Preparation method of LaOCl dielectric film based on rare earth oxychloride and construction method of LaOCl / MoS2 field effect transistor
LaOCl film was prepared by solution method and integrated with MoS2 to construct LaOCl/MoS2 field effect transistors, which solved the problems of large-area LaOCl film preparation and transistor integration, significantly improved the transistor performance and output characteristics of multi-layer MoS2, and achieved a flat film and the effect of high switching current.
Patent Information
- Application Number
- CN202411004563.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-08
AI Technical Summary
The prior art is difficult to achieve the preparation of large-area rare earth oxychloride LaOCl films and their effective integration in field effect transistors, resulting in a short channel effect after the transistor size is reduced, affecting the performance of electronic devices.
LaOCl dielectric film was prepared by solution method, and a flat LaOCl film was formed on the P-Si substrate through cleaning and spin coating technology, and integrated with multi-layer MoS2 single crystals to construct LaOCl/MoS2 field effect transistors, and electron beam lithography was used. Electrodes were prepared by thermal evaporation coating system.
The preparation of large-area LaOCl film and the construction of LaOCl/MoS2 field effect transistors are realized, which significantly regulates the output characteristics of multi-layer MoS2 and improves the performance of the transistor. Especially under the optimization conditions of temperature and precursor solution concentration, the film surface is uniform. The performance and switching current performance are significantly improved.
Smart Images

Figure CN118919413A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of field effect transistor devices, and in particular relates to a method for preparing a rare earth oxychloride LaOCl dielectric film and constructing a LaOCl / MoS2 field effect transistor. Background Art
[0002] In order to meet the ever-evolving technological demands and improve the performance of electronic devices (including speed, power consumption, and computing power), the size of traditional silicon-based field-effect transistors (FETs) is being reduced. However, this size reduction has also caused the so-called short channel effect, which is an undesirable phenomenon. It has been reported that the use of ultrathin channel materials and dielectric layers with high dielectric constants (κ) can effectively reduce the size of transistors. Integrating high-mobility two-dimensional (2D) semiconductor channels with ultrathin high-κ gate dielectrics in transistors is expected to alleviate the above effects. However, the subsequent manufacturing is hindered by the lack of suitable 2D high-κ gate dielectrics.
[0003] LaOCl has been proven to have wide bandgap and high dielectric constant properties and is considered to be a promising gate dielectric material. In recent years, reports have pointed out the potential for LaOCl to be used in next-generation electronic devices. The preparation of LaOCl reported so far is at the micrometer scale, and the preparation and application of large-area LaOCl films are relatively rare. Summary of the invention
[0004] In view of the above-mentioned deficiencies in the prior art, the present invention provides a method for preparing a LaOCl dielectric film based on rare earth oxychloride and constructing a LaOCl / MoS2 field effect transistor, so as to realize the preparation of large-area LaOCl, which is expected to promote the development of field effect transistors.
[0005] The present invention provides a method for preparing a rare earth oxychloride LaOCl dielectric film, comprising the following steps:
[0006] Step 1: Clean the substrate and place the P-Si <100> After the wafer is cut into 15mm*15mm squares, it is cleaned with deionized water, acetone, and anhydrous ethanol in turn, blown dry with N2, and cleaned with ultraviolet ozone.
[0007] Step 2: Dissolve LaCl3 hexahydrate in N,N-dimethylformamide (DMF) to obtain a transparent precursor solution.
[0008] Step 3: Coat the precursor solution obtained in step 2 on the substrate in step 1 and perform a pre-annealing treatment on a hot plate.
[0009] Step 4: After the pre-annealing in step 3, the film is quickly placed in a muffle furnace for secondary annealing to obtain a film.
[0010] In step 2, the concentration of the precursor solution is 0.2M-0.5M, such as 0.2M, 0.3M, 0.4M, 0.5M.
[0011] In step 3, the precursor solution obtained in step 2 is coated on the substrate in step 1 by spin coating, and the spin coating parameters are firstly spin coating at a low speed of 500 rpm for 5 seconds, and then spin coating at 4000 rpm for 20-30 seconds.
[0012] In step 3, the pre-annealing temperature is 150° C. and the time is 10 min.
[0013] In step 4, the temperature of the secondary annealing is 300° C.-600° C., and the time is 30 min-60 min.
[0014] The method for constructing the LaOCl / MoS2 field effect transistor of the present invention comprises the following steps:
[0015] Step 5: Use tape to mechanically exfoliate bulk single crystal MoS2 into multilayer (>3 layers) MoS2.
[0016] Step 6: Use a two-dimensional material transfer platform to transfer the MoS2 peeled off in step 4 to the LaOCl film obtained in step 4.
[0017] Step 7: Use electron beam lithography to expose the electrode pattern on the transferred MoS2.
[0018] Step 8: Prepare In-Au electrodes using an electron beam-thermal evaporation coating system.
[0019] The beneficial effects of the present invention are embodied in:
[0020] The present invention provides a method for preparing a LaOCl dielectric film and a method for constructing a LaOCl / MoS2 field effect transistor. The LaOCl dielectric film is prepared by a solution method. The film has no pinholes or hillocks and is relatively flat. After the LaOCl / MoS2 field effect transistor is constructed by using a P-Si substrate as a conductive gate to regulate the semiconductor MoS2 channel, the output characteristics of the multilayer MoS2 can be significantly regulated. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is the TGA diagram of the decomposition of LaCl3·6H2O in the present invention. TGA proves the decomposition process of LaCl3 hydrate, which will be transformed into LaOCl at 300-700℃.
[0022] Figure 2 The XRD pattern of the LaOCl film prepared in the present invention is shown in Figure 1. X-ray diffraction proves that the prepared film is LaOCl phase.
[0023] Figure 3 , Figure 4 The AFM images of the LaOCl thin film prepared in Example 1 of the present invention under different annealing conditions are as follows: morphology ( Figure 3 ); Roughness( Figure 4 ). When the temperature increases from 300℃ to 600℃, the film has the best surface uniformity at 400℃, and the roughness increases with the increase of temperature. This is because the thermal expansion mismatch between the Si substrate and the film causes the residual stress between the film and the substrate, which increases with the increase of temperature, so the film is rough.
[0024] Figure 5 , Figure 6 The transmittance diagram of LaOCl thin films prepared with different precursor solution concentrations in Example 2 of the present invention ( Figure 5 )、Tauc plot( Figure 6 ). The band gap of LaOCl film can be roughly estimated to be about 4.22 eV from the Tauc plot.
[0025] Figure 7 This is the XPS spectrum of La 3d of the LaOCl film prepared in Example 3 of the present invention. Figure 8 This is the XPS spectrum of O1s of the LaOCl film prepared in Example 3 of the present invention. Fig. 9 The XPS spectrum of Cl 2p of the LaOCl film prepared in Example 3 of the present invention is shown in Figure 3. The XPS spectrum proves that for the prepared LaOCl film, the peaks at 851.1 eV and 855.4 eV correspond to La 3d 3 / 2 states, while the other pair of peaks (834.2 eV and 838.4 eV) corresponds to the La 3d 5 / 2 The two peaks at ≈198.7 eV and ≈200.1 eV can be attributed to the spin-orbit phenomenon, corresponding to the Cl 2p 1 / 2 and Cl 2p 3 / 2 orbitals, which are consistent with the presence of metal chlorides. Cl 2p and La 4p 3 / 2 The binding energy ranges of the peaks show overlap, requiring the inclusion of an additional peak in the Cl 2p binding energy range. This additional peak corresponds to the La 4p at 195.5 eV. 3 / 2 The above findings confirm the existence of La-O and La-Cl.
[0026] Fig.10 This is a cross-sectional SEM image of the LaOCl film prepared on Si / SiO2 in Example 3 of the present invention. Fig.11This is the EDS spectrum of the LaOCl film prepared on Si / SiO2 in Example 3 of the present invention. From the cross-sectional SEM, it can be seen that the thickness of the LaOCl film is about 60nm, and the EDS spectrum confirms that the element ratio La:Cl=1:1.
[0027] Fig.12 Schematic diagram of the LaOCl / MoS2 FET device structure prepared in Examples 4 and 5 of the present invention.
[0028] Fig.13 a) Output characteristics and b) Transfer characteristics of the LaOCl / MoS2 FET device prepared in Example 4 of the present invention. The transfer curve shows that the LaOCl / MoS2 FET device prepared in Example 4 has a threshold voltage Vth = -1.24V, a subthreshold swing (SS) of up to 0.239V / dec, and a switching current of up to (I on / I off )=2.7×10 4 .
[0029] Fig.14 The transfer curves show that the LaOCl / MoS2 FET device prepared in Example 5 has a threshold voltage Vth = 0.54V, a subthreshold swing (SS) of up to 0.188V / dec, and a switching current of up to (I on / I off )=4.79×10 4 . DETAILED DESCRIPTION
[0030] In order to make the purpose, technical scheme and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. In addition, the technical features involved in each embodiment of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0031] The present invention provides a simple method for preparing LaOCl thin film, which can be used as a dielectric layer of a field effect transistor. On the other hand, it provides a method for preparing a field effect transistor using the thin film and multilayer MoS2 single crystal.
[0032] The specific implementation steps are as follows:
[0033] Step 1: Clean the substrate and place the heavily doped P-Si <100> After the wafer is cut into 15mm*15mm squares, it is cleaned in deionized water, acetone, and anhydrous ethanol in turn. After cleaning, it is blown dry with N2 and surface treated with ultraviolet ozone to improve hydrophilicity.
[0034] Step 2: Dissolve LaCl3·6H2O in N,N-dimethylformamide (DMF) and stir for 12 h using a magnetic stirring rotor to obtain a transparent and clear precursor solution;
[0035] Step 3: Coat the above solution on the substrate in step 1 and perform annealing on a heating plate.
[0036] Step 4: After the pre-annealing in step 3, the film is quickly placed in a muffle furnace for the next step of annealing to obtain a film.
[0037] Next is a method for preparing a LaOCl / MoS2 FET device based on LaOCl, comprising the following steps:
[0038] Step 5: Mechanically exfoliate bulk single crystal MoS2 into multilayer MoS2 using tape.
[0039] Step 6: Use a two-dimensional material transfer platform to transfer the MoS2 peeled off in step 4 to the prepared LaOCl film.
[0040] Step 7: Use electron beam lithography to expose the electrode pattern on the transferred MoS2.
[0041] Step 8: Prepare In-Au electrodes using an electron beam-thermal evaporation coating system.
[0042] The following describes it in detail through specific embodiments.
[0043] In the following embodiments, XRD represents X-ray diffraction test, AFM represents atomic force microscope test, SEM represents scanning electron microscope test, and XPS represents X-ray photoelectron spectroscopy test.
[0044] Embodiment 1:
[0045] According to the LaOCl film and preparation method thereof provided by the present invention:
[0046] 106 mg of LaCl3·6H2O crystals were dissolved in 1 mL of N,N-dimethylformamide (DMF) and stirred for 12 h by a magnetic stirring rotor to prepare a transparent and clear precursor solution with a concentration of 0.3 mol / L. The solution was filtered using a syringe and a 0.22 μm nylon filter.
[0047] Four cleaned and ozone-surface-treated P-Si substrates were used as substrates, and the substrates were fixed on a coater in turn. 100 μL of the precursor solution was dropped onto the substrates, and a thin film was obtained with spin coating parameters of 500 rpm, 5 s; 4000 rpm, 30 s.
[0048] The films were immediately removed, placed on a 150°C heating table for annealing for 10 min, then removed, and immediately placed in a muffle furnace at 300°C, 400°C, 500°C, and 600°C for annealing for 60 min.
[0049] The purpose of this embodiment is to test the AFM of thin films prepared at different annealing temperatures and analyze the phase information and surface roughness of the thin films.
[0050] Embodiment 2:
[0051] According to the LaOCl film and preparation method thereof provided by the present invention:
[0052] 106 mg, 141 mg, and 176 mg of LaCl3·6H2O crystals were respectively dissolved in 1 mL of N,N-dimethylformamide (DMF), and stirred for 12 h using a magnetic stirring rotor to prepare transparent and clear precursor solutions with concentrations of 0.3 mol / L, 0.4 mol / L, and 0.5 mol / L. The solution was filtered using a syringe and a 0.22 μm nylon filter.
[0053] Three cleaned and ozone-surface-treated glass sheets were used as substrates, and the substrates were fixed on a coating machine. 100 μL of the precursor solution was dropped onto the substrates respectively, and thin films were obtained with spin coating parameters of 500 rpm, 5 s; 4000 rpm, 30 s.
[0054] The film was immediately removed and placed on a 150°C heating table for annealing for 10 min, then removed and immediately placed in a 500°C muffle furnace for annealing for 60 min.
[0055] The purpose of this example is to test the transmittance and absorption spectrum of the thin film prepared from precursor solutions of different concentrations, and to obtain a Tauc plot based on the absorption spectrum to estimate its band gap.
[0056] Embodiment 3:
[0057] According to the LaOCl film and preparation method thereof provided by the present invention:
[0058] 106 mg of LaCl3·6H2O crystals were dissolved in 1 mL of N,N-dimethylformamide (DMF) and stirred for 12 h by a magnetic stirring rotor to prepare a transparent and clear precursor solution with a concentration of 0.3 mol / L. The solution was filtered using a syringe and a 0.22 μm nylon filter.
[0059] Take the cleaned and ozone-surface-treated Si / SiO2 as the substrate, fix the substrate on the spin coater in turn, take 100 μL of the precursor solution and drop it on the substrate, and obtain a thin film with the spin coating parameters of 500 rpm, 5 s; 4000 rpm, 30 s.
[0060] The films were immediately removed one by one, placed on a 150°C heating table for annealing for 10 min, then removed and immediately placed in a 500°C muffle furnace for annealing for 60 min.
[0061] The purpose of this embodiment is to test the XPS spectrum, SEM cross section and EDS spectrum of the prepared film and analyze the element information of the film.
[0062] Embodiment 4:
[0063] According to the LaOCl film and preparation method thereof provided by the present invention:
[0064] 106 mg of LaCl3·6H2O crystals were dissolved in 1 mL of N,N-dimethylformamide (DMF) and stirred for 12 h by a magnetic stirring rotor to prepare a transparent and clear precursor solution with a concentration of 0.3 mol / L. The solution was filtered using a syringe and a 0.22 μm nylon filter.
[0065] The cleaned and ozone-surface-treated P-Si substrate was fixed on a spin coater, 100 μL of the precursor solution was dropped onto the substrate, and a thin film was obtained with spin coating parameters of 500 rpm, 5 s; 4000 rpm, 30 s.
[0066] The film was immediately removed and placed on a 150°C heating table for annealing for 10 min, then removed and immediately placed in a 500°C muffle furnace for annealing for 60 min.
[0067] Bulk single crystal MoS2 was mechanically exfoliated into multilayer MoS2 using adhesive tape.
[0068] The exfoliated MoS2 was transferred to the prepared LaOCl film using a two-dimensional material transfer platform.
[0069] Electron beam lithography was used to expose the electrode pattern on the transferred MoS2.
[0070] In-Au was prepared using an electron beam-thermal evaporation coating system, where the In / Au electrode thickness was approximately 10nm / 50nm.
[0071] At this point, the preparation of LaOCl / MoS2 FET devices has been completed.
[0072] Embodiment 5:
[0073] According to the LaOCl film and preparation method thereof provided by the present invention:
[0074] 141 mg of LaCl3·6H2O crystals were dissolved in 1 mL of N,N-dimethylformamide (DMF) and stirred for 12 h by a magnetic stirring rotor to prepare a transparent and clear precursor solution with a concentration of 0.4 mol / L. The solution was filtered using a syringe and a 0.22 μm nylon filter.
[0075] The substrate is P-Si that has been cleaned and surface treated with ozone. The substrate is fixed on a spin coater, 100 μL of the precursor solution is dropped onto the substrate, and a thin film is obtained with spin coating parameters of 500 rpm, 5 s; 4000 rpm, 30 s.
[0076] The film was immediately removed and placed on a 150°C heating table for annealing for 10 min, then removed and immediately placed in a 500°C muffle furnace for annealing for 60 min.
[0077] The device preparation is consistent with Example 4.
Claims
1. A method for preparing a rare earth oxychloride LaOCl dielectric film, Features The steps include: Step 1: Clean the substrate and place the P-Si <100> After the wafer is cut into the required size, it is cleaned with deionized water, acetone, and anhydrous ethanol in sequence. 2 Blow dry and clean with UV ozone; Step 2: LaCl 3 The hexahydrate was dissolved in N, N-dimethylamide to obtain a transparent precursor solution; Step 3: coating the precursor solution obtained in step 2 on the substrate in step 1, and performing a pre-annealing treatment on a heating plate; Step 4: After the pre-annealing in step 3, the film is quickly placed in a muffle furnace for secondary annealing to obtain a LaOCl dielectric film.
2. The preparation method according to claim 1, Features: In step 2, the concentration of the precursor solution is 0.2M-0.5M.
3. The preparation method according to claim 1, Features: In step 3, the precursor solution obtained in step 2 is coated on the substrate in step 1 by spin coating, and the spin coating parameters are firstly spin coating at a low speed of 500 rpm for 5 seconds, and then spin coating at 4000 rpm for 20-30 seconds.
4. The preparation method according to claim 1, Features: In step 3, the pre-annealing temperature is 150° C. and the time is 10 min.
5. The preparation method according to claim 1, Features: In step 4, the temperature of the secondary annealing is 300° C.-600° C., and the time is 30 min-60 min.
6. LaOCl / MoS dielectric film prepared by the preparation method of any one of claims 1 to 5 2 Field Effect Transistor Method, Features: Mechanically exfoliated multilayer MoS was transferred using dry transfer 2 The single crystal was transferred to the LaOCl dielectric film and In-Au electrodes were prepared by electron beam lithography to obtain LaOCl / MoS 2 FET devices.