Phosphorus-antimony co-doping process method

By using a phosphorus-antimony co-doping process, combined with feed doping and equipment supplementation, the problem of resistivity uniformity in monocrystalline silicon rods was solved, achieving uniformity of resistivity at both ends and improving the production efficiency of silicon wafers.

CN118910724APending Publication Date: 2024-11-08包头美科硅能源有限公司 +1
View PDF 0 Cites 6 Cited by

Patent Information

Application Number
CN202410959998.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing technologies make it difficult to achieve consistent resistivity during phosphorus-antimony co-doping in the production of single-crystal silicon rods, resulting in large differences in resistivity between the beginning and end, which affects the efficiency of silicon wafers.

Method used

The phosphorus-antimony co-doping process is adopted, which combines feed doping and device-assisted doping to utilize the phosphorus and antimony metals to jointly compensate for resistivity, control the volatilization coefficient of antimony metal and the segregation coefficient of phosphorus metal, and ensure resistivity consistency.

Benefits of technology

This achieved a resistivity difference of less than 0.1Ω between the head and tail of a single-crystal silicon rod, thus improving the production efficiency of silicon wafers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004949992970000021
    Figure BDA0004949992970000021
  • Figure BDA0004949992970000051
    Figure BDA0004949992970000051
  • Figure FDA0004949992950000011
    Figure FDA0004949992950000011
Patent Text Reader

Abstract

The invention relates to the technical field of monocrystalline silicon manufacturing, in particular to a phosphorus-antimony co-doping process method. Comprising the steps of feeding doping and device supplementary doping. The step of feeding and doping refers to the step of feeding and doping during normal feeding of a coil base; the supplementary doping of the device is supplementary doping when the coil base is not charged; in the step of adding and doping, the doping amount of antimony metal and phosphorus metal is calculated according to the target resistance of the head, and then adding and doping are carried out; the supplementary doping of the device is that the supplementary doping amount of the antimony alloy is calculated according to a supplementary doping formula, and then a doping device is used for supplementary doping; according to the method, the resistivity consistency is realized through phosphorus and antimony doped metal common compensation, antimony metal dominates and influences the resistivity in the early stage, antimony metal volatilizes in the later stage and phosphorus metal resistance compensation, the resistivity difference between the head resistivity and the tail resistivity is 0.1 omega finally, and the silicon wafer efficiency is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of single crystal silicon manufacturing, and in particular to a phosphorus-antimony co-doping process method. Background Art

[0002] At present, the vast majority of single crystal N-type silicon rods on the market are pulled using phosphorus-doped crystal rods as the dopant. Since the segregation coefficient of phosphorus-doped crystal rods is 0.35<1 and the volatility is small, the resistivity distribution is high at the head and low at the tail. Although the segregation coefficient of the new antimony-doped crystal rods is 0.023<1, they are very volatile, resulting in the output crystal rod having low resistance at the head and high resistance at the tail. The resistivity of the crystal rods produced by the above two dopants has a large difference between the head and tail, and the resistivity consistency is poor, which affects the efficiency of the final silicon wafer.

[0003] Patent technical document CN202311131542.8 discloses a resistivity supplementary doping control method, including step 1, calculating the weight of dopants required for the target resistivity of the head, step 2, calculating the weight of dopants contained therein, and deducting the weight of dopants brought into the circulating material, step 3, calculating the volatilization and condensation of dopants, and obtaining the pre-doping constant, step 4, calculating the first resistance doping, step 5, obtaining the doping weight M after segmented calculation, step 6, obtaining the doping weight m in the raw material after graded calculation, step 7, according to the number of feedings RCZ given coefficient, step 8, according to the difference between the theoretical value and the output, formulate the correction amount. The invention can accurately calculate and correct the dopant loss according to factors such as differences in single crystal furnaces, different volatilization in different temperature ranges, and the influence of dopants brought into the circulating material, so as to ensure the resistance uniformity of the crystal output and avoid dopant loss or increase that affects the final resistance of the crystal. However, this supplementary doping method is not suitable for resistance compensation by phosphorus-antimony co-doping, because in the actual production process, the single crystal furnace has the phenomenon of difficult crystallization and multiple temperature adjustment and release. The temperature is relatively high during the temperature adjustment process, which will accelerate the volatilization of antimony metal and cause the resistivity to increase, and the resistivity consistency cannot be guaranteed. Summary of the invention

[0004] In view of this, the purpose of the present invention is to propose a phosphorus-antimony co-doping process method, through phosphorus-antimony doped metal joint compensation, the antimony metal mainly affects the resistivity in the early stage, the antimony metal volatilizes in the later stage, and the phosphorus metal resistance compensation achieves resistivity consistency. The final resistivity can achieve a head-tail resistivity difference of between 0.1Ω, thereby improving the efficiency of the silicon wafer.

[0005] Based on the above purpose, the present invention provides a phosphorus-antimony co-doping process method, including material adding and doping and device supplementary doping; the material adding and doping is doping when the furnace is normally charged; the device supplementary doping is doping when the furnace is not charged.

[0006] Furthermore, the doping is performed by first calculating the doping amount of antimony metal and phosphorus metal according to the target resistance of the head, and then doping.

[0007] Furthermore, the device performs supplementary doping by first calculating the supplementary doping amount of the antimony alloy according to a supplementary doping formula, and then using a doping device for supplementary doping.

[0008] The further doping formula is as follows:

[0009]

[0010] The residual material amount is the total weight of the residual material in the furnace when antimony alloy needs to be added after multiple releases, the total material input amount is the total weight added before the furnace is released, the supplementary doping coefficient is calculated based on the actual volatilization and segregation coefficients, and the initial antimony alloy is the weight of the antimony alloy added through the barrel before the furnace is released.

[0011] Furthermore, the supplementary doping coefficient is an empirical value. According to different thermal insulation and volatilization in different thermal fields, after actual measurement, the furnace is temperature-adjusted and released 1-3 times. The supplementary doping coefficient is between 10% and 30% to ensure the consistent output resistivity after supplementary doping.

[0012] Furthermore, during the doping, the antimony metal doping amount is 70%-80% of the head target resistance, and the phosphorus metal doping amount is 20%-30% of the head target resistance. In the early stage, the phosphorus, antimony and metals jointly reach the head target resistance. During the crystal pulling process, the antimony metal volatilizes severely, and the phosphorus metal segregation coefficient is 0.35<1. Therefore, as the crystal is pulled, the phosphorus metal doping concentration increases and the antimony metal concentration decreases. Overall, the dopant concentration in the crystal rod remains unchanged, and the resistivity consistency of the head and tail can be achieved.

[0013] Furthermore, the doping barrel number during the doping process requires the last barrel to be added in the middle of the barrel, the purpose of which is to reduce the time and temperature of doping the antimony alloy and ensure the consistency of resistance of different furnaces. In the process of melting materials in a single crystal furnace, the raw materials melt slowly from the outside to the inside, and the temperature of the melt is low in the center and high at the edge. The higher the temperature, the more serious the volatilization of the antimony alloy. Therefore, adding the doping position in the middle of the barrel can ensure that the antimony alloy is at the center of the material block during the melting process, with the lowest temperature, reduce the influence of the melt temperature on the volatilization of the antimony alloy, and thus ensure the consistency of the resistivity of the furnace.

[0014] Furthermore, when the last barrel of material is added and the main power is reduced before the temperature adjustment starts, the dry pump opening is adjusted from 100% to 40%-60%, and the furnace pressure is increased from 7-10torr to 15-20torr. The purpose is to reduce the volatilization of the doped antimony alloy when the last barrel of molten material is added and ensure the consistency of the resistance of different furnaces.

[0015] Furthermore, the last barrel is the last barrel to be charged into the single crystal furnace.

[0016] Furthermore, the doping device is used for supplementary doping every 1-3 times when the furnace is temperature-adjusted and released.

[0017] Furthermore, when the doping device is used to supplement the antimony alloy, the antimony alloy is required to be added into the furnace 5-10 minutes before temperature adjustment, and when the antimony alloy is added, the water cooling screen is at the highest position, 200-300 mm away from the molten silicon liquid surface.

[0018] Furthermore, the antimony alloy is added to the molten silicon liquid surface as solid metal. The molten silicon temperature is the highest during the temperature adjustment. In order to prevent the alloy from bursting due to a large difference between hot and cold and affecting the resistance, it is added 5-10 minutes before the temperature adjustment to reduce the temperature difference and prevent the antimony alloy from bursting.

[0019] Furthermore, the antimony alloy is added from the auxiliary chamber port using the supplementary doping device. Due to the influence of gravity, the addition of the antimony alloy will cause slight silicon splashing on the liquid surface. In order to prevent the splashing of silicon onto the water-cooling screen and affecting crystal pulling, the water-cooling screen must be in the highest position when the antimony alloy is added.

[0020] Beneficial effects of the present invention:

[0021] The phosphorus-antimony co-doping process provided by the present invention is used for resistance compensation, and the material doping method and the device supplementary doping method are adjusted together. In the early stage, the antimony metal mainly affects the resistivity, and in the later stage, the antimony metal volatilizes, and the phosphorus metal resistance compensation realizes the resistivity consistency. The final resistivity can achieve a head-tail resistivity difference of between 0.1Ω, thereby improving the efficiency of the silicon wafer. DETAILED DESCRIPTION

[0022] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments.

[0023] 1. Adding materials

[0024] (1) The total amount of material added is 950kg, and the target silicon wafer resistivity is 1.0. According to the national standard formula, the pure antimony metal doping amount is 24.67g, and the pure phosphorus doping amount is 482g (0.0025 phosphorus silicon alloy). Because this is phosphorus-antimony co-doping, the antimony metal is calculated as 70-80% of the target resistance, and the phosphorus metal is calculated as 20-30% of the target resistance. Calculated based on 70% antimony metal and 30% phosphorus metal, the antimony metal doping amount this time is 17.27g, and the phosphorus metal doping amount this time is 144g.

[0025] (2) Use an electronic scale to weigh out the corresponding antimony alloy and phosphorus alloy.

[0026] (3) Add 30kg of conventional re-feed material to the last bucket, stop adding material after adding and notify the dosing personnel to do the dosing. After the dosing is completed, add 20-30kg of conventional re-feed material on top to ensure that the alloy is added in the middle of the material block.

[0027] (4) Check the weight of added materials and the amount of additives added. After completion, the barrel will be sent to the site.

[0028] (5) Check the number of barrels to be added. Before the last barrel is added, the dry pump opening is changed from 100% to 50%. At this time, the pressure in the furnace changes from 7 torr to 16 torr. Confirm that the furnace pressure is appropriate. At this time, open the rotary valve to add material. After the addition is completed, the dry pump and furnace pressure remain unchanged until the material is mixed. When the temperature adjustment begins, the main power becomes low and then the dry pump opening and normal furnace pressure are restored.

[0029] 2. Supplementary doping device

[0030] The material is added normally, and the temperature is adjusted and released normally after the addition is completed. If the crystal rod is not produced after two temperature adjustments and releases, the crystal needs to be pulled again without adding material, and the supplementary doping device needs to be used for supplementary doping.

[0031] (1) Record the furnace number, the amount of remaining material in the furnace, the number of times the material was released, the time of adding the admixture, etc.

[0032] (2) The formula for calculating the amount of antimony alloy added is as follows:

[0033]

[0034] Due to the second release, the supplementary doping coefficient is calculated as 20%. According to the above formula, the alloy to be added this time is: 890 / 950*20%*17.27=3.23g

[0035] (3) Weigh the antimony alloy and send it to the production furnace in time. According to the process requirements, lift the water cooling screen to the upper limit. At this time, the water cooling screen is 250mm away from the molten silicon liquid surface. At this time, it is not allowed to increase the temperature for temperature adjustment. Put the antimony alloy into the supplementary doping device and complete the addition within 5 minutes.

[0036] (4) After the antimony alloy is added, the water cooling screen can be lowered and the temperature can be raised to adjust the temperature.

[0037] After testing, the final single crystal N-type silicon rod has a head resistance of 1.01Ω, a tail resistivity difference of 1.06Ω, and a final single crystal N-type silicon rod has a head resistivity difference of 0.05Ω.

[0038] Those skilled in the art should understand that the discussion of any of the above embodiments is merely illustrative and is not intended to imply that the scope of the present invention is limited to these examples. Under the concept of the present invention, the technical features in the above embodiments or different embodiments may be combined, the steps may be implemented in any order, and there are many other variations of the different aspects of the present invention as described above, which are not provided in detail for the sake of simplicity.

Claims

1. A phosphorus-antimony co-doping process, characterized in that: It includes material addition and device supplementary addition; the material addition refers to the addition when the furnace is normally added with material; the device supplementary addition refers to the supplementary addition when the furnace is not added with material; The doping step includes first calculating the doping amount of antimony metal and phosphorus metal according to the target resistance of the head, and then doping. The device supplementary doping comprises first calculating the supplementary doping amount of the antimony alloy according to the supplementary doping formula, and then using the doping device for supplementary doping; The doping formula is as follows: The residual material amount is the total weight of the residual material in the furnace when antimony alloy needs to be added after multiple releases, the total material input amount is the total weight added before the furnace is released, the supplementary doping coefficient is calculated based on the actual volatilization and segregation coefficients, and the initial antimony alloy is the weight of the antimony alloy added through the barrel before the furnace is released.

2. The phosphorus-antimony co-doping process according to claim 1, characterized in that: During the doping, the antimony metal doping amount is 70%-80% of the head target resistance, and the phosphorus metal doping amount is 20%-30% of the head target resistance.

3. The phosphorus-antimony co-doping process according to claim 1, characterized in that: The doping device is used for supplementary doping every 1-3 times when the furnace is temperature-adjusted and released.

4. The phosphorus-antimony co-doping process according to claim 1, characterized in that: When the doping device is used to supplement the antimony alloy, the antimony alloy is required to be added into the furnace 5-10 minutes before temperature adjustment, and when the antimony alloy is added, the water cooling screen is at the highest position, 200-300 mm away from the molten silicon liquid surface.

Citation Information

Cited By

  • Drawing method of silicon single crystal rod

    CN119265690A

  • Method for controlling resistivity of fifth main group element doped crystal bar

    CN119392360A

  • A method for controlling the resistivity of a Group V element-doped crystal rod

    CN119392360B

  • Method for controlling resistivity of N-type crystal bar by using phosphorus and antimony

    CN120797174A

  • Method for controlling resistivity of group v element-doped crystal ingot