Sodium-ion battery positive electrode material as well as preparation method and application thereof

By using fluoroaluminum magnesium sodaite structure and metal doping technology in the positive electrode material of sodium ion battery, the triangular phase of the P3121 space group is formed, and the low capacity, poor rate performance and poor long cycle performance of sodium ion battery positive electrode material is solved. Problem, high stability and high capacity battery performance are achieved.

CN118919718APending Publication Date: 2024-11-08ZHENGZHOU NEW CENTURY MATERIALS GENOME INST CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410952943.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing positive electrode materials of sodium ion batteries have problems such as low capacity, poor rate performance and poor long cycle performance, resulting in low energy density and poor battery life of sodium ion batteries.

Method used

The positive electrode material of sodium ion battery based on fluoroaluminum magnesium sodaite structure is adopted. The chemical formula is NaaMb1M”b2M’1-b1-b2NcN’1-cX7+d. The metal and X are strengthened by doping of M, M” and N metals. The chemical bonds of the P3121 space group form the triangular phase, improve the stability of the structural skeleton and the electronic conductivity, avoid structural collapse, and improve capacity and rate performance.

Benefits of technology

The high ionic conductivity, good electronic conductivity and zero volume changes of sodium ion batteries are achieved, which significantly improves the battery cycle stability and capacity retention rate, and solves the problems of low energy density and poor endurance of sodium ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919718A_ABST
    Figure CN118919718A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of secondary batteries, and particularly relates to a sodium ion battery positive electrode material and a preparation method and application thereof. The chemical formula of the positive electrode material of the sodium ion battery is NaaMb1M'b2M '1-b1-b2NcN' 1-cX7 + d, M is trivalent metal, N is divalent metal, M'and M 'are different trivalent transition metal, N' is divalent transition metal, X is halogen element, 1.75 < = a < = 2.25, 0 < = b1 < = 0.05, 0 < = b2 < = 0.33, 0 < = c < = 0.05,-0.25 < = d < = 0.25, and b1, b2 and c are not 0 at the same time. On the basis of the structural characteristics of the fluorine-aluminum-magnesium-sodium stone type, large surface spacing is beneficial to rapid transportation of sodium ions, chemical bonds between metal and X are strengthened through doping of M and / or N metal, the structural framework stability is greatly improved, the electronic conductivity is further enhanced, the problem of structural collapse of Na2TiFeF7 in the battery circulation process is avoided, and the service life of the Na2TiFeF7 battery is prolonged. The long cycle stability is greatly improved, and the capacity and the rate capability can be greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of secondary batteries, and in particular to a sodium ion battery positive electrode material and a preparation method and application thereof. Background Art

[0002] Nowadays, lithium-ion batteries (LIBs) are widely used as power sources in portable electronic devices and electric vehicles due to their high energy density and long cycle life. However, the limited global lithium reserves have raised concerns about a resource crisis, which may hinder the sustainable development and utilization of LIBs. This issue has become more urgent as the transition to a low-carbon economy drives increasing demand. Therefore, there is an urgent need to develop next-generation metal-ion batteries that rely on more sustainable resources, including but not limited to Na + , K + Mg 2+ 、Zn 2+ and other viable options.

[0003] Taking sodium-ion batteries as an example, currently, commercial cathode materials for sodium-ion batteries mainly include layered transition metal oxides, Prussian blue / white compounds, and polyanionic compounds. However, there are many shortcomings in materials, such as the poor battery cycle stability of layered transition metal oxides; the introduction of toxic groups CN- in the synthesis and preparation of Prussian blue / white compounds poses a great safety hazard; and polyanionic compounds cannot achieve high sodium storage capacity due to their heavy skeletons.

[0004] Fluoride sodium ion batteries have good advantages in high voltage resistance. The large ionic radius of sodium ions makes it difficult to transport in densely packed fluorinated octahedron or fluorinated tetrahedron structures. Therefore, in a fluorinated chemical environment, in order to achieve rapid diffusion of sodium ions, the sodium electrode material needs to have a cage-like or large lattice gap, and the coordination number between sodium ions and surrounding F ions must be greater than six. In addition, sodium ions with large ionic radius will cause drastic changes in the volume of active materials during the embedding or de-embedding process of the positive electrode, and even cause complex irreversible phase changes, resulting in battery capacity loss.

[0005] The Korean patent application with application publication number KR1020230037373A, which was published on March 16, 2023, discloses a positive electrode material for a sodium battery, comprising a sodium metal fluoride having a trigonal crystal structure and a three-dimensional sodium ion channel for embedding or de-embedding sodium ions in the crystal structure, with a chemical formula of Na x M yF7, M is a transition metal, 0≤x≤3, 1≤y≤3, through the three-dimensional sodium ion channel, it is easy to produce a three-dimensional ion diffusion path of sodium ions to the negative electrode material body. In the negative electrode material with a three-dimensional sodium ion channel, the insertion or desorption of sodium ions proceeds as a single-phase reaction without phase change. x M y F7 still has problems of low capacity and poor rate performance.

[0006] On March 3, 2022, Jungmin Kang et al. published in Highly Stable Fe 2+ / Ti 3+ -Based FluorideCathode Enabling Low-Cost and High-Performance Na-Ion Batteries" discloses that Na2TiFeF7 composed of three-dimensionally interconnected (Fe,Ti)F6 octahedra has a performance of 185 mAh g at C / 20. -1 The specific capacity of Na2TiFeF7 is 71% after 600 cycles at 1C. However, the structure of Na2TiFeF7 is unstable. During the battery cycle, the structure collapses, and the battery cannot be cycled stably for a long time. The capacity is low and the rate performance is poor. In addition, the research and development of high-load sodium positive electrodes is of great significance, which greatly improves the energy storage capacity of sodium batteries at this stage, thereby extending the use time without charging. This is especially beneficial for various high-energy consumption applications that require a reliable and long-lasting source of electricity. Summary of the invention

[0007] The purpose of the present invention is to provide a sodium ion battery positive electrode material to solve the problems of low capacity, poor rate performance and poor long cycle performance in the prior art.

[0008] The second object of the present invention is to provide a method for preparing a positive electrode material for a sodium ion battery, so as to solve the problems of low capacity, poor rate performance and poor long cycle performance existing in the prior art.

[0009] The third object of the present invention is to provide an application of a sodium ion battery positive electrode material to solve the problems of low energy density and poor endurance of sodium ion batteries.

[0010] In order to solve the above technical problems, the technical solution of the sodium ion battery positive electrode material of the present invention is:

[0011] A sodium ion battery positive electrode material, the chemical formula of the positive electrode material is Na a M b1 M” b2 M' 1-b1-b2 N c N'1- c X 7+d , wherein M is a trivalent metal, N is a divalent metal, M” and M’ are different trivalent transition metals respectively, N’ is a divalent transition metal, X is a halogen element, 1.75 ≤ a ≤ 2.25, 0 ≤ b1 ≤ 0.05, 0 ≤ b2 ≤ 0.33, 0 ≤ c ≤ 0.05, -0.25 ≤ d ≤ 0.25, and b1, b2, and c are not simultaneously 0.

[0012] The present invention is an improvement on the prior art, providing a cathode material for a sodium-ion battery. Based on the structural characteristics of the fluoroaluminosodiummagnesite type, it belongs to the trigonal phase of the P3121 space group and is composed of MX6 sharing common vertices to form a stacked cage structure. Na + has small structural changes during the delamination / intercalation process and has a large interplanar spacing greater than on the (022) plane. The large interplanar spacing helps the rapid transport of sodium ions. Through the doping of M, M”, and N metals, the chemical bond between the metal and X is strengthened, greatly enhancing the stability of its structural framework, further enhancing the electronic conductivity, avoiding the problem of structural collapse of Na2TiFeF7 during the battery cycling process, greatly improving the long-term cycling stability, and being able to significantly improve the capacity and rate performance.

[0013] The cathode material for a sodium-ion battery provided by the present invention has three-dimensional equivalent ultrafast sodium-ion transport ability and stable thermodynamic properties. Compared with traditional sodium-ion battery cathodes, it has advantages such as ultra-high ionic conductivity, good electronic conductivity, zero volume change, excellent battery cycling stability, and no resource problems.

[0014] To further improve the stability of the structural framework and improve the capacity and rate performance, preferably, M’ is Ti, M” is Mn, M is Al, N’ is Fe, and N is Mg.

[0015] To further improve the chemical bonding between the metal and X, preferably, X is F.

[0016] To further improve the doping effect of the metal, preferably, the chemical formula of the cathode material is Na2Al b1 Ti 1- b1 Mg c Fe 1-c F7, wherein 0 < b1 ≤ 0.05, 0 < c ≤ 0.02; or it is Na2Al b1 Mn b2 Ti 1-b1-b2FeF7, where 0 < b1 ≤ 0.05 and 0 < b2 ≤ 0.33. Under the doping of Al and Mg, the structural framework stability is greatly improved, making it an excellent cathode material for sodium-ion batteries, enabling stable long cycling. After 200 cycles, the capacity retention rate is still above 90%. Na2Al b1 Ti 1-b1 Mg c Fe 1-c F7 can be used as the standard stoichiometry. When a deviates from the standard stoichiometry (the deviation amount is less than 15%), under the condition of ensuring the electroneutrality of the material, the stoichiometric ratio of M or F will deviate accordingly (the deviation amount is less than 15%).

[0017] To further improve the sodium-ion mobility, preferably, the crystal structure of the cathode material belongs to the trigonal phase of the P3121 space group, and the interplanar spacing of the (022) crystal plane is greater than

[0018] To further improve the electrochemical performance, preferably, the chemical formula of the cathode material is Na2Al 0.05 Ti 0.95 FeF7 or Na2Mg 0.05 TiFe 0.95 F7 or Na2Al 0.05 Ti 0.95 Mg 0.01 Fe 0.99 F7 or Na2Al 0.02 Ti 0.98 Mg 0.02 Fe 0.98 F7 or Na2Al 0.01 Ti 0.66 Mn 0.33 FeF7.

[0019] The technical solution of the preparation method of the cathode material for sodium-ion batteries of the present invention is as follows:

[0020] A preparation method of a cathode material for sodium-ion batteries includes the following steps: Mix the metal fluorides of Na, M, M', M", N, and N' under an inert gas condition and then perform ball milling treatment to obtain a precursor, and then cool the precursor after vacuum heat treatment. The temperature of the vacuum heat treatment is 500 - 650 °C, and the time of the vacuum heat treatment is 60 - 90 min.

[0021] The method for preparing a positive electrode material for a sodium ion battery provided by the present invention has a triangular phase of a P3121 space group, a large interplanar spacing is conducive to the rapid transport of sodium ions, and the chemical bond between the metal and X is strengthened by doping with M and / or N metals, thereby greatly improving the stability of its structural skeleton, further enhancing the electronic conductivity, avoiding the problem of structural collapse of Na2TiFeF7 during battery cycling, greatly improving long-cycle stability, and being able to greatly improve capacity and rate performance, and can be obtained by simple heat treatment, with a simple and efficient process, and being suitable for large-scale industrial production.

[0022] In order to further improve the doping uniformity, preferably, the rotation speed of the ball milling treatment is 300-500 rpm, and the time of the ball milling treatment is 12-18 hours. It should be noted that the time of the ball milling treatment refers to the effective time of the ball milling treatment.

[0023] The technical solution for the application of the sodium ion battery positive electrode material of the present invention is:

[0024] An application of a sodium ion battery positive electrode material, wherein the sodium ion battery positive electrode material, a conductive material and a binder are mixed and then rolled to obtain a positive electrode sheet.

[0025] The application of the sodium ion battery positive electrode material provided by the present invention is based on the positive electrode material with a triangular phase of the P3121 space group, which can maintain high ionic conductivity and excellent electronic conductivity throughout the entire charge and discharge process, and is composited with a conductive material to prepare a high-load electrode sheet with high loading capacity and high utilization rate of active materials without obvious capacity decay, thereby solving the problems of low energy density and poor endurance of sodium ion batteries; due to its own high ionic and electronic conductivity, the electric field within the high load is uniform, there is no serious polarization problem, and the active material in the high-load positive electrode sheet can be fully mobilized.

[0026] In order to further improve the conductivity of the positive electrode plate, preferably, the conductive material is selected from one or more of conductive carbon black, graphene and carbon nanotubes.

[0027] In order to further improve the conductivity of the positive electrode sheet, preferably, the mass ratio of the sodium ion battery positive electrode material, conductive carbon black, graphene and carbon nanotubes is (80-90): (8.65-9.5): (8.65-9.5): (2.7-3). By compounding with high-quality graphene with extremely low lattice defect rate, the charge transfer and ion transport are effectively improved, and the high-load electrode sheet prepared has a loading capacity of 10-13 mg / cm 2 .

[0028] In order to further improve the stability of the positive electrode sheet, preferably, the sodium ion battery positive electrode material and the conductive material are mixed to form a positive electrode active material, and the mass ratio of the positive electrode active material to the binder is (90-95):(5-10).

[0029] In order to further improve the uniformity of the positive electrode sheet, preferably, the sodium ion battery positive electrode material and the conductive material are ball-milled to obtain a positive electrode active material, and then the positive electrode active material and the binder are mixed and roll-pressed to obtain a positive electrode sheet.

[0030] In order to further improve the uniformity of the ball milling treatment, preferably, when the sodium ion battery positive electrode material and the conductive material are ball milled, the rotation speed of the ball milling treatment is 150-200 rpm, and the ball milling treatment time is 8-12 hours. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 is the crystal structure diagram of Na2MNX7;

[0032] Figure 2 The sodium ion positive electrode material Na2Al of Example 4 0.02 Ti 0.98 Mg 0.02 Fe 0.98 XRD pattern of F7;

[0033] Figure 3 The sodium ion positive electrode material Na2Al of Example 4 0.02 Ti 0.98 Mg 0.02 Fe 0.98 TEM image of F7;

[0034] Figure 4 The sodium ion positive electrode material Na2Al of Example 4 0.02 Ti 0.98 Mg 0.02 Fe 0.98 F7 electronic conductivity test results diagram;

[0035] Figure 5 The sodium ion positive electrode material Na2Al of Example 4 0.02 Ti 0.98 Mg 0.02 Fe 0.98 Impedance spectrum of F7;

[0036] Figure 6 The sodium ion positive electrode material Na2Al of Example 4 0.02 Ti 0.98 Mg 0.02 Fe 0.98 Comparison chart of F7’s charge and discharge performance test. DETAILED DESCRIPTION

[0037] The technical concept of the sodium ion battery positive electrode material provided by the present invention is as follows:

[0038] A sodium ion battery positive electrode material, the chemical formula of the positive electrode material is Na a M b1 M” b2 M' 1-b1-b2 N c N' 1- c X 7+d , wherein M is a trivalent metal, N is a divalent metal, M” and M’ are different trivalent transition metals, N’ is a divalent transition metal, X is a halogen element, 1.75≤a≤2.25, 0≤b1≤0.05, 0≤b2≤0.33, 0≤c≤0.05, -0.25≤d≤0.25, and b1, b2, and c are not all 0 at the same time.

[0039] The sodium ion battery cathode material provided by the present invention is based on the structural characteristics of fluorinated aluminum magnesium sodium nitrite. The crystal structure of Na2MNX7 is as follows: Figure 1 As shown, the triangular phase belongs to the P3121 space group, which is composed of MX6 vertices forming a cage-like structure. The M' and N' sublattices are mainly occupied by ions. The M' and / or N' sublattices contain a small amount of metal ions of the same valence, that is, M and / or M" doping the M' sublattice, or N doping the N' sublattice. The doped ion radius is smaller than the main ion radius. The X sublattice is mainly occupied by halogen anions. A small amount of X sublattice can be doped by other halogen anions or anion functional groups. Na + The structural change during the delamination / intercalation process is small, and the (022) plane has a larger The large interplanar spacing is conducive to the rapid transport of sodium ions. The chemical bond between the metal and X is strengthened by the doping of M, M”, and N metals, which greatly improves the stability of its structural skeleton and the electronic conductivity. The problem of structural collapse of Na2TiFeF7 during battery cycling is avoided, the long-cycle stability is greatly improved, and the capacity and rate performance can be greatly improved.

[0040] The sodium ion battery cathode material provided by the present invention has three-dimensional equivalent ultrafast sodium ion transmission capability and stable thermodynamic properties. Compared with the traditional sodium battery cathode, it has the advantages of ultra-high ionic conductivity, good electronic conductivity, zero volume change, excellent battery cycle stability, and no resource problems.

[0041] The embodiments of the present invention are further described below in conjunction with specific examples. The chemical reagents involved in the following examples are all commercially available conventional products unless otherwise specified.

[0042] 1. Specific embodiments of the sodium ion battery positive electrode material of the present invention

[0043] The chemical formula of the sodium ion battery positive electrode material of the present invention is shown in Table 1.

[0044] Table 1 Chemical formula of the sodium ion battery positive electrode material of the present invention

[0045] Chemical formula Example 1 <![CDATA[Na2Al 0.05 Of 0.95 FeF7]]> Example 2 <![CDATA[Na2Mg 0.05 If you like 0.95 F7]]> Example 3 <![CDATA[Na2Al 0.05 Of 0.95 Mg 0.01 Want 0.99 F7]]> Example 4 <![CDATA[Na2Al 0.02 Of 0.98 Mg 0.02 Want 0.98 F7]]> Example 5 <![CDATA[Na2Al 0.01 Of 0.66 Mn 0.33 FeF7]]>

[0046] The chemical formula of the sodium ion battery positive electrode material of Example 1 is Na a M b1 M” b2 M' 1-b1-b2 N c N' 1-c X 7+d , where M is Al, M' is Ti, N' is Fe, X is F, a=2, b1=0.05, b2=0, c=0, d=0, specifically Na2Al 0.05 Ti 0.95 FeF7.

[0047] The chemical formula of the sodium ion battery positive electrode material of Example 2 is Na a M b1 M” b2 M' 1-b1-b2 N c N' 1-c X 7+d , where M' is Ti, N is Mg, N' is Fe, X is F, a=2, b1=0, b2=0, c=0.05, d=0, specifically Na2Mg 0.05 TiFe 0.95 F7.

[0048] The chemical formula of the sodium ion battery positive electrode material of Example 3 is Na a M b1 M” b2 M' 1-b1-b2 N c N' 1-c X 7+d , where M is Al, N is Mg, M' is Ti, N' is Fe, X is F, a=2, b1=0.05, b2=0, c=0.01, d=0, specifically Na2Al 0.05 Ti 0.95 Mg 0.01 Fe 0.99 F7.

[0049] The chemical formula of the sodium ion battery positive electrode material of Example 4 is Na a M b1 M”b2 M' 1-b1-b2 N c N' 1-c X 7+d , where M is Al, N is Mg, M' is Ti, N' is Fe, X is F, a=2, b1=0.02, b2=0, c=0.02, d=0, specifically Na2Al 0.02 Ti 0.98 Mg 0.02 Fe 0.98 F7.

[0050] The chemical formula of the sodium ion battery positive electrode material of Example 5 is Na a M b1 M” b2 M' 1-b1-b2 N c N' 1-c X 7+d , where M is Al, N is Mn, M' is Ti, N' is Fe, X is F, a=2, b1=0.01, b2=0.33, c=0, d=0, specifically Na2Al 0.01 Ti 0.66 Mn 0.33 FeF7.

[0051] 2. Specific embodiments of the method for preparing the positive electrode material for sodium ion batteries of the present invention

[0052] Example 6

[0053] The preparation method of the sodium ion battery positive electrode material of this embodiment is as follows:

[0054] 1) Under the protection of argon atmosphere in a glove box, weigh sodium fluoride (NaF), iron difluoride (FeF2), titanium trifluoride (TiF3) and aluminum trifluoride (AlF3) in a molar ratio of 2:1:0.95:0.05, mix the above powders evenly and put them into an alumina ball milling jar, put 20 zirconium oxide ball milling beads with a diameter of 10 mm into the jar and seal it tightly. Take the tightly sealed ball milling jar out of the glove box and put it into a ball mill for ball milling treatment; set the ball mill speed to 300rmp, the ball mill is milled for 10 minutes, and then cooled for 5 minutes. The effective time of ball milling treatment is 12 hours to obtain a precursor.

[0055] 2) The precursor is taken out and placed in a vacuum tube furnace for vacuum heat treatment. The vacuum heat treatment temperature is 600° C. and the vacuum heat treatment time is 60 min. After the vacuum heat treatment is completed, the furnace is cooled to room temperature. The obtained powder is the sodium ion battery positive electrode material Na2Al 0.05 Ti0.95 FeF7.

[0056] Example 7

[0057] The preparation method of the sodium ion battery positive electrode material of this embodiment is as follows:

[0058] 1) Under the protection of argon atmosphere in a glove box, weigh sodium fluoride (NaF), iron difluoride (FeF2), titanium trifluoride (TiF3) and magnesium difluoride (MgF2) in a molar ratio of 2:0.95:1:0.05, mix the above powders evenly and put them into an alumina ball milling jar, put 20 zirconium oxide ball milling beads with a diameter of 10 mm into the jar and seal it tightly. Take the tightly sealed ball milling jar out of the glove box and put it into a ball mill for ball milling treatment; set the ball mill speed to 300rmp, the ball mill is milled for 10 minutes, and then cooled for 5 minutes. The effective time of ball milling treatment is 12 hours to obtain a precursor.

[0059] 2) The precursor is taken out and placed in a vacuum tube furnace for vacuum heat treatment. The vacuum heat treatment temperature is 650° C. and the vacuum heat treatment time is 90 min. After the vacuum heat treatment is completed, the precursor is cooled to room temperature in the furnace. The obtained powder is the sodium ion battery positive electrode material Na2Mg 0.05 TiFe 0.95 F7.

[0060] Example 8

[0061] The preparation method of the sodium ion battery positive electrode material of this embodiment is as follows:

[0062] 1) Under the protection of argon atmosphere in a glove box, sodium fluoride (NaF), iron difluoride (FeF2), titanium trifluoride (TiF3), aluminum trifluoride (AlF3) and magnesium difluoride (MgF2) are weighed in a molar ratio of 2:0.99:0.95:0.01:0.05. The above powders are uniformly mixed and loaded into an alumina ball milling jar. 20 zirconium oxide ball milling beads with a diameter of 10 mm are loaded into the jar and sealed tightly. The tightly sealed ball milling jar is taken out of the glove box and loaded into a ball mill for ball milling treatment; the ball mill speed is set to 300 rpm for ball milling treatment, the ball mill is milled for 10 minutes, and then cooled for 5 minutes. The effective time of ball milling treatment is 12 hours to obtain a precursor.

[0063] 2) The precursor is taken out and placed in a vacuum tube furnace for vacuum heat treatment. The vacuum heat treatment temperature is 500° C. and the vacuum heat treatment time is 60 min. After the vacuum heat treatment is completed, the furnace is cooled to room temperature. The obtained powder is the sodium ion battery positive electrode material Na2Al 0.05 Ti 0.95 Mg 0.01 Fe 0.99 F7.

[0064] Example 9

[0065] The preparation method of the sodium ion battery positive electrode material of this embodiment is as follows:

[0066] 1) Under the protection of argon atmosphere in a glove box, weigh sodium fluoride (NaF), iron difluoride (FeF2), titanium trifluoride (TiF3), aluminum trifluoride (AlF3) and magnesium difluoride (MgF2) according to a molar ratio of 2:0.98:0.98:0.02:0.02. After mixing the above powders evenly, put them into an alumina ball milling jar, and put 20 zirconium oxide ball milling beads with a diameter of 10 mm into the jar and seal it tightly. Take the tightly sealed ball milling jar out of the glove box and put it into a ball mill for ball milling treatment; set the ball mill speed to 300 rpm, the ball mill is milled for 10 minutes, and then cooled for 5 minutes. The effective time of ball milling treatment is 12 hours to obtain a precursor.

[0067] 2) The precursor is taken out and placed in a vacuum tube furnace for vacuum heat treatment. The vacuum heat treatment temperature is 500° C. and the vacuum heat treatment time is 90 min. After the vacuum heat treatment is completed, the furnace is cooled to room temperature. The obtained powder is the sodium ion battery positive electrode material Na2Al 0.02 Ti 0.98 Mg 0.02 Fe 0.98 F7.

[0068] Example 10

[0069] The preparation method of the sodium ion battery positive electrode material of this embodiment is as follows:

[0070] 1) Under the protection of argon atmosphere in a glove box, weigh sodium fluoride (NaF), iron difluoride (FeF2), titanium trifluoride (TiF3), aluminum trifluoride (AlF3) and manganese trifluoride (MnF3) according to a molar ratio of 2:1:0.66:0.01:0.33, weigh sodium fluoride powder, iron difluoride powder, titanium trifluoride powder, aluminum trifluoride powder and manganese trifluoride powder, mix the above powders evenly and put them into an alumina ball milling jar, put 20 zirconium oxide ball milling beads with a diameter of 10 mm into the jar and seal it tightly. Take the tightly sealed ball milling jar out of the glove box and put it into a ball mill for ball milling treatment; set the ball mill speed to 300rmp for ball milling treatment, the ball mill is milled for 10 minutes, and then cooled for 5 minutes. The effective time of ball milling treatment is 12 hours to obtain a precursor.

[0071] 2) The precursor is taken out and placed in a vacuum tube furnace for vacuum heat treatment. The vacuum heat treatment temperature is 600° C. and the vacuum heat treatment time is 90 min. After the vacuum heat treatment is completed, the furnace is cooled to room temperature. The obtained powder is the sodium ion battery positive electrode material Na2Al 0.01 Ti 0.66 Mn 0.33 FeF7.

[0072] 3. Specific Examples of Application of the Sodium Ion Battery Positive Electrode Material of the Present Invention

[0073] Embodiment 11

[0074] The sodium ion positive electrode material, conductive carbon black (Super P), graphene and carbon nanotubes of any embodiment are weighed in a mass ratio of 80:8.65:8.65:2.7, mixed evenly and put into a ball mill, 20 zirconium oxide ball milling beads with a diameter of 10 mm are put into the jar and sealed tightly, the tightly sealed ball milling jar is taken out from the glove box, and put into a ball mill for ball milling treatment; the ball milling treatment is set to a speed of 150 rpm, the ball mill is milled for 10 min, and the ball mill is cooled for 5 min, and the total effective ball milling time is 8 h to obtain a positive electrode active material, the positive electrode active material and the binder PTFE are mixed evenly in a mass ratio of 95:5, and then rolled to prepare a sodium ion battery positive electrode sheet with a loading of 10-13 mg cm -2 .

[0075] 4. Comparative Proportion

[0076] Comparative Example 1

[0077] The chemical formula of the sodium ion battery positive electrode material in this comparative example is Na2TiFeF7.

[0078] The preparation method of the sodium ion battery positive electrode material of this comparative example is as follows:

[0079] 1) Under the protection of argon atmosphere in a glove box, weigh sodium fluoride (NaF), iron difluoride (FeF2), and titanium trifluoride (TiF3) in a molar ratio of 2:1:1, mix the above powders evenly and put them into an alumina ball milling jar, put 20 zirconium oxide ball milling beads with a diameter of 10 mm into the jar and seal it tightly. Take the tightly sealed ball milling jar out of the glove box and put it into a ball mill for ball milling; set the ball mill speed to 300rmp, the ball mill mills for 10 minutes each time, and then cools for 5 minutes. The total effective ball milling time is 12 hours to obtain a precursor.

[0080] 2) The precursor is taken out and placed in a vacuum tube furnace for heat treatment at a temperature of 600°C for 60 minutes. After the heat treatment, it is quickly cooled to room temperature. The obtained powder is the sodium ion battery positive electrode material Na2TiFeF7 of this comparative example.

[0081] The chemical formula and process parameters of the sodium ion positive electrode materials of the embodiment and comparative example are shown in Table 2.

[0082] Table 2 Chemical formula and process parameters of sodium ion cathode materials

[0083]

[0084] V. Experimental Examples

[0085] Experimental Example 1

[0086] This experimental example characterizes the crystal structure of the sodium ion positive electrode material. Figure 2 The sodium ion positive electrode material Na2Al of Example 4 0.02 Ti 0.98 Mg 0.02 Fe 0.98 XRD pattern of F7, Figure 2 The blue line below is the data from the standard diffraction PDF card (card number: PDF#24-1098). Figure 2 It can be seen that the main peaks of the sodium ion positive electrode material provided by the present invention are near 30°, 50° and 60°, which are consistent with the PDF#24-1098 card, and there are no other impurity peaks, indicating that it is a pure phase (i.e., a crystal structure of fluoroaluminum magnesium sodium stone); it shows that the precursor in the preparation method provided by the present invention is fully reacted and there is no other second phase substance.

[0087] Figure 3 The sodium ion positive electrode material Na2Al of Example 4 0.02 Ti 0.98 Mg 0.02 Fe 0.98 Transmission electron microscopy (TEM) image of F7, from Figure 3 It can be seen that the particle edges are clean, there is no amorphous phase, the lattice fringes are clearly discernible, belonging to the trigonal phase of the P3121 space group, with a significant spacing of 0.606 nm, which corresponds to the (022) plane of the lattice.

[0088] Experimental Example 2

[0089] This experimental example tests the electrochemical performance of sodium ion positive electrode materials.

[0090] 1) Electronic conductivity test

[0091] The electronic conductivity test method in this experimental example is as follows: the sodium ion positive electrode materials of Example 4 and Comparative Example 1 are pressed into sheets as the positive electrode using a mold, and the pressed sheets are clamped with two gaskets, and assembled into a 2032-type button battery in the following order: positive electrode shell, gasket, spring sheet, positive electrode, diaphragm (glass fiber diaphragm model GF / D), sodium sheet, spring sheet, gasket, and negative electrode shell, and the electrolyte is NaClO4; the test is carried out in Chenhua (CHI660e) electrochemical work, the mode is selected as it-Amperometricit Curve, a voltage of 1V is applied, and the duration is 3000s.

[0092] Figure 4 The sodium ion positive electrode material Na2Al of Example 4 0.02 Ti 0.98 Mg 0.02 Fe 0.98 F7 electronic conductivity test results, from Figure 4 It can be seen that the sodium ion positive electrode material Na2Al 0.02 Ti 0.98 Mg 0.02 Fe 0.98 The electronic conductivity of F7 is 5.22*10 -6 S cm -1 , while the electronic conductivity of the sodium ion positive electrode material Na2TiFeF7 in Comparative Example 2 is 4.05*10 -6 S cm -1 , indicating that doping with Al and Mg can greatly improve the electronic conductivity and has good electronic conductivity.

[0093] 2) Impedance test

[0094] The impedance test method in this experimental example is as follows: Referring to Example 11, the positive electrode sheet prepared from the positive electrode materials of Example 4 and Comparative Example 4 is used as the positive electrode, and the sodium sheet is used as the negative electrode. The positive electrode shell, gasket, spring sheet, positive electrode, diaphragm (glass fiber diaphragm model GF / D), sodium sheet, spring sheet, gasket, negative electrode shell are assembled into a 2032-type button battery, and the electrolyte is NaClO4; the test is carried out in Chenhua (CHI660e) electrochemical work, the mode is selected as IMP-AC.Impedance, and the high frequency area is 10 5 Hz, the low frequency area is 0.1Hz, and the amplitude is 0.005V.

[0095] Figure 5 The sodium ion positive electrode material Na2Al of Example 4 0.02 Ti 0.98 Mg 0.02 Fe 0.98 The impedance spectrum of F7, from Figure 5 It can be seen that the sodium ion positive electrode material Na2Al 0.02 Ti 0.98 Mg 0.02 Fe 0.98 F7 shows lower impedance than the sodium ion positive electrode material Na2TiFeF7 of comparative example 2, indicating that doping with Al and Mg can reduce impedance, indicating that the sodium ion positive electrode material provided has low impedance and is a good conductor of sodium ions.

[0096] 3) Charge and discharge performance test

[0097] The charge and discharge performance test method in this experimental example is as follows: Referring to Example 11, the positive electrode sheet prepared from the positive electrode materials of the embodiment and the comparative example is used as the positive electrode, and the sodium sheet is used as the negative electrode. The positive electrode shell, gasket, spring sheet, positive electrode, diaphragm (glass fiber diaphragm model GF / D), sodium sheet, spring sheet, gasket, and negative electrode shell are assembled into a 2032-type button battery, and the electrolyte is NaClO4. Then, the charge and discharge curve of the sodium ion battery is tested, and the test voltage is 1.5-4.3V. The test results are shown in Table 3.

[0098] Table 3 Test results of charge and discharge performance of sodium ion positive electrode materials of the embodiments and comparative examples

[0099]

[0100] It can be seen from Table 3 that compared with Comparative Example 1, the sodium ion positive electrode materials of Examples 1-5 show higher specific capacity at any rate, indicating that Al and / or Mg or Al and Mn doping can greatly improve the specific capacity of the positive electrode material; and the capacity retention rate is still maintained at more than 90% after 200 cycles, which is 3 times that of the positive electrode material Na2TiFeF7 in Comparative Example 1, proving that Na2TiFeF7 is obviously structurally unstable and prone to structural collapse under long cycle conditions, resulting in poor long cycle performance. The present invention greatly improves the structural stability of the positive electrode material by doping with Al and / or Mg, Al and Mn, so that the positive electrode material obtains better long cycle stability.

[0101] The charge and discharge performance test comparison diagram of the sodium ion positive electrode material of Example 4 is as follows Figure 6 As shown. Figure 6 (a) is the first cycle charge and discharge curve of the sodium ion positive electrode material of Example 4 and Comparative Example 1, Figure 6 (b) is a comparison chart of the capacities of the sodium ion positive electrode materials of Example 4 and Comparative Example 1 under different rates and different cycle numbers. Figure 6 (a) and (b) show that under the load condition (0.05C), the first-week capacity of Na2TiFeF7 is only about 121.07 mAh / g, while Na2Al 0.02 Ti 0.98 Mg 0.02 Fe 0.98 The first week capacity of F7 can reach 169mAh / g, which is nearly 30% higher than that of Na2Al 0.02 Ti 0.98 Mg 0.02 Fe 0.98 F7 still shows a higher specific capacity than Na2TiFeF7 under different rates and different cycle numbers. In addition, the capacity of Na2TiFeF7 decays sharply to 40mAh / g under the condition of 20 cycles and 1C, while Na2Al 0.02 Ti 0.98 Mg 0.02 Fe 0.98 The capacity of F7 can still be maintained at 100 mAh / g, indicating that the rate performance of the positive electrode material of the present invention is significantly better than that of Comparative Example 1; at 0.05C, Na2Al 0.02 Ti 0.98 Mg 0.02 Fe 0.98The first-week discharge capacity of F7 is 169 mAh / g, and the capacity retention rate after 200 cycles is 91.79%, while the first-week discharge capacity of Na2TiFeF7 is 121.07 mAh / g, and the capacity retention rate after 200 cycles is 31.77%; 6 (c) is a comparison of the long-cycle stability performance of the sodium ion positive electrode materials of Example 4 and Comparative Example 1. Figure 6 (c) It can be seen that under 1C conditions, as the number of cycles increases, Na2Al 0.02 Ti 0.98 Mg 0.02 Fe 0.98 The specific capacity of F7 does not change much, while the specific capacity of Na2TiFeF7 decays significantly, especially after 80 cycles. After 200 cycles, the specific capacity decays from 30mAh / g to almost below 15mAh / g, indicating that Na2TiFeF7 has obvious structural instability problems. Its structure collapses under long cycle conditions, so it cannot be used as a suitable positive electrode material for sodium batteries to achieve stable long cycles. 0.02 Ti 0.98 Mg 0.02 Fe 0.98 Under the action of Al and Mg doping, the structural skeleton stability of F7 is greatly improved, making it an excellent positive electrode material for sodium batteries and achieving stable and long cycles.

[0102] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A sodium ion battery positive electrode material, characterized in that: The chemical formula of the positive electrode material is Na a M b1 M” b2 M' 1-b1- b2 N c N' 1-c X 7+d , wherein M is a trivalent metal, N is a divalent metal, M” and M’ are different trivalent transition metals, N’ is a divalent transition metal, X is a halogen element, 1.75≤a≤2.25, 0≤b1≤0.05, 0≤b2≤0.33, 0≤c≤0.05, -0.25≤d≤0.25, and b1, b2, and c are not all 0 at the same time.

2. The sodium ion battery positive electrode material according to claim 1, characterized in that The M' is Ti, M" is Mn, the M is Al, the N' is Fe, and the N is Mg.

3. The sodium ion battery positive electrode material according to claim 1, characterized in that The X is F.

4. The sodium ion battery positive electrode material according to claim 1, characterized in that The chemical formula of the positive electrode material is Na2Al b1 Ti 1-b1 Mg c Fe 1-c F7, where 0 < b1 ≤ 0.05 and 0 < c ≤ 0.02; or it is Na2Al b1 Mn b2 Ti 1-b1-b2 FeF7, where 0 < b1 ≤ 0.05 and 0 < b2 ≤ 0.

33.

5. The sodium ion battery positive electrode material according to claim 1, characterized in that The crystal structure of the positive electrode material belongs to the trigonal phase of the P3121 space group, and the interplanar spacing of the (022) crystal plane is greater than 6. The sodium ion battery positive electrode material according to claim 1, characterized in that The chemical formula of the positive electrode material is Na2Al 0.05 Ti 0.95 FeF7 or Na2Mg 0.05 TiFe 0.95 F7 or Na2Al 0.05 Ti 0.95 Mg 0.01 Fe 0.99 F7 or Na2Al 0.02 Ti 0.98 Mg 0.02 Fe 0.98 F7 or Na2Al 0.01 Ti 0.66 Mn 0.33 FeF7.

7. A method for preparing a positive electrode material for a sodium ion battery according to claims 1-6, characterized in that: The following steps are involved: Under inert gas conditions, metal fluorides of Na, M, M', M", N and N' are mixed and ball-milled to obtain a precursor, and the precursor is vacuum-heat-treated and then cooled. The vacuum heat-treatment temperature is 500-650° C. and the vacuum heat-treatment time is 60-90 min.

8. An application of the sodium ion battery positive electrode material according to claims 1-6, characterized in that: The sodium ion battery positive electrode material, the conductive material and the binder are mixed and then rolled to obtain a positive electrode sheet.

9. The use of the sodium ion battery positive electrode material according to claim 8, characterized in that: The conductive material is selected from one or more of conductive carbon black, graphene and carbon nanotubes.

10. The use of the sodium ion battery positive electrode material according to claim 9, characterized in that: The mass ratio of the sodium ion battery positive electrode material, conductive carbon black, graphene and carbon nanotubes is (80-90): (8.65-9.5): (8.65-9.5): (2.7-3).