Positive electrode active material and preparation method thereof, positive electrode plate, battery and electric equipment
By optimizing the structural and interface stability of the positive electrode active material in the nickel-cobalt-manganese ternary layered material, the problem of degradation of battery performance caused by the reduction of cobalt element is solved, and higher circulation performance and safety performance are achieved.
Patent Information
- Application Number
- CN202411218275.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-08
AI Technical Summary
The decrease in the proportion of cobalt elements in nickel-cobalt-manganese ternary layered materials leads to the problem of decreasing the first charge and discharge efficiency of the battery, deteriorating the rate performance, deteriorating the cycle performance and increasing impedance.
A positive electrode active material is proposed. The characteristic peaks of (018) and (110) crystal planes in the XRD map are bimodal. By controlling the intensity ratio and position of the characteristic peaks, combined with the use of doped elements and cladding layers, the structure is improved. and interface stability to reduce the degree of Li/Ni mixed displacement.
It effectively improves the battery's cycle performance, first charge and discharge efficiency, discharge capacity and safety performance, while reducing the initial impedance and impedance increase.
Smart Images

Figure CN118919699A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the field of batteries, and specifically relates to a positive electrode active material and a preparation method thereof, a positive electrode sheet, a battery and an electrical device. Background Art
[0002] Lithium-ion batteries have become the main power source for portable electronic devices, electric vehicles and energy storage systems due to their high energy density, long cycle life and environmental friendliness. At present, the most widely used positive electrode materials for lithium-ion batteries on the market mainly include lithium cobalt oxide, nickel-cobalt-manganese ternary layered materials, lithium iron phosphate, lithium iron manganese phosphate and lithium manganese oxide spinel positive electrode materials. Among them, nickel-cobalt-manganese ternary layered materials are considered to be an ideal choice for lithium-ion battery positive electrode materials due to their high theoretical specific capacity (about 274mAh / g). However, the cobalt element has problems such as scarce resources, high prices and environmental pollution, so the research and development and application of low-cobalt or even cobalt-free positive electrode materials have received widespread attention.
[0003] In nickel-cobalt-manganese ternary layered materials, the reduction in the proportion of cobalt elements will lead to problems such as decreased initial charge and discharge efficiency of the battery, poor rate performance, deterioration of cycle performance, and increased impedance, which seriously restricts the promotion and application of low-cobalt and cobalt-free layered positive electrode materials. Summary of the invention
[0004] The present application aims to solve at least one of the technical problems in the related art to a certain extent. To this end, one purpose of the present application is to propose a positive electrode active material and a preparation method thereof, a positive electrode sheet, a battery and an electrical device to solve the problem that the reduction in the proportion of cobalt elements leads to a decrease in the initial charge and discharge efficiency of the battery, a deterioration in rate performance, a deterioration in cycle performance and an increase in impedance.
[0005] In one aspect of the present application, the present application proposes a positive electrode active material. According to an embodiment of the present application, the positive electrode active material includes:
[0006] In the XRD spectrum of the positive electrode active material, the characteristic peak C(018) corresponding to the (018) crystal plane of the positive electrode active material is distributed in a bimodal manner, including a first characteristic peak C(018) located at a small angle side. 1 (018) and the second characteristic peak C at the high angle side 2 (018);
[0007] The characteristic peak D(110) corresponding to the (110) crystal plane of the positive electrode active material is distributed in a bimodal manner, including a first characteristic peak D 1 (110) and the second characteristic peak D at the high angle side 2 (110);
[0008] I C1The first characteristic peak C corresponding to the (018) crystal plane of the positive electrode active material 1 The strength of (018), I D1 The first characteristic peak D corresponding to the (110) crystal plane of the positive electrode active material is represented by 1 The strength of (110) satisfies 0.80≤I D1 / I C1 ≤1.00.
[0009] According to the positive electrode active material of the embodiment of the present application, the structural stability and interface stability of the positive electrode active material are effectively improved, and the degree of Li / Ni mixing of the positive electrode material is effectively reduced, thereby effectively improving the cycle performance, initial charge and discharge efficiency, discharge capacity and safety performance of the battery, and effectively reducing the initial impedance and impedance increase of the battery.
[0010] In addition, the positive electrode active material according to the above embodiment of the present application may also have the following additional technical features:
[0011] In some embodiments of the present application, I C1 and I D1 Satisfy 0.85≤I D1 / I C1 ≤0.95.
[0012] In some embodiments of the present application, A C1 The first characteristic peak C corresponding to the (018) crystal plane of the positive electrode active material 1 The peak area of (018), A D1 The first characteristic peak D corresponding to the (110) crystal plane of the positive electrode active material 1 The peak area of (110) satisfies 0.80≤A D1 / A C1 ≤1.05, preferably, 0.85≤A D1 / A C1 ≤1.00.
[0013] In some embodiments of the present application, S C1 The first characteristic peak C corresponding to the (018) crystal plane of the positive electrode active material 1 (018) position, S D1 The first characteristic peak D corresponding to the (110) crystal plane of the positive electrode active material 1 (110) position, satisfying 0.35°≤S D1 -S C1 ≤0.65°, preferably, 0.40°≤S D1 -S C1 ≤0.60°.
[0014] In some embodiments of the present application, I C2 The second characteristic peak C corresponding to the (018) crystal plane of the positive electrode active material 2 The strength of (018), I D2 The second characteristic peak D corresponding to the (110) crystal plane of the positive electrode active material 2 The strength of (110) satisfies 1.77≤Ic1 / I C2 ≤1.98,1.78≤I D1 / I D2 ≤2.19, preferably, 1.80≤Ic1 / I C2 ≤1.95,1.80≤I D1 / I D2 ≤2.00.
[0015] In some embodiments of the present application, F C1 The first characteristic peak C corresponding to the (018) crystal plane of the positive electrode active material 1 The half-peak width of (018), F D1 The first characteristic peak D corresponding to the (110) crystal plane of the positive electrode active material 1 The half-peak width of (110) satisfies 0°<F C1 ≤0.20°, 0°<F D1 ≤0.20°, preferably, 0.05°≤F C1 ≤0.15°, 0.05°≤F D1 ≤0.15°.
[0016] In some embodiments of the present application, the positive electrode active material includes: a matrix, the matrix is a single crystal matrix, the matrix includes a chemical formula of Li a (Ni x Co y Mn z M b R c )O2 material, wherein 0.95≤a≤1.10, 0.50≤x≤0.95, 0≤y≤0.05, 0≤z≤0.45, 0≤b≤0.05, 0≤c≤0.03, and at least one of b and c is not equal to 0; M and R are both doping elements, and M and R are independently selected from at least one of B, Mg, Sr, Ba, Fe, Cu, Ni, Co, Mn, Sc, Y, La, Ce, Sm, Eu, Gd, Tb, Dy, Yb, Lu, Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, W, Ru, Rh, Ir, Zn, Al, Ga, In, Si, Pb, Cd, Ge, Sn, Sb, Bi and Te.
[0017] In some embodiments of the present application, the positive electrode active material further includes: a coating layer, and the coating layer is provided on at least a portion of the surface of the substrate.
[0018] In some embodiments of the present application, the coating layer includes a continuous coating layer and a coating protruding from the surface of the continuous coating layer, and the coating includes at least one of a point-shaped coating and an island-shaped coating.
[0019] In some embodiments of the present application, the continuous coating layer includes at least one of lithium cobalt oxide of Al, lithium cobalt oxide of W, lithium cobalt oxide of Zr, and lithium cobalt oxide of B; and / or the coating includes at least one of aluminum oxide, tungsten oxide, titanium oxide, boron oxide, strontium oxide, lithium oxide of Al, lithium oxide of W, lithium oxide of Ti, lithium oxide of B, and lithium oxide of Sr.
[0020] In the second aspect of the present application, the present application proposes a method for preparing the above-mentioned positive electrode active material, comprising:
[0021] Mixing a nickel-cobalt-manganese precursor, a first lithium source, and a first doping additive according to a stoichiometric ratio, and performing a first sintering to obtain a first sintered product;
[0022] The first sintered product, the second lithium source, and the optional second doping additive are mixed according to a stoichiometric ratio, and sintered for a second time to obtain a second sintered product;
[0023] The second sintered product and the coating agent are mixed and sintered for a third time to obtain a positive electrode active material.
[0024] According to the method for preparing the above-mentioned positive electrode active material in the embodiment of the present application, by adding lithium source in batches during two sinterings (i.e., adding a portion of lithium source in the first sintering, and adding another portion of lithium source in the second sintering), the formation of impurity phases in the process of preparing a single crystal matrix at high temperature and with excessive lithium source can be prevented, and the generation of microscopic stress can be reduced, so that the single crystallization of the matrix material is more complete. Doping additives are added in the two sinterings respectively, so as to obtain a structurally stable matrix material with both solid phase doping and surface doping, and the surface of the matrix material is coated to modify the surface interface of the matrix material. On the one hand, the direct contact between the positive electrode active material and the electrolyte can be effectively isolated, and the side reactions can be reduced, thereby effectively improving the electrochemical performance and safety performance of the battery. On the other hand, the ionic and electronic conductivity of the positive electrode material can be effectively improved, thereby effectively improving the discharge capacity and cycle performance of the battery.
[0025] In some embodiments of the present application, the first sintering includes a first heating stage and a first constant temperature stage, the heating rate of the first heating stage is 1°C / min~15°C / min, the temperature of the first constant temperature stage is 600°C~1000°C, and the time of the first constant temperature stage is 2h~20h; and / or, the second sintering includes a second heating stage, a third heating stage and a second constant temperature stage, the heating rate of the second heating stage is greater than the heating rate of the third heating stage, and the difference in heating rate between the second heating stage and the third heating stage is 1°C / min~5°C / min, the temperature of the second constant temperature stage is 600°C~1200°C, and the time of the second constant temperature stage is 2h~24h.
[0026] In some embodiments of the present application, the first doping additive is selected from at least one of an oxide and a hydroxide containing a doping element M; and / or, the second doping additive is selected from at least one of an oxide and a hydroxide containing a doping element R; and / or, the first lithium source includes lithium carbonate, the second lithium source includes lithium hydroxide, and the molar ratio of the first lithium source to the second lithium source is (30~90):(10~70).
[0027] In some embodiments of the present application, the mixing of the second sintered product and the coating agent and sintering for a third time includes the following steps: mixing the second sintered product and the first coating agent and sintering for a third time to obtain a third sintered product; mixing the third sintered product and the second coating agent and sintering for a fourth time to obtain a positive electrode active material.
[0028] In some embodiments of the present application, the third sintering includes a fourth heating stage and a third constant temperature stage, the heating rate of the fourth heating stage is 1°C / min to 15°C / min, the temperature of the third constant temperature stage is 500°C to 1000°C, and the time of the third constant temperature stage is 2h to 20h; and / or, the fourth sintering includes a fifth heating stage and a fourth constant temperature stage, the heating rate of the fifth heating stage is 1°C / min to 15°C / min, the temperature of the fourth constant temperature stage is 200°C to 800°C, and the time of the fourth constant temperature stage is 2h to 20h.
[0029] In some embodiments of the present application, the first coating agent is selected from at least one of oxides, hydroxides, carbonates containing Al, W, Zr or B; and / or, the second coating agent is selected from at least one of oxides, hydroxides, carbonates containing Al, W, Ti, B or Sr; and / or, the mass of the first coating agent is 0.01% to 2% of the mass of the second sintered product; and / or, the mass of the second coating agent is 0.01% to 2% of the mass of the third sintered product.
[0030] In a third aspect of the present application, the present application proposes a positive electrode sheet. According to an embodiment of the present application, the positive electrode sheet includes the positive electrode active material described in the first aspect of the present application.
[0031] In a fourth aspect of the present application, the present application provides a battery. According to an embodiment of the present application, the battery includes the positive electrode sheet described in the third aspect of the present application.
[0032] In a fifth aspect of the present application, the present application proposes an electric device. According to an embodiment of the present application, the electric device includes the battery described in the fourth aspect of the present application.
[0033] Additional aspects and advantages of the present application will be given in part in the description below, and in part will become apparent from the description below, or will be learned through the practice of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 is the XRD diagram of the low-cobalt layered positive electrode material of Example 3 and Comparative Example 4;
[0035] Figure 2 is the SEM image of Example 1 after four sinterings;
[0036] Figure 3 It is a graph of the cycle retention rate of batteries made from the low-cobalt layered positive electrode materials of Example 1, Example 3, Example 4, Example 7 and Comparative Example 1. DETAILED DESCRIPTION
[0037] Embodiments of the present application are described in detail below, and examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present application, and should not be construed as limiting the present application.
[0038] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0039] This application is proposed by the inventor based on the following issues:
[0040] The inventors found that in the nickel-cobalt-manganese ternary layered material, the reduction in the proportion of cobalt elements will lead to serious Li / Ni mixing of the positive electrode material, poor electronic conductivity, and slow lithium ion migration, which will lead to problems such as decreased initial charge and discharge efficiency of the battery, poor rate performance, deterioration of cycle performance, and increased impedance, which seriously restricts the promotion and application of low-cobalt and cobalt-free layered positive electrode materials. Therefore, how to eliminate the adverse effects of decobaltization on the structure and performance of the positive electrode material so that it can exert high energy density and continue to maintain good structural stability during the electrochemical cycle is a technical problem to be solved by this application.
[0041] In view of this, in one aspect of the present application, the present application proposes a positive electrode active material. According to an embodiment of the present application, the above-mentioned positive electrode active material has a specific structure. In the XRD spectrum of the above-mentioned positive electrode active material, the characteristic peak C(018) corresponding to the (018) crystal plane of the positive electrode active material is bimodal, including a first characteristic peak C(018) located at a small angle side. 1 (018) and the second characteristic peak C at the high angle side 2 (018); The characteristic peak D(110) corresponding to the (110) crystal plane of the positive electrode active material is distributed in a bimodal manner, including the first characteristic peak D 1 (110) and the second characteristic peak D at the high angle side 2 (110). C1 The first characteristic peak C corresponding to the (018) crystal plane of the positive electrode active material 1 The strength of (018), I D1 The first characteristic peak D corresponding to the (110) crystal plane of the positive electrode active material 1 The intensity of (110) is measured by XRD and the intensity ratio of the diffraction peak satisfies the following relationship: 0.80≤I D1 / I C1 ≤1.00. Due to the high activity of the (110) crystal plane of the positive electrode active material, excessive exposure of the (110) crystal plane can easily lead to an irreversible phase change of the positive electrode material during the cycle, from a layered structure to a spinel phase (space group Fd-3m), and then to a rock salt phase (space group Fm-3m), thereby deteriorating the cycle stability of the battery. D1 / I C1 ≤1.00 is controlled within the above range, which can appropriately reduce the exposure of the active crystal surface, effectively inhibit the side reaction between the positive electrode material and the electrolyte and the surface phase change, thereby effectively improving the cycle stability of the positive electrode material under high pressure. Preferably, 0.85≤I D1 / I C1≤0.95. The present application effectively improves the structural stability and interface stability of the positive electrode active material, and also effectively reduces the degree of Li / Ni mixing of the positive electrode material, thereby effectively improving the cycle performance, initial charge and discharge efficiency, discharge capacity and safety performance of the battery, and also effectively reducing the initial impedance and impedance increase of the battery.
[0042] According to some specific embodiments of the present application, S C1 The first characteristic peak C corresponding to the (018) crystal plane of the positive electrode active material 1 (018) position, S D1 The first characteristic peak D corresponding to the (110) crystal plane of the positive electrode active material 1 (110) position, satisfying 0.35°≤S D1 -S C1 ≤0.65°. The greater the degree of splitting of the characteristic peak C(018) corresponding to the (018) crystal plane of the positive electrode active material and the characteristic peak D(110) corresponding to the (110) crystal plane, the more obvious the layered characteristics of the positive electrode material are and the lower the degree of Li / Ni mixing. The present application controls the degree of splitting of the characteristic peak C(018) and the characteristic peak D(110) to 0.35°≤S D1 -S C1 ≤0.65°, a layered positive electrode material with high capacity and excellent cycle performance can be obtained. Preferably, 0.40°≤S D1 -S C1 ≤0.60°.
[0043] According to some further specific embodiments of the present application, A C1 The first characteristic peak C corresponding to the (018) crystal plane of the positive electrode active material 1 The peak area of (018), A D1 The first characteristic peak D corresponding to the (110) crystal plane of the positive electrode active material 1 The peak area of (110) and the area ratio of the diffraction peak measured by XRD satisfy the following relationship: 0.80≤A D1 / A C1 ≤1.05. Due to the high activity of the (110) crystal plane of the positive electrode active material, excessive exposure of the (110) crystal plane can easily lead to irreversible phase change of the positive electrode material during the cycle, from the layered structure to the spinel phase (space group Fd-3m), and then to the rock salt phase (space group Fm-3m), thereby deteriorating the cycle stability of the battery. D1 / A C1≤1.05 is controlled within the above range, which can further reduce the exposure of the active crystal surface, further effectively inhibit the side reaction between the positive electrode material and the electrolyte and the surface phase change, thereby further effectively improving the cycle stability of the positive electrode material under high pressure. Preferably, 0.85≤A D1 / A C1 ≤1.00.
[0044] According to some further specific embodiments of the present application, C2 The second characteristic peak C corresponding to the (018) crystal plane of the positive electrode active material 2 The strength of (018), I D2 The second characteristic peak D corresponding to the (110) crystal plane of the positive electrode active material 2 The strength of (110) satisfies 1.77≤Ic1 / I C2 ≤1.98,1.78≤I D1 / I D2 ≤2.19. The second characteristic peak C 2 (018) and D 2 (110) comes from the diffraction peak caused by multiphase. If C 2 (018) and D 2 If the ratio of (110) is too high, it will easily lead to a decrease in the capacity, initial efficiency and cycle characteristics of the battery. 2 (018) and D 2 When the ratio of (110) is too low, the crystallinity of the positive electrode active material is poor, which will also cause the performance of the manufactured battery, such as cycle and DCR increase, to deteriorate. The inventors have found that by 1 (018) and the second characteristic peak C 2 (018) intensity ratio and the first characteristic peak D 1 (110) and the second characteristic peak D 2 The intensity ratio of (110) is within the specified range, and the positive electrode active material exhibits good battery performance. Preferably, 1.80≤Ic1 / I C2 ≤1.95,1.80≤I D1 / I D2 ≤2.00.
[0045] According to some further specific embodiments of the present application, F C1 The first characteristic peak C corresponding to the (018) crystal plane of the positive electrode active material 1 The half-peak width of (018), F D1 The first characteristic peak D corresponding to the (110) crystal plane of the positive electrode active material 1 The half-peak width of (110) satisfies 0°<F C1 ≤0.20°, 0°<FD1 ≤0.20°. The smaller the grain size, the larger the half-peak width of the diffraction peak. Therefore, this application defines 0°<F C1 ≤0.20°, 0°<F D1 ≤0.20°, which can effectively eliminate randomly oriented grain boundaries, reduce the contact area between the positive electrode material and the electrolyte, and obtain higher mechanical strength, which can effectively inhibit the generation of particle microcracks and harmful surface phase changes / side reactions, thereby helping to improve the cycle stability of the battery. Preferably, 0.05°≤F C1 ≤0.15°, 0.05°≤F D1 ≤0.15°.
[0046] Half-peak width: is the straight-line distance from the half-peak point on one side of the peak to the half-peak point on the other side. Half-peak intensity: is half of the peak intensity. Peak intensity: is the top or highest intensity point of the peak.
[0047] According to some specific embodiments of the present application, the above-mentioned positive electrode active material includes: a matrix, the matrix is a single crystal matrix, and the matrix includes a chemical formula of Li a (Ni x Co y Mn z M b R c)O2 material, wherein 0.95≤a≤1.10 (as an example a can be 0.95 / 1.00 / 1.05 / 1.10, etc.), 0.50≤x≤0.95 (as an example x can be 0.50 / 0.60 / 0.70 / 0.80 / 0.90 / 0.95, etc.), 0≤y≤0.05 (as an example y can be 0 / 0.01 / 0.02 / 0.03 / 0.04 / 0.05), 0≤z≤0.45 (as an example z can be 0 / 0.05 / 0.10 / 0.20 / 0.30 / 0.40 / 0.45), 0≤b≤0.05 (as an example b can be 0 / 0.01 / 0 .02 / 0.03 / 0.04 / 0.05), 0≤c≤0.03 (as an example c can be 0 / 0.01 / 0.02 / 0.03), and at least one of b and c is not equal to 0; M and R are both doping elements, and M and R are independently selected from at least one of B, Mg, Sr, Ba, Fe, Cu, Ni, Co, Mn, Sc, Y, La, Ce, Sm, Eu, Gd, Tb, Dy, Yb, Lu, Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, W, Ru, Rh, Ir, Zn, Al, Ga, In, Si, Pb, Cd, Ge, Sn, Sb, Bi and Te. Thus, the single crystal matrix includes doping elements M and R, thereby obtaining a structurally stable matrix material with both phase doping and surface doping, which can effectively improve the structural stability and interface stability of the positive electrode active material, and at the same time reduce the degree of Li / Ni mixing of the positive electrode material, thereby effectively improving the cycle performance, discharge capacity and safety performance of the battery.
[0048] According to some preferred embodiments of the present application, 1.00≤a≤1.05, 0.60≤x≤0.80, 0≤y≤0.03, 0.05≤z≤0.30, 0.01≤b≤0.03, 0≤c≤0.02, x+y+z+b+c=1.
[0049] According to some further preferred embodiments of the present application, M and R are different, and M is selected from at least one of B, Mg, Fe, Cu, Ni, Co, Mn, Sc, Ti, Zr, Cr, Zn, Al, Ga, In, Si, Pb, Ge, Sn and Sb, and more preferably at least one of B, Mg, Ti, Zr, Zn, Al, Si. R is selected from at least one of Sr, Ba, Y, La, Ce, Sm, Eu, Gd, Tb, Dy, Yb, Lu, Hf, V, Nb, Ta, Mo, W, Ru, Rh, Ir, Cd, Bi and Te, and more preferably at least one of Sr, Ba, Y, La, Al, Nb, Ta, Mo, W. The above-mentioned doping elements M and R can further effectively improve the structural stability and interface stability of the positive electrode active material, and at the same time can further reduce the degree of Li / Ni mixing of the positive electrode material, thereby further effectively improving the cycle performance, discharge capacity and safety performance of the battery.
[0050] According to some other specific embodiments of the present application, the positive electrode active material further includes: a coating layer, which is disposed on at least part of the surface of the substrate. Thus, the coating layer is disposed on the surface of the substrate material to modify the surface interface of the substrate material. On the one hand, it can effectively isolate the direct contact between the positive electrode active material and the electrolyte, reduce side reactions, and thus effectively improve the electrochemical performance and safety performance of the battery. On the other hand, it can also effectively improve the ionic and electronic conductivity of the positive electrode material, thereby effectively improving the initial charge and discharge efficiency, discharge capacity and cycle performance of the battery, while reducing the initial impedance and impedance increase of the battery.
[0051] According to some other specific embodiments of the present application, the coating layer includes a continuous coating layer and a coating protruding from the surface of the continuous coating layer, and the coating includes at least one of a point-shaped coating and an island-shaped coating. Among them, the continuous coating layer can effectively improve the ionic and electronic conductivity of the positive electrode material, thereby improving the discharge capacity and cycle performance of the battery, while reducing the impedance of the battery. The discontinuous coating can effectively improve the stability of the positive electrode material, reduce the reaction between the positive electrode material and the electrolyte, and effectively improve the ionic and electronic conductivity of the positive electrode material, thereby improving the charge and discharge performance of the battery.
[0052] It can be understood that a continuous coating layer refers to a coating layer with a smooth and continuous surface without obvious particles and dot-shaped / island-shaped coatings, and dot-shaped / island-shaped coatings refer to dot-shaped and / or island-shaped coatings that obviously protrude from the surface of the coating layer.
[0053] According to some other specific embodiments of the present application, the continuous coating layer includes at least one of Al lithium cobalt oxide, W lithium cobalt oxide, Zr lithium cobalt oxide, and B lithium cobalt oxide. Thus, the above-mentioned continuous coating layer can further effectively improve the ionic and electronic conductivity of the positive electrode material, thereby further improving the discharge capacity and cycle performance of the battery, while further reducing the impedance of the battery.
[0054] According to some other specific embodiments of the present application, the coating includes at least one of aluminum oxide, tungsten oxide, titanium oxide, boron oxide, strontium oxide, lithium oxide of Al, lithium oxide of W, lithium oxide of Ti, lithium oxide of B, and lithium oxide of Sr. Thus, the coating can further improve the stability of the positive electrode material, further reduce the reaction between the positive electrode material and the electrolyte, and at the same time can further effectively improve the ionic and electronic conductivity of the positive electrode material, thereby further improving the charge and discharge performance of the battery.
[0055] According to some specific embodiments of the present application, the thickness of the continuous coating layer is in the range of 0.1 μm to 0.5 μm, and the height of the coating protruding from the surface of the coating layer is in the range of 0.1 μm to 0.5 μm.
[0056] In a second aspect of the present application, the present application proposes a method for preparing the above-mentioned positive electrode active material. According to an embodiment of the present application, the method comprises:
[0057] S100: mixing a nickel-cobalt-manganese precursor, a first lithium source, and a first doping additive according to a stoichiometric ratio, and performing a first sintering to obtain a first sintered product;
[0058] In this step, the nickel-cobalt-manganese precursor, the first lithium source, and the first doping additive are mixed in a stoichiometric ratio, and then the first sintering is performed under air / oxygen, and the obtained product is crushed to obtain a bulk-doped first sintered product, which is a compound containing lithium, nickel, cobalt, manganese and the first doping element, and the compound is a smaller grain. By doping the first doping additive in the positive electrode active material, the structural stability of the positive electrode active material can be effectively improved, and the degree of Li / Ni mixing of the positive electrode material can also be reduced, thereby effectively improving the cycle performance and capacity of the battery and inhibiting gas production.
[0059] In an embodiment of the present application, the nickel-cobalt-manganese precursor is a hydroxide solid solution containing nickel-cobalt-manganese.
[0060] According to some specific embodiments of the present application, the first doping additive is selected from at least one of oxides and hydroxides containing a doping element M, wherein M is selected from at least one of B, Mg, Sr, Ba, Fe, Cu, Ni, Co, Mn, Sc, Y, La, Ce, Sm, Eu, Gd, Tb, Dy, Yb, Lu, Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, W, Ru, Rh, Ir, Zn, Al, Ga, In, Si, Pb, Cd, Ge, Sn, Sb, Bi and Te. The first doping additive of the above type can effectively improve the structural stability of the positive electrode active material, and can also reduce the degree of Li / Ni mixing of the positive electrode material.
[0061] According to some further specific embodiments of the present application, the first sintering includes a first heating stage and a first constant temperature stage. The heating rate of the first heating stage is 1°C / min to 15°C / min (as an example, it can be 1°C / min, 3°C / min, 5°C / min, 7°C / min, 10°C / min, 12°C / min, 15°C / min, etc.). Thus, both the heating efficiency and the impurity elements in the first lithium source and the first doping additive can be ensured to be fully discharged from the reaction system.
[0062] According to some other specific embodiments of the present application, the temperature of the first constant temperature stage is 600°C to 1000°C (as an example, it can be 600°C, 700°C, 800°C, 900°C, 1000°C, etc.), and the time of the first constant temperature stage is 2h to 20h (as an example, it can be 2h, 4h, 6h, 8h, 10h, 12h, 14h, 16h, 18h, 20h, etc.), thereby further ensuring that the nickel-cobalt-manganese precursor, the first lithium source, and the first doping additive fully react to form a first sintered product of bulk doping.
[0063] S200: mixing the first sintered product, the second lithium source, and the optional second doping additive according to a stoichiometric ratio, and performing a second sintering to obtain a second sintered product;
[0064] In this step, the first sintered product, the second lithium source, and the optional second doping additive are mixed in a stoichiometric ratio, and then sintered for a second time under air / oxygen, and the obtained product is crushed to obtain a single-crystal low-cobalt or cobalt-free matrix material (i.e., the second sintered product). In this step, the second doping element and the second lithium source are mainly doped in the surface layer of the material. By doping the second doping additive in the positive electrode active material, the interfacial stability of the positive electrode active material can be effectively improved, thereby improving the cycle performance of the battery and inhibiting gas production. At the same time, this step is a grain growth process, and the above-mentioned second sintered product grows into a larger single crystal.
[0065] According to some other specific embodiments of the present application, the second doping additive is selected from at least one of oxides and hydroxides containing a doping element R, wherein R is selected from at least one of B, Mg, Sr, Ba, Fe, Cu, Ni, Co, Mn, Sc, Y, La, Ce, Sm, Eu, Gd, Tb, Dy, Yb, Lu, Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, W, Ru, Rh, Ir, Zn, Al, Ga, In, Si, Pb, Cd, Ge, Sn, Sb, Bi and Te. The above-mentioned second doping additive can further effectively improve the interfacial stability of the positive electrode active material, thereby improving the cycle performance of the battery and inhibiting gas production.
[0066] According to some other specific embodiments of the present application, the first lithium source includes lithium carbonate, and the second lithium source includes lithium hydroxide. The present application adds the lithium source in batches during the two sinterings, and adds lithium carbonate in the first sintering, and adds lithium hydroxide in the second sintering, which can effectively prevent the formation of impurity phases in the process of preparing a single crystal matrix at high temperature and excessive lithium source, and can also reduce the generation of micro stress, so that the single crystal of the matrix material is more sufficient. Further, the molar ratio of the first lithium source to the second lithium source is (30-90): (10-70), thereby further effectively promoting the single crystal of the matrix material. Preferably, the molar ratio of the first lithium source to the second lithium source is (40-90): (10-60), more preferably (50-90): (20-60).
[0067] According to some other specific embodiments of the present application, the second sintering includes a second heating stage, a third heating stage and a second constant temperature stage, the heating rate of the second heating stage is greater than the heating rate of the third heating stage, and the difference between the heating rates of the second heating stage and the third heating stage is 1°C / min to 5°C / min, the heating rate of the second heating stage can be 3°C / min to 10°C / min (as an example, it can be 3°C / min, 4°C / min, 5°C / min, 6°C / min, 7°C / min, 8°C / min, 9°C / min, 10°C / min, etc.), and the heating rate of the third heating stage can be 1°C / min to 5°C / min (as an example, it can be 1°C / min, 2°C / min, 3°C / min, 4°C / min, 5°C / min). By limiting the heating rate of the second heating stage within the above range, it is beneficial to ensure that the impurity elements in the second lithium source and the second doping additive are fully discharged from the reaction system, and by limiting the heating rate of the third heating stage within the above range, it is beneficial to the growth of the positive electrode material grains.
[0068] According to some other specific embodiments of the present application, the temperature of the second constant temperature stage is 600℃~1200℃ (as an example, it can be 600℃, 700℃, 800℃, 900℃, 1000℃, 1100℃, 1200℃, etc.), and the time of the second constant temperature stage is 2h~24h (as an example, it can be 2h, 4h, 6h, 8h, 10h, 12h, 14h, 16h, 18h, 20h, 22h, 24h, etc.), thereby further ensuring that the first sintered product, the second lithium source, and the second doping additive fully react to form a structurally stable matrix material with both solid phase doping and surface doping.
[0069] S300: mixing the second sintered product and the coating agent, and performing a third sintering to obtain a positive electrode active material;
[0070] According to some specific embodiments of the present application, the above step S300 includes:
[0071] S310: mixing the second sintered product and the first coating agent, and performing a third sintering to obtain a third sintered product;
[0072] In this step, the second sintered product and the first coating agent are mixed, and then sintered for the third time under air / oxygen to form a continuous coating layer on at least part of the surface of the base material, and the obtained product is crushed to obtain a third sintered product. By forming a continuous coating layer on the surface of the base material, the ionic and electronic conductivity of the positive electrode material can be effectively improved, thereby improving the discharge capacity and cycle performance of the battery, while reducing the impedance of the battery.
[0073] According to some other specific embodiments of the present application, the first coating agent is selected from at least one of oxides, hydroxides, carbonates containing Al, W, Zr or B, such as aluminum oxide, aluminum hydroxide, aluminum carbonate, etc., and the above-mentioned first coating agent forms lithium cobalt oxide containing Al, W, Zr or B after sintering.
[0074] According to some other specific embodiments of the present application, the mass of the first coating agent is 0.01% to 2% of the mass of the second sintered product, and as an example it can be 0.01%, 0.5%, 1%, 1.5%, 2%, etc., thereby further effectively improving the ionic and electronic conductivity of the positive electrode material.
[0075] According to some other specific embodiments of the present application, the third sintering includes a fourth heating stage and a third constant temperature stage. The heating rate of the fourth heating stage is 1°C / min to 15°C / min (as an example, it can be 1°C / min, 3°C / min, 5°C / min, 7°C / min, 10°C / min, 12°C / min, 15°C / min, etc.). Thus, both the heating efficiency and the impurity elements in the first coating agent can be ensured to be fully discharged from the reaction system.
[0076] According to some other specific embodiments of the present application, the temperature of the third constant temperature stage is 500℃~1000℃ (as an example, it can be 500℃, 600℃, 700℃, 800℃, 900℃, 1000℃, etc.), and the time of the third constant temperature stage is 2h~20h (as an example, it can be 2h, 4h, 6h, 8h, 10h, 12h, 14h, 16h, 18h, 20h, etc.), thereby further ensuring that the first coating agent fully reacts to form a continuous coating layer.
[0077] S320: mixing the third sintered product and the second coating agent, and performing a fourth sintering to obtain a positive electrode active material;
[0078] In this step, the third sintered product and the second coating agent are mixed, and then sintered for the fourth time under air / oxygen to form a discontinuous coating on part of the surface of the continuous coating layer, the coating protruding from the surface of the continuous coating layer, and the coating includes at least one of a point-shaped coating and an island-shaped coating. Finally, the obtained product is crushed, cooled, screened, and demagnetized to obtain a positive electrode active material. By forming a discontinuous coating on the surface of the continuous coating layer, the stability of the positive electrode material can be effectively improved, the reaction between the positive electrode material and the electrolyte can be reduced, and the ionic and electronic conductivity of the positive electrode material can be effectively improved, thereby improving the charge and discharge performance of the battery.
[0079] According to some other specific embodiments of the present application, the second coating agent is selected from at least one of oxides, hydroxides, carbonates containing Al, W, Ti, B or Sr, such as aluminum oxide, aluminum hydroxide, aluminum carbonate, etc., and the above-mentioned second coating agent forms aluminum oxide or lithium oxide containing Al, W, Ti, B or Sr after sintering.
[0080] According to some other specific embodiments of the present application, the mass of the second coating agent is 0.01% to 2% of the mass of the third sintered product, and as an example it can be 0.01%, 0.5%, 1%, 1.5%, 2%, etc., thereby further ensuring the improvement of the stability of the positive electrode material and further effectively improving the ionic and electronic conductivity of the positive electrode material.
[0081] According to some other specific embodiments of the present application, the fourth sintering includes a fifth heating stage and a fourth constant temperature stage. The heating rate of the fifth heating stage is 1°C / min to 15°C / min (as an example, it can be 1°C / min, 3°C / min, 5°C / min, 7°C / min, 10°C / min, 12°C / min, 15°C / min, etc.). Thus, both the heating efficiency and the impurity elements in the second coating agent can be ensured to be fully discharged from the reaction system.
[0082] The temperature of the fourth constant temperature stage is 200°C to 800°C (as an example, it can be 200°C, 300°C, 400°C, 500°C, 600°C, 700°C, 800°C, etc.), and the time of the fourth constant temperature stage is 2h to 20h (as an example, it can be 2h, 4h, 6h, 8h, 10h, 12h, 14h, 16h, 18h, 20h, etc.). This can further ensure that the second coating agent is fully reacted to form a discontinuous coating.
[0083] Therefore, the present application prevents the formation of impurity phases in the process of preparing a single crystal matrix at high temperature and with excessive lithium source by adding lithium source in batches during two sinterings (i.e., adding a portion of lithium source in the first sintering and adding another portion of lithium source in the second sintering), and at the same time, can reduce the generation of micro stress, so that the single crystallization of the matrix material is more complete. Doping additives are added in the two sinterings respectively, so as to obtain a structurally stable matrix material with both phase doping and surface doping, and the surface of the matrix material is coated to modify the surface interface of the matrix material, which can effectively isolate the direct contact between the positive electrode active material and the electrolyte, reduce side reactions, and thus effectively improve the electrochemical performance and safety performance of the battery, and on the other hand, can effectively improve the ionic and electronic conductivity of the positive electrode material, so as to effectively improve the discharge capacity and cycle performance of the battery.
[0084] In the third aspect of the present application, the present application proposes a positive electrode plate. According to an embodiment of the present application, the positive electrode plate includes a positive electrode current collector and a positive electrode active material layer disposed on at least one side of the positive electrode current collector, and the positive electrode active material layer includes the positive electrode active material described in the first aspect of the present application, or the positive electrode active material prepared by the method described in the second aspect.
[0085] According to an embodiment of the present application, the positive electrode plate includes a positive electrode collector and a positive electrode active material layer arranged on the positive electrode collector, the positive electrode active material layer includes the above-mentioned positive electrode active material, wherein the positive electrode collector can be a metal foil or a composite current collector (the metal material can be arranged on a polymer substrate to form a composite current collector), for example, the positive electrode collector can be aluminum foil.
[0086] According to some embodiments of the present application, the positive electrode active material layer may further optionally include a binder. As an example, the binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, or fluorine-containing acrylate resin.
[0087] According to some embodiments of the present application, the positive electrode active material layer may further optionally include a conductive agent. As an example, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, or carbon nanofibers.
[0088] According to some embodiments of the present application, the positive electrode sheet can be prepared in the following manner: the components for preparing the positive electrode sheet, such as the positive electrode active material, the conductive agent, the binder and any other components are dispersed in a solvent (such as N-methylpyrrolidone) to form a positive electrode slurry; the positive electrode slurry is coated on the positive electrode collector, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained.
[0089] It should be noted that the features and advantages described above for the positive electrode active material and the preparation method thereof are also applicable to the positive electrode plate and will not be described in detail here.
[0090] In the fourth aspect of the present application, the present application proposes a battery. According to an embodiment of the present application, the battery includes at least one of the positive electrode sheets of the third aspect. Thus, the initial charge and discharge efficiency, discharge capacity, cycle performance and safety performance of the battery can be effectively improved, while reducing the initial impedance and impedance increase of the battery.
[0091] As an example, a battery includes a positive electrode sheet, a negative electrode sheet, an electrolyte and a separator, and the separator is located between the positive electrode sheet and the negative electrode sheet. During the charge and discharge process of the battery, active ions are embedded and removed back and forth between the positive electrode sheet and the negative electrode sheet. The electrolyte plays the role of conducting ions between the positive electrode sheet and the negative electrode sheet. The separator is arranged between the positive electrode sheet and the negative electrode sheet, mainly to prevent the positive and negative electrodes from short-circuiting, while allowing ions to pass through.
[0092] According to an embodiment of the present application, the negative electrode plate includes a negative electrode current collector and a negative electrode active material layer arranged on the negative electrode current collector, the negative electrode active material layer includes a negative electrode active material, wherein the negative electrode current collector can be a metal foil or a composite current collector (the metal material can be arranged on a polymer substrate to form a composite current collector), for example, the positive electrode current collector can be a copper foil.
[0093] According to some embodiments of the present application, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, sodium titanate, etc.
[0094] According to some embodiments of the present application, the negative electrode active material layer may further include a conductive agent, which may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, or carbon nanofibers.
[0095] According to some embodiments of the present application, the negative electrode active material layer may further optionally include other additives, such as a thickener (eg, sodium carboxymethyl cellulose (CMC-Na)).
[0096] According to some embodiments of the present application, the negative electrode sheet can be prepared in the following manner: the above-mentioned components for preparing the negative electrode sheet, such as the negative electrode active material, the conductive agent, and the adhesive are dispersed in a solvent (such as deionized water) to form a negative electrode slurry; the negative electrode slurry is coated on the negative electrode collector, and after drying, cold pressing and other processes, the negative electrode sheet can be obtained.
[0097] According to some further embodiments of the present application, the negative electrode plate may include a metal sodium plate or a sodium alloy, such as a sodium-indium alloy.
[0098] According to some other embodiments of the present application, there is no particular restriction on the type of isolation membrane, and any known porous structure isolation membrane with good chemical stability and mechanical stability can be selected. As an example, the material of the isolation membrane may include at least one of glass fiber, non-woven fabric, polyethylene, polypropylene or polyvinylidene fluoride. The isolation membrane can be a single-layer film or a multi-layer composite film without particular restriction. When the isolation membrane is a multi-layer composite film, the materials of each layer can be the same or different without particular restriction.
[0099] According to some other embodiments of the present application, the type of electrolyte is not specifically limited and can be selected according to needs. According to some specific embodiments of the present application, the electrolyte is an electrolyte solution, and the electrolyte solution includes a lithium salt and a solvent.
[0100] According to some specific embodiments of the present application, the lithium salt may include lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium bis(fluorosulfonyl)imide (LiFSI), lithium phosphate (LiBOB), lithium difluorophosphate (LiPO2F2)
[0101] According to some specific embodiments of the present application, the solvent may include at least one of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, butylene carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, cyclopentane sulfone, dimethyl sulfone, ethylene glycol dimethyl ether, methyl ethyl sulfone or diethyl sulfone.
[0102] In some embodiments of the present application, the electrolyte may further include additives. For example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, and may also include additives that can improve certain battery properties, such as additives that improve battery overcharge performance, additives that improve battery high or low temperature performance, etc.
[0103] It should be noted that the above-mentioned features and advantages described for the positive electrode plate are also applicable to the solid-state battery and will not be repeated here.
[0104] In a fifth aspect of the present application, the present application proposes an electric device. According to an embodiment of the present application, the electric device includes the above-mentioned battery. The features and advantages described above for the battery are also applicable to the electric device and will not be repeated here.
[0105] Specifically, the electrical equipment may be, but is not limited to, mobile phones, tablets, laptops, electric toys, electric tools, battery cars, electric cars, ships, spacecraft, etc. Electric toys may include fixed or mobile electric toys, such as game consoles, electric car toys, electric ship toys, and electric airplane toys, etc. Spacecraft may include airplanes, rockets, space shuttles, and spacecraft, etc.
[0106] Hereinafter, the embodiments of the present application will be described. The embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If no specific techniques or conditions are indicated in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. If the manufacturer is not indicated in the reagents or instruments used, they are all conventional products that can be obtained commercially.
[0107] Example 1
[0108] (1) lithium carbonate, a nickel-cobalt-manganese precursor, and zirconium oxide are uniformly mixed in a high-speed mixer according to a ratio of n(Li):n(Ni):n(Co):n(Mn):n(Zr)=0.52:0.763:0.015:0.219:0.003 to obtain a mixture I;
[0109] (2) Mixture I was heated to 875°C at a rate of 5.5°C / min in an air atmosphere, kept at that temperature for 8.5 h, cooled naturally to room temperature, and crushed by a colloid mill to obtain product I, whose D50 was 4.2 μm;
[0110] (3) Process product I and lithium hydroxide are divided into n(Li 0.52 Ni 0.763 Co 0.015 Mn 0.219 Zr 0.003 ):n(Li)=1:0.52, and uniformly mixed in a high-speed mixer to obtain a mixture II;
[0111] (4) sintering the mixture II for the second time in an oxygen atmosphere, heating the mixture to 650°C at a rate of 4.5°C / min, and then heating the mixture to 920°C at a rate of 2.5°C / min, maintaining the temperature for 8 hours, cooling the mixture naturally to room temperature, and crushing the mixture to obtain the in-process product II;
[0112] (5) uniformly mixing the process product II with aluminum oxide and cobalt oxyhydroxide in a high-speed mixer at a mass ratio of 100:0.19:0.76 to obtain a mixture III;
[0113] (6) performing a third sintering in air, heating to 750°C at a rate of 3°C / min, maintaining the temperature for 8 h, cooling naturally to room temperature, and crushing the obtained product to obtain process product III;
[0114] (7) uniformly mixing the process product III with aluminum oxide, tungsten oxide, and titanium oxide in a mass ratio of 100:0.28:0.25:0.30 in a high-speed mixer to obtain a mixture IV;
[0115] (8) The fourth sintering was carried out in air, the temperature was raised to 410°C at 3°C / min, the temperature was kept for 8 hours, and the obtained product was naturally cooled to room temperature. The obtained product was crushed and passed through a 400-mesh sieve to obtain a low-cobalt layered positive electrode material A1, whose composition is Li 1.04 Ni 0.747 Co 0.023 Mn 0.214 Zr 0.003 Al 0.009 W 0.001 Ti 0.003 O2.
[0116] Example 2
[0117] (1) lithium carbonate, a nickel-cobalt-manganese precursor, zirconium oxide, and aluminum oxide are uniformly mixed in a high-speed mixer according to a ratio of n(Li):n(Ni):n(Co):n(Mn):n(Zr):n(Al)=0.78:0.761:0.015:0.219:0.002:0.003 to obtain a mixture I;
[0118] (2) In an oxygen atmosphere, the mixture I was heated to 895°C at a rate of 5.5°C / min, kept at this temperature for 8.5 h, cooled naturally to room temperature, and crushed by a colloid mill to obtain the process product I with a D50 of 4.5 μm;
[0119] (3) Process product I and lithium hydroxide are divided into n(Li 0.78 Ni 0.761 Co 0.015 Mn 0.219 Zr 0.002 Al 0.003 O2):n(Li)=1:0.26 ratio, uniformly mixed in a high speed mixer to obtain mixture II;
[0120] (4) sintering the mixture II for the second time in an oxygen atmosphere, heating the mixture to 650°C at 4.5°C / min, and then heating the mixture to 900°C at 2.5°C / min, keeping the temperature for 8 hours, cooling the mixture naturally to room temperature, and crushing the mixture to obtain the in-process product II;
[0121] (5) uniformly mixing the process product II with aluminum oxide and cobalt oxyhydroxide in a high-speed mixer at a mass ratio of 100:0.19:0.76 to obtain a mixture III;
[0122] (6) performing a third sintering in air, heating to 750°C at a rate of 3°C / min, maintaining the temperature for 8 h, cooling naturally to room temperature, and crushing the obtained product to obtain process product III;
[0123] (7) uniformly mixing the process product III with aluminum oxide, tungsten oxide, and titanium oxide in a mass ratio of 100:0.28:0.25:0.30 in a high-speed mixer to obtain a mixture IV;
[0124] (8) The fourth sintering was performed under air, the temperature was raised to 410°C at 3°C / min, the temperature was kept for 8 hours, and the obtained product was naturally cooled to room temperature. The obtained product was crushed and passed through a 400-mesh sieve to obtain a low-cobalt layered positive electrode material A2, whose composition is Li 1.04 Ni 0.745 Co 0.023 Mn 0.214 Zr 0.002 Al 0.012 W 0.001 Ti 0.003 O2.
[0125] Example 3
[0126] (1) lithium carbonate, a nickel-cobalt-manganese precursor, zirconium oxide, and aluminum oxide are uniformly mixed in a high-speed mixer according to a ratio of n(Li):n(Ni):n(Co):n(Mn):n(Zr):n(Al)=0.78:0.761:0.015:0.219:0.002:0.003 to obtain a mixture I;
[0127] (2) In an oxygen atmosphere, the mixture I was heated to 895°C at a rate of 5.5°C / min, kept at this temperature for 8.5 h, cooled naturally to room temperature, and crushed by a colloid mill to obtain the process product I with a D50 of 4.5 μm;
[0128] (3) Process product I, lithium hydroxide and yttrium oxide are mixed according to n(Li 0.78 Ni 0.761 Co 0.015 Mn 0.219 Zr 0.002 Al 0.003O2):n(Li):n(Y)=1:0.26:0.002, and uniformly mixed in a high-speed mixer to obtain a mixture II;
[0129] (4) sintering the mixture II for the second time in an oxygen atmosphere, heating the mixture to 650°C at 4.5°C / min, and then heating the mixture to 900°C at 2.5°C / min, keeping the temperature for 8 hours, cooling the mixture naturally to room temperature, and crushing the mixture to obtain the in-process product II;
[0130] (5) uniformly mixing the process product II with aluminum oxide and cobalt oxyhydroxide in a high-speed mixer at a mass ratio of 100:0.19:0.76 to obtain a mixture III;
[0131] (6) performing a third sintering in air, heating to 750°C at a rate of 3°C / min, maintaining the temperature for 8 h, cooling naturally to room temperature, and crushing the obtained product to obtain process product III;
[0132] (7) uniformly mixing the process product III with aluminum oxide, tungsten oxide, and titanium oxide in a mass ratio of 100:0.28:0.25:0.30 in a high-speed mixer to obtain a mixture IV;
[0133] (8) The fourth sintering was performed under air, the temperature was raised to 410°C at 3°C / min, the temperature was kept for 8 hours, and the product was naturally cooled to room temperature. The obtained product was crushed and passed through a 400-mesh sieve to obtain a low-cobalt layered positive electrode material A3, whose composition is Li 1.04 Ni 0.744 Co 0.022 Mn 0.214 Zr 0.002 Y 0.002 Al 0.012 W 0.001 Ti 0.003 O2.
[0134] Example 4
[0135] (1) lithium carbonate, a nickel-cobalt-manganese precursor, zirconium oxide, and aluminum oxide are uniformly mixed in a high-speed mixer according to a ratio of n(Li):n(Ni):n(Co):n(Mn):n(Zr):n(Al)=0.78:0.761:0.015:0.219:0.002:0.003 to obtain a mixture I;
[0136] (2) In an oxygen atmosphere, the mixture I was heated to 895°C at a rate of 5.5°C / min, kept at this temperature for 8.5 h, cooled naturally to room temperature, and crushed by a colloid mill to obtain the process product I with a D50 of 4.5 μm;
[0137] (3) Process product I, lithium hydroxide and yttrium oxide are mixed according to n(Li 0.78 Ni 0.761 Co0.015 Mn 0.219 Zr 0.002 Al 0.003 O2):n(Li):n(Y)=1:0.26:0.002, and uniformly mixed in a high-speed mixer to obtain a mixture II;
[0138] (4) sintering the mixture II for the second time in an oxygen atmosphere, heating the mixture to 650°C at 4.5°C / min, and then heating the mixture to 900°C at 2.5°C / min, keeping the temperature for 8 hours, cooling the mixture naturally to room temperature, and crushing the mixture to obtain the in-process product II;
[0139] (5) uniformly mixing the process product II with aluminum oxide, tungsten oxide, and titanium oxide in a mass ratio of 100:0.28:0.25:0.30 in a high-speed mixer to obtain a mixture III;
[0140] (6) The third sintering was carried out in air, the temperature was raised to 410°C at 3°C / min, the temperature was kept for 8 hours, and the product was naturally cooled to room temperature. The obtained product was crushed and passed through a 400-mesh sieve to obtain a low-cobalt layered positive electrode material A4, whose composition is Li 1.04 Ni 0.753 Co 0.015 Mn 0.216 Zr 0.002 Y 0.002 Al 0.008 W 0.001 Ti 0.003 O2.
[0141] Example 5
[0142] (1) lithium carbonate, nickel-cobalt-manganese precursor, zirconium oxide, aluminum oxide, and boron oxide are uniformly mixed in a high-speed mixer according to a ratio of n(Li):n(Ni):n(Co):n(Mn):n(Zr):n(Al):n(B)=0.832:0.757:0.015:0.218:0.002:0.003:0.005 to obtain a mixture I;
[0143] (2) In an oxygen atmosphere, the mixture I was heated to 895°C at a rate of 5.5°C / min, kept at this temperature for 8.5 h, cooled naturally to room temperature, and crushed by a colloid mill to obtain the process product I with a D50 of 4.5 μm;
[0144] (3) Process product I, lithium hydroxide and yttrium oxide are mixed according to n(Li 0.832 Ni 0.757 Co 0.015 Mn 0.218 Zr 0.002 Al 0.00 3B 0.005O2):n(Li):n(Y)=1:0.208:0.002, uniformly mixed in a high-speed mixer to obtain a mixture II;
[0145] (4) sintering the mixture II for the second time in an oxygen atmosphere, heating the mixture to 650°C at 4.5°C / min, and then heating the mixture to 900°C at 2.5°C / min, keeping the temperature for 8 hours, cooling the mixture naturally to room temperature, and crushing the mixture to obtain the in-process product II;
[0146] (5) uniformly mixing the process product II with aluminum oxide and cobalt oxyhydroxide in a high-speed mixer at a mass ratio of 100:0.19:0.76 to obtain a mixture III;
[0147] (6) performing a third sintering in air, heating to 750°C at a rate of 3°C / min, maintaining the temperature for 8 h, cooling naturally to room temperature, and crushing the obtained product to obtain process product III;
[0148] (7) uniformly mixing the process product III with aluminum oxide, tungsten oxide, and titanium oxide in a mass ratio of 100:0.28:0.25:0.30 in a high-speed mixer to obtain a mixture IV;
[0149] (8) The fourth sintering was performed under air, the temperature was raised to 410°C at 3°C / min, the temperature was kept for 8 hours, and the product was naturally cooled to room temperature. The obtained product was crushed and passed through a 400-mesh sieve to obtain a low-cobalt layered positive electrode material A5, whose composition is Li 1.04 Ni 0.740 Co 0.022 Mn 0.213 Zr 0.002 Y 0.002 B 0.005 Al 0.012 W 0.001 Ti 0.003 O2.
[0150] Example 6
[0151] (1) lithium carbonate, a nickel-cobalt-manganese precursor, titanium oxide, and aluminum oxide are uniformly mixed in a high-speed mixer according to a ratio of n(Li):n(Ni):n(Co):n(Mn):n(Ti):n(Al)=0.78:0.745:0:0.249:0.002:0.004 to obtain a mixture I;
[0152] (2) In an oxygen atmosphere, the mixture I was heated to 895°C at a rate of 5.5°C / min, kept at this temperature for 8.5 h, cooled naturally to room temperature, and crushed by a colloid mill to obtain the process product I with a D50 of 4.5 μm;
[0153] (3) Mix process product I, lithium hydroxide, zirconium oxide and yttrium oxide according to n(Li 0.78 Ni0.745 Mn 0.249 Ti 0.002 Al 0.00 4O2):n(Li):n(Zr):n(Y)=1:0.26:0.002:0.002, and uniformly mix in a high-speed mixer to obtain a mixture II;
[0154] (4) sintering the mixture II for the second time in an oxygen atmosphere, heating the mixture to 650°C at 4.5°C / min, and then heating the mixture to 910°C at 2.5°C / min, keeping the temperature for 8 hours, cooling the mixture to room temperature naturally, and crushing the mixture to obtain the in-process product II;
[0155] (5) uniformly mixing the process product II with aluminum oxide and cobalt oxyhydroxide in a high-speed mixer at a mass ratio of 100:0.19:1.9 to obtain a mixture III;
[0156] (6) performing a third sintering in air, heating to 750°C at a rate of 3°C / min, maintaining the temperature for 8 h, cooling naturally to room temperature, and crushing the obtained product to obtain process product III;
[0157] (7) uniformly mixing the process product III with aluminum oxide, tungsten oxide, and titanium oxide in a mass ratio of 100:0.28:0.25:0.30 in a high-speed mixer to obtain a mixture IV;
[0158] (8) The fourth sintering was performed under air, the temperature was raised to 410°C at 3°C / min, the temperature was kept for 8 hours, and the product was naturally cooled to room temperature. The obtained product was crushed and passed through a 400-mesh sieve to obtain a low-cobalt layered positive electrode material A6, which has a composition of Li 1.04 Ni 0.718 Co 0.020 Mn 0.239 Zr 0.002 Y 0.002 Al 0.013 W 0.001 Ti 0.005 O2.
[0159] Example 7
[0160] (1) lithium carbonate, a nickel-cobalt-manganese precursor, titanium oxide, and aluminum oxide are uniformly mixed in a high-speed mixer according to a ratio of n(Li):n(Ni):n(Co):n(Mn):n(Ti):n(Al)=0.78:0.800:0.005:0.189:0.002:0.004 to obtain a mixture I;
[0161] (2) In an oxygen atmosphere, the mixture I was heated to 895°C at a rate of 5.5°C / min, kept at this temperature for 8.5 h, cooled naturally to room temperature, and crushed by a colloid mill to obtain the process product I with a D50 of 4.5 μm;
[0162] (3) Mix process product I, lithium hydroxide, zirconium oxide and yttrium oxide according to n(Li 0.78 Ni 0.800 Co 0.005 Mn 0.189 Ti 0.002 Al 0.004 O2):n(Li):n(Zr):n(Y)=1:0.26:0.002:0.002, and uniformly mix in a high-speed mixer to obtain a mixture II;
[0163] (4) sintering the mixture II for the second time in an oxygen atmosphere, heating the mixture to 650°C at 4.5°C / min, and then heating the mixture to 900°C at 2.5°C / min, keeping the temperature for 8 hours, cooling the mixture naturally to room temperature, and crushing the mixture to obtain the in-process product II;
[0164] (5) uniformly mixing the process product II with aluminum oxide and cobalt oxyhydroxide in a high-speed mixer at a mass ratio of 100:0.19:1.42 to obtain a mixture III;
[0165] (6) performing a third sintering in air, heating to 750°C at a rate of 3°C / min, maintaining the temperature for 8 h, cooling naturally to room temperature, and crushing the obtained product to obtain process product III;
[0166] (7) uniformly mixing the process product III with aluminum oxide, tungsten oxide, and titanium oxide in a mass ratio of 100:0.28:0.25:0.30 in a high-speed mixer to obtain a mixture IV;
[0167] (8) The fourth sintering was carried out in air, the temperature was raised to 410°C at 3°C / min, the temperature was kept for 8 hours, and the product was naturally cooled to room temperature. The obtained product was crushed and passed through a 400-mesh sieve to obtain a low-cobalt layered positive electrode material A7, whose composition is Li 1.04 Ni 0.775 Co 0.019 Mn 0.183 Zr 0.002 Y 0.002 Al 0.013 W 0.001 Ti 0.005 O2.
[0168] Example 8
[0169] The preparation method of this embodiment is basically the same as that of embodiment 5, except that:
[0170] (1) Replacing zirconium oxide with magnesium oxide to obtain a low-cobalt layered cathode material A8, which is composed of Li 1.04 Ni 0.740 Co 0.022 Mn 0.213 Mg 0.002Y 0.002 B 0.005 Al 0.012 W 0.001 Ti 0.003 O2.
[0171] Example 9
[0172] The preparation method of this embodiment is basically the same as that of embodiment 5, except that:
[0173] (1) Replacing zirconium oxide with silicon oxide to obtain a low-cobalt layered cathode material A9, which is composed of Li 1.04 Ni 0.740 Co 0.02 2Mn 0.213 Si 0.002 Y 0.002 B 0.005 Al 0.012 W 0.001 Ti 0.003 O2.
[0174] Example 10
[0175] The preparation method of this embodiment is basically the same as that of embodiment 5, except that:
[0176] (3) Replacing yttrium oxide with tantalum oxide to obtain a low-cobalt layered cathode material A10, which has a composition of Li 1.04 Ni 0.740 Co 0.022 Mn 0.213 Zr 0.002 Ta 0.002 B 0.005 Al 0.012 W 0.001 Ti 0.003 O2.
[0177] Embodiment 11
[0178] The preparation method of this embodiment is basically the same as that of embodiment 5, except that:
[0179] (3) Replacing yttrium oxide with tungsten oxide to obtain a low-cobalt layered cathode material A11, whose composition is Li 1.04 Ni 0.740 Co 0.022 Mn 0.213 Zr 0.002 B 0.005 Al 0.012 W 0.003 Ti 0.003 O2.
[0180] Comparative Example 1
[0181] (1) lithium carbonate, a nickel-cobalt-manganese precursor, zirconium oxide, and aluminum oxide are uniformly mixed in a high-speed mixer according to a ratio of n(Li):n(Ni):n(Co):n(Mn):n(Zr)=1.04:0.763:0.015:0.219:0.003: to obtain a mixture I;
[0182] (2) In an oxygen atmosphere, the mixture I is heated to 650°C at 4.5°C / min, then heated to 940°C at 2.5°C / min, kept at this temperature for 8 hours, cooled naturally to room temperature, and crushed to obtain the process product I;
[0183] (3) uniformly mixing the process product I with aluminum oxide and cobalt oxyhydroxide in a high-speed mixer at a mass ratio of 100:0.19:0.76 to obtain a mixture II;
[0184] (4) performing a second sintering in air, heating to 750°C at a rate of 3°C / min, maintaining the temperature for 8 hours, cooling naturally to room temperature, and crushing the obtained product to obtain process product II;
[0185] (5) uniformly mixing the process product II with aluminum oxide, tungsten oxide, and titanium oxide in a mass ratio of 100:0.28:0.25:0.30 in a high-speed mixer to obtain a mixture III;
[0186] (6) The third sintering was carried out in air, the temperature was raised to 410°C at 3°C / min, the temperature was kept for 8 hours, and the product was naturally cooled to room temperature. The obtained product was crushed and passed through a 400-mesh sieve to obtain a low-cobalt layered positive electrode material D1, which has a composition of Li 1.04 Ni 0.747 Co 0.023 Mn 0.214 Zr 0.003 Al 0.009 W 0.001 Ti 0.003 O2, the specific data parameters are shown in Table 1 and Table 2.
[0187] Comparative Example 2
[0188] (1) According to the method of comparative example 1, the difference is that the lithium source used in the mixture I is lithium hydroxide, the temperature of the constant temperature stage I in the first sintering process is T1 = 910 ° C, and the rest is the same to obtain a low-cobalt layered positive electrode material D2. The composition of D2 is Li 1.04 Ni 0.747 Co 0.023 Mn 0.214 Zr 0.003 Al 0.009 W 0.001 Ti 0.003 O2, the specific data parameters are shown in Table 1 and Table 2.
[0189] Comparative Example 3
[0190] (1) lithium carbonate, lithium hydroxide, nickel-cobalt-manganese precursor, zirconium oxide and aluminum oxide are uniformly mixed in a high-speed mixer according to a ratio of n(Li2CO3):n(LiOH):n(Ni):n(Co):n(Mn):n(Zr)=0.26:0.52:0.763:0.015:0.219:0.003: to obtain a mixture I;
[0191] (2) In an oxygen atmosphere, the mixture I is heated to 650°C at 4.5°C / min, then heated to 900°C at 2.5°C / min, kept at this temperature for 8 hours, cooled naturally to room temperature, and crushed to obtain the process product I;
[0192] (3) uniformly mixing the process product I with aluminum oxide and cobalt oxyhydroxide in a high-speed mixer at a mass ratio of 100:0.19:0.76 to obtain a mixture II;
[0193] (4) performing a second sintering in air, heating to 750°C at a rate of 3°C / min, maintaining the temperature for 8 hours, cooling naturally to room temperature, and crushing the obtained product to obtain process product II;
[0194] (5) uniformly mixing the process product II with aluminum oxide, tungsten oxide, and titanium oxide in a mass ratio of 100:0.28:0.25:0.30 in a high-speed mixer to obtain a mixture III;
[0195] (6) The third sintering was carried out in air, the temperature was raised to 410°C at 3°C / min, the temperature was kept for 8 hours, and the product was naturally cooled to room temperature. The obtained product was crushed and passed through a 400-mesh sieve to obtain a low-cobalt layered positive electrode material D3, whose composition is Li 1.04 Ni 0.747 Co 0.023 Mn 0.214 Zr 0.003 Al 0.009 W 0.001 Ti 0.003 O2, the specific data parameters are shown in Table 1 and Table 2.
[0196] Comparative Example 4
[0197] (1) The method of Comparative Example 3 is followed, except that the ratio of lithium carbonate, lithium hydroxide, nickel-cobalt-manganese precursor, zirconium oxide, and aluminum oxide in the mixture I is n(Li2CO3):n(LiOH):n(Ni):n(Co):n(Mn):n(Zr):n(Al):n(Y)=0.39:0.26:0.760:0.015:0.218:0.002:0.003:0.002, the holding temperature of the constant temperature stage I during the first sintering process is T1=940°C, and the rest are the same, to obtain a low-cobalt layered positive electrode material D4. The composition of D4 is Li 1.04 Ni 0.744 Co 0.022 Mn 0.214 Zr 0.002 Y 0.002 Al 0.012 W 0.001 Ti 0.003 O2, the specific data parameters are shown in Table 1 and Table 2.
[0198] Comparative Example 5
[0199] (1) lithium carbonate, lithium hydroxide, nickel-cobalt-manganese precursor, zirconium oxide, and aluminum oxide are uniformly mixed in a high-speed mixer at a ratio of n(Li2CO3):n(LiOH):n(Ni):n(Co):n(Mn):n(Zr):n(Al)=0.39:0.26:0.761:0.015:0.219:0.002:0.003 to obtain a mixture I;
[0200] (2) In an oxygen atmosphere, the mixture I was heated to 895°C at a rate of 5.5°C / min, kept at this temperature for 8.5 h, cooled naturally to room temperature, and crushed by a colloid mill to obtain the process product I with a D50 of 4.5 μm;
[0201] (3) Mix process product I and yttrium oxide according to n(Li 1.04 Ni 0.761 Co 0.015 Mn 0.219 Zr 0.002 Al 0.003 O2):n(Y)=1:0.002, and uniformly mix in a high-speed mixer to obtain a mixture II;
[0202] (4) The mixture II is sintered for the second time in an oxygen atmosphere by heating the mixture to 650°C at a rate of 4.5°C / min and then heating the mixture to 940°C at a rate of 2.5°C / min. The mixture is kept at this temperature for 8 hours and cooled naturally to room temperature. After crushing, the product II is obtained.
[0203] (5) uniformly mixing the process product II with aluminum oxide and cobalt oxyhydroxide in a high-speed mixer at a mass ratio of 100:0.19:0.76 to obtain a mixture III;
[0204] (6) performing a third sintering in air, heating to 750°C at a rate of 3°C / min, maintaining the temperature for 8 h, cooling naturally to room temperature, and crushing the obtained product to obtain process product III;
[0205] (7) uniformly mixing the process product III with aluminum oxide, tungsten oxide, and titanium oxide in a mass ratio of 100:0.28:0.25:0.30 in a high-speed mixer to obtain a mixture IV;
[0206] (8) The fourth sintering was carried out in air, the temperature was raised to 410°C at 3°C / min, the temperature was kept for 8 hours, and the product was naturally cooled to room temperature. The obtained product was crushed and passed through a 400-mesh sieve to obtain a low-cobalt layered positive electrode material D5, whose composition is Li 1.04 Ni 0.744 Co 0.022 Mn 0.214 Zr 0.002 Y 0.002 Al 0.012 W 0.001 Ti 0.003 O2, the specific data parameters are shown in Table 1 and Table 2.
[0207] The SEM observations were performed on the products after four sinterings in Example 1. Figure 2 As shown in Figure 2, it can be seen that process product I is a single crystal with smaller grains, process product II has grown into a single crystal with larger grain size, process product III forms a continuous coating layer on the surface of the base material, and positive electrode material A1 forms a discontinuous point-shaped coating or an island-shaped coating on part of the surface of the continuous coating layer.
[0208] XRD tests were performed on the positive electrode materials prepared in Examples 1 to 11 and Comparative Examples 1 to 5, and S D1 -S C1 ,I D1 / I C1 、F C1 and F D1 The results are shown in Table 1. Figure 1 It is the XRD diagram of the positive electrode materials of Example 3 and Comparative Example 4.
[0209] The charging capacity, discharge capacity, first coulombic efficiency (i.e., first efficiency), 80-week cycle retention rate, and 80-week DCR increase of lithium-ion half-cells (4.45V) prepared from the positive electrode materials prepared in Examples 1 to 11 and Comparative Examples 1 to 5 were tested respectively, and the results are shown in Table 2.
[0210] Charge and discharge capacity and first coulomb efficiency test:
[0211] Shenzhen Xinwell Battery Testing System was used to test the electrochemical performance of CR2025 button cells. The charge and discharge current density at 0.1C was 175mA / g. The charge and discharge voltage range was controlled to be 3.0V-4.45V. At room temperature, the button cells were charged and discharged at 0.1C to evaluate the charge and discharge specific capacity of the positive electrode material. The first coulomb efficiency % = first discharge specific capacity / first charge specific capacity*100%.
[0212] 80-week cycle retention test method:
[0213] In both the embodiment and the comparative example, the charge and discharge voltage range is controlled to be 3.0V-4.45V. At a constant temperature of 45°C, the button battery is charged and discharged once at 0.1C, and then charged and discharged 80 times at 1C to evaluate the high temperature cycle capacity retention rate of the positive electrode material.
[0214] 80-week DCR (impedance) gain test method:
[0215] Before the battery is cycled at high temperature, the impedance at 50% SOC is measured after it is fully charged, which is the initial impedance. After the battery is tested for high temperature cycling, the impedance at 50% SOC is measured after it is fully charged, which is the final impedance. The impedance growth rate % = (final impedance - initial impedance) / initial impedance × 100%.
[0216] Table 1
[0217]
[0218]
[0219] Table 2
[0220]
[0221]
[0222] It can be seen from Table 1 and Table 2 that compared with Comparative Examples 1 to 5, the charging capacity, discharge capacity, first efficiency, and 80-week cycle retention rate of Examples 1 to 11 are significantly improved, and the 80-week DCR increase is significantly reduced. The 80-week high-temperature cycle capacity retention rate of Examples 1 to 11 of the present application is above 89%, and the DCR increase is below 160%, while the 80-week high-temperature cycle capacity retention rate of Comparative Examples 1 to 5 is below 86%, and the DCR increase is above 220%. It can be seen that by limiting 0.80≤I D1 / I C1 ≤1.00、0.80≤A D1 / A C1 ≤1.05、0.35°≤S D1 -S C1≤0.65°、1.77≤Ic1 / I C2 ≤1.98、1.78≤I D1 / I D2 ≤2.19, 0°<F C1 ≤0.20° and 0°<F D1 ≤0.20°, which can effectively improve the initial charge and discharge efficiency, discharge capacity and cycle performance of the battery, and effectively reduce the initial impedance and impedance increase of the battery. And by comparing Examples 1 to 11, it can be seen that compared with Examples 1, 4, 10, and 11, the charging capacity, discharge capacity, first efficiency, and 80-week cycle retention rate of Examples 3 and Examples 5-7 are further improved, and the 80-week DCR increase is further reduced. In particular, the comprehensive performance of Example 7 is the best. It can be seen that by limiting 0.85≤I D1 / I C1 ≤0.95、0.85≤A D1 / A C1 ≤1.00、0.40°≤S D1 -S C1 ≤0.60°、1.80≤Ic1 / I C2 ≤1.95、1.80≤I D1 / I D2 ≤2.00, 0.05°≤F C1 ≤0.15° and 0.05°≤F D1 ≤0.15°, which can further improve the battery's initial charge and discharge efficiency, discharge capacity and cycle performance, while further reducing the battery's initial impedance and impedance increase.
[0223] Attached Figure 3 It is a schematic diagram of the cycle retention rate of batteries made of the low-cobalt layered positive electrode materials of Example 1, Example 3, Example 4, Example 7 and Comparative Example 1, with the horizontal axis representing the number of cycles and the vertical axis representing the capacity retention rate; the battery is tested for cycle life at 45 degrees Celsius, at a charge and discharge rate of 1C, and in a voltage range of 3.0V to 4.45V.
[0224] from Figure 3 It can be seen that compared with Comparative Example 1, the cycle retention rates of Example 1, Example 3, Example 4, and Example 7 are significantly improved. D1 / I C1 ≤1.00、0.80≤A D1 / A C1 ≤1.05、0.35°≤S D1 -S C1 ≤0.65°、1.77≤Ic1 / I C2 ≤1.98、1.78≤I D1 / I D2≤2.19, 0°<F C1 ≤0.20° and 0°<F D1 ≤0.20°, which can effectively improve the cycle performance of the battery.
[0225] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present application. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
[0226] Although the embodiments of the present application have been shown and described above, it can be understood that the above embodiments are exemplary and cannot be understood as limitations on the present application. Ordinary technicians in this field can change, modify, replace and modify the above embodiments within the scope of the present application.
Claims
1. A positive electrode active material, characterized in that: In the XRD spectrum of the positive electrode active material, the characteristic peak C(018) corresponding to the (018) crystal plane of the positive electrode active material is distributed in a bimodal manner, including a first characteristic peak C(018) located at a small angle side. 1 (018) and the second characteristic peak C at the high angle side 2 (018); The characteristic peak D(110) corresponding to the (110) crystal plane of the positive electrode active material is distributed in a bimodal manner, including a first characteristic peak D 1 (110) and the second characteristic peak D at the high angle side 2 (110); I C1 The first characteristic peak C corresponding to the (018) crystal plane of the positive electrode active material 1 The strength of (018), I D1 The first characteristic peak D corresponding to the (110) crystal plane of the positive electrode active material 1 The strength of (110) satisfies 0.80≤I D1 / I C1 ≤1.
00.
2. The positive electrode active material according to claim 1, characterized in that I C1 Japanese I D1 full foot 0.85≤I D1 / I C1 ≤0.
95.
3. The positive electrode active material according to claim 1, characterized in that A C1 The first characteristic peak C corresponding to the (018) crystal plane of the positive electrode active material 1 The peak area of (018), A D1 The first characteristic peak D corresponding to the (110) crystal plane of the positive electrode active material 1 The peak area of (110) satisfies 0.80≤A D1 / A C1 ≤1.05, preferably, 0.85≤A D1 / A C1 ≤1.
00.
4. The positive electrode active material according to claim 1, characterized in that S C1 The first characteristic peak C corresponding to the (018) crystal plane of the positive electrode active material 1 (018) position, S D1 The first characteristic peak D corresponding to the (110) crystal plane of the positive electrode active material 1 (110) position, satisfying 0.35°≤S D1 -S C1 ≤0.65°, preferably, 0.40°≤S D1 -S C1 ≤0.60°.
5. The positive electrode active material according to claim 1, characterized in that I C2 The second characteristic peak C corresponding to the (018) crystal plane of the positive electrode active material 2 The strength of (018), I D2 The second characteristic peak D corresponding to the (110) crystal plane of the positive electrode active material 2 The strength of (110) satisfies 1.77≤Ic1 / I C2 ≤1.98,1.78≤I D1 / I D2 ≤2.19, preferably, 1.80≤Ic1 / I C2 ≤1.95,1.80≤I D1 / I D2 ≤2.
00.
6. The positive electrode active material according to claim 1, characterized in that F C1 The first characteristic peak C corresponding to the (018) crystal plane of the positive electrode active material 1 The half-peak width of (018), F D1 The first characteristic peak D corresponding to the (110) crystal plane of the positive electrode active material 1 The half-peak width of (110) satisfies 0°<F C1 ≤0.20°, 0°<F D1 ≤0.20°, preferably, 0.05°≤F C1 ≤0.15°, 0.05°≤F D1 ≤0.15°.
7. The positive electrode active material according to any one of claims 1 to 6, characterized in that The positive electrode active material comprises: The matrix is a single crystal matrix, and the matrix includes a chemical formula of Li a (Ni x Co y Mn z M b R c )O2 material, wherein 0.95≤a≤1.10, 0.50≤x≤0.95, 0≤y≤0.05, 0≤z≤0.45, 0≤b≤0.05, 0≤c≤0.03, and at least one of b and c is not equal to 0; M and R are both doping elements, and M and R are independently selected from at least one of B, Mg, Sr, Ba, Fe, Cu, Ni, Co, Mn, Sc, Y, La, Ce, Sm, Eu, Gd, Tb, Dy, Yb, Lu, Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, W, Ru, Rh, Ir, Zn, Al, Ga, In, Si, Pb, Cd, Ge, Sn, Sb, Bi and Te.
8. The positive electrode active material according to claim 7, characterized in that The positive electrode active material also includes: A coating layer is provided on at least a portion of the surface of the substrate.
9. The positive electrode active material according to claim 8, characterized in that The coating layer includes a continuous coating layer and a coating protruding from the surface of the continuous coating layer, and the coating includes at least one of a point-shaped coating and an island-shaped coating.
10. The positive electrode active material according to claim 9, characterized in that The continuous coating layer comprises at least one of lithium cobalt oxide of Al, lithium cobalt oxide of W, lithium cobalt oxide of Zr, and lithium cobalt oxide of B; And / or, the coating includes at least one of aluminum oxide, tungsten oxide, titanium oxide, boron oxide, strontium oxide, lithium oxide of Al, lithium oxide of W, lithium oxide of Ti, lithium oxide of B, and lithium oxide of Sr.
11. A method for preparing the positive electrode active material according to any one of claims 1 to 10, characterized in that: include: Mixing a nickel-cobalt-manganese precursor, a first lithium source, and a first doping additive according to a stoichiometric ratio, and performing a first sintering to obtain a first sintered product; The first sintered product, the second lithium source, and the optional second doping additive are mixed according to a stoichiometric ratio, and sintered for a second time to obtain a second sintered product; The second sintered product and the coating agent are mixed and sintered for a third time to obtain a positive electrode active material.
12. The method according to claim 11, characterized in that The first sintering includes a first heating stage and a first constant temperature stage, the heating rate of the first heating stage is 1°C / min-15°C / min, the temperature of the first constant temperature stage is 600°C-1000°C, and the time of the first constant temperature stage is 2h-20h; And / or, the second sintering includes a second heating stage, a third heating stage and a second constant temperature stage, the heating rate of the second heating stage is greater than the heating rate of the third heating stage, and the difference in heating rate between the second heating stage and the third heating stage is 1°C / min to 5°C / min, the temperature of the second constant temperature stage is 600°C to 1200°C, and the time of the second constant temperature stage is 2h to 24h.
13. The method according to claim 11, characterized in that The first doping additive is selected from at least one of an oxide and a hydroxide containing a doping element M; and / or, the second doping additive is selected from at least one of an oxide and a hydroxide containing a doping element R; And / or, the first lithium source includes lithium carbonate, the second lithium source includes lithium hydroxide, and the molar ratio of the first lithium source to the second lithium source is (30-90):(10-70).
14. The method according to claim 11, characterized in that The mixing of the second sintered product and the coating agent and the third sintering comprises the following steps: The second sintered product and the first coating agent are mixed and sintered for a third time to obtain a third sintered product; The third sintered product and the second coating agent are mixed and sintered for the fourth time to obtain a positive electrode active material.
15. The method according to claim 14, characterized in that The third sintering includes a fourth heating stage and a third constant temperature stage, the heating rate of the fourth heating stage is 1°C / min to 15°C / min, the temperature of the third constant temperature stage is 500°C to 1000°C, and the time of the third constant temperature stage is 2h to 20h; And / or, the fourth sintering includes a fifth heating stage and a fourth constant temperature stage, the heating rate of the fifth heating stage is 1°C / min to 15°C / min, the temperature of the fourth constant temperature stage is 200°C to 800°C, and the duration of the fourth constant temperature stage is 2h to 20h; And / or, the first coating agent is selected from at least one of oxides, hydroxides and carbonates containing Al, W, Zr or B; And / or, the second coating agent is selected from at least one of oxides, hydroxides and carbonates containing Al, W, Ti, B or Sr; and / or, the mass of the first coating agent is 0.01% to 2% of the mass of the second sintered product; And / or, the mass of the second coating agent is 0.01% to 2% of the mass of the third sintered product.
16. A positive electrode plate, characterized in that: The invention comprises the positive electrode active material according to any one of claims 1 to 10 or the positive electrode active material prepared by the method according to any one of claims 11 to 15.
17. A battery, characterized in that: Including the positive electrode sheet as described in claim 16.
18. An electrical equipment, characterized in that: Comprising the battery of claim 17.
Citation Information
Cited By
Positive electrode material and preparation method thereof, positive electrode plate, battery and electric equipment
CN119153667A
Positive plate, lithium ion battery and electric device
CN120749117A
Positive electrode active material and preparation method therefor, positive electrode sheet, battery, and electrical device
EP4819233A1
Positive electrode active material and preparation method therefor, positive electrode sheet, battery, and electrical device
WO2026044873A1