High-rate positive electrode material and preparation method thereof, positive plate and sodium ion battery
By using a high-ratio cathode material with three-dimensional connected nanopore structure in the sodium ion battery positive electrode material, the problem of insufficient magnification performance of sodium ion battery is solved, and higher battery performance is achieved to meet the needs of diversified application.
Patent Information
- Application Number
- CN202410965824.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-08
AI Technical Summary
The rate performance of the cathode material of sodium ion battery is poor, and the existing improvement strategy has limited effect, making it difficult to meet higher application needs.
Using a high-ratio positive electrode material with three-dimensional connected nanopore structure, it is mixed with a nickel ferromanganese carbonate precursor and a copper source to form a loose porous structure, and calcined with the sodium source to maintain the nanopore structure, increasing electrolyte contact and electrons Conductivity.
It significantly improves the rate performance of sodium ion batteries, ensuring that the rate performance of 2C/0.2C and 5C/0.2C reaches 0.90 and 0.85 respectively, respectively, meeting higher application needs.
Smart Images

Figure CN118919712A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of positive electrode materials for sodium ion batteries, and in particular to a high-rate positive electrode material and a preparation method thereof, a positive electrode sheet and a sodium ion battery. Background Art
[0002] Since sodium has the advantages of abundant resources and cheap raw materials, sodium-ion secondary batteries are considered to be very likely to replace lithium-ion secondary batteries to solve the problem of lithium resource shortage, thereby achieving cheap large-scale energy storage and large-scale commercial applications.
[0003] Compared with lithium-ion layered oxides, sodium ions have a larger radius, so it is relatively difficult to deintercalate, which is manifested as poor rate performance. Currently, the rate performance is mainly improved by strategies such as doping and coating, small particle size, and proportion adjustment, but the improvement is often small. In order to meet more application needs, it is necessary to develop more effective strategies to improve the rate performance of sodium-ion cathode materials.
[0004] In view of this, the present invention is proposed. Summary of the invention
[0005] The first purpose of the present invention is to provide a high-rate positive electrode material, which has a three-dimensionally connected nanopore structure, which can increase the contact and wetting effect between the electrolyte and the positive electrode material, shorten the sodium ion transmission path, and the three-dimensionally connected layer structure can effectively improve the electron conduction ability. Therefore, the positive electrode material provided by the present invention has excellent rate performance.
[0006] The second object of the present invention is to provide a method for preparing a high-rate positive electrode material, which is conducive to forming a positive electrode material with a three-dimensionally connected nanopore structure, thereby improving its rate performance.
[0007] The third object of the present invention is to provide a positive electrode sheet, the battery produced by the positive electrode sheet has excellent rate performance.
[0008] A fourth object of the present invention is to provide a sodium ion battery having good rate performance, wherein the rate performance is 2C / 0.2C>0.90 and 5C / 0.2C>0.85.
[0009] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:
[0010] The present invention first provides a high-rate positive electrode material, the chemical formula of which is Na k Cu 1-h M h O2, wherein 0.8≤k≤1, 0.95≤h<1, and M includes at least Ni, Mn and Fe elements;
[0011] The high-rate positive electrode material includes secondary particles having a three-dimensionally connected nanopore structure formed by stacking and interlacing nanosheet layered primary particles.
[0012] Preferably, the thickness d1 of the nanosheet layered primary particles satisfies 0.05 μm<d1<0.5 μm.
[0013] Preferably, the pore diameter d2 of the nanopore structure satisfies 0.1 μm<d2<0.9 μm.
[0014] Preferably, the shape of the secondary particles includes a spherical shape.
[0015] Preferably, the particle size D of the high-rate positive electrode material is 50 Satisfy 8μm<D 50 <15μm.
[0016] Preferably, M further includes at least one of the elements Zn, Ti, Mg, Zr, Y, Ca, Sr, B, Co, Al and La.
[0017] Preferably, the high-rate positive electrode material is an O3 phase layered oxide.
[0018] Preferably, the specific surface area BET of the high rate positive electrode material satisfies 1 m 2 / g<BET<2.5m 2 / g.
[0019] Preferably, the tap density TD of the high-rate positive electrode material satisfies 1 g / cm 3 <TD<1.8g / cm 3 .
[0020] Preferably, the rate performance of a battery containing the high-rate positive electrode material satisfies: 2C / 0.2C>0.90, 5C / 0.2C>0.85.
[0021] The present invention further provides a method for preparing the high-rate positive electrode material, comprising the following steps:
[0022] The nickel-iron-manganese carbonate precursor and the copper source are mixed and sintered to obtain copper-nickel-iron-manganese oxide;
[0023] The copper-nickel-iron-manganese oxide is mixed with a sodium source and then calcined to obtain the high-rate positive electrode material.
[0024] Preferably, the specific surface area of the nickel-iron-manganese carbonate precursor is greater than 30 m 2 / g, the bulk density AD meets 0.8g / cm 3 <AD<1.5g / cm 3 , particle size D 50 8~15μm.
[0025] Preferably, the sintering temperature is 500-700° C., and the insulation time is ≥10 h.
[0026] Preferably, the calcination temperature is 770-870° C., and the insulation time is ≥10 h.
[0027] Preferably, in the process of mixing the copper-nickel-iron-manganese oxide with the sodium source, a dopant containing at least one element selected from the group consisting of Zn, Ti, Mg, Zr, Y, Ca, Sr, B, Co, Al and La is also added.
[0028] Preferably, the copper source comprises a nano copper source.
[0029] Preferably, the preparation method of the nickel-iron-manganese carbonate precursor comprises: mixing a nickel-iron-manganese ternary salt solution with a precipitant solution and conducting a co-precipitation reaction, and obtaining the nickel-iron-manganese carbonate precursor after solid-liquid separation; wherein the precipitant solution comprises a mixed solution of sodium carbonate solution and ammonia water, and the molar ratio of sodium carbonate to ammonia monohydrate in the precipitant solution is greater than 20:1.
[0030] Preferably, the total molar concentration of the metal elements in the nickel-iron-manganese ternary salt solution is 0.2-0.8 mol / L.
[0031] Preferably, the molar concentration of sodium carbonate in the precipitant solution is 0.2-0.8 mol / L.
[0032] Preferably, the coprecipitation reaction temperature is 40-70°C.
[0033] Preferably, the pH of the coprecipitation reaction is 8-10.
[0034] The present invention further provides a positive electrode sheet, comprising the high-rate positive electrode material.
[0035] The present invention also provides a sodium ion battery, comprising the positive electrode sheet.
[0036] Compared with the prior art, the present invention has the following beneficial effects:
[0037] (1) The high-rate positive electrode material provided by the present invention has a special three-dimensional pore structure, specifically, thin nanosheets are stacked and staggered to form three-dimensional interconnected nanopores, which can increase the contact and wetting effect between the electrolyte and the positive electrode material, shorten the sodium ion transmission path, and the three-dimensionally connected sheet structure can effectively improve the electron conduction ability. Therefore, the positive electrode material provided by the present invention has excellent rate performance.
[0038] (2) The high-rate positive electrode material provided by the present invention has a larger specific surface area and a smaller tap density.
[0039] (3) The high-rate positive electrode material provided by the present invention can produce a battery with a rate performance of 2C / 0.2C>0.90 and 5C / 0.2C>0.85.
[0040] (4) The preparation method of the high-rate positive electrode material provided by the present invention comprises the following steps: firstly mixing and sintering a nickel-iron-manganese carbonate precursor and a copper source, wherein the Cu element has a fluxing effect, and helps to coordinate the melting and decomposition of the nickel-iron-manganese carbonate precursor to obtain a copper-nickel-iron-manganese oxide with a loose porous structure; the structure is conducive to the embedding of sodium ions during the next step of mixing and calcining with a sodium source, and the inherent loose porous structure of the oxide raw material is maintained to the greatest extent during the calcination process, thereby obtaining a positive electrode material with a three-dimensionally connected nanopore structure. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0042] Figure 1 The XRD diagram of the high-rate positive electrode material prepared in Example 1 provided by the present invention;
[0043] Figure 2 This is a SEM image of the high-rate positive electrode material prepared in Example 1 provided by the present invention. DETAILED DESCRIPTION
[0044] The technical scheme of the present invention will be clearly and completely described below in conjunction with the accompanying drawings and specific embodiments, but it will be understood by those skilled in the art that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work are within the scope of protection of the present invention. If specific conditions are not specified in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not specified in the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0045] If there is no special explanation, in the present invention, "the first aspect", "the second aspect", "the third aspect", "the fourth aspect", etc. are only used for descriptive purposes and cannot be understood as indicating or implying relative importance or quantity, nor can they be understood as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "the first", "the second", "the third", "the fourth", etc. only serve the purpose of non-exhaustive enumeration and description, and it should be understood that they do not constitute a closed limitation on quantity.
[0046] If there is no special explanation, the "include" and "comprising" mentioned in the present invention represent open-ended or closed-ended expressions. For example, the "include" and "comprising" may represent that other components not listed may also be included or only the listed components may be included or only the listed components may be included.
[0047] If there is no special explanation, in the present invention, "one or more" or "at least one" refers to any one, any two or more of the listed items. Among them, "several" refers to any two or more of the listed items.
[0048] In a first aspect, the present invention provides a high-rate cathode material having three-dimensional nanopores for sodium ion batteries, wherein the chemical formula of the high-rate cathode material is Na k Cu 1-h M h O2, wherein 0.8≤k≤1, 0.95≤h<1, and M includes at least Ni, Mn and Fe elements.
[0049] Among them, k includes but is not limited to any one of the point values of 0.8, 0.85, 0.9, 0.95, and 1, or a range of values between any two of them; h includes but is not limited to any one of the point values of 0.95, 0.96, 0.97, 0.98, 0.99, and 0.999, or a range of values between any two of them.
[0050] The high-rate positive electrode material includes secondary particles having a three-dimensionally connected nanopore structure formed by stacking and interlacing nanosheet layered primary particles.
[0051] The particles of the high-rate positive electrode material provided by the present invention have a special three-dimensional structure, specifically, thin nanosheets are stacked and interlaced to form three-dimensionally connected nanopores.
[0052] The high-rate positive electrode material provided by the present invention contains a specific content of Cu element, and the Cu element in the positive electrode material at least has the functions of fluxing and promoting the formation of a three-dimensional interconnected nano-pore structure.
[0053] Among them, the three-dimensional pore structure can increase the contact and wetting effect between the electrolyte and the positive electrode material, shorten the sodium ion transmission path, and the three-dimensional connected layer structure can effectively improve the electron conduction ability. Therefore, the positive electrode material provided by the present invention has excellent rate performance.
[0054] In some specific embodiments, the morphology of the nanosheet layered primary particles is thin sheet-like, and the thickness d1 of the nanosheet layered primary particles satisfies 0.05μm<d1<0.5μm; including but not limited to any point value of 0.06μm, 0.1μm, 0.15μm, 0.2μm, 0.25μm, 0.3μm, 0.35μm, 0.4μm, 0.45μm, 0.49μm or the range value between any two of them.
[0055] In some specific embodiments, the three-dimensional pore size d2 of the nanopore structure satisfies 0.1μm<d2<0.9μm; including but not limited to any point value of 0.11μm, 0.2μm, 0.3μm, 0.4μm, 0.5μm, 0.6μm, 0.7μm, 0.8μm, 0.85μm, 0.89μm or the range value between any two of them.
[0056] In some specific embodiments, the shape of the secondary particles includes a spherical shape; it can be understood that the spherical shape includes a quasi-spherical shape.
[0057] That is to say, the high-rate positive electrode material is a spherical secondary particle formed by stacking and interlacing flaky primary particles, and the surface of the spherical secondary particle has a plurality of nanopore structures.
[0058] In some specific embodiments, the particle size D of the high rate positive electrode material is 50 Satisfy 8μm<D 50 <15μm; including but not limited to any point value of 8.1μm, 9μm, 10μm, 11μm, 12μm, 13μm, 14μm, 14.8μm or a range value between any two of them.
[0059] In some specific embodiments, M also includes at least one of the elements Zn, Ti, Mg, Zr, Y, Ca, Sr, B, Co, Al and La, for example, two, three, four or more thereof.
[0060] In some specific embodiments, the high-rate positive electrode material is an O3 phase layered oxide.
[0061] The three-dimensional pore structure enables the high-rate cathode material provided by the present invention to have a large specific surface area. In some specific embodiments, the specific surface area of the high-rate cathode material satisfies BET of 1 m 2 / g<BET<2.5m 2 / g; including but not limited to 1.1m 2 / g, 1.3m 2 / g, 1.5m 2 / g, 1.8m 2 / g, 2m 2 / g, 2.1m 2 / g, 2.2m 2 / g, 2.3m 2 / g, 2.4m 2 / g, 2.49m 2 / g, or a range of values between them.
[0062] Moreover, the large number of nanopore structures enables the high-rate positive electrode material provided by the present invention to have a smaller tap density.
[0063] In some specific embodiments, the tap density TD of the high-rate positive electrode material satisfies 1 g / cm 3 <TD<1.8g / cm 3 , where TD includes but is not limited to 1.1 g / cm 3 , 1.2g / cm 3 , 1.3g / cm 3 , 1.4g / cm 3 , 1.5g / cm 3 , 1.6g / cm 3 , 1.7g / cm 3 Any point value in or any range of values between them.
[0064] In some specific embodiments, the rate performance of the battery containing the high-rate positive electrode material is 2C / 0.2C>0.90, including but not limited to any point value of 0.91, 0.92, 0.93, 0.94, 0.95, 0.96, 0.98 or a range value between any two of them; 5C / 0.2C>0.85, including but not limited to any point value of 0.86, 0.88, 0.90, 0.91, 0.92, 0.93, 0.95 or a range value between any two of them.
[0065] It can be seen that the secondary battery prepared by using the high-rate positive electrode material provided by the present invention has good rate performance.
[0066] In some specific embodiments, the molar amounts of Ni, Fe, Mn and Zn, Ti, Mg, Zr, Y, Ca, Sr, B, Co, Al and La elements in the high-rate positive electrode material include any molar ratios commonly used in the art.
[0067] As an example, the molar ratio of Ni, Fe, and Mn elements in the high-rate positive electrode material is 0.2-0.4: 0.1-0.4: 0.3-0.6, but it is not limited thereto.
[0068] The other elements in the high-rate positive electrode material except Cu, Ni, Fe, and Mn are trace added elements. As an example, their usage is controlled to be less than 0.05 (that is, the ratio of the molar amount of the Na element to the total molar amount of the other elements except Cu, Ni, Fe, and Mn is 0.8-1:0.05), but it is not limited to this.
[0069] In some specific embodiments, the high-rate positive electrode material is mainly obtained by mixing a nickel-iron-manganese carbonate precursor with a copper source and calcining it once, and then mixing it with a sodium source and calcining it twice.
[0070] In a second aspect, the present invention provides a method for preparing the above-mentioned high-rate positive electrode material, comprising the following steps:
[0071] The nickel-iron-manganese carbonate precursor and the copper source are uniformly mixed and sintered, and copper-nickel-iron-manganese oxide is obtained after cooling.
[0072] The chemical formula of copper-nickel-iron-manganese oxide is Cu 1-a M a O y , wherein the oxygen coefficient satisfies 1<y<2, the M value satisfies 0.95≤a<1, and M includes at least Ni, Mn and Fe elements.
[0073] The Cu element added in this step has a fluxing effect, which helps to coordinate the melting decomposition of the nickel-iron-manganese carbonate precursor to obtain a copper-nickel-iron-manganese oxide with a loose porous structure; this structure is conducive to the embedding of sodium ions in the next calcination process, and maintains the inherent loose porous structure of the oxide raw material to the greatest extent during the calcination process.
[0074] The copper-nickel-iron-manganese oxide is mixed with a sodium source and then calcined, and then cooled to obtain the high-rate positive electrode material.
[0075] The method for preparing a high-rate positive electrode material provided by the present invention is conducive to forming a loose and porous positive electrode material with a three-dimensionally connected nanopore structure, thereby improving its rate performance.
[0076] In some specific embodiments, the nickel iron manganese carbonate precursor is a fluffy carbonate material. Specifically, the specific surface area of the nickel iron manganese carbonate precursor is greater than 30 m 2 / g, including but not limited to 30.5m 2 / g, 31m 2 / g, 31.5m 2 / g, 32m 2 / g or any point value or range value between any two; the bulk density AD of the nickel-iron-manganese carbonate precursor satisfies 0.8 g / cm 3 <AD<1.5g / cm 3 , including but not limited to 0.81g / cm 3 , 0.85g / cm 3 , 0.9g / cm 3 , 1g / cm 3 , 1.1g / cm 3 , 1.2g / cm 3 , 1.3g / cm 3 , 1.4g / cm 3 , 1.48g / cm 3 Any point value or any range value between the two; The particle size D of the nickel iron manganese carbonate precursor 50 It is 8 to 15 μm, including but not limited to any point value of 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, and 14.8 μm, or a range value between any two of them.
[0077] In some specific embodiments, the sintering temperature is 500-700°C, including but not limited to any one of 500°C, 550°C, 600°C, 650°C, and 700°C, or a range between any two of them; the holding time is ≥10h, including but not limited to any one of 10h, 12h, 14h, 15h, 18h, 20h, 22h, 24h, 30h, and 48h, or a range between any two of them.
[0078] In some specific embodiments, the sintering is performed in an oxygen-containing atmosphere, such as an air atmosphere or an oxygen atmosphere.
[0079] In some specific embodiments, the calcination temperature is 770-870°C, including but not limited to any one of 770°C, 780°C, 790°C, 800°C, 810°C, 820°C, 830°C, 840°C, 850°C, 870°C or any range between two of them; the insulation time is ≥10h, including but not limited to any one of 10h, 12h, 14h, 15h, 18h, 20h, 22h, 24h, 30h, 48h or any range between two of them.
[0080] In some specific embodiments, the calcination is performed in an oxygen-containing atmosphere, such as an air atmosphere or an oxygen atmosphere.
[0081] In some specific embodiments, during the process of mixing the copper-nickel-iron-manganese oxide with the sodium source, a dopant containing at least one element selected from the group consisting of Zn, Ti, Mg, Zr, Y, Ca, Sr, B, Co, Al and La is also added.
[0082] In some specific embodiments, the dopant containing at least one element among Zn, Ti, Mg, Zr, Y, Ca, Sr, B, Co, Al and La includes an oxide, hydroxide or carbonate containing at least one element among Zn, Ti, Mg, Zr, Y, Ca, Sr, B, Co, Al and La, such as calcium carbonate, zirconium oxide, aluminum hydroxide, magnesium hydroxide, etc., but is not limited thereto.
[0083] In some specific embodiments, the copper source includes a nano copper source. The use of a nano copper source can make the sintering and fluxing uniform, and improve the purity of the obtained positive electrode material.
[0084] In some specific embodiments, the nano copper source includes but is not limited to nano copper oxide.
[0085] In some specific embodiments, the sodium source includes a sodium-containing compound, such as sodium carbonate, but is not limited thereto.
[0086] In some specific embodiments, the preparation method of the nickel-iron-manganese carbonate precursor includes: mixing a nickel-iron-manganese ternary salt solution with a precipitant solution and performing a co-precipitation reaction, and after the co-precipitation reaction is completed, separating the solid and the liquid, washing and drying to obtain the nickel-iron-manganese carbonate precursor.
[0087] Wherein, the precipitant solution comprises a mixed solution of sodium carbonate solution and ammonia water, and the molar ratio of sodium carbonate to ammonia monohydrate in the precipitant solution is greater than 20:1, including but not limited to any point value of 21:1, 22:1, 23:1, 24:1, 25:1, 26:1, 28:1, 30:1 or a range value between any two of them. Wherein, ammonia monohydrate is mainly used to provide an alkaline co-precipitation environment and a complexing effect; sodium carbonate is mainly used to provide sufficient carbonate ions for precipitating metals. The above molar ratio is conducive to the formation of a nickel-iron-manganese carbonate precursor with fine whiskers and a fluffy shape.
[0088] In some specific embodiments, the total molar concentration of the metal elements in the nickel-iron-manganese ternary salt solution is 0.2-0.8 mol / L, including but not limited to any point value of 0.2 mol / L, 0.3 mol / L, 0.4 mol / L, 0.5 mol / L, 0.6 mol / L, 0.7 mol / L, 0.8 mol / L or a range value between any two of them. The total molar concentration of the metal elements refers to the sum of the molar concentrations of the three elements nickel, iron and manganese.
[0089] In some specific embodiments, the molar concentration of sodium carbonate in the precipitant solution is 0.2-0.8 mol / L, including but not limited to any one of 0.2 mol / L, 0.3 mol / L, 0.4 mol / L, 0.5 mol / L, 0.6 mol / L, 0.7 mol / L, 0.8 mol / L or a range between any two of them.
[0090] In some specific embodiments, the coprecipitation reaction temperature is 40-70°C, including but not limited to any point value of 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C or any range value between two of them.
[0091] In some specific embodiments, the pH of the coprecipitation reaction is 8-10, including but not limited to any one of 8, 8.5, 9, 9.5, 10 or a range between any two of them.
[0092] By controlling the coprecipitation reaction to meet the above reaction conditions (including the total molar concentration of metal elements in the nickel-iron-manganese ternary salt solution, the molar concentration of sodium carbonate in the precipitant solution, the molar ratio of sodium carbonate to ammonia monohydrate, the pH of the coprecipitation reaction, etc.), it is beneficial to obtain whiskers that are finer and fluffy and meet the required specific surface area, bulk density and particle size D 50 Nickel-iron-manganese carbonate precursor.
[0093] In some specific implementations, the pH is maintained between 8 and 10 by adjusting the addition ratio of the nickel-iron-manganese ternary salt solution and the precipitant solution.
[0094] In a third aspect, the present invention provides a positive electrode sheet comprising the above-mentioned high-rate positive electrode material.
[0095] The battery made from the positive electrode sheet has excellent rate performance.
[0096] Optionally, the positive electrode sheet further includes at least one of a binder and a conductive agent, which is not limited in the present invention.
[0097] In a fourth aspect, the present invention provides a sodium ion battery comprising the above-mentioned positive electrode sheet.
[0098] The sodium ion battery has good rate performance, with rate performance of 2C / 0.2C>0.90 and 5C / 0.2C>0.85.
[0099] Optionally, the sodium ion battery further includes a negative electrode sheet, a separator and an electrolyte, and any materials or reagents commonly used in the art may be used, and the present invention is not limited thereto.
[0100] The embodiments of the present invention will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present invention and should not be considered as limiting the scope of the present invention. If no specific conditions are specified in the examples, the conditions are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be obtained commercially.
[0101] Example 1
[0102] The high-rate positive electrode material Na 0.8 Cu 0.05 Ni 0.25 Fe 0.2 Mn 0.5 The preparation method of O2 comprises the following steps:
[0103] (1) Preparation of nickel iron manganese carbonate precursor Ni 0.25 Fe 0.2 Mn 0.5 (CO3) 0.95 :
[0104] Nickel sulfate, ferrous sulfate, manganese sulfate and water are prepared into a nickel-iron-manganese ternary salt solution, in which the total molar concentration of the metal elements is 0.5 mol / L, and the molar ratio of Ni, Fe and Mn elements is 0.25:0.2:0.5.
[0105] A concentrated sodium carbonate solution is selected and added with a small amount of ammonia water to prepare a precipitant solution. The molar ratio of sodium carbonate to ammonia monohydrate in the obtained precipitant solution is 21:1, and the molar concentration of sodium carbonate in the precipitant solution is 0.5 mol / L.
[0106] Under nitrogen protection, the following steps are performed: using the precipitant solution as the base liquid, slowly adding the nickel-iron-manganese ternary salt solution and the precipitant solution into the base liquid at the same time, controlling the coprecipitation reaction temperature to 60°C, and adjusting the addition ratio of the nickel-iron-manganese ternary salt solution and the precipitant solution to keep the pH at 9, and always in a uniform and slow stirring state. After the coprecipitation reaction is completed, the obtained precipitated product is filtered, washed, and dried to obtain a nickel-iron-manganese carbonate precursor.
[0107] (2) The nickel iron manganese carbonate precursor obtained in step (1) is fully mixed with nano copper oxide according to the target molecular formula ratio, and sintered in a 600° C. high-temperature atmosphere furnace in an air atmosphere for 10 h to obtain copper-nickel iron-manganese oxide.
[0108] (3) The copper-nickel-iron-manganese oxide obtained in step (2) is uniformly mixed with sodium carbonate according to the target molecular formula ratio, and calcined in an air furnace at 850° C. for 10 h, crushed, and sieved to obtain the target high-rate positive electrode material.
[0109] like Figure 1 The XRD pattern of the high rate positive electrode material prepared in this embodiment is shown. Figure 1 It can be seen that the high-rate positive electrode material prepared in this embodiment is an O3 phase layered oxide.
[0110] like Figure 2 The SEM image of the high rate positive electrode material prepared in this embodiment is shown. Figure 2 It can be seen that the high-rate positive electrode material prepared in this embodiment is a three-dimensional interconnected nanopore structure formed by stacking and interlacing thin nanosheets.
[0111] Example 2
[0112] Referring to the preparation method of Example 1, a high-rate positive electrode material Na1Cu was prepared according to the target molecular formula ratio. 0.02 Ni 0.35 Fe 0.25 Mn 0.37 Mg 0.01 O2, the difference is that in step (1), the nickel iron manganese carbonate precursor Ni 0.35 Fe 0.25 Mn 0.37 (CO3) 0.97 The molar ratio of Ni, Fe and Mn elements in the nickel-iron-manganese ternary salt solution is 0.35:0.25:0.37; the sintering temperature in step (2) is 500°C and the temperature is kept for 12 hours; and, in step (3), the copper-nickel-iron-manganese oxide is uniformly mixed with sodium carbonate and magnesium hydroxide according to the target molecular formula ratio, and the calcination temperature is 770°C and the temperature is kept for 12 hours.
[0113] Example 3
[0114] Referring to the preparation method of Example 1, a high-rate positive electrode material Na 0.89 Cu 0.01 Ni 0.25 Fe 0.35 Mn 0.37 Ti 0.01 Ca 0.01 O2, the difference is that in step (1), the nickel iron manganese carbonate precursor Ni 0.25 Fe 0.35 Mn 0.37 (CO3) 0.97 The molar ratio of Ni, Fe and Mn elements in the nickel-iron-manganese ternary salt solution is 0.25:0.35:0.37; the sintering temperature in step (2) is 700°C and the temperature is kept for 15 hours; and, in step (3), the copper-nickel-iron-manganese oxide is uniformly mixed with sodium carbonate, titanium dioxide and calcium carbonate according to the target molecular formula ratio, and the calcination temperature is 870°C and the temperature is kept for 15 hours.
[0115] Example 4
[0116] Referring to the preparation method of Example 1, a high-rate positive electrode material Na 0.9 Cu 0.03 Ni 0.3 Fe 0.22 Mn 0.44 Zn 0.002 Sr 0.002 La 0.002 Zr 0.004 O2, the difference is that in step (1), the nickel iron manganese carbonate precursor Ni 0.3 Fe 0.22 Mn 0.44 (CO3) 0.96 The molar ratio of Ni, Fe and Mn elements in the nickel-iron-manganese ternary salt solution is 0.3:0.22:0.44; the sintering temperature in step (2) is 600°C and the temperature is kept for 15 hours; and, in step (3), copper-nickel-iron-manganese oxide is uniformly mixed with sodium carbonate, zinc oxide, strontium oxide, lanthanum oxide and zirconium dioxide according to the target molecular formula ratio, and the calcination temperature is 800°C and the temperature is kept for 15 hours.
[0117] Example 5
[0118] Referring to the preparation method of Example 4, a high-rate positive electrode material Na 0.9 Cu 0.03 Ni 0.3 Fe 0.22 Mn 0.44 Y 0.002 B 0.002 Co 0.002 Al 0.004 O2, the difference is that in step (3), the copper-nickel-iron-manganese oxide is uniformly mixed with sodium carbonate, yttrium oxide, boron trioxide, cobalt oxide and aluminum hydroxide according to the target molecular formula ratio.
[0119] Example 6
[0120] The high-rate positive electrode material Na 0.8 Cu 0.05 Ni 0.25 Fe 0.2 Mn 0.5 The preparation method of O2 is basically the same as that of Example 1, except that in step (1), during the coprecipitation reaction, the ratio of the nickel-iron-manganese ternary salt solution and the precipitant solution is adjusted so that the pH is maintained at 10.
[0121] Comparative Example 1
[0122] Referring to the preparation method of Example 1, the positive electrode material Na0.8 Cu 0.053 Ni 0.249 Fe 0.199 Mn 0.499 O2, the difference is that the Cu content in the target material increases from 0.05 to 0.053, and correspondingly, in order to meet the balancing requirements, the amounts of Ni, Fe and Mn are simultaneously reduced by 0.001.
[0123] Comparative Example 2
[0124] The positive electrode material Na1Cu 0.02 Ni 0.35 Fe 0.25 Mn 0.37 Mg 0.01 The preparation method of O2 is basically the same as that of Example 2, except that nano copper oxide is not added in step (2), but nickel sulfate, ferrous sulfate, manganese sulfate, copper sulfate and water are configured into a copper-nickel-iron-manganese quaternary salt solution in step (1). Specifically, in step (1), a copper-nickel-iron-manganese carbonate precursor Cu 0.02 Ni 0.35 Fe 0.25 Mn 0.37 (CO3) 0.99 .
[0125] Comparative Example 3
[0126] The positive electrode material Na 0.89 Ni 0.253 Fe 0.353 Mn 0.373 Ti 0.01 Ca 0.01 The preparation method of O2 is basically the same as that of Example 3, except that nano copper oxide is not added in step (2).
[0127] Comparative Example 4
[0128] The positive electrode material Na 0.9 Cu 0.03 Ni 0.3 Fe 0.22 Mn 0.44 Zn 0.002 Sr 0.002 La 0.002 Zr 0.004 The preparation method of O2 is basically the same as that of Example 4, except that step (2) is not performed, but the nickel iron manganese carbonate precursor obtained in step (1) is directly mixed with sodium carbonate and nano copper oxide according to the target molecular formula ratio, and then calcination in step (3) and subsequent steps are performed.
[0129] Comparative Example 5
[0130] The positive electrode material Na 0.8 Cu 0.05 Ni 0.25 Fe 0.2 Mn 0.5 The preparation method of O2 comprises the following steps: according to the target molecular formula ratio, Cu 0.05 Ni 0.25 Fe 0.2 Mn 0.5 (OH)2 and sodium carbonate were mixed evenly, calcined in an air furnace at 850°C for 10 h, crushed and sieved to obtain a positive electrode material.
[0131] Comparative Example 6
[0132] The positive electrode material Na 0.8 Cu 0.05 Ni 0.25 Fe 0.2 Mn 0.5 The preparation method of O2 comprises the following steps: 0.25 Fe 0.2 Mn 0.5 (OH) 1.9 The copper-nickel-iron-manganese oxide was mixed with nano-copper oxide according to the target molecular formula ratio, and sintered in a 600°C high-temperature atmosphere furnace in an air atmosphere for 10 hours to obtain copper-nickel-iron-manganese oxide. The copper-nickel-iron-manganese oxide was mixed with sodium carbonate according to the target molecular formula ratio, and calcined in an air furnace at 850°C for 10 hours, crushed and sieved to obtain the positive electrode material. Among them, the specific surface area of the nickel-iron-manganese hydroxide precursor is 25m 2 / g, bulk density is 1.88g / cm 3 , particle size D 50 It is 11.5μm.
[0133] The specific surface area, bulk density and particle size D of the nickel iron manganese carbonate precursor (or copper nickel iron manganese carbonate precursor, comparative example 2) prepared in the above embodiments and comparative examples are as follows: 50 As shown in Table 1. The particle size D of the copper-nickel-iron-manganese oxide (or nickel-iron-manganese oxide, comparative example 3) prepared in each embodiment and each comparative example is 50 As shown in Table 1.
[0134] Table 1 Some indicators of intermediate products
[0135]
[0136] Experimental example
[0137] The thickness d1 of the nanosheet-like primary particles of the positive electrode materials prepared in each embodiment and each comparative example, the pore size d2 of the nanopore structure, and the particle size D 50, the specific surface area BET of the positive electrode material, and the tap density TD of the positive electrode material. The results are shown in Table 2.
[0138] The calculation method of d1 and d2 is as follows: the thickness of the lamella and the pore size on a single particle are counted by SEM, and the average value is taken. Considering the statistical accuracy error, the approximate value is taken with the minimum unit of 0.05 μm.
[0139] D 50 Test: Malvern particle size analyzer was used for testing.
[0140] Tap density TD test: Use a conventional tap density meter to test (unit: g / cm 3 ).
[0141] Furthermore, the positive electrode materials prepared in each embodiment and each comparative example were used as positive electrode active materials, and the positive electrode active materials, SP and PVDF were mixed in a mass ratio of 90:5:5, and NMP was added to make a viscous glue, which was coated on aluminum foil and baked in a vacuum drying oven at 120°C for 12 hours to obtain a positive electrode sheet. A metal sodium sheet was used as a counter electrode, glass fiber (Waterman) was used as a diaphragm, 1 mol / L NaPF6, EC:DMC (volume ratio) = 1:1 were configured as electrolytes, and 2032 button cells were assembled in an Ar protective glove box. Then, each battery was tested for rate performance as follows: in the voltage range of 2.5-4.0V, a small current of 0.2C was used for charging, and a small current of 0.2C was used for discharging to test the capacity of 0.2C (unit: mAh / g); similarly, in the voltage range of 2.5-4.0V, a large current of 2C was used for charging, and a large current of 2C was used for discharging to test the capacity of 2C (unit: mAh / g); the rate value of 2C / 0.2C was calculated, and the rate value of 5C / 0.2C was calculated by the same method.
[0142] Table 2 Some product indicators and battery rate performance results
[0143]
[0144] According to the data of each embodiment in Table 1 and Table 2, the final product obtained by the present invention is a thin nanosheet layer stacked and staggered to form a three-dimensional interconnected nanopore; the treated copper-nickel-iron-manganese oxide and the product D 50All meet 8μm<D50<15μm, the product has a relatively large specific surface area, and due to the large number of nanopores, it has a small tap density; in terms of performance, the button battery has excellent rate performance. This is because the three-dimensional pore structure and large BET can increase the contact and wetting effect between the electrolyte and the material, shorten the sodium ion transmission path, and the three-dimensional interconnected sheet structure can effectively improve the electronic conductivity. The comprehensive effect is that the material has excellent rate performance.
[0145] Comparative Example 1: Compared with Example 1, the amount of Cu added was adjusted from 0.05 to 0.053. The Cu content was too high, resulting in a significant decrease in the rate performance of the product. The main reason for the decrease was that the thickness of the sheet layer increased and the pore size became smaller.
[0146] Comparative Example 2: Compared with Example 2, the timing of adding the copper element is not suitable, and the final result is also a significant decrease in the rate performance. The main reason for the decrease is that the flakes are smaller (0.1μm) and the nanopores almost disappear (<0.05μm). It is speculated that the change in the timing of addition affects the sintering and pore-forming process of copper-nickel-iron-manganese oxide, causing the product morphology to deviate from the target morphology.
[0147] Comparative Example 3: Compared with Example 3, without adding the Cu element, the final result is that the rate performance is significantly reduced. The main reason for the reduction is that the thickness of the layer is very small and the pore size almost disappears, indicating that the lack of the fluxing effect of the copper element makes it impossible to generate a layer structure of appropriate size, and it is also impossible to further construct a three-dimensional hole structure.
[0148] Comparative Example 4: Compared with Example 4, no pre-sintering process is performed, which is consistent with the conclusion of Comparative Example 3, indicating that this process is indispensable.
[0149] Comparative Example 5: Compared with Example 1, the same proportion of materials were prepared using the conventional hydroxide precursor process in the industry, and the final d1 thickness was 0.4 μm, but it did not have a pore-forming effect, that is, there was no nanopore size. It was further manifested in a higher tap density and a smaller BET. The rate performance was significantly lower than that of Example 1, indicating that conventional processes cannot achieve the effects of the present invention.
[0150] Comparative Example 6: Compared with Example 1, a conventional hydroxide precursor was used for mono- and di-calcination. Similar to the conclusion of Comparative Example 5, the rate performance was significantly lower than that of Example 1, indicating that conventional processes cannot achieve the effects of the present invention.
[0151] Although the present invention has been illustrated and described with specific embodiments, it should be appreciated that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Those skilled in the art should understand that the technical solutions described in the above embodiments may be modified, or some or all of the technical features thereof may be replaced by equivalents without departing from the spirit and scope of the present invention. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention. Therefore, this means that all such replacements and modifications within the scope of the present invention are included in the appended claims.
Claims
1. A high rate positive electrode material, characterized in that: The chemical formula of the high-rate positive electrode material is Na k Cu 1-h M h O2, wherein 0.8≤k≤1, 0.95≤h<1, and M includes at least Ni, Mn and Fe elements; The high-rate positive electrode material includes secondary particles having a three-dimensionally connected nanopore structure formed by stacking and interlacing nanosheet layered primary particles.
2. The high-rate positive electrode material according to claim 1, characterized in that: At least one of the following conditions is met: (1) The thickness d1 of the nanosheet-like primary particles satisfies 0.05 μm<d1<0.5 μm; (2) The pore size d2 of the nanopore structure satisfies 0.1 μm<d2<0.9 μm; (3) The shape of the secondary particles includes spherical; (4) The particle size D of the high-rate positive electrode material 50 Satisfy 8μm<D 50 <15μm.
3. The high-rate positive electrode material according to claim 1, characterized in that: At least one of the following conditions is met: (1) M further includes at least one of Zn, Ti, Mg, Zr, Y, Ca, Sr, B, Co, Al and La; (2) The high-rate positive electrode material is an O3 phase layered oxide; (3) The specific surface area of the high-rate positive electrode material satisfies the BET requirement of 1 m 2 / g<BET<2.5m 2 / g; (4) The tap density TD of the high-rate positive electrode material satisfies 1 g / cm 3 <TD<1.8g / cm 3 .
4. The high-rate positive electrode material according to claim 1, characterized in that: The rate performance of the battery containing the high-rate positive electrode material satisfies: 2C / 0.2C>0.90, 5C / 0.2C>0.
85.
5. The method for preparing a high-rate positive electrode material according to any one of claims 1 to 4, characterized in that: The steps include: The nickel-iron-manganese carbonate precursor and the copper source are mixed and sintered to obtain copper-nickel-iron-manganese oxide; The copper-nickel-iron-manganese oxide is mixed with a sodium source and then calcined to obtain the high-rate positive electrode material.
6. The method for preparing a high-rate positive electrode material according to claim 5, characterized in that: At least one of the following conditions is met: (1) The specific surface area of the nickel-iron-manganese carbonate precursor is greater than 30 m 2 / g, the bulk density AD meets 0.8g / cm 3 <AD<1.5g / cm 3 , particle size D 50 8~15μm; (2) The sintering temperature is 500-700° C. and the holding time is ≥10 h; (3) The calcination temperature is 770-870° C. and the holding time is ≥10 h; (4) in the process of mixing the copper-nickel-iron-manganese oxide with the sodium source, a dopant containing at least one element selected from the group consisting of Zn, Ti, Mg, Zr, Y, Ca, Sr, B, Co, Al and La is also added; (5) The copper source includes a nano copper source.
7. The method for preparing a high-rate positive electrode material according to claim 5, characterized in that: The preparation method of the nickel-iron-manganese carbonate precursor comprises: mixing a nickel-iron-manganese ternary salt solution with a precipitant solution and performing a coprecipitation reaction, and obtaining the nickel-iron-manganese carbonate precursor after solid-liquid separation; The precipitant solution comprises a mixed solution of sodium carbonate solution and ammonia water, and the molar ratio of sodium carbonate to ammonia monohydrate in the precipitant solution is greater than 20:
1.
8. The method for preparing a high-rate positive electrode material according to claim 7, characterized in that: At least one of the following conditions is met: (1) The total molar concentration of metal elements in the nickel-iron-manganese ternary salt solution is 0.2-0.8 mol / L; (2) the molar concentration of sodium carbonate in the precipitant solution is 0.2 to 0.8 mol / L; (3) The temperature of the coprecipitation reaction is 40 to 70° C.; (4) The pH of the coprecipitation reaction is 8-10.
9. A positive electrode sheet, characterized in that: It comprises the high-rate positive electrode material as claimed in any one of claims 1 to 4.
10. A sodium ion battery, characterized in that: Comprising the positive electrode sheet as claimed in claim 9.
Citation Information
Cited By
Sodium battery positive electrode material and preparation method and application thereof
CN119764437A
Positive electrode material, preparation method thereof and sodium ion battery
CN120690856A