutting is 2mm;
[0112] (2) Laminating and pressurizing the cut battery strips;
[0113] Among them, the number of battery strips in the stacking pressurization process is 200, and the applied pressure is equal to 250N;
[0114] (3) The passivating agents in Examples 1-16 are respectively applied to the cut surfaces of the laminated battery strips to passivate the edge defects;
[0115] Among them, the coating thickness of the passivating agent is 0.1mm;
[0116] (4) drying the battery strip coated with the passivating agent in a nitrogen atmosphere to obtain a repaired battery strip;
[0117] Among them, the nitrogen flow rate is 11L / min; the drying temperature is 90°C; and the drying time is 2min.
[0118] Embodiment 35
[0119] This embodiment provides a TopCon solar cell passivation method, which differs from Embodiment 23 in that the nitrogen flow rate is 5 L / min, and the rest is consistent with Embodiment 23.
[0120] Embodiment 36
[0121] This embodiment provides a TopCon solar cell passivation method, which differs from Embodiment 23 in that the drying temperature is 150° C., and the rest is consistent with Embodiment 23.
[0122] Embodiment 37
[0123] This embodiment provides a TopCon solar cell passivation method, which differs from Embodiment 23 in that the drying time is 10 minutes, and the rest is consistent with Embodiment 23.
[0124] Comparative Example 1
[0125] This comparative example provides a passivating agent for solar cells, which differs from Example 5 in that its components do not contain metal oxide nanoparticles, and the rest is consistent with Example 5.
[0126] Comparative Example 2
[0127] This comparative example provides a passivator for solar cells, which differs from Example 5 in that its components do not contain polytetrafluoroethylene dispersion, and the rest are consistent with Example 5.
[0128] Comparative Examples 3-4
[0129] This comparative example provides a TopCon solar cell passivation method, in which the passivating agents in comparative examples 1-2 are respectively applied to the cut surfaces of the laminated cell strips to passivate the edge defects, and the remaining steps are consistent with Example 23.
[0130] Test Case
[0131] Test samples: TopCon solar cells passivated in Examples 17-34 and TopCon solar cells passivated in Comparative Examples 3-4.
[0132] Test method: The cut battery strips are spliced into complete battery sheets and tested in an IV test machine.
[0133] The test results are shown in Table 1.
[0134] Table 1
[0135]
[0136]
[0137] It can be seen from the data in Table 1 that, through the data in Examples 19-23, when aluminum oxide nanoparticles and magnesium oxide nanoparticles are used together, the efficiency of the battery cell is better; through Examples 24-37 and Comparative Examples 3-4, it can be seen that by using the passivator provided by the present invention and the relevant parameters in the passivation method provided by the present invention, the efficiency of the battery cell is better.
[0138] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A passivating agent for solar cells, characterized in that: The solar cell passivator comprises the following components: polytetrafluoroethylene dispersion and metal oxide nanoparticles; Wherein, the metal oxide nanoparticles include at least one of aluminum oxide nanoparticles and magnesium oxide nanoparticles.
2. The passivator for solar cells according to claim 1, characterized in that: The weight ratio of polytetrafluoroethylene and metal oxide nanoparticles is (2:1)-(1:1); Preferably, the concentration of the polytetrafluoroethylene dispersion is 10%-30%; Preferably, the polytetrafluoroethylene dispersion is synthesized by low-pressure dispersion polymerization.
3. The passivator for solar cells according to claim 1, characterized in that: The weight ratio of the aluminum oxide nanoparticles to the magnesium oxide nanoparticles is (1:1)-(3:1); Preferably, the particle size of the aluminum oxide nanoparticles is 10nm-30nm; Preferably, the particle size of the magnesium oxide nanoparticles is 10 nm-30 nm.
4. The passivator for solar cells according to claim 1, characterized in that: The solid content of the passivating agent for solar cells is 20%-40%.
5. Use of the solar cell passivator according to any one of claims 1 to 4 in passivating solar cells.
6. A TopCon solar cell passivation method, characterized in that: The TopCon solar cell passivation method comprises the following steps: The solar cell passivator according to any one of claims 1 to 4 is applied to the cut surface of the cell strip after cutting to passivate the cell strip.
7. The TopCon solar cell passivation method according to claim 6, characterized in that: The coating thickness of the solar cell passivator is 0.05-0.2 mm.
8. The TopCon solar cell passivation method according to claim 6, characterized in that: Using laser to cut the battery sheet to obtain several battery strips; Preferably, a non-destructive laser process is used to cut the battery cells; Preferably, the temperature of the cutting process is 150-250°C and the power range is 5-50W; Preferably, two ends of the battery cell are grooved relative to each other, and the groove length is 0-3 mm.
9. The TopCon solar cell passivation method according to claim 6, characterized in that: The TopCon solar cell passivation method further comprises the following steps: before applying a passivating agent to the cell strips, laminating and pressing the cut cell strips; Preferably, during the lamination pressurization process, the applied pressure is greater than or equal to 200N; Preferably, during the lamination and pressurization process, the number of battery strips is greater than or equal to 2.
10. The TopCon solar cell passivation method according to claim 6, characterized in that: The TopCon solar cell passivation method further comprises the following steps: drying the cell strip after the passivation agent is applied to obtain the passivated cell strip; Preferably, the battery strip after applying the passivating agent is dried in a nitrogen atmosphere; Preferably, the flow rate of the nitrogen is 10-15 L / min; Preferably, the drying temperature is 80-100°C; Preferably, the drying time is 1-3 min.
Citation Information
Patent Citations
Solar cell back sheet, preparation method thereof and solar cell
CN102956730A
Method for removing damage to solar cell slice
CN112490323A
Solar cell module production method and solar cell module
CN112786734A
Solar cell cutting surface polishing and passivating method and device
CN113903827A
Silicon heterojunction solar cell laser cutting and passivating method
CN117754158A