Sodium ion composite all-solid-state electrolyte and preparation method thereof

By doping sodium salt and sulfide electrolyte in polymer electrolyte, the conductivity and interface stability of sodium ion all-solid electrolyte are improved, the low conductivity and stability of existing electrolytes are solved, and the performance of sodium batteries is improved and security.

CN118919830APending Publication Date: 2024-11-08HUNAN XIANNA TECH CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411291193.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-14
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The ionic conductivity of existing sodium ion all-solid electrolytes is relatively low and the interface chemical stability is insufficient, resulting in battery performance and safety hazards, limiting the commercial application of sodium batteries.

Method used

The sodium salt and sulfide electrolyte Na3-xPS4-xClx powder are uniformly dispersed in the polymer electrolyte matrix. By optimizing the electrolyte material, the conductivity and interface stability are improved, and the mechanical properties are improved, and the sodium ion composite all-solid electrolyte is prepared.

Benefits of technology

It improves the charge and discharge efficiency, cycle stability and safety of the battery, broadens the electrochemical window, inhibits interface reactions and dendrites, and enhances the overall performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919830A_ABST
    Figure CN118919830A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of batteries, and particularly provides a sodion composite solid electrolyte which comprises a polymer electrolyte matrix, the powder particles of sodium salt and sulfide electrolyte Na3-xPS4-xClx are uniformly dispersed in the matrix, and x is more than 0 and less than or equal to 2.0; wherein the mass ratio of the sodium salt in the sodium ion composite solid electrolyte is 10%-40%, the mass ratio of the Na < 3-x > PS < 4-x > Cl < x > in the sodium ion composite solid electrolyte is 0.5%-10%, and the balance is the polymer electrolyte matrix. Compared with a traditional polymer solid electrolyte membrane, the composite polymer electrolyte shows remarkable advantages including higher sodium ion conductivity, a more stable interface and lower impedance. In practical application, an all-solid-state battery assembled by the electrolyte shows excellent cycling stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of electrochemistry, and in particular relates to a sodium ion composite all-solid electrolyte and a preparation method thereof. Background Art

[0002] Sodium-ion batteries, as a battery technology that has received much attention in recent years, have shown great application potential in the field of new energy with their abundant sodium resources, low cost and potential high performance advantages. Traditional sodium-ion batteries are limited by the lack of organic liquid electrolytes and it is difficult to achieve higher energy density and higher safety requirements. All-solid-state batteries can solve the safety hazards that may be caused by liquid electrolytes. Although sodium-ion all-solid-state batteries have many potential advantages, their commercialization process also faces some challenges, especially in the selection of electrolyte materials. Traditional single solid electrolytes are often difficult to meet the requirements of sodium-ion batteries in electrochemical and mechanical properties. Therefore, the development of a new type of composite electrolyte material to improve the comprehensive performance of sodium-ion batteries has become the focus of current research.

[0003] Chinese patent application CN108199083A discloses a composite electrolyte between liquid and solid and a preparation method thereof, wherein the electrolyte solvent accounts for 30-75%, the sodium salt accounts for 7-15%, the polymer accounts for 8-12%, and the ceramic powder accounts for 5-55%. The design of this composite electrolyte is intended to improve the safety and cycle performance of sodium ion batteries, while improving the interface contact between the electrolyte and the electrode. However, the sodium ion battery electrolyte in this scheme is not completely solid, but an electrolyte containing a certain amount of liquid solvent, thus forming a semi-solid electrolyte; although this design may improve the ion conductivity of the electrolyte to a certain extent, it may also introduce safety risks brought by the liquid electrolyte, such as leakage, short circuit and other problems. Secondly, the organic solvents used are volatile, flammable, and toxic, which not only brings safety hazards to the production, storage and use of batteries, but also pollutes the environment. Especially when abnormal conditions such as thermal runaway occur in the battery, these organic solvents may aggravate the combustion or explosion of the battery.

[0004] Chinese patent application CN115663274A mainly relates to a method for preparing a sodium ion composite solid electrolyte, which records that Na 3 PS 4The composite solid electrolyte is obtained by air flow pulverization and tableting, realizing the uniform compounding of sodium ion solid electrolyte by solvent-free process, in which the composite agent mainly acts as a binder. This method not only improves the ionic conductivity of the composite solid electrolyte to 0.71mS / cm, but also avoids the problems of uneven dispersion and agglomeration that may occur in the preparation process of traditional solid phase method. However, the composite solid electrolyte membrane prepared by dry process has poor interface wettability and poor contact with electrode, resulting in high interface resistance. The solid electrolyte prepared by this technology has the main component of Na 3 PS 4 , the dosage is 99%-99.8%, and the proportion of the composite agent is very small. During the preparation process and after the battery is assembled, the sulfide solid electrolyte is easy to react with moisture and oxygen, the interface chemical stability is insufficient, and the interface reaction is easy to occur, resulting in battery performance attenuation and safety hazards. Chinese patent application CN115763801A discloses a solid electrolyte membrane with an organic porous membrane as a carrier, and a first electrolyte coating and a second electrolyte coating are distributed on the front and back of the organic porous membrane. The first electrolyte coating and the second electrolyte coating are independently selected from aqueous electrolyte coatings or oily electrolyte coatings. The thickness of the solid electrolyte membrane is controllable and has good thermal stability and good mechanical properties, which improves the poor processability and flexibility of inorganic solid electrolyte membranes. However, this technology may still have safety risks such as leakage and explosion when a small amount of electrolyte is injected during the preparation process, and the organic porous membrane is a non-electrolyte material, which has a lower energy density than all-solid-state batteries.

[0005] Based on the analysis of existing technologies, the current sodium ion all-solid-state electrolytes have the following problems that limit the performance and commercial application of all-solid-state sodium batteries:

[0006] (1) Compared with liquid electrolytes, the ionic conductivity of solid electrolytes is generally lower. The lack of ionic conductivity means that the ion migration rate is slower during the battery charging and discharging process, which affects the battery's charging and discharging efficiency, thereby limiting the battery's overall performance.

[0007] (2) The chemical stability of the interface between solid electrolytes and electrode materials is a key factor restricting their application. Sulfide solid electrolytes easily react with water and oxygen, resulting in performance degradation. At the same time, when assembled with electrode materials such as layered oxide positive electrode materials and metallic sodium negative electrodes, the electrolyte-electrode interface chemical stability is insufficient, and interfacial reactions are prone to occur, leading to battery performance degradation and safety hazards.

[0008] Therefore, the inventors hope to propose a sodium ion all-solid-state electrolyte with high ionic conductivity and high interfacial chemical stability and a preparation scheme thereof, so as to improve the comprehensive performance and market competitiveness of all-solid-state sodium batteries. Summary of the invention

[0009] 1. Technical issues to be resolved

[0010] In view of the above-mentioned shortcomings and deficiencies of the prior art, the present invention provides a sodium ion composite all-solid-state electrolyte and a preparation method thereof, which optimizes the electrolyte material, improves the conductivity of the all-solid-state electrolyte and the interface stability between the all-solid-state electrolyte and the electrode, avoids problems such as interface reaction and dendrite growth, and improves the mechanical properties of the all-solid-state electrolyte, thereby improving the electrochemical performance and cycle stability of the sodium ion battery, and provides a possibility for realizing the application of metallic sodium electrodes in solid-state batteries.

[0011] (II) Technical solution

[0012] In a first aspect, the present invention provides a sodium ion composite solid electrolyte, which comprises a polymer electrolyte matrix; a sodium salt and a sulfide electrolyte Na uniformly dispersed in the matrix; 3-x PS 4-x Cl x Powder particles, wherein 0<x≤2.0; wherein the mass proportion of sodium salt in the sodium ion composite solid electrolyte is 10%-40%, Na 3-x PS 4-x Cl x The mass proportion in the sodium ion composite solid electrolyte is 0.5%-10%, and the remainder is the polymer electrolyte matrix.

[0013] Preferably, wherein x=0.1-0.3; and Na 3-x PS 4-x Cl x The mass proportion in the sodium ion composite solid electrolyte is 1%-2%, and more preferably 1.5%.

[0014] According to a preferred embodiment of the present invention, the polymer electrolyte matrix is ​​at least one of polyethylene oxide (PEO), polyethylene carbonate (PEC), polypropylene carbonate (PPC) and polyacrylonitrile (PAN), and its weight average molecular weight is 10 5 -10 6 order of magnitude.

[0015] According to a preferred embodiment of the present invention, the sodium salt is sodium bis(trifluoromethylsulfonyl)imide (NaTFSI), sodium bis(fluorosulfonyl)imide (NaFSI), sodium perchlorate (NaClO 4 ) and sodium hexafluorophosphate (NaPF 6 ) at least one of.

[0016] According to a preferred embodiment of the present invention, Na 3-x PS 4-x Cl xThe mass proportion of sodium ion in the sodium ion composite solid electrolyte is 0.5%-5.5%, and more preferably not more than 2.5%. 3-x PS 4-x Cl x When the proportion of sodium ion composite solid electrolyte is too high or too low, it is not conducive to improving the ionic conductivity and capacity retention rate of the solid electrolyte. When it is too high or too low, it will also lead to excessive crystallinity χc (%), which means that the interaction between the polymer electrolyte matrix segments is enhanced, thereby causing the ion conductivity of the electrolyte to decrease.

[0017] According to a preferred embodiment of the present invention, the mass proportion of sodium salt in the sodium ion composite solid electrolyte is 30%-38%.

[0018] In a second aspect, the present invention provides a method for preparing a sodium ion composite solid electrolyte, comprising the following steps:

[0019] S1, adding the polymer electrolyte matrix and the sodium salt into an organic solvent and dispersing them uniformly to obtain a primary dispersion;

[0020] S2. Add Na to the primary dispersion 3-x PS 4-x Cl x The powder particles are fully stirred to obtain a uniform secondary dispersion;

[0021] S3, pouring the secondary dispersion into a mold to cast a film, drying and solidifying it to obtain a sodium ion composite solid electrolyte;

[0022] Among them, S2-S3 are operated under the protection of dry inert atmosphere.

[0023] According to a preferred embodiment of the present invention, in S2, Na 3-x PS 4-x Cl x The powder particles are encapsulated and stored in O 2 <0.1ppm, H 2 O<0.1ppm in a sealed environment; for example, it can be stored in an argon-filled glove box.

[0024] According to a preferred embodiment of the present invention, steps S2-S3 are performed in 2 <0.1ppm, H 2 O < 0.1 ppm; for example, in an argon-filled glove box.

[0025] According to a preferred embodiment of the present invention, the organic solvent in S1 is at least one of acetonitrile (ACN), dimethylformamide (DMF), acetone (Acetone) and tetrahydrofuran (THF); preferably acetonitrile, which has a low boiling point, is easy to dry and recover, has appropriate polarity, and has good dispersibility in polymer electrolyte matrices (organic matter) and sodium salts (inorganic matter).

[0026] According to a preferred embodiment of the present invention, in S1, the polymer electrolyte matrix and the sodium salt are first vacuum dried to reduce moisture before use, and the vacuum drying is performed in a vacuum drying oven at a temperature of 50-120° C. for 8-24 hours.

[0027] According to a preferred embodiment of the present invention, in S3, the drying and curing is performed in a vacuum drying oven at a temperature of 50-120° C. for 8-24 hours to completely evaporate the organic solvent.

[0028] In a third aspect, the present invention also provides a sodium ion all-solid-state battery, which comprises a positive electrode, a negative electrode and the above-mentioned sodium ion composite solid electrolyte.

[0029] According to a preferred embodiment of the present invention, the negative electrode is a sodium sheet. According to a preferred embodiment of the present invention, the positive electrode active material used in the positive electrode is O 3 -Na[Ni 1 / 3 Fe 1 / 3 Mn 1 / 3 ]O 2 , O 3 -Na 0.9 [Cu 0.22 Fe 0.3 Mn 0.48 ]O 2 and O 3 -Na[Ni 0.5 Fe 0.5 ]O 2 At least one of .

[0030] (III) Beneficial effects

[0031] The technical effects of the present invention are:

[0032] 1. Reduce the interface impedance and improve the contact effect with the electrode: through Na 3-x PS 4-x Cl x(0<x≤2.0) The reaction between the surface groups and the polymer electrolyte matrix (such as PEO) chain segments reduces the amorphous transition temperature of the polymer electrolyte, thereby improving the flexibility of the polymer chain segments; the improvement in the flexibility of the solid electrolyte material makes the contact between the solid electrolyte and the sodium metal electrode interface closer, and the solid electrolyte surface can be embedded in the pore structure of the electrode surface, which helps to reduce the interface resistance and improve the battery capacity retention rate.

[0033] 2. Improve the ionic conductivity of solid electrolytes: through Na 3-x PS 4-x Cl x (0<x≤2.0) The surface groups serve as cross-linking points between the polymer electrolyte matrix (such as PEO) chain segments and anions, changing the structure of the polymer chain segments at the interface and providing more channels for sodium ion transmission; this helps to improve the ionic conductivity of the solid electrolyte, thereby accelerating the charge and discharge speed of the battery and improving the charge and discharge efficiency.

[0034] 3. Broaden the electrochemical window: Compared with pure polymer electrolyte matrix (such as PEO), PEO-Na 3-x PS 4-x Cl x (0<x≤2.0) The composite electrolyte has a higher oxidation potential, which means it is compatible with more high-voltage electrode materials. The broadening of the electrochemical window provides a basis for achieving high energy density batteries.

[0035] 4. Inhibit the interfacial reaction and dendrite growth between the solid electrolyte and the metallic sodium negative electrode: The addition of sulfide electrolyte not only improves the sodium ion conductivity of the polymer electrolyte, but also enhances the interfacial stability. This stability helps to inhibit the interfacial reaction and dendrite growth that may occur during the charge and discharge process of the sodium metal, thereby extending the cycle life and safety of the battery.

[0036] In summary, the present invention dopes a small amount of Na into the polymer solid electrolyte. 3-x PS 4-x Cl x (0<x≤2.0), successfully prepared a composite solid polymer electrolyte with high ionic conductivity, excellent interface stability and a wide electrochemical window, promoted the application of metallic sodium electrodes in all-solid-state batteries, and provided strong technical support for the development of solid-state batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 The EIS impedance spectra of the composite solid electrolytes of Examples 1 and 3 and Comparative Examples 1 and 3-4 are shown. DETAILED DESCRIPTION

[0038] In order to better explain the present invention and facilitate understanding, the present invention is described in detail below through specific implementation modes in conjunction with the accompanying drawings.

[0039] Example 1

[0040] This embodiment provides a method for preparing a sodium ion composite solid electrolyte, the steps are as follows:

[0041] (1) PEO and NaTFSI were dried in a vacuum oven at 60°C for 12 h. In an argon-filled glove box, PEO "EO" (ethoxy) and NaTFSI were added to acetonitrile (ACN) solvent in a molar ratio of 1:18, and stirred until completely dissolved to obtain a primary dispersion.

[0042] (2) In an argon-filled glove box, add Na 2.9 PS 3.9 Cl 0.1 The powder is fully stirred to obtain a uniform secondary dispersion.

[0043] (3) In an argon-filled glove box, the secondary dispersion was poured into a polytetrafluoroethylene mold to cast a film, and dried in a vacuum drying oven at 60°C for 18 hours to completely evaporate the acetonitrile (for recycling), thereby finally producing a composite polymer electrolyte membrane. 2 <0.1ppm, H 2 O<0.1ppm. In the composite polymer electrolyte membrane, Na 2.9 PS 3.9 Cl 0.1 The powder accounts for 1.5 wt% of the total mass of the composite polymer electrolyte membrane.

[0044] Example 2

[0045] The preparation method of the sodium ion composite solid electrolyte in this embodiment is the same as that in embodiment 1, except that Na 2.9 PS 3.9 Cl 0.1 The amount of powder used is Na 2.9 PS 3.9 Cl 0.1 The powder accounts for 0.5 wt% of the total mass of the composite polymer electrolyte membrane.

[0046] Example 3

[0047] The preparation method of the sodium ion composite solid electrolyte in this embodiment is the same as that in embodiment 1, except that Na 2.9 PS 3.9 Cl 0.1 The amount of powder used is to make Na 2.9 PS3.9 Cl 0.1 The powder accounts for 2.5 wt% of the total mass of the composite polymer electrolyte membrane.

[0048] Example 4

[0049] The preparation method of the sodium ion composite solid electrolyte in this embodiment is the same as that in embodiment 1, except that Na 2.9 PS 3.9 Cl 0.1 The amount of powder used is to make Na 2.9 PS 3.9 Cl 0.1 The powder accounts for 5.5 wt% of the total mass of the composite polymer electrolyte membrane.

[0050] Example 5

[0051] The preparation method of the sodium ion composite solid electrolyte in this embodiment is the same as that in embodiment 1, except that the Na 2.9 PS 3.9 Cl 0.1 Powder replaced with Na 2.7 PS 3.7 Cl 0.3 Powder, Na 2.7 PS 3.7 Cl 0.3 The powder accounts for 1.5 wt % in the composite polymer electrolyte membrane.

[0052] Comparative Example 1

[0053] This comparative example provides a method for preparing a sodium ion composite solid electrolyte, the steps are as follows:

[0054] (1) PEO and NaTFSI were dried in a vacuum oven at 60°C for 12 h. In an argon-filled glove box, PEO "EO" (ethoxy) and NaTFSI were added to acetonitrile (ACN) solvent in a molar ratio of 1:18, and stirred until completely dissolved to obtain a primary dispersion.

[0055] (2) In an argon-filled glove box, the primary dispersion was poured into a polytetrafluoroethylene mold to cast a film, and then dried in a vacuum drying oven at 60°C for 18 hours to completely evaporate the acetonitrile to obtain a polymer electrolyte membrane. The polymer electrolyte membrane does not contain Na 2.9 PS 3.9 Cl 0.1 powder.

[0056] Comparative Example 2

[0057] This comparative example is based on Example 1, which greatly reduces Na 2.9 PS3.9 Cl 0.1 The amount of powder used is to make Na 2.9 PS 3.9 Cl 0.1 The powder accounts for 0.1 wt % in the composite polymer electrolyte membrane.

[0058] Comparative Example 3

[0059] This comparative example is based on Example 1, and Na 2.9 PS 3.9 Cl 0.1 The amount of powder used is to make Na 2.9 PS 3.9 Cl 0.1 The powder accounts for 11 wt % in the composite polymer electrolyte membrane.

[0060] Comparative Example 4

[0061] This comparative example is based on Example 1, and the Na 2.9 PS 3.9 Cl 0.1 Powder replaced with Na 3 PS 4 Powder, Na 3 PS 4 The powder accounts for 1.5 wt % in the composite polymer electrolyte membrane.

[0062] Comparative Example 5

[0063] This comparative example is based on Example 1, and the Na 2.9 PS 3.9 Cl 0.1 Powder replaced with Na 3 Sb 4 Powder, Na 3 Sb 4 The powder accounts for 1.5 wt % in the composite polymer electrolyte membrane.

[0064] Comparative Example 6

[0065] This comparative example is based on Example 1, and the Na 2.9 PS 3.9 Cl 0.1 Powder replaced with Na 3 PsE 4 Powder, Na 3 PsE 4 The powder accounts for 1.5 wt % in the composite polymer electrolyte membrane.

[0066] Electrochemical performance test

[0067] 1. Test items

[0068] (1) Electrochemical impedance spectroscopy (EIS): By testing the AC impedance spectrum of the sodium ion blocking electrode / solid electrolyte / sodium ion blocking electrode symmetrical battery through EIS, the dynamics of the solid electrolyte corresponding battery can be known. During the test, the frequency range is set to: 1MHz-10mHz, and the amplitude is set to 10mV. The impedance diagram of the electrolyte is obtained, and the ionic conductivity of the electrolyte at 80℃ is calculated.

[0069] (2) Crystallinity χc (%) detection: Differential scanning calorimetry is mainly used to measure the specific heat capacity and melting enthalpy parameters of the sample and then calculate the crystallinity of the electrolyte. The prepared polymer solid electrolyte was analyzed by differential scanning calorimetry (DSC) using a differential thermal analyzer. The test temperature range was -60 to 80 °C, and the heating rate was 10 °C / min.

[0070] (3) Battery assembly and battery performance testing:

[0071] ①Battery assembly method: In a glove box, 3- Na[Ni 1 / 3 Fe 1 / 3 Mn 1 / 3 ]O 2 , conductive carbon black and PVDF were weighed and mixed in a mass ratio of 8:1:1 to prepare the raw material mixed powder for the positive electrode sheet. N-methylpyrrolidone (NMP) was added to the mixed powder and stirred evenly for 10 hours to obtain the positive electrode slurry, which was coated on a smooth aluminum foil current collector (the loading amount of the positive electrode material was 2.8 mg / cm 2 ), and then placed in a vacuum drying oven at 80°C for 12 hours to completely dry the NMP solvent to obtain the prepared positive electrode plate. The positive electrode material / polymer electrolyte / Na battery is assembled in a glove box filled with argon. The positive electrode plate (14 mm) prepared above is the positive electrode, and the sodium sheet (15.6 mm) is used as the negative electrode. The polymer electrolyte membrane (thickness of 19 mm) prepared in the above embodiments and comparative examples is sandwiched between the positive electrode plate and the metallic sodium to form a sandwich structure, and the sandwich structure is sealed in a CR2032 button battery shell by a sealing machine.

[0072] ②Test conditions: Cycle life test at 60°C, working voltage range 2.0-4.0V. Battery charge and discharge test at a rate of 0.2C (1C = 130mA / g).

[0073] 2. Test results

[0074] The EIS impedance spectra of Examples 1 and 3 and Comparative Examples 1 and 3-4 obtained by electrochemical impedance spectroscopy (EIS) were combined into one figure, as shown in FIG. Figure 1 As shown in the figure, the EIS impedance of the solid electrolyte is in the following order: Comparative Example 1>Comparative Example 3>Comparative Example 4>Example 3>Example 1.

[0075] The crystallinity χc (%), ionic conductivity and battery capacity retention rate of the solid electrolytes prepared in each embodiment and comparative example and assembled into CR2032 button batteries are shown in Table 1.

[0076] Table 1: Crystallinity χc (%), ionic conductivity and battery capacity retention of composite solid electrolytes

[0077]

[0078]

[0079] As can be seen from Table 1, the crystallinity x of Example 1 c The lowest is only 32.3%. Low crystallinity means that the interaction between PEO segments is weakened, thereby enhancing the ion conductivity of the solid electrolyte. This is due to the Na 2.9 PS 3.9 Cl 0.1 The surface groups can serve as crosslinking points between PEO segments and anions, changing the structure of polymer segments at the interface and increasing the channels for sodium ion transmission, which reduces the possibility of ion pair formation. This effect increases the number of free ions and thus improves the sodium ion conductivity of the polymer electrolyte.

[0080] At 80°C, the sodium ion conductivity of Example 1 is 10.05×10 -4 S / cm, while the sodium ion conductivity of Comparative Example 1 is only 4.02×10 -4 S / cm, which means Na 2.9 PS 3.9 Cl 0.1 The addition of can improve the sodium ion conductivity of the polymer electrolyte. It can also be seen from Example 1 and Examples 3-4 in Table 1 that Na 2.9 PS 3.9 Cl 0.1 The sodium ion conductivity of the solid electrolyte is the highest when the proportion of Na in the solid electrolyte is 1.5wt%. 2.9 PS 3.9 Cl 0.1 As the proportion of solid electrolytes increases, the ionic conductivity of electrolytes decreases. This is because Na 2.9 PS 3.9 Cl 0.1After the ratio increases, it is not completely dispersed in the polymer electrolyte, resulting in particle agglomeration. In addition, it can be seen from Example 1 and Example 2 in Table 1 that as the Na 2.9 PS 3.9 Cl 0.1 The proportion of solid electrolytes decreases, and the ionic conductivity of electrolytes also decreases. This is mainly due to the decrease of Na 2.9 PS 3.9 Cl 0.1 The ratio is too low, and the weakening effect on the interaction between PEO segments is insufficient. It can be seen from Example 1 and Example 5 in Table 1 that when Na 3-x PS 4-x Cl x When x=0.1 or 0.3, the solid electrolyte can be modified well, but the modification effect of x=0.3 is not as good as that of x=0.1.

[0081] Since the PEO / NaTFSI electrolyte is reduced during charging, a relatively rough and loose solid electrolyte interface (SEI) is generated on the surface of the sodium metal, resulting in continuous side reactions between PEO / NaTFSI and the sodium metal electrode, which is the reason why the cycle stability of Comparative Example 1 is the worst. The good cycle stability of Example 1 depends on the formation of a smooth and dense SEI film on the surface of the metal sodium electrode.

[0082] It can be seen from Example 1 and Comparative Examples 1-3 in Table 1 that when Na 2.9 PS 3.9 Cl 0.1 When the addition amount of is reduced to 0.1wt% or even 0 or increased to 11wt%, the sodium ion conductivity of the solid electrolyte is significantly reduced, which is much smaller than that of Examples 1-5. As can be seen from Examples 1 and 5 and Comparative Examples 4-6 in Table 1, Na 3-x PS 4-x Cl x Through the unique lattice structure and cross-linking point effect, the sodium ion diffusion rate and cycle stability of the solid electrolyte are improved, and the improvement effect is better than other sulfides (Na 3 PS 4 , Na 3 Sb 4 ) or similar (Na 3 PsE 4 ).

[0083] Combining Table 1 and Figure 1(Sodium metal symmetric battery AC impedance diagram) It can be seen that the cycle life of the all-solid-state battery is greatly affected by the overall impedance of the battery, and the overall impedance is closely related to the interface resistance of the sodium metal / electrolyte. The interface compatibility of pure PEO-based polymer electrolytes and sodium metal electrodes is poor. By infiltrating appropriate inorganic particles into the polymer electrolyte, the amorphous transition temperature of the polymer electrolyte is reduced, the flexibility of the solid electrolyte material is improved, and the contact tightness of the interface between the solid electrolyte and the sodium metal electrode is improved; the inorganic material also effectively improves the interface compatibility between the electrolyte and the sodium electrode. Therefore, the addition of sulfide electrolyte improves the sodium ion conductivity and interface stability of the polymer electrolyte, thereby inhibiting the interface reaction and dendrite growth of metallic sodium to a certain extent.

[0084] The present invention adopts solution casting method to form Na 3-x PS 4-x Cl x (0<x≤2.0) was added as a filler into the polymer electrolyte matrix to prepare a composite electrolyte with a sulfide electrolyte and a polymer electrolyte. The sulfide electrolyte contains sodium ions and is a sodium supplement as well as a dopant. Compared with traditional polymer solid electrolyte membranes, this composite polymer electrolyte exhibits significant advantages, including higher sodium ion conductivity, more stable interface, and lower impedance. In practical applications, all-solid-state batteries assembled with this solid electrolyte exhibit excellent cycle stability. The fundamental reason is the synergistic effect between sulfide and polymer electrolyte, which quickly forms an electrochemically stable SEI film on the surface of the sodium electrode. Na 3-x PS 4-x Cl x (0<x≤2.0) As a sulfide electrolyte with excellent ionic conductivity, the composite with the polymer matrix not only achieves high ionic conductivity, but also ensures good mechanical strength and superior interface stability.

[0085] The present invention essentially provides a composite polymer electrolyte that integrates the advantages of sulfide electrolytes and polymer electrolytes, and is expected to provide strong technical support for the further development of sodium ion batteries. Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit them; although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in this field should understand that they can still modify the technical solutions recorded in the above embodiments, or replace some or all of the technical features therein; and these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A sodium ion composite solid electrolyte, characterized in that: It comprises a polymer electrolyte matrix; sodium salt and sulfide electrolyte Na uniformly dispersed in the matrix 3-x PS 4-x Cl x Powder particles, wherein 0<x≤2.0; wherein the mass proportion of sodium salt in the sodium ion composite solid electrolyte is 10%-40%, Na 3-x PS 4-x Cl x The mass proportion in the sodium ion composite solid electrolyte is 0.5%-10%, and the remainder is the polymer electrolyte matrix.

2. The sodium ion composite solid electrolyte according to claim 1, characterized in that The polymer electrolyte matrix is ​​at least one of PEO, PEC, PPC and PAN, and its weight average molecular weight is 10 5 -10 6 order of magnitude.

3. The sodium ion composite solid electrolyte according to claim 1, characterized in that The sodium salt is at least one of sodium bis(trifluoromethylsulfonyl)imide, sodium bis(fluorosulfonyl)imide, sodium perchlorate and sodium hexafluorophosphate.

4. The sodium ion composite solid electrolyte according to claim 1, characterized in that Na 3-x PS 4-x Cl x The mass share in the sodium ion composite solid electrolyte is 0.5%-5.5%.

5. The sodium ion composite solid electrolyte according to claim 1, characterized in that: The mass proportion of sodium salt in the sodium ion composite solid electrolyte is 30%-38%.

6. A method for preparing the sodium ion composite solid electrolyte according to any one of claims 1 to 5, characterized in that: It includes the following steps: S1, adding the polymer electrolyte matrix and the sodium salt into an organic solvent and dispersing them uniformly to obtain a primary dispersion; S2. Add Na to the primary dispersion 3-x PS 4-x Cl x The powder particles are fully stirred to obtain a uniform secondary dispersion; S3, pouring the secondary dispersion into a mold to cast a film, drying and solidifying it to obtain a sodium ion composite solid electrolyte; Among them, S2-S3 are operated under the protection of dry inert atmosphere.

7. The preparation method according to claim 6, characterized in that: In S2, Na 3-x PS 4-x Cl x The powder particles are packaged and stored in a sealed environment with O2<0.1ppm, H2O<0.1ppm.

8. The preparation method according to claim 6, characterized in that: The S2-S3 steps were operated under the conditions of O2<0.1ppm and H2O<0.1ppm.

9. The preparation method according to claim 6, characterized in that: The organic solvent in S1 is at least one of acetonitrile, dimethylformamide, acetone and tetrahydrofuran.

10. The preparation method according to claim 6, characterized in that: In S1, the polymer electrolyte matrix and sodium salt are first vacuum dried to reduce moisture before use, and the vacuum drying is performed in a vacuum drying oven at a temperature of 50-120° C. for 8-24 hours; in S3, the drying and curing is performed in a vacuum drying oven at a temperature of 50-120° C. for 8-24 hours to completely evaporate the organic solvent.

Citation Information

Cited By

  • Polymer solid electrolyte and solid sodium battery based on polymer solid electrolyte

    CN119601766A

  • Sodium ion composite solid electrolyte, preparation method thereof and sodium solid-state battery

    CN120453474A