Lithium ion secondary battery

By using carbon nanotube conductive agent, ethyl acetate and lithium difluorophosphate in lithium-ion batteries, the relationship between its content and the positive electrode sheet density is adjusted, and the problems of insufficient wettability and increased impedance of the electrolyte are solved, and the battery is improved Energy density and high temperature performance.

CN118919822APending Publication Date: 2024-11-08ZHEJIANG COSMX BATTERY CO LTD
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411220103.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the process of increasing the energy density of existing lithium-ion batteries, the increase in the electrode surface density leads to insufficient wetting of the electrolyte, increasing impedance and lithium extraction problems, affecting battery performance.

Method used

Add carbon nanotube conductive agent to the positive electrode sheet, add ethyl acetate and lithium difluorophosphate to the electrolyte, and adjust the relationship between its mass percentage content and the double-side density of the positive electrode sheet to meet a specific ratio to improve the battery cell Wetting ability and migration speed of lithium ions.

Benefits of technology

It effectively solves the problems of poor cell infiltration, increased impedance and lithium extraction, and improves the energy density and high-temperature performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005022779330000171
    Figure BDA0005022779330000171
  • Figure BDA0005022779330000181
    Figure BDA0005022779330000181
  • Figure BDA0005022779330000182
    Figure BDA0005022779330000182
Patent Text Reader

Abstract

The invention relates to the technical field of lithium ion batteries, and provides a lithium ion secondary battery which comprises a positive plate, a diaphragm, a negative plate and an electrolyte, the double-sided surface density of the positive plate is recorded as X mg / cm < 2 >; the positive plate comprises a positive active material and a conductive agent, the conductive agent comprises a carbon nano tube, and the tube diameter of the carbon nano tube is marked as Y nm; the electrolyte comprises ethyl acetate and lithium difluorophosphate; based on the total mass of the electrolyte, the mass percentage content of the ethyl acetate is recorded as a%, and the mass percentage content of the lithium difluorophosphate is recorded as b%; and when X, Y, a and b meet the condition that (a + Y * b) / X is more than or equal to 0.6 and less than or equal to 1.5, the wettability of the battery cell can be effectively improved, the migration speed of lithium ions is increased, and the problems of poor wettability, impedance increase, lithium separation and the like of the battery cell are effectively solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a lithium ion secondary battery. Background Art

[0002] Compared with traditional batteries, lithium-ion batteries have advantages such as high specific energy, long cycle life, no pollution, and high operating voltage, so they have been widely used in many fields such as portable electronic devices, energy storage, and automotive power. With the rapid growth of lithium battery market demand, consumers have higher and higher requirements for the energy density of lithium batteries.

[0003] At present, one of the mainstream methods in the industry to improve energy density is to increase the surface density of the pole piece to form a thick electrode. However, the thick electrode will bring about the problem of insufficient electrolyte wettability. At the same time, the thick electrode will also significantly reduce the migration speed of lithium ions, which will eventually lead to problems such as poor wetting, increased impedance, and lithium precipitation in the battery cell. Summary of the invention

[0004] The purpose of the present invention is to overcome the above-mentioned problems existing in the prior art and provide a lithium ion secondary battery, in which a carbon nanotube conductive agent is added to the positive electrode sheet, and ethyl acetate (EA) and lithium difluorophosphate are added to the electrolyte. By adjusting the diameter of the carbon nanotubes, the mass percentage of ethyl acetate and lithium difluorophosphate in the electrolyte, and the double-sided surface density of the positive electrode sheet, the wettability of the battery cell can be effectively improved, the migration speed of lithium ions can be increased, and the problems of poor battery cell wetting, increased impedance, lithium precipitation, etc. can be effectively solved.

[0005] In order to achieve the above object, the present invention provides a lithium ion secondary battery, the lithium ion secondary battery comprises a positive electrode sheet, a separator, a negative electrode sheet and an electrolyte; the double-sided surface density of the positive electrode sheet is X mg / cm 2 ;

[0006] The positive electrode sheet includes a positive electrode active material and a conductive agent, the conductive agent includes carbon nanotubes, and the diameter of the carbon nanotubes is denoted as Y nm;

[0007] The electrolyte includes ethyl acetate; the mass percentage of ethyl acetate is recorded as a% based on the total mass of the electrolyte;

[0008] The electrolyte includes lithium difluorophosphate; based on the total mass of the electrolyte, the mass percentage of lithium difluorophosphate is recorded as b%;

[0009] X, Y, a and b satisfy: 0.6≤(a+Y*b) / X≤1.5.

[0010] The present invention adopts the above technical solution to achieve the following beneficial effects:

[0011] The lithium ion secondary battery provided by the present invention comprises ethyl acetate and lithium difluorophosphate added to the electrolyte, and the mass percentage of ethyl acetate in the electrolyte (a%) and the mass percentage of lithium difluorophosphate in the electrolyte (b%) are adjusted, and carbon nanotubes as a conductive agent are added to the positive electrode sheet, and the diameter of the carbon nanotubes (Y nm) is adjusted, and the double-sided surface density (X mg / cm 2 )When the four meet 0.6≤(a+Y*b) / X≤1.5, the wettability of the battery cell can be effectively improved, the migration speed of lithium ions can be increased, and the problems of poor battery cell wetting, increased impedance and lithium deposition can be effectively solved.

[0012] The endpoints and any values ​​of the range disclosed in this article are not limited to the precise range or value, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article. Herein, in the absence of special instructions, data ranges include endpoints. DETAILED DESCRIPTION

[0013] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0014] Unless otherwise defined, all scientific and technical terms used in the present invention have the same meanings as commonly understood by one of ordinary skill in the art to which the present invention relates.

[0015] In the present invention, the terms "battery", "lithium battery", "lithium-ion battery" and "lithium-ion secondary battery" all have the same meaning and refer to lithium-ion secondary batteries, which generally include an electrode assembly (such as a positive electrode sheet, a negative electrode sheet and a separator), a container (shell) for accommodating the electrode assembly, and an electrolyte.

[0016] In the present invention, the terms "primary particles" and "secondary particles" have the conventional meanings in the art. The term "primary particle" refers to a single negative electrode active particle; the term "secondary particle" refers to a particle formed by agglomeration of several primary particles, for example: the secondary particle is a particle formed by agglomeration of 2 primary particles, a particle formed by agglomeration of 5 primary particles, a particle formed by agglomeration of 10 primary particles, a particle formed by agglomeration of 50 primary particles, or a particle formed by agglomeration of 100 primary particles.

[0017] In the present invention, the term "average particle size" refers to the average value of the geometric diameters of several samples, for example, obtained by measuring several particles, for example, the average value of the geometric diameters can be obtained by measuring a dozen particles or dozens of particles. The average particle size can be measured using a laser particle size analyzer, and in the present invention, it is measured by a Malvern Mastersizer 3000 laser particle size analyzer.

[0018] The present invention provides a lithium ion secondary battery, which comprises a positive electrode sheet, a separator, a negative electrode sheet and an electrolyte; the double-sided surface density of the positive electrode sheet is X mg / cm 2 ;

[0019] The positive electrode sheet includes a positive electrode active material and a conductive agent, the conductive agent includes carbon nanotubes, and the diameter of the carbon nanotubes is denoted as Y nm;

[0020] The electrolyte includes ethyl acetate; the mass percentage of ethyl acetate is recorded as a% based on the total mass of the electrolyte;

[0021] The electrolyte includes lithium difluorophosphate; based on the total mass of the electrolyte, the mass percentage of lithium difluorophosphate is recorded as b%;

[0022] X, Y, a and b satisfy: 0.6≤(a+Y*b) / X≤1.5. The value of (a+Y*b) / X can be, for example, 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5 or any point value in the range formed by any two of the above point values.

[0023] The larger X is, the thicker the positive electrode sheet is. A thick electrode sheet can improve the energy density of the battery, but a thick electrode sheet itself will lead to a large battery impedance and poor wettability. In order to solve the problems of thick electrode sheets, the present invention adds ethyl acetate (EA) to the electrolyte. The viscosity of EA is relatively small, which can reduce the viscosity of the electrolyte and help improve the wettability of the thick electrode sheet. Conventional conductive agents used in batteries, such as carbon black, are point-to-point contacts that cannot form a good conductive network and have a poor effect on improving battery impedance. The present invention uses a carbon nanotube conductive agent and adjusts the diameter of the carbon nanotubes so that the carbon nanotube conductive agent is point-to-line contact that can form a good conductive network and thus reduce battery impedance. In addition, the spatial structure of the electrode sheet is more conducive to the rapid entry of EA into the interior of the electrode sheet. The combined use of carbon nanotubes and EA is more conducive to improving the wettability of thick electrode sheets. EA and Li + There is an interaction force between them, and the desolvation energy is high; a large number of functional groups on the surface of carbon nanotubes can interact with EA, weakening the interaction between EA and Li + The interaction between them reduces the desolvation energy and reduces the Li +The charge transfer impedance in the double layer is more favorable for Li + The shuttle between the two terminals can reduce the problem of increased impedance caused by thick electrodes.

[0024] The present invention has found that although the combination of EA and carbon nanotubes can effectively solve the problems of poor wettability and high impedance of thick pole pieces, when EA is added as a solvent in the electrolyte, the SEI film formed by EA at the negative electrode is loose and unstable, and consumes more active lithium electrolyte additives; and the higher the EA content, the easier it is for EA to oxidize and decompose to produce gas when the battery is at high temperature, and the more side reactions of the electrolyte lead to electrolyte degradation, and the high temperature performance of the battery is poor. Furthermore, the present invention adds lithium difluorophosphate to the electrolyte, and the decomposition products of lithium difluorophosphate (such as LiF, Li3PO4, etc.) have high ion conductivity and chemical stability. The decomposition products of lithium difluorophosphate can be embedded in the SEI film, improve the composition structure of the SEI film, and improve the density and stability of the SEI film. The antioxidant properties of lithium difluorophosphate help prevent the occurrence of EA oxidation reaction, maintain the stability of the electrolyte, and improve the high temperature performance of the battery.

[0025] In summary, the present invention uses a thick electrode with a double-sided surface density of X. By adjusting the mass percentage of EA (a%) and the mass percentage of lithium difluorophosphate (b%) in the electrolyte, and adjusting the tube diameter (Y nm) of the carbon nanotubes, when the formula 0.6≤(a+Y*b) / X≤1.5 is satisfied, the problems of poor cell wetting, increased impedance, lithium precipitation, etc. can be effectively solved.

[0026] In some embodiments, X, Y, a and b satisfy: 0.8≤(a+Y*b) / X≤1.3, and the value of (a+Y*b) / X can be, for example, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3 or any point value in the range of any two of the above point values. When 0.8≤(a+Y*b) / X≤1.3 is satisfied, the wettability of the battery cell can be further improved, the migration speed of lithium ions can be increased, the impedance can be reduced, and the high temperature performance of the battery can be improved.

[0027] In the present invention, the values ​​of X, Y, a and b can be set with reference to the conventional value ranges of X, Y, a and b in the art. As long as the relationship among X, Y, a and b satisfies 0.8≤(a+Y*b) / X≤1.3, it is within the protection scope of the present invention.

[0028] In order to further improve the battery performance, under the premise of satisfying 0.8≤(a+Y*b) / X≤1.3, the present invention further provides a selectable value range of X, Y, a and b, as follows:

[0029] In some embodiments, the double-sided surface density X of the positive electrode sheet satisfies: 40≤X≤60, and the value of X can be, for example, 40, 42, 44, 46, 48, 50, 52, 54, 56, 58, 60 or any point value in the range of any two of the above point values, preferably 45≤X≤50. When X, Y, a and b satisfy 0.6≤(a+Y*b) / X≤1.5, when the value of X is adjusted within the above range, the thickness of the positive electrode sheet is relatively high, which can improve the energy density of the battery, so that the battery has both high energy density and good wetting ability.

[0030] In some embodiments, in the present invention, the term "tube diameter" of the carbon nanotube refers to the inner diameter of the carbon nanotube. The diameter Y of the carbon nanotube satisfies: 1≤Y≤30, and the value of Y can be, for example, 1, 2, 3, 5, 8, 10, 12, 14, 16, 18, 20, 22, 24, 26, 28, 29, 30 or any point value in the range of the above two point values, preferably 5≤Y≤11. When X, Y, a and b satisfy 0.6≤(a+Y*b) / X≤1.5, when the value of Y is adjusted to meet the above range, the carbon nanotubes can be evenly dispersed in the positive electrode sheet, and the carbon nanotubes are in point-line contact with the positive electrode active material, which can form a better conductive network, accelerate the electrolyte to penetrate into the inside of the electrode sheet through the carbon nanotubes, and provide better thermal conductivity, further improve the wettability of the thick electrode sheet and reduce the temperature rise of the battery.

[0031] In some embodiments, the mass percentage a of ethyl acetate satisfies: 10≤a≤70. Based on the total mass of the electrolyte, the mass percentage of EA (a%) can be, for example, 10%, 12%, 14%, 16%, 18%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 62%, 64%, 66%, 68%, 70% or any point value in the range composed of any two of the above point values, preferably 30≤a≤50. When X, Y, a and b satisfy 0.6≤(a+Y*b) / X≤1.5, when the mass percentage of EA is adjusted to meet the above range, EA can better reduce the viscosity of the electrolyte and improve Li + The transmission efficiency is improved, which enables the electrolyte to penetrate into the electrode faster through the carbon nanotubes, thereby improving the wetting performance of thick electrode sheets.

[0032] In some embodiments, the mass percentage b of lithium difluorophosphate satisfies: 0.1≤b≤1.0. Based on the total mass of the electrolyte, the mass percentage (b%) of lithium difluorophosphate can be, for example, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0 or any point value in the range of any two of the above points, preferably 0.3≤b≤0.5. When X, Y, a and b satisfy 0.6≤(a+Y*b) / X≤1.5, when b is adjusted to meet the above range, lithium difluorophosphate can better improve the density and stability of the SEI film formed at the negative electrode, and further reduce the SEI film impedance.

[0033] In some embodiments, based on the total mass of the positive electrode sheet, the mass percentage of the carbon nanotubes is within 2%, such as 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0% or any point value in the range formed by any two of the above points. When X, Y, a and b satisfy 0.6≤(a+Y*b) / X≤1.5, when the mass percentage of the carbon nanotubes is adjusted to meet the above range, the agglomeration and accumulation of the carbon nanotubes caused by excessive carbon nanotubes can be prevented, the uniformity of the electrode material can be improved, and the battery can be ensured to have a higher energy density while promoting the electrolyte to infiltrate the electrode.

[0034] In some embodiments, the carbon nanotubes include single-walled carbon nanotubes and / or multi-walled carbon nanotubes. The diameters of the single-walled carbon nanotubes and / or multi-walled carbon nanotubes are all between 1-30 nm. For example, the carbon nanotubes are single-walled carbon nanotubes, the carbon nanotubes are multi-walled carbon nanotubes, or the carbon nanotubes are a mixture of single-walled carbon nanotubes and multi-walled carbon nanotubes.

[0035] In some embodiments, the conductive agent may include at least one of conductive carbon black, conductive graphite, acetylene black, Ketjen black, graphene, conductive carbon fiber, carbon nanotubes, metal powder and carbon fiber in addition to carbon nanotubes. When the conductive agent is mixed with carbon nanotubes, the electrode conductivity can be further improved, the electrode conductive network is more abundant, and the electrolyte is promoted to infiltrate the positive electrode.

[0036] In some embodiments, the positive electrode active material includes lithium iron phosphate (LiFePO4, LFP). LFP is an olivine structure, and the olivine structure makes the lithium iron phosphate lithium ion transmission channel relatively limited, mainly a one-dimensional channel, which affects the lithium ion diffusion performance. When X, Y, a and b satisfy 0.6≤(a+Y*b) / X≤1.5, it is used in combination with the lithium iron phosphate positive electrode active material to improve the wettability of the positive electrode sheet and the dynamics of the electrolyte, thereby alleviating the obstruction of lithium ion transmission caused by lithium iron phosphate, which is conducive to improving the transmission of ions.

[0037] As the particle size of the positive electrode active material increases, the compaction of the battery positive electrode material increases, which can significantly improve the battery energy density. However, as the particle size increases, it will lead to Li + The transfer rate continues to decrease and makes the wetting of the electrode more difficult.

[0038] In order to solve the above problems, the present invention further proposes: the surface of the lithium iron phosphate has a coating layer, the coating layer includes Ti element, the total mass of the lithium iron phosphate is recorded as M ppm; the lithium iron phosphate includes primary particles and / or secondary particles, the average particle size of the primary particles is recorded as D nm; M, D and a satisfy:

[0039] The Ti content in the lithium iron phosphate surface coating layer can be measured by EDS (Energy Dispersive X-ray Spectroscopy) test; and / or ICP (Inductively Coupled Plasma) test.

[0040] The value of can be, for example, 0.1, 0.5, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15 or any point value in the range consisting of any two of the above point values.

[0041] On the basis that X, Y, a and b satisfy 0.6≤(a+Y*b) / X≤1.5, by doping Ti element in the surface coating layer of the positive electrode active material lithium iron phosphate, on the basis that When Li-Ti-O fast ion conductors are formed on the positive electrode surface, they provide fast ion transport paths, increase the effective electrode reaction area, improve kinetics, and increase Li + Transmission rate. At the same time, add the conditions that satisfy 0.6≤(a+Y*b) / X≤1.5 and The specific mass percentage of EA (a%) can better reduce the viscosity of the electrolyte and further improve the Li +The transmission rate can effectively solve the wetting difficulty problem caused by the increase of primary particles and / or secondary particles of the positive electrode material of the battery, and improve the wettability of the battery electrode.

[0042] In some embodiments, M, D and a satisfy: The value of can be, for example, 0.3, 0.5, 1.0, 2.0, 3.0, 4.0, 5.0, 6.0, 7.0, 8.0, or any point value in the range consisting of any two of the above point values. When the above range is met, the wettability of the electrode can be better improved.

[0043] In some embodiments, based on the total mass of lithium iron phosphate, the content M (ppm) of the Ti element satisfies: 500≤M≤5000. The content of the Ti element can be, for example, 500ppm, 550ppm, 600ppm, 650ppm, 700ppm, 1000ppm, 1500ppm, 2000ppm, 2500ppm, 3000ppm, 3500ppm, 4000ppm, 4500ppm, 4700ppm, 5000ppm or any point value in the range of any two of the above point values. When X, Y, a and b satisfy 0.6≤(a+Y*b) / X≤1.5, M, D and a satisfy When M is adjusted to meet the above range, the distribution of Ti element in the coating layer can be more uniform, the electronic conductivity of the positive electrode active material can be improved, and the Li between the active material particles can be increased. + Transmission efficiency can also stabilize the material structure, reduce the formation of lattice defects and reduce internal resistance.

[0044] In some embodiments, the average particle size D (nm) of the primary particles satisfies: 100≤D≤800. The average particle size of the primary particles can be, for example, 100nm, 200nm, 220nm, 240nm, 300nm, 350nm, 400nm, 450nm, 500nm, 550nm, 600nm, 750nm, 770nm, 800nm ​​or any point value in the range of any two of the above points. When X, Y, a and b satisfy 0.6≤(a+Y*b) / X≤1.5, M, D and a satisfy When D is adjusted to meet the above range, the contact area between particles can be increased, the density of particles can be increased, which is beneficial to improve the energy density of the battery, improve the electrode structure, and increase Li + Transmission efficiency, improve the charging and discharging efficiency of the battery.

[0045] In some embodiments, the average particle size of the secondary particles is 0.5 μm-3 μm. The average particle size of the secondary particles can be, for example, 0.5 μm, 0.8 μm, 1.0 μm, 1.2 μm, 1.4 μm, 1.6 μm, 1.8 μm, 2.0 μm, 2.2 μm, 2.4 μm, 2.6 μm, 2.8 μm, 3.0 μm, or any point value in the range of any two of the above points. When X, Y, a and b satisfy 0.6≤(a+Y*b) / X≤1.5, M, D and a satisfy When the average particle size of the secondary particles is adjusted to meet the above range, the conductivity and wettability of the electrode sheet can be further improved.

[0046] In order to further improve the wettability of the electrode sheet, the present invention further proposes that: the contact angle θ between the positive electrode sheet and the electrolyte is 5° to 35°. The value of the contact angle θ can be, for example, 5°, 8°, 10°, 12°, 14°, 16°, 18°, 20°, 22°, 24°, 26°, 28°, 30°, 32°, 35° or any point value in the range of any two of the above point values, preferably 5° to 15°. When X, Y, a and b satisfy 0.6≤(a+Y*b) / X≤1.5, M, D and a satisfy When θ is adjusted to meet the above range, the electrolyte can be evenly spread on the surface of the positive electrode sheet, promoting uniform infiltration of the electrolyte, and at the same time avoiding the problem of further deterioration of the high temperature performance of the battery due to excessively small contact angle θ and excessive EA content in the electrolyte, thereby ensuring that the battery has better high temperature performance and better wettability of the battery electrode sheet.

[0047] The contact angle θ can be measured using the sessile drop method, which includes the following steps: prepare a flat electrode plate, measure the contact angle of the electrolyte on the electrode plate by the sessile drop method, use a 1 μL water droplet as the electrolyte, test 10 times in a row and take the average value, θ average = (θ1+θ2+…+θ10) / 10.

[0048] In the present invention, when EA is added to the electrolyte, a high EA content will cause the high temperature performance of the battery to deteriorate. At the same time, due to the poor kinetic performance of the thick electrode, the impedance of the SEI film is large, and the resistance of lithium ions passing through the SEI film is large. To further solve the above problems, the present invention further proposes the following solutions:

[0049] In some embodiments, a sulfur (S) additive is added to the electrolyte; the mass percentage of the sulfur additive is 0.05%-3% based on the total mass of the electrolyte. The mass percentage of the sulfur additive can be, for example, 0.05%, 0.1%, 0.5%, 1.0%, 1.5%, 2.0%, 2.5%, 2.8%, 3.0% or any point value in the range composed of two points above, preferably 0.1%-1.0%. Exemplarily, the sulfur additive includes at least one of methylene disulfonate (MMDS), vinyl sulfate (DTD), thiophene, and vinyl sulfite. Adding a sulfur additive to the electrolyte can generate inorganic components such as Li2SO3 when the SEI film is formed at the negative electrode, reduce the film formation impedance, increase the speed of lithium ions passing through the SEI film, and at the same time improve the high temperature resistance of the SEI film, further make up for the high temperature degradation defects caused by adding EA to the electrolyte, and improve the high temperature performance of the battery. In addition to the above functions, the addition of thiophene to the electrolyte can also complex the H atoms of HF and H2O in the electrolyte due to the action of lone pair electrons, which has the effect of removing water and inhibiting acid, and can effectively prevent HF from corroding the SEI film, enhance the negative electrode interface protection, and improve the high-temperature cycle performance of the battery.

[0050] In some embodiments, the electrolyte further includes a nitrogen (N) additive and / or a phosphorus (P) additive; based on the total mass of the electrolyte, the mass percentage of the N additive and / or the P additive is 0.1%-1%; the mass percentage of the N additive and / or the P additive can be 0.05%, 0.1%, 0.5%, 1.0%, 1.5%, 2.0%, 2.5%, 2.8%, 3.0% or any point value in the range composed of any two of the above point values, preferably 0.1%-1%. Exemplarily, the nitrogen-containing additives include but are not limited to pyridine additives (e.g., 2-fluoropyridine), pyrazine additives, pyridazine additives, triazine additives (e.g., trifluorotriazine), preferably 2-fluoropyridine, and the P-containing additives include but are not limited to tris(trimethylsilyl)phosphite (TMSP), tris(trimethylsilyl)phosphite (TMSPi), 1-propyl phosphoric anhydride, 1-butyl phosphoric anhydride, tris(pyrrolidin-1-yl)phosphine, and ethoxypentafluorocyclotriphosphazene. The N atom in the N-containing additive or the P atom in the P-containing additive can also complex the H atoms of HF and H2O in the electrolyte through the action of lone pairs of electrons, remove water and suppress acid, effectively prevent HF from corroding the SEI film, enhance the negative electrode interface protection, and improve the high temperature cycle performance of the battery.

[0051] In some embodiments, the double-sided surface density of the negative electrode sheet is 20-30 mg / cm 2 The double-sided surface density of the negative electrode sheet can be, for example, 20 mg / cm 2 , 21mg / cm 2, 22mg / cm 2 , 23mg / cm 2 , 24mg / cm 2 , 25mg / cm 2 、26mg / cm 2 , 27mg / cm 2 、28mg / cm 2 , 29mg / cm 2 、30mg / cm 2 Or any point value in the range of the above two point values. In some embodiments, the compaction density of the negative electrode sheet is 1.4-1.8 mg / cm 3 The compaction density of the negative electrode sheet can be, for example, 1.40 mg / cm 3 、1.45mg / cm 3 、1.50mg / cm 3 、1.55mg / cm 3 、1.60mg / cm 3 、1.65mg / cm 3 、1.70mg / cm 3 、1.75mg / cm 3 、1.80mg / cm 3 Or any point value in the range of the above two point values. When the double-sided surface density and / or compaction density of the negative electrode sheet meets the above range, the Li ions released from the positive electrode can be effectively suppressed. + The lithium plating problem caused by the inability of the negative electrode to accommodate lithium can work together with the double-sided surface density of the positive electrode to significantly improve the energy density of the battery.

[0052] In some embodiments, the ratio NP of the negative electrode sheet capacity to the positive electrode sheet capacity is 1.08-1.20. The value of NP can be, for example, 1.08, 1.10, 1.12, 1.14, 1.16, 1.18, 1.20 or any point value in the range composed of the above two point values. Exemplarily, the calculation method of the ratio NP of the negative electrode sheet capacity to the positive electrode sheet capacity is: NP = gram capacity of negative electrode active material * loading (negative electrode active material content) * negative electrode surface density / gram capacity of positive electrode active material * loading (positive electrode active material content) * positive electrode surface density. When NP meets the above range, the risk of battery failure caused by lithium plating caused by too low NP ratio can be avoided, and the problem of low battery capacity and reduced battery energy density caused by excessive N / P and irreversible capacity loss of the battery can also be avoided. The ratio NP of the negative electrode sheet capacity to the positive electrode sheet capacity is 1.08-1.20, which can give full play to the positive electrode gram capacity and take into account the high temperature performance and safety performance of the battery.

[0053] In some embodiments, the separator includes a base film, and the base film includes a polyolefin material. Exemplarily, the polyolefin material includes at least one of a polypropylene material and a polyethylene material.

[0054] In some embodiments, the porosity of the base film is 30%-60%. The porosity of the base film can be, for example, 30%, 35%, 40%, 45%, 50%, 55%, 60%, or any point value in the range of two points above. When the porosity of the base film meets the above range, the kinetics can be improved and the Li in the electrolyte can be promoted. + The transmission can also further improve the wettability of the electrolyte to the thick electrode.

[0055] In some embodiments, the thickness of the base film is 3 μm-25 μm. The thickness of the base film can be, for example, 3 μm, 4 μm, 5 μm, 8 μm, 10 μm, 12 μm, 14 μm, 16 μm, 18 μm, 20 μm, 22 μm, 24 μm, 25 μm, or any point value in the range of the above two point values. When the thickness of the base film meets the above range, it can help the electrolyte to better penetrate and fill the internal pores of the base film, increase the contact area between the electrolyte and the electrode, facilitate the infiltration of the electrolyte, and thus reduce the internal resistance of the battery.

[0056] In some embodiments, the positive electrode sheet includes a positive electrode active material layer, the positive electrode active material layer includes a positive electrode active material and a conductive agent, and further includes at least one of a binder, an anti-cracking agent, and a dispersant.

[0057] In some embodiments, the positive electrode sheet further includes a binder, and the mass percentage of the binder is 1% to 3.5% based on the total mass of the positive electrode active material layer.

[0058] Exemplarily, the binder includes at least one of polyvinylidene fluoride, polytetrafluoroethylene, polyethylene oxide, sodium carboxymethyl cellulose, and styrene-butadiene rubber (SBR). Adding a binder to the positive electrode sheet can improve the mechanical strength of the electrode sheet, adjust the battery structure, improve the conductivity, and facilitate the infiltration of the electrolyte.

[0059] In some embodiments, the positive electrode sheet further includes an anti-cracking agent, and the mass percentage of the anti-cracking agent is 0.05% to 0.5%, preferably 0.2%, based on the total mass of the positive electrode active material layer. Exemplarily, the anti-cracking agent includes at least one of a polyether compound and a polyester compound. Adding an anti-cracking agent to the positive electrode sheet can stabilize the electrode sheet structure, enhance the mechanical strength of the electrode sheet, improve the high temperature resistance of the battery, and prevent cracking.

[0060] In some embodiments, the positive electrode sheet further includes a dispersant, and the mass percentage of the dispersant is 0.05% to 0.5%, preferably 0.2%, based on the total mass of the positive electrode active material layer. Exemplarily, the dispersant includes at least one of a polyether compound, a polyester compound, and a cyclic compound (including a compound containing a benzene ring). Adding a dispersant to the positive electrode sheet can evenly disperse the active material in the electrode sheet, prevent particle agglomeration, increase the specific surface area of ​​the electrode sheet, and improve battery performance.

[0061] In some embodiments, the electrolyte further comprises a carbonate solvent; preferably, based on the total mass of the electrolyte, the mass proportion of the carbonate solvent is 40%-90%, for example, it can be 40%, 45%, 50%, 60%, 70%, 80%, 90% or any point value in the range of the above two point values. The carbonate solvent includes but is not limited to at least one of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate and ethyl methyl carbonate and fluorinated products thereof. The addition of a carbonate solvent to the electrolyte can make the interface generated by the electrolyte at the negative electrode more stable, improve the cycle performance of the battery, and improve the safety performance of the battery.

[0062] In some embodiments, the electrolyte further includes an electrolyte lithium salt, and the amount of the electrolyte lithium salt is 0.3 to 1.8 mol / L based on the total mass of the electrolyte.

[0063] Exemplarily, the electrolyte lithium salt includes at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium bis(fluorosulfonyl)imide, and lithium bis(trifluoromethylsulfonyl)imide. The above lithium salt additive is added to the electrolyte, and the lithium salt additive can improve the ionic conductivity of the electrolyte, make the migration rate of lithium ions in the electrolyte faster, and improve the battery performance.

[0064] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0065] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources.

[0066] The present invention is described in detail below in conjunction with specific embodiments, which are used to understand but not to limit the present invention.

[0067] The batteries of the examples and comparative examples of the present invention were prepared according to the following preparation method, and the differences from Example 1-1 are shown below.

[0068] Example 1-1

[0069] (1) Preparation of electrolyte

[0070] In an argon glove box with a water content of <0.1ppm and an oxygen content of <0.1ppm, ethylene carbonate (EC), ethyl methyl carbonate (EMC) and ethyl acetate (EA) are mixed evenly, and fully dried lithium hexafluorophosphate (LiPF6) is added thereto for stirring and dissolution, the mass of LiPF6 added is 12.5% ​​of the total mass of the electrolyte, 0.5% of lithium difluorophosphate based on the total mass of the electrolyte is added, 2.3% of vinylene carbonate (VC), 0.5% of fluoroethylene carbonate (FEC), 0.5% of vinyl sulfate (DTD), 0.3% of tris(trimethylsilyl) phosphite (TMSP), 0.3% of thiophene and 0.2% of 2-fluoropyridine are added based on the total mass of the electrolyte, and stirred evenly, the mass proportion of EA in the electrolyte is 40%, the mass proportion of EC and EMC (the mass ratio of the two is 1:1) in the electrolyte can be obtained by calculation, and the electrolyte is obtained after passing the physical property test.

[0071] (2) Preparation of positive electrode

[0072] Lithium iron phosphate (LFP), polyvinylidene fluoride and conductive agent (acetylene black and carbon nanotubes, mass ratio 5:3) were put into a vacuum mixer according to a mass ratio of 97:1.5:1.3, and N-methylpyrrolidone (NMP) was added. They were fully mixed under the action of the vacuum mixer until a uniform and fluid positive electrode slurry was formed, wherein the solid content was 55wt%, wherein the LFP positive electrode material was purchased from Hubei Rongtong High-Tech Advanced Materials Group Co., Ltd., the content M of the encapsulated Ti element was 1500ppm, and the particle size value D of the primary particles was 530nm; the above positive electrode slurry was evenly coated on an aluminum foil with a thickness of 13μm, and the coating double-sided surface density was 48mg / cm 2 , drying, rolling, slitting and punching to obtain the positive electrode sheet.

[0073] (3) Preparation of negative electrode sheet

[0074] Graphite, styrene-butadiene rubber, sodium carboxymethyl cellulose and acetylene black were put into a vacuum mixer in a mass ratio of 96.5:1.45:1.05:1, and deionized water was added to fully mix them under the action of the vacuum mixer to finally form a uniform and fluid negative electrode slurry with a solid content of 45wt%. The negative electrode slurry was evenly coated on a copper foil with a thickness of 8μm, dried, rolled and die-cut to obtain a negative electrode sheet, and the double-sided surface density of the negative electrode sheet was 21.50mg / cm 2 , compacted density is 1.55g / cm 3 , the NP ratio is 1.13.

[0075] (4) Preparation of batteries

[0076] The positive electrode sheet obtained in step (1), the negative electrode sheet obtained in step (2) and the separator (a polyethylene separator with a thickness of 8 μm and a porosity of 35% provided by Asahi Kasei Corporation) are wound to obtain a bare battery cell; the bare battery cell is welded with a pole ear and placed in a battery casing, and the electrolyte prepared in step (3) is injected into the dried and qualified battery cell, and a battery is obtained after standing, aging, formation, exhaust, aging, sorting and other processes.

[0077] (5) Test battery

[0078] (i) 45℃ high temperature cycle test

[0079] The batteries prepared in the examples and comparative examples were subjected to a 45°C high temperature cycle test. The specific test method is as follows:

[0080] Place the battery in a 45±1℃ environment, leave it for 180min, discharge it to 2.2V at 0.5C constant current, leave it for 30min, charge it to 3.65V at 0.25C constant current and constant voltage, cut off current 0.05C, leave it for 30min, discharge it to 2.2V at 0.25C constant current, record the discharge capacity C0, leave it for 30min, charge it to 3.65V at 0.5C0 constant current and constant voltage, cut off current 0.05C0, leave it for 30min, discharge it to 2.2V at 0.5C0 constant current, when the cycle reaches n times, record the last discharge capacity Cn, the capacity retention rate of the nth time is calculated as follows: Capacity retention rate (%) = Cn / C0×100%.

[0081] (ii) 25℃ 0.5C / 0.5C cycle 50T dissection test

[0082] Place the battery in a 25±1℃ environment, leave for 120min, discharge at 0.5C constant current to 2.2V, leave for 30min, charge at 0.25C constant current and constant voltage to 3.65V, cut-off current 0.05C, leave for 30min, discharge at 0.25C constant current to 2.2V, record discharge capacity C0, leave for 30min, charge at 0.5C0 constant current and constant voltage to 3.65V, cut-off current 0.05C0, leave for 30min, discharge at 0.5C0 constant current to 2.2V, when the cycle reaches 50 cycles, charge at 0.5C0 constant current and constant voltage to 3.65V, cut-off current 0.05C0, and dissect after full charge.

[0083] (iii) 25°C 50% SOC EIS test (Electrochemical Impedance Spectroscopy test)

[0084] The battery was placed in a 25±1℃ environment, left for 60 min, discharged at 0.5C constant current to 2.2V, left for 30 min, charged at 0.5C constant current and constant voltage to 3.65V, with a cutoff current of 0.05C, left for 30 min, discharged at 0.5C constant current to 2.2V, and the discharge capacity C0 was recorded. Left for 30 min, charged at 1.0C0 constant current and constant voltage to 3.65V, with a cutoff current of 0.05C0, left for 30 min, discharged at 0.5C0 constant current to 50% SOC, and then subjected to EIS test.

[0085] (iv) Drop test

[0086] The drip test is used to characterize the wettability of the electrolyte on the electrode.

[0087] First, prepare a flat electrode plate, several 1mL syringes and a stopwatch, then gently drop a drop of electrolyte on the electrode plate and start timing until the drop completely disappears on the electrode plate, stop timing and record the time. For each electrolyte, make three drop samples in parallel on the positive electrode plate and calculate the average, taverage = (t1+t2+t3) / 3.

[0088] With reference to Example 1-1, the proportion of ethyl acetate in Example 1 was changed to a, the proportion of lithium difluorophosphate in Example 2 was changed to b, the diameter of carbon nanotubes Y was changed in Example 3, and the double-sided surface density of the positive electrode sheet X was changed in Example 4. The changes in the values ​​of a, b, and X in Comparative Examples 1 and 2 resulted in the formula not satisfying 0.6≤(a+Y*b) / X≤1.5, the change in the value of a in Comparative Example 3 resulted in the formula not satisfying 0.6≤(a+Y*b) / X≤1.5, lithium difluorophosphate was not added in Comparative Example 4, and the change in the value of Y in Comparative Example 5 resulted in the formula not satisfying 0.6≤(a+Y*b) / X≤1.5. The specific data are shown in Table 1.

[0089] Table 1

[0090]

[0091]

[0092] Note: "*" indicates that the corresponding parameter in this embodiment or comparative example is the same as that in Example 1-1. " / " indicates that the corresponding parameter was not tested.

[0093] As can be seen from Table 1, the present invention can effectively improve the wettability of the battery cell while taking into account the high temperature performance of the battery, and effectively solve the problems of poor battery cell wettability, increased impedance, lithium precipitation, etc. by adding a conductive agent to the positive electrode sheet, using an electrolyte containing ethyl acetate and lithium difluorophosphate, and adjusting the diameter of the carbon nanotubes in the conductive agent, and the contents of ethyl acetate and lithium difluorophosphate to meet 0.6≤(a+Y*b) / X≤1.5.

[0094] Referring to Example 1-1, in Example 5 group, Example 5-1 and Example 5-2 change the average particle size D of the lithium iron phosphate primary particles, and Example 5-3 and Example 5-4 change the content M of the Ti element doped in the lithium iron phosphate surface coating layer. The specific data are shown in Table 2.

[0095] Table 2

[0096]

[0097] Note: "*" indicates that the corresponding parameter in this embodiment or comparative example is the same as that in Example 1-1. " / " indicates that the corresponding parameter was not tested, and the specific data are shown in Table 3.

[0098] As can be seen from Table 2, in the present invention, on the basis that X, Y, a and b satisfy 0.6≤(a+Y*b) / X≤1.5, lithium iron phosphate is selected as the positive electrode active material, and Ti element is doped in the surface coating layer of lithium iron phosphate to satisfy When Li-Ti-O fast ion conductors are formed on the positive electrode surface, they provide fast ion transport paths, increase the effective electrode reaction area, improve kinetics, and increase Li + transmission rate, improving the high temperature performance of the battery. At the same time, adding The specific mass percentage of EA (a%) can better reduce the viscosity of the electrolyte and further improve the Li + The transmission rate can effectively solve the wetting difficulty problem caused by the increase of primary particles and / or secondary particles of the positive electrode material of the battery, and improve the wettability of the battery electrode.

[0099] Referring to Example 1-1, in Example 6, the nitrogen-containing additive and the phosphorus-containing additive were not added in Example 6-1; the sulfur-containing additive and the phosphorus-containing additive were not added in Example 6-2; the sulfur-containing additive and the nitrogen-containing additive were not added in Example 6-3; and the sulfur-containing additive, the nitrogen-containing additive, and the phosphorus-containing additive were not added in Example 6-4.

[0100] Table 3

[0101]

[0102] It can be seen from Table 3 that the present invention, by adding S-containing additives, N-containing additives and P-containing additives to the electrolyte, can complex the H atoms of HF and H2O in the electrolyte through the action of lone pair electrons, remove water and inhibit acid, effectively prevent HF from corroding the SEI film, enhance the negative electrode interface protection, and improve the high temperature cycle performance of the battery.

[0103] It should be noted that, in this article, the terms "comprise", "include" or any other variant thereof are intended to cover non-exclusive inclusion, so that the process, method, article or device including a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise one..." do not exclude the presence of other identical elements in the process, method, article or device including the element. In addition, it should be pointed out that the scope of the methods and devices in the embodiments of the present application is not limited to performing functions in the order shown or discussed, and may also include performing functions in a substantially simultaneous manner or in reverse order according to the functions involved, for example, the described method may be performed in an order different from that described, and various steps may also be added, omitted, or combined. In addition, the features described with reference to certain examples may be combined in other examples.

[0104] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A lithium ion secondary battery, characterized in that: The lithium-ion secondary battery comprises a positive electrode sheet, a separator, a negative electrode sheet and an electrolyte; the double-sided surface density of the positive electrode sheet is recorded as X mg / cm 2 ; The positive electrode sheet includes a positive electrode active material and a conductive agent, the conductive agent includes carbon nanotubes, and the diameter of the carbon nanotubes is denoted as Y nm; The electrolyte includes ethyl acetate; the mass percentage of ethyl acetate is recorded as a% based on the total mass of the electrolyte; The electrolyte includes lithium difluorophosphate; based on the total mass of the electrolyte, the mass percentage of lithium difluorophosphate is recorded as b%; X, Y, a and b satisfy: 0.6≤(a+Y*b) / X≤1.

5.

2. The battery according to claim 1, characterized in that X, Y, a and b satisfy: 0.8≤(a+Y*b) / X≤1.3; Preferably, X satisfies: 40≤X≤60, more preferably 45≤X≤50; Preferably, Y satisfies: 1≤Y≤30, more preferably 5≤Y≤11.

3. The battery according to claim 1, characterized in that a satisfies: 10≤a≤70, preferably 30≤a≤50; And / or, b satisfies: 0.1≤b≤1.0, preferably 0.3≤b≤0.

5.

4. The battery according to claim 1, characterized in that The positive electrode active material includes lithium iron phosphate; the surface of the lithium iron phosphate has a coating layer, and the coating layer includes a Ti element; the content of the Ti element is recorded as M ppm based on the total mass of the lithium iron phosphate; The lithium iron phosphate includes primary particles and / or secondary particles, and the average particle size of the primary particles is denoted as Dnm; M, D and a satisfy:

5. The battery according to claim 4, characterized in that M, D and a satisfy: Preferably, M satisfies: 500≤M≤5000; and / or, D satisfies: 100≤D≤800; Preferably, the average particle size of the secondary particles is 0.5 μm to 3 μm.

6. The battery according to claim 1, characterized in that The contact angle θ between the positive electrode sheet and the electrolyte is 5° to 35°, preferably 5° to 15°.

7. The battery according to any one of claims 1 to 6, characterized in that: The electrolyte further comprises a sulfur-containing additive; based on the total mass of the electrolyte, the mass percentage of the sulfur-containing additive is 0.05%-3%; Preferably, the sulfur-containing additive includes at least one of methylene methanedisulfonate, vinyl sulfate, thiophene, and vinyl sulfite.

8. The battery according to any one of claims 1 to 6, characterized in that: The electrolyte further comprises a nitrogen-containing additive and / or a phosphorus-containing additive; based on the total mass of the electrolyte, the mass percentage of the nitrogen-containing additive and / or the phosphorus-containing additive is 0.05%-3%; Preferably, the nitrogen-containing additive includes at least one of pyridine additives, pyrazine additives, pyridazine additives, and triazine additives, and more preferably 2-fluoropyridine; Preferably, the phosphorus-containing additive includes at least one of tris(trimethylsilyl)phosphite, tris(trimethylsilyl)phosphite, 1-propyl phosphoric anhydride, 1-butyl phosphoric anhydride, tris(pyrrolidin-1-yl)phosphine, and ethoxypentafluorocyclotriphosphazene.

9. The battery according to any one of claims 1 to 6, characterized in that: The double-sided surface density of the negative electrode sheet is 20-30 mg / cm 2 ; And / or, the compaction density of the negative electrode sheet is 1.4-1.8 mg / cm 3 ; And / or, the ratio NP of the negative electrode sheet capacity to the positive electrode sheet capacity is 1.08-1.

20.

10. The battery according to any one of claims 1 to 6, characterized in that: The separator includes a base film, and the base film includes a polyolefin material; Preferably, the porosity of the base film is 30%-60%; Preferably, the base film has a thickness of 3 μm-25 μm.

Citation Information

Cited By

  • Solvent composition for solid-state battery, slurry composition for battery,

    CN120527443A

  • Solvent composition for solid-state battery, slurry composition for battery, battery, and method for producing the same

    CN120527443B

  • Battery cell, battery device, and electric device

    CN122393288A