Method for improving cycling stability of battery, carbon-coated current collector and battery positive plate
By introducing WTe2-WO3 heterojunctions, graphite, and carbon nanotubes into the carbon-coated current collector of sodium-ion batteries, the problem of poor cycle stability of sodium-ion batteries was solved, thereby improving battery performance and reducing costs.
Patent Information
- Application Number
- CN202411012638.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-08
AI Technical Summary
Sodium-ion batteries are difficult to insert and deintercalate ions, have poor cycle stability, and therefore have high energy storage costs.
A WTe2-WO3 heterojunction structure is introduced into the carbon coating layer of the carbon-coated current collector, and graphite and carbon nanotubes are added to form a mixed carbon coating slurry, which is then coated onto the positive electrode foil to prepare the positive electrode sheet of the battery.
It significantly improves the cycle stability and electrical performance of the battery, and reduces the cost of energy storage.
Smart Images

Figure CN118919735A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of batteries, and in particular to a method for improving battery cycle stability, a carbon-coated current collector and a battery positive electrode sheet. Background Art
[0002] The over-exploitation and utilization of traditional fossil energy has inevitably caused energy crises and environmental pollution. With the advancement of contemporary technology, the research and application of new energy sources are becoming more and more extensive. However, some new energy sources, such as solar energy and wind energy, are heavily dependent on natural conditions such as weather, seasons, and locations, and are intermittent and unstable. Therefore, how to further develop convenient and efficient large-scale energy storage devices and their applications is crucial to technological progress.
[0003] In recent decades, lithium-ion batteries have achieved considerable development as a popular power source for electronic systems and renewable energy, and the limited resources of lithium metal and the gradual expansion of energy storage demand have pushed up the price of lithium.
[0004] Sodium-ion batteries have also attracted widespread interest among researchers as a potential energy storage system. Sodium has similar chemical properties to lithium, with abundant natural reserves and low redox potential. Na ions have a higher ionic radius than Li ions, so sodium-ion batteries have the same ion migration difficulties as lithium-ion batteries, and ion deintercalation during charging and discharging is more difficult.
[0005] Therefore, in order to reduce the cost of the energy storage industry and alleviate the energy pressure of lithium-ion batteries, sodium-ion batteries, etc., the need to explore new energy storage systems is imminent. Summary of the invention
[0006] The purpose of the present invention is to provide a method for improving the cycle stability of a battery, a carbon-coated current collector and a battery positive electrode sheet, and to improve the conductivity of the carbon-coated layer by the strategy of doping and constructing a heterojunction structure, thereby optimizing the cycle stability of the battery.
[0007] The present invention is achieved through the following technical solutions:
[0008] The present invention provides a carbon-coated current collector for improving the cycle stability of a battery. The carbon-coated layer of the carbon-coated current collector contains a WTe2-WO3 heterojunction, graphite and carbon nanotubes. The carbon-coated current collector is used to prepare a positive electrode sheet of a battery.
[0009] The present invention also provides a method for improving the cycle stability of a battery, wherein WTe2-WO3 is added to a carbon-coated slurry to construct a heterojunction, and graphite and carbon nanotubes are added to form a mixed carbon-coated slurry, which is evenly coated on a positive electrode foil to obtain a carbon-coated current collector, and the carbon-coated current collector is used to prepare a battery positive electrode sheet.
[0010] Furthermore, WO3 is added to the mixed carbon-coated slurry.
[0011] Specifically, the preparation of the mixed carbon coating slurry comprises the following steps:
[0012] S1: After mixing the binder with water, add the conductive agent and WO3 thereto and disperse them evenly to form the first slurry;
[0013] S2: Add a conductive agent and WTe2-WO3 to the first slurry and disperse them evenly to form a second slurry;
[0014] S3: adding water to the second slurry to dilute it and disperse it evenly to form a third slurry;
[0015] S4: adding graphite and carbon nanotubes to the third slurry and dispersing them evenly to form a fourth slurry;
[0016] S5: adding a wetting agent to the fourth slurry and dispersing it evenly to form a fifth slurry;
[0017] S6: sand-grind the fifth slurry to obtain a mixed carbon-coated slurry.
[0018] The binder is selected from at least one of acrylate, polyacrylic acid, modified polyacrylic acid and waterborne polyurethane; the conductive agent is carbon black; and the wetting agent is selected from at least one of polyether siloxane, modified polyether siloxane and alcohol reagents.
[0019] Preferably, the binder is a modified polyacrylic acid with a solid content of 15-30% and a viscosity of 200-1500 mPa.s; and the wetting agent is a modified polyether siloxane.
[0020] Among them, the conductive agent is added twice in steps S1 and S2 respectively, and the mass proportion of the conductive agent in the second slurry after the two additions is 40%-90%; the mass proportion of graphite and carbon nanotubes added in step S4 in the fourth slurry is 0%-10% respectively, and 0% is not included; the mass proportion of the wetting agent added in step S5 in the fifth slurry is 5%-20%.
[0021] The preparation method of WTe2-WO3 is to deposit tellurium elements on a WO3 precursor by electrochemical deposition of a tellurium source to obtain WTe2-WO3; the tellurium source is a telluride soluble in water.
[0022] The uniform dispersion in the steps S1 to S4 is performed by high-speed dispersion in a stirring device at a rotation speed of 2000-2600 rpm / min for 30-60 min; the uniform dispersion in the step S5 is performed by low-speed stirring in a stirring device at a rotation speed of 10-15 rpm / min for 30-45 min; and the sand grinding in the step S6 is performed by sand grinding in a sand grinding tank for 6-8 times.
[0023] The present invention also provides a battery positive electrode sheet, which uses the above-mentioned carbon-coated current collector for improving battery cycle stability as the positive current collector, and a positive active material layer is provided on the surface of the positive current collector; preferably, the positive active material layer includes a sodium-based positive electrode material.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] The present invention provides a strategy for improving the cycle stability of the battery. The WTe2-WO3 heterojunction structure is obtained by introducing tellurium elements into the carbon-coated layer of the carbon-coated current collector while maintaining the nanobelt morphology of WO3. The addition of tellurium elements can accelerate the electrochemical reaction kinetic rate, thereby improving the electronic conductivity of the material. At the same time, the construction of the heterojunction structure can increase the reaction active phase. The increase in active sites is also beneficial to improving the electrical performance of the battery and increasing the reaction rate when the battery is working.
[0026] The present invention also obtains a final composite material by physically mixing the material doped with WTe2-WO3 heterojunction with carbon nanotubes and graphite. The addition of carbon nanotubes and graphite can improve the conductivity of the slurry, which is beneficial to prevent the volume expansion of the composite material during processing from affecting the charging and discharging process, and the deformation of the battery is controlled to a minimum when the battery is overcharged and over-discharged. In addition, the reasonable ratio of carbon nanotubes and graphite can help improve electron transfer and ion migration, so that the carbon nanotubes and graphite can cooperate with the influence of the WTe2-WO3 heterojunction on the electrical properties of the battery, significantly enhance the ion transmission / diffusion capacity, ensure the rapid kinetic process during the ion storage process, and obtain excellent rate performance and cycle stability.
[0027] The present invention also adds WO3 to the carbon coating slurry to increase the dispersibility of the slurry. WO3 is soluble in water, and WO3 reacts with H2O to generate a portion of H2WO4, which is weakly acidic and can adjust the pH of the slurry to 5-7. When the pH of the slurry exceeds 7, it is easy to cause changes in the structure of the binder itself, causing the slurry to become thick and unable to be coated smoothly.
[0028] The solution of the present invention can be applied to lithium batteries, sodium batteries, etc., significantly improving battery cycle stability and reducing energy storage costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 : Electron microscope image of the carbon-coated current collector for improving battery cycle stability of the present invention, wherein the magnification of (a) is 1 micron, and the magnification of (b) is 10 microns. DETAILED DESCRIPTION
[0030] The above contents of the present invention are further described in detail below in the form of embodiments, but this should not be understood as the scope of the above subject matter of the present invention being limited to the following embodiments, and all technologies realized based on the above contents of the present invention belong to the scope of the present invention.
[0031] The experimental methods used in the following examples are all conventional methods unless otherwise specified, and the reagents, methods and equipment used are all conventional reagents, methods and equipment in the technical field unless otherwise specified.
[0032] The WO3 in the present invention is a conventional powder additive material. The WO3 powder can be purchased or obtained by using tungsten salt through a high-temperature hydrothermal method.
[0033] The WO3 in the embodiment of the present invention is prepared by the following method:
[0034] Sodium tungstate and weakly acidic hydrochloric acid solution with a pH of 2-3 are mixed and stirred evenly until a clear and transparent solution is obtained, which is called solution A. Potassium chloride solution is added dropwise to solution A to adjust the pH to about 5. The solution after the pH adjustment is called solution B. Solution B is transferred to a reactor and reacted at 120°C for 6 hours. After the reaction is completed, the solution is cooled to room temperature and transferred to a centrifuge and dispersed at 6000r / min for 10 minutes. After dispersion, the precipitated material at the bottom of the centrifuge tube is removed and dried in a vacuum drying oven at 60°C for 12 hours to obtain pure WO3 crystals.
[0035] The WTe2-WO3 heterojunction in the embodiment of the present invention is prepared by the following method:
[0036] Sodium tellurate was dissolved in deionized water, potassium chloride solution was added to the sodium tellurate solution, the pH was adjusted to about 3, and the solution was transferred to an electrolytic cell for standby use; the WO3 precursor powder was then dispersed with Nafion solution and evenly applied on a platinum electrode sheet, which was used as the positive electrode of the power supply; in addition, a graphite rod was selected as the negative electrode of the power supply; the voltage was selected to be -0.9V, and the reaction time was 20 minutes; as the color of the positive electrode sheet changed from white to dark red, it indicated that the Te element was successfully deposited on the WO3 precursor; the deposited material on the positive platinum sheet was removed and dried in a vacuum drying oven at 60°C for 12 hours to obtain a WTe2-WO3 heterojunction.
[0037] In the above preparation method of WTe2-WO3 heterojunction, sodium tellurite can be replaced by other tellurium source materials. The tellurium source material selects conventional water-soluble tellurides, such as tellurium dioxide and telluric acid solution.
[0038] The carbon-coated current collector in the embodiment of the present invention is obtained by uniformly coating a mixed carbon-coated slurry formed by a carbon-coated slurry doped with WTe2-WO3 to form a heterojunction and graphite and carbon nanotubes on the positive electrode foil, and then the carbon-coated current collector is used to prepare the battery positive electrode sheet.
[0039] The conductive agent in the embodiment of the present invention is added in two times to avoid the situation where the viscosity of the slurry is too high after adding it once.
[0040] In the following examples of adding graphite and carbon nanotubes, the addition amount is 1% each. However, according to tests, similar effects can be achieved at addition amounts of 0%-10% (excluding 0%).
[0041] After the mixed carbon coating slurry in the embodiment of the present invention is coated on the positive electrode foil, a drying treatment is performed. The drying treatment can be carried out by drying in a vacuum environment at 120° C. for 8 hours.
[0042] Example 1
[0043] 1. Preparation of positive electrode carbon-coated current collector, the process is as follows:
[0044] Mixing deionized water with the binder to reduce the solid content of the binder;
[0045] Add carbon black conductive agent and WO3, and disperse at high speed of 2000-2600rpm / min in a 200L Double Star stirring tank for 30-60min;
[0046] Add carbon black conductive agent and WTe2-WO3, and disperse at high speed of 2000-2600rpm / min in a 200L Double Star stirring tank for 30-60min;
[0047] Add appropriate amount of deionized water to reduce the slurry concentration, and disperse at high speed of 2000-2600rpm / min in a 200L Double Star stirring tank for 30min;
[0048] Add graphite and carbon nanotubes as additives and disperse them at a high speed of 2000-2600 rpm / min in a 200L Double Star stirring tank for 30-60 minutes;
[0049] Add wetting agent, stir at low speed of 10-15rpm / min in a 200L double star stirring tank for 30-45min, then discharge;
[0050] Sand the slurry in a sand mill 7 times;
[0051] The slurry is uniformly coated on an aluminum current collector or a composite current collector to obtain a carbon-coated current collector.
[0052] Among them, the mass ratio of carbon black: WTe2-WO3: graphite: carbon nanotubes used is 95:3:1:1, the wetting agent accounts for 10%, the binder is modified PAA (modified polyacrylic acid), and the wetting agent is modified polyether siloxane. The carbon-coated aluminum foil is prepared according to the above steps.
[0053] 2. Preparation of positive electrode sheet:
[0054] The positive electrode active material sodium iron phosphate (NaFePO4), conductive carbon black (SP), and binder polyvinylidene fluoride (PVDF) are mixed evenly in a mass ratio of 96:2:2 and dispersed in a solvent N-methylpyrrolidone (NMP) to prepare a positive electrode slurry; the positive electrode slurry is evenly coated on the two surfaces of the positive electrode current collector carbon-coated aluminum foil to form a positive electrode active coating, and dried at 120°C for 8 hours in a vacuum environment, and then cold pressed and slit to obtain a positive electrode sheet.
[0055] 3. Preparation of negative electrode sheet:
[0056] Graphite negative electrode active material, conductive carbon black (SP), Li4Ti5O 12 The mixture was uniformly mixed in a mass ratio of 93:5:2 and dispersed in a solvent of deionized water to obtain a negative electrode slurry; the mixed powder was pressed into the shape of a negative electrode sheet, and dried at 120° C. for 4 hours to obtain a negative electrode sheet.
[0057] 4. Preparation of sodium ion batteries:
[0058] The positive electrode sheet and the negative electrode sheet are stacked in order, and the electrolyte is injected. After vacuum packaging, standing, forming, shaping and other processes, a sodium ion battery is obtained.
[0059] 5.Battery assembly and testing:
[0060] The sodium ion batteries of the embodiments and comparative examples were tested at room temperature (25° C.), and the button-type symmetrical batteries were charged at constant current and constant voltage to 3-4.5V at a rate of 0.2C, 0.3C, 0.5C, 1C, 2C, 3C, and 5C, with a cut-off current of 0.15-3A. Then, the button-type symmetrical batteries were discharged at constant current to …… 3-4.5V at a rate of 0.2C, 0.3C, 0.5C, 1C, 2C, 3C, and 5C, which was regarded as one charge and discharge cycle. The button-type symmetrical batteries were charged and discharged for 100 cycles in accordance with the above method, and the discharge capacity of the button-type symmetrical batteries before and after the cycle was tested. The capacity retention rate of the button-type symmetrical batteries after 100 cycles was calculated according to the following formula: Capacity retention rate of the button-type symmetrical battery after 100 cycles (%) = (discharge capacity of the 100th cycle / first discharge capacity) × 100%.
[0061] Example 2
[0062] The mass ratio was adjusted to carbon black:WTe2-WO3:graphite:carbon nanotube=90:8:1:1, and the others were the same as in Example 1;
[0063] Example 3
[0064] The mass ratio was adjusted to carbon black:WTe2-WO3:graphite:carbon nanotube=85:13:1:1, and the others were the same as in Example 1;
[0065] Example 4
[0066] The mass ratio was adjusted to carbon black:WTe2-WO3:graphite:carbon nanotube=80:18:1:1, and the others were the same as in Example 1;
[0067] Example 5
[0068] The mass ratio was adjusted to carbon black: WTe2-WO3: graphite: carbon nanotube = 75:23:1:1, and the rest was the same as in Example 1; Comparative Example 1
[0069] The mass ratio was adjusted to carbon black: WTe2-WO3: graphite: carbon nanotube = 70:28:1:1, and the rest was the same as in Example 1; Comparative Example 2
[0070] The mass ratio was adjusted to carbon black: WTe2-WO3: graphite: carbon nanotube = 80:20:0:0, and the rest was the same as in Example 1; Comparative Example 3
[0071] The mass ratio was adjusted to carbon black:WTe2-WO3:graphite:carbon nanotube=98:0:1:1, and the others were the same as in Example 1;
[0072] Comparative Example 4
[0073] The mass ratio was adjusted to carbon black:WTe2-WO3:graphite:carbon nanotube=100:0:0:0:0, and the rest was the same as in Example 1.
[0074] The test results of the above embodiments and comparative examples are compared in Table 1:
[0075] Table 1 Test results of embodiments and comparative examples
[0076]
[0077]
[0078] The above embodiments and comparative examples have investigated whether to add WTe2-WO3, graphite, carbon nanotubes and the addition ratio. Experiments have proved that the scheme of the present invention can significantly improve the first efficiency and cycle capacity retention rate of sodium batteries, which is significantly better than the comparative examples. Among them, Example 3 has better performance in both the first efficiency and cycle capacity retention rate of sodium batteries.
[0079] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Any technician familiar with the profession, without departing from the scope of the technical solution of the present invention, according to the technical essence of the present invention, any simple modification, equivalent replacement and improvement made to the above embodiment still falls within the protection scope of the technical solution of the present invention.
Claims
1. A carbon-coated current collector for improving battery cycle stability, Features: The carbon-coated layer of the carbon-coated current collector contains WTe 2 -WO 3 Heterojunction, graphite and carbon nanotubes, the carbon-coated current collector is used to prepare a positive electrode sheet of a battery.
2. A method for improving battery cycle stability, Features: Add WTe to the carbon coating slurry 2 -WO 3 A heterojunction is constructed, and graphite and carbon nanotubes are added to form a mixed carbon-coated slurry, which is evenly coated on the positive electrode foil to obtain a carbon-coated current collector, and the carbon-coated current collector is used to prepare a battery positive electrode sheet.
3. The method for improving battery cycle stability according to claim 2, Features: WO is also added to the mixed carbon coating slurry. 3 .
4. The method for improving battery cycle stability according to claim 2 or 3, Features: The preparation of the mixed carbon coating slurry specifically comprises the following steps: S1: After mixing the binder with water, add the conductive agent and WO 3 , dispersed evenly to form a first slurry; S2: Add conductive agent and WTe to the first slurry 2 -WO 3 , dispersed evenly to form a second slurry; S3: adding water to the second slurry to dilute it and disperse it evenly to form a third slurry; S4: adding graphite and carbon nanotubes to the third slurry and dispersing them evenly to form a fourth slurry; S5: adding a wetting agent to the fourth slurry and dispersing it evenly to form a fifth slurry; S6: sand-grind the fifth slurry to obtain a mixed carbon-coated slurry.
5. The method for improving battery cycle stability according to claim 4, Features: The binder is selected from at least one of acrylate, polyacrylic acid, modified polyacrylic acid and waterborne polyurethane; the conductive agent is carbon black; and the wetting agent is selected from at least one of polyether siloxane, modified polyether siloxane and alcohol reagents.
6. The method for improving battery cycle stability according to claim 4, Features: The binder is modified polyacrylic acid with a solid content of 15-30% and a viscosity of 200-1500 mPa.s; and the wetting agent is modified polyether siloxane.
7. The method for improving battery cycle stability according to claim 4, Features: The conductive agent is added twice in steps S1 and S2, and the mass proportion of the conductive agent in the second slurry after the two additions is 40%-90%; the mass proportions of graphite and carbon nanotubes added in step S4 in the fourth slurry are 0%-10%, respectively, and 0% is not included; the mass proportion of the wetting agent added in step S5 in the fifth slurry is 5%-20%.
8. The method for improving battery cycle stability according to claim 4, Features: The WTe 2 -WO 3 The preparation method is to make a tellurium source on WO by electrochemical deposition. 3 Tellurium is deposited on the precursor to obtain WTe 2 -WO 3 ; The tellurium source is a water-soluble telluride.
9. The method for improving battery cycle stability according to claim 4, Features: The uniform dispersion in the steps S1 to S4 is performed by high-speed dispersion in a stirring device at a rotation speed of 2000-2600 rpm / min for 30-60 min; the uniform dispersion in the step S5 is performed by low-speed stirring in a stirring device at a rotation speed of 10-15 rpm / min for 30-45 min; and the sand grinding in the step S6 is performed by sand grinding in a sand grinding tank for 6-8 times.
10. A positive electrode sheet for a battery, Features: The carbon-coated current collector for improving battery cycle stability according to claim 1 is used as a positive electrode current collector, and a positive electrode active material layer is provided on the surface of the positive electrode current collector; preferably, the positive electrode active material layer includes a sodium-based positive electrode material.
Citation Information
Cited By
Carbon-coated current collector and preparation method thereof, pole piece and battery
CN120784378A
Carbon-coated current collector, preparation method thereof, pole piece and battery
CN120784378B