Ion liquid crystal interface modified solid-state battery and preparation method thereof

By using imidazole-quaternary ammonium salt composite ion liquid crystal as a buffer layer in solid-state batteries, the problem of poor battery cycle performance under low temperature conditions is solved, and more efficient ion transmission and better battery adaptability are achieved.

CN118919835APending Publication Date: 2024-11-08CHAOWEI POWER GROUP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410997638.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The solid-state battery has a large interface impedance and large interface stress of solid-state electrolytes and electrodes under low temperature conditions, resulting in poor battery circulation performance. In the prior art, the design cost of solid-state electrolytes and electrode interface modifications is high and the application range is limited.

Method used

Using ionic liquid crystal as buffer layer material, the imidazole halogen, quaternary ammonium salt containing diallyl chains and additives are prepared to form an ionic liquid crystal buffer layer with flexibility and conductivity, and placed between the solid electrolyte and the electrode. , use its self-assembly to form an efficient ion transport channel to reduce interface impedance.

Benefits of technology

Under low temperature conditions, the ionic liquid crystals maintain a good sorting state, improving the circulation performance of solid-state batteries, reducing interface impedance, enhancing the environmental adaptability of the battery, and reducing the battery's energy density and reducing the risk.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919835A_ABST
    Figure CN118919835A_ABST
Patent Text Reader

Abstract

The invention relates to an ion liquid crystal interface modified solid-state battery and a preparation method thereof, belongs to the technical field of solid-state batteries, and solves the problem of poor battery cycle performance caused by large interface impedance and large interface stress of a solid electrolyte and an electrode of an existing solid-state battery under a low-temperature condition. The solid-state battery comprises a positive electrode, a solid-state electrolyte and a negative electrode which are sequentially stacked, a buffer layer is arranged between the positive electrode and the solid-state electrolyte or / and between the negative electrode and the solid-state electrolyte, and the buffer layer is made of ionic liquid crystals. The flexibility, orderliness and conductivity of the ion liquid crystal are utilized, an ion buffer layer is formed between the solid electrolyte and the electrode material, the compatibility of the solid electrolyte and the electrode material is improved, and the interface resistance is reduced; and moreover, the ion liquid crystals still present a good sequencing state under a low-temperature condition, so that a good migration channel is provided for ion transmission, and the cycle performance of the solid-state battery under the low-temperature state is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of solid-state batteries, and in particular to an ionic liquid crystal interface modified solid-state battery and a preparation method thereof. Background Art

[0002] At present, traditional lithium-ion batteries still use flammable and explosive organic electrolytes, which bring a series of safety hazards. In recent years, researchers have proposed using solid electrolytes as electrolytes for lithium-ion batteries. Compared with traditional organic electrolytes, solid electrolytes have higher safety and energy density.

[0003] Although solid electrolytes have been studied and developed to a certain extent, there are still some challenges. For example, the ionic conductivity of solid electrolytes is poor, usually below 10 -4 -10 -6 S / cm; the interface between the solid electrolyte and the electrode is unstable, and the defects therein increase the ion migration impedance, weakening the high energy density advantage of the solid electrolyte battery. Therefore, it is very important to modify the interface between the solid electrolyte and the electrode to reduce the defects therein.

[0004] At present, the use of conductive polymers with good flexibility for filling or modification is a common method. To a certain extent, it improves the compatibility between the solid electrolyte and the electrode and reduces the interface impedance. However, it also has shortcomings. Especially at low temperatures, the conductive polymer will be affected by the freezing effect, resulting in reduced flexibility and conductivity, thereby increasing the impedance between the solid electrolyte and the electrode. In addition, in the prior art, the interface modification between the solid electrolyte and the electrode is mainly designed for a specific solid-state battery, which has high design costs and limited application scope.

[0005] In view of the common interface problems between solid electrolytes and electrode materials, there is an urgent need for a universal new material to modify the interface between solid electrolytes and electrode materials. This new material not only has flexibility and conductivity, but also plays a role in improving the compatibility between the two and reducing interface resistance; and under low temperature conditions, it can overcome the problem of increased interface impedance between solid electrolytes and electrodes, which leads to poor battery cycle performance, so as to improve the adaptability of solid-state batteries to the environment. Summary of the invention

[0006] In view of the above analysis, the embodiments of the present invention aim to provide a solid-state battery modified with an ionic liquid crystal interface and a preparation method thereof, so as to solve at least one of the problems of existing solid-state batteries, namely, large interface impedance and large interface stress between solid electrolyte and electrode under low temperature conditions, resulting in poor battery cycle performance.

[0007] In a first aspect, an embodiment of the present invention provides a solid-state battery, comprising a positive electrode, a solid electrolyte and a negative electrode stacked in sequence, a buffer layer is provided between the positive electrode and the solid electrolyte or / and between the negative electrode and the solid electrolyte, and the material constituting the buffer layer is ionic liquid crystal.

[0008] Furthermore, the conductivity of the ionic liquid crystal is 10 -7 -10 -3 S / cm, viscosity is 10 -2 -10 3 Pa·s.

[0009] And / or, the elastic modulus of the ionic liquid crystal is 0.01-1000 MPa.

[0010] Furthermore, the melting point of the ionic liquid crystal is (-50)-10°C, and the clearing point is 40-200°C.

[0011] Furthermore, the thickness of the buffer layer is 1%-20% of the thickness of the positive electrode material or the negative electrode material of the solid-state battery.

[0012] Furthermore, the ionic liquid crystal is prepared from imidazole halides, quaternary ammonium salts containing bisallyl chains and additives.

[0013] Furthermore, the imidazole halide is selected from one or more of 1-methyl-3-decyl imidazole halide, 1-ethyl-3-methyl imidazole halide, 1-butyl-3-methyl imidazole halide, and 1-octyl-3-methyl imidazole halide.

[0014] Furthermore, the quaternary ammonium salt containing a diallyl chain is one or more of dimethyldiallylammonium chloride, diethyldiallylammonium chloride, and allyldimethylalkylammonium bromide.

[0015] Furthermore, the additive is a hydrogen bond donor or a hydrogen bond acceptor.

[0016] Furthermore, the molar ratio of the imidazole halide, the quaternary ammonium salt and the additive is 1:0.001-1000:10-1000.

[0017] In a first aspect, an embodiment of the present invention provides a method for preparing the solid-state battery described in the first aspect, the method comprising: placing the ionic liquid crystal between the solid electrolyte and the positive electrode or / and negative electrode material, and cold pressing;

[0018] Preferably, the cold pressing temperature is (-200)-(15)°C, the pressure is 10-100 KPa, and the time is 30s-30min.

[0019] Compared with the prior art, the present invention can achieve at least one of the following beneficial effects:

[0020] 1. The present invention provides an ionic liquid crystal buffer layer between the electrolyte and the electrode of the solid-state battery to solve the problems of unstable interface and high impedance between the solid-state electrolyte and the electrode in the prior art. The flexibility, orderliness and conductivity of the ionic liquid crystal are utilized to form an ionic buffer layer between the solid-state electrolyte and the electrode material, thereby improving the compatibility between the two and reducing the interface impedance. Moreover, under low temperature conditions, the ionic liquid crystal can still present a good sorting state, providing a good migration channel for ion transport, thereby improving the cycle performance of the solid-state battery under low temperature conditions.

[0021] 2. The ionic liquid crystal material of the present invention forms an effective ion transmission channel through self-assembly. Under the action of the electric field, ions can pass smoothly, forming an efficient ion channel at the interface between the solid electrolyte and the electrode, reducing the interface impedance, thereby improving the ion transmission rate. The conductivity of the ionic liquid crystal of the present invention is 10 -7 -10 -3 S / cm, viscosity is 10 -2 -10 3 Pa·s, elastic modulus is 0.01-1000MPa.

[0022] 3. The melting point and clearing point of the ionic liquid crystal of the present invention determine the phase state of the ionic liquid crystal at different temperatures, and ultimately determine the operating temperature of the solid-state battery using the ionic liquid crystal buffer layer. In order to make the solid-state battery adapt to the actual complex and changeable ambient temperature, the melting point of the ionic liquid crystal of the present invention is (-50)-10°C, and the clearing point is 40-200°C.

[0023] 4. On the one hand, the present invention enables ionic liquid crystal to buffer the strain defects between the electrode material and the electrolyte, thereby improving the electrochemical cycle performance of the battery under low temperature conditions; on the other hand, in order to prevent the reduction of the energy density of the solid-state battery, the present invention sets the thickness of the buffer layer to 1%-20% of the thickness of the solid-state positive electrode material or negative electrode material.

[0024] 5. The present invention preferably adopts imidazole-quaternary ammonium salt composite ionic liquid crystal. This type of ionic liquid crystal not only has the planarity and rigidity of imidazole ring, but also because of the ionic property of quaternary ammonium salt, it shows good compatibility and stability. The introduction of bisallyl chain increases the flexibility and adjustability of the molecule, helps to form various liquid crystal phases, such as nematic phase, smectic phase, etc.; Therefore, effective ion transmission channels are formed inside the imidazole-quaternary ammonium salt composite ionic liquid crystal material of the present invention, and ions can pass smoothly under the action of electric field, thereby forming efficient ion channels at the interface between solid electrolyte and electrode, reducing interface impedance, thereby improving ion transmission rate.

[0025] 6. The present invention adopts cold pressing to place ionic liquid crystal between the positive electrode and the solid electrolyte or / and between the negative electrode and the solid electrolyte, so as to improve the binding force between the ionic liquid crystal and the electrode and the solid electrolyte, realize the uniformity and densification of the interface bonding, maximize the interface modification effect of the buffer layer, reduce the interface impedance, and improve the battery cycle performance.

[0026] In the present invention, the above-mentioned technical solutions can also be combined with each other to achieve more preferred combination solutions. Other features and advantages of the present invention will be described in the subsequent description, and some advantages can become obvious from the description, or can be understood by practicing the present invention. The purpose and other advantages of the present invention can be realized and obtained through the contents particularly pointed out in the description and the drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] The drawings are only for the purpose of illustrating particular embodiments and are not to be considered limiting of the present invention. Like reference symbols denote like components throughout the drawings.

[0028] Figure 1 (1) is a schematic diagram of the interface state and ion migration of the solid electrolyte and electrode of the solid-state battery 1 prepared in Example 1 of the present invention; (2) is a schematic diagram of the interface state and ion migration of the solid electrolyte and electrode of the solid-state battery 7 prepared in Comparative Example 1;

[0029] Figure 2 Electrochemical impedance diagrams of solid-state batteries prepared in Examples 1-4 and Comparative Example 1 of the present invention;

[0030] Figure 3 The electrochemical cycle performance diagram of the solid-state batteries prepared in Examples 1-4 of the present invention and Comparative Examples 1 and 2;

[0031] Reference numerals:

[0032] 1-electrode; 2-solid electrolyte; 3-buffer layer. DETAILED DESCRIPTION

[0033] The preferred embodiments of the present invention will be described in detail below in conjunction with the accompanying drawings, wherein the accompanying drawings constitute a part of the present invention and are used together with the embodiments of the present invention to illustrate the principles of the present invention, but are not used to limit the scope of the present invention.

[0034] Although solid electrolytes have been studied and developed to a certain extent, there are still some challenges. For example, the interface between the solid electrolyte and the electrode is unstable. The defects in it increase the ion migration impedance, which weakens the high energy density advantage of the solid electrolyte battery. Therefore, it is very important to modify the interface between the solid electrolyte and the electrode to reduce the defects in it.

[0035] At present, the use of conductive polymers with good flexibility for filling or modification is a common method. To a certain extent, it improves the compatibility between the solid electrolyte and the electrode and reduces the interface impedance. However, it also has shortcomings. Especially at low temperatures, the conductive polymer will be affected by the freezing effect, resulting in reduced flexibility and conductivity, thereby increasing the impedance between the solid electrolyte and the electrode. In addition, in the prior art, the interface modification between the solid electrolyte and the electrode is mainly designed for a specific solid-state battery, which has high design costs and limited application scope.

[0036] Therefore, the present invention discloses a solid-state battery, which comprises a positive electrode, a solid electrolyte and a negative electrode stacked in sequence, wherein a buffer layer is provided between the positive electrode and the solid electrolyte or / and between the negative electrode and the solid electrolyte, and the material constituting the buffer layer is ionic liquid crystal.

[0037] Ionic liquid crystal (ILC) is a material with self-assembly ability, high stability and fluidity. It is a new type of liquid crystal material formed by the combination of ionic liquid and liquid crystal. It has the fluidity of liquid and the anisotropy of crystal. In addition to the general characteristics of liquid crystal, ionic liquid crystal also has unique properties due to its ionic characteristics. For example, ionic liquid crystal has good conductivity and can change its phase or properties under the action of electric or magnetic fields. In addition, the liquid crystal phase of ionic liquid crystal is also more diverse, including smectic phase, nematic phase, columnar phase and even three-dimensional cubic phase. The properties of ionic liquid crystal are stable over a wide temperature range, and the design of ionic liquid crystal is flexible and changeable. Liquid crystal molecules can be self-assembled and designed according to specific situations and needs. The mobile phase and conductivity of ionic liquid crystal are conducive to the transmission of ions, and the unique ordered self-assembly structure can provide an efficient ion transmission path, which is expected to greatly improve ionic conductivity.

[0038] The present invention provides an ionic liquid crystal buffer layer between the electrolyte and the electrode of the solid-state battery to solve the problems of unstable interface and high impedance between the solid-state electrolyte and the electrode in the prior art. The flexibility, orderliness and conductivity of the ionic liquid crystal are utilized to form an ionic buffer layer between the solid-state electrolyte and the electrode material, thereby improving the compatibility between the two and reducing the interface resistance. Moreover, under low temperature conditions, the ionic liquid crystal still presents a good sorting state, providing a good migration channel for ion transmission, thereby improving the cycle performance of the solid-state battery under low temperature conditions.

[0039] It should be noted that the solid-state battery of the present invention is a conventional solid-state battery in the prior art, and the electrodes and solid electrolyte in the solid-state battery are also conventional; according to a preferred embodiment of the present invention, the positive electrode in the solid-state battery adopts lithium iron phosphate, the negative electrode adopts metallic lithium, and the solid electrolyte is lithium bis(trifluoromethanesulfonyl)imide filled with polyethylene oxide.

[0040] It should be noted that the ionic liquid crystal used as a buffer layer in the present invention does not react with electrodes or electrolytes.

[0041] It should be noted that in order to ensure the ionic conductivity between the solid electrolyte and the electrodes, the present invention limits the conductivity of the ionic liquid crystal.

[0042] Specifically, the conductivity of the ionic liquid crystal of the present invention is 10 -7 -10 -3 S / cm, viscosity is 10 -2 -10 3 Pa·s; The viscosity of ionic liquid crystals will directly affect the mobility of ions therein. In ionic liquid crystals, the conduction of ions is achieved by jumping or diffusing between molecules or in the channels formed. Ionic liquid crystals with higher viscosity have greater internal friction between molecules, which will hinder the migration of ions, thereby reducing the mobility of ions and affecting the conductivity of ionic liquid crystals.

[0043] It should be noted that in order to buffer the structural strain of the positive electrode material or the negative electrode material during the cycle within a certain range and fill the gap defects between the positive electrode material or the negative electrode material and the electrolyte caused by stress, the ionic liquid crystal buffer layer needs to have a certain flexibility.

[0044] Specifically, the elastic modulus of the ionic liquid crystal of the present invention is 0.01-1000MPa. If the elastic modulus of the ionic liquid crystal is too large, the ionic liquid crystal responds very slowly to the strain defects between the positive electrode material or the negative electrode material and the electrolyte and cannot play a buffering role; if the elastic modulus of the ionic liquid crystal is too small, it is easy to produce stress concentration locally when subjected to external force, which may cause the material to be damaged prematurely in the area, thereby affecting the conductivity of ions in the ionic liquid crystal.

[0045] The melting point and clearing point of ionic liquid crystals are two key temperature parameters that describe their phase transitions. The melting point refers to the temperature at which the liquid crystal changes from a solid state to a liquid crystal state, while the clearing point refers to the temperature at which the liquid crystal changes from a liquid crystal state to a liquid state, i.e., the highest temperature at which the liquid crystal state can exist. These two parameters are very important for the application of ionic liquid crystals because they determine the behavior and stability of the material at a specific temperature.

[0046] It should be noted that in order to make the solid-state battery adapt to the complex and changeable ambient temperature of actual use, the present invention needs to limit the phase transition temperature of the ionic liquid crystal.

[0047] Specifically, the melting point of the ionic liquid crystal of the present invention is (-50)-10°C, and the clearing point is 40-200°C. If the melting point of the ionic liquid crystal is too high, the ionic liquid crystal buffer layer will present a solid phase at the application temperature of the solid-state battery, and will not have the mechanical strength and flexibility of the liquid crystal phase, and the interface stress will increase, resulting in a decrease in the battery conductivity; if the clearing point of the ionic liquid crystal is too low, the ionic liquid crystal buffer layer will easily present a liquid phase at the application temperature of the solid-state battery, and the orderly arrangement structure of the liquid crystal will be lost, becoming a disordered liquid state, affecting the ionic conductivity.

[0048] It should be noted that in order to ensure the energy density of the solid-state battery, the present invention needs to limit the thickness of the buffer layer.

[0049] Specifically, the thickness of the buffer layer of the present invention is 1%-20% of the thickness of the solid positive electrode material or negative electrode material. If the thickness of the buffer layer is too large, the energy density of the solid-state battery will be reduced; if the thickness of the buffer layer is too small, it will not effectively buffer the strain defects between the positive and negative electrode materials and the electrolyte.

[0050] According to a preferred embodiment of the present invention, the ionic liquid crystal preferably adopts imidazole-quaternary ammonium salt composite ionic liquid crystal, which is composited by imidazole halides and quaternary ammonium salts containing bisallyl chains. This type of ionic liquid crystal not only has the planarity and rigidity of imidazole rings, but also because of the ionic properties of quaternary ammonium salts, it shows good compatibility and stability, and the introduction of bisallyl chains increases the flexibility and adjustability of molecules, which helps to form various liquid crystal phases, such as nematic phases, smectic phases, etc.; Therefore, effective ion transmission channels are formed inside the imidazole-quaternary ammonium salt composite ionic liquid crystal material of the present invention, and ions can pass smoothly under the action of an electric field, thereby forming efficient ion channels at the interface between a solid electrolyte and an electrode, reducing interface impedance, thereby improving ion transmission rate.

[0051] It should be noted that the imidazole-quaternary ammonium salt composite ionic liquid crystal of the present invention can be purchased and / or prepared by any existing method.

[0052] According to a preferred embodiment of the present invention, the method for preparing the imidazole-quaternary ammonium salt composite ionic liquid crystal comprises:

[0053] (1) mixing an imidazole halide and a quaternary ammonium salt containing a bisallyl chain at a temperature of 1 and stirring;

[0054] (2) adding a hydrogen bond donor or a hydrogen bond acceptor to the mixed solution obtained in step (1), mixing and stirring at temperature II;

[0055] (3) The system prepared in step (2) is allowed to stand at room temperature (25° C.) for a certain period of time to obtain the ionic liquid crystal.

[0056] Preferably, the imidazole halide in step (1) is one or more of 1-methyl-3-octyl imidazole halide, 1-ethyl-3-methyl imidazole halide, 1-butyl-3-methyl imidazole halide, and 1-octyl-3-methyl imidazole halide.

[0057] More preferably, the imidazole halide is 1-butyl-3-methylimidazolium chloride, 1-ethyl-3-methylimidazolium chloride, 1-methyl-3-n-octylimidazolium chloride, or 1-octyl-3-methylimidazolium chloride.

[0058] Preferably, the quaternary ammonium salt containing a diallyl chain in step (1) is one or more of dimethyldiallylammonium chloride, diethyldiallylammonium chloride, and allyldimethylalkylammonium bromide. Among them, the allyldimethylalkylammonium bromide is at least one of allyldimethylhexadecylammonium bromide and allyldimethyloctadecylammonium bromide.

[0059] In order to make the obtained composite ionic liquid crystal have suitable properties such as ionic conductivity and thermal stability, the molar ratio of the imidazole halide to the quaternary ammonium salt in the present invention is 1:0.001-1000.

[0060] Preferably, the temperature I in step (1) refers to room temperature, which is 15-35°C.

[0061] In the design process of the imidazole-quaternary ammonium salt composite ionic liquid crystal, it is necessary to add hydrogen bond acceptors or donors to regulate the properties of the liquid crystal molecules. The hydrogen bond is achieved through the interaction force between molecules and the orderliness of the molecular arrangement. The stronger the hydrogen bond between liquid crystal molecules, the higher the corresponding melting point and clearing point will be.

[0062] Preferably, the hydrogen bond donor or hydrogen bond acceptor in step (2) can be alcohols, amides, urea, acetamide, water molecules, ethers, carbonyl compounds, carboxylic acids, amines, nitriles, halide ions, etc.; the amount of the hydrogen bond donor or hydrogen bond acceptor added is regulated according to the required melting point or clearing point of the ionic liquid crystal, and the molar ratio of the imidazole halide to the hydrogen bond donor or hydrogen bond acceptor in the present invention is 1:10-1000.

[0063] Preferably, the temperature II in step (2) is 25°C-200°C, preferably 40-80°C.

[0064] Preferably, the certain time in step (3) is 10-24 hours, preferably 12-20 hours.

[0065] The performance parameters of the ionic liquid crystal prepared by the above method will vary depending on the type of imidazole halide selected, the type of quaternary ammonium salt with a bisallyl chain, their molar ratio, and the type and dosage of the hydrogen bond acceptor or donor used. The performance parameters of the ionic liquid crystal prepared, such as conductivity, viscosity, elastic modulus, melting point, clearing point, etc., can be measured by characterization means such as DC conductivity test, rotational rheometer, dynamic mechanical analysis, differential scanning calorimetry, polarizing microscope, etc.

[0066] The present invention also discloses a method for preparing a solid-state battery, the method comprising: adding the ionic liquid crystal between the solid-state electrolyte and the positive electrode or / and negative electrode material, and cold pressing.

[0067] Preferably, the cold pressing temperature is generally lower than the melting point of the liquid crystal material, generally lower than room temperature, and is (-200)-(15)°C, the pressure is 10-100KPa, and the duration is 30s-30min. If the cold pressing temperature is too low, the material may be brittle in the solid state during the cold pressing process, and strain and breakage of the material may occur easily. If the cold pressing temperature is too high, the material may be completely liquid during the cold pressing process and cannot be placed between the electrolyte and the electrode material. If the cold pressing time is too short, the liquid crystal material and the electrode or electrolyte are not tightly combined. If the cold pressing time is too long, the material is continuously subjected to stress, which may cause strain damage to the material.

[0068] At a temperature lower than the melting point of the ionic liquid crystal, the ionic liquid crystal is transformed into a solid state, so that the composite material that is transformed into a solid state at low temperature is fixed between the positive electrode and the solid electrolyte or between the negative electrode and the solid electrolyte by pressure. During the temperature rise process after cold pressing, the composite material gradually returns to the ionic liquid crystal state, and realizes a firm and uniform densification combination with the electrode and the solid electrolyte, respectively, so that the ionic liquid crystal buffer layer plays an interface modification role to the maximum extent, reduces the interface impedance, and improves the battery cycle performance; when the composite material has a solid-liquid crystal mixed state (melting point) or a pure liquid crystal state (greater than the melting point), cold pressing can also enable the ionic liquid crystal to achieve a firm and uniform densification combination with the electrode and the solid electrolyte. Among them, the pressure increase rate per second is 10-50%.

[0069] The positive electrode of the solid-state battery is lithium iron phosphate with a thickness of 100μm; the negative electrode is metallic lithium with a thickness of 10μm; the solid-state electrolyte is polyethylene oxide-filled lithium bis(trifluoromethanesulfonyl)imide with a thickness of 50μm.

[0070] Example 1

[0071] A method for preparing a solid-state battery 1, comprising:

[0072] (1) 0.1 mol of 1-butyl-3-methylimidazolium chloride and 1 mol of a 60% aqueous solution of dimethyldiallylammonium chloride were mixed, and stirred at room temperature (25° C.) and a stirring speed of 500 rpm for 10 min;

[0073] (2) adding 6 mol of urea, 12 mol of acetamide and 2 mol of isopropanol to the mixed solution obtained in step (1) in sequence, stirring at a constant temperature of 60° C. for 20 min to obtain a clear and transparent liquid;

[0074] (3) The clear and transparent liquid obtained in step (2) was allowed to stand at room temperature of 25° C. for 24 h to obtain ionic liquid crystal 1. The conductivity of ionic liquid crystal 1 was measured to be 2.5×10 -5 S / cm, viscosity is 3Pa·s, elastic modulus is 500Mpa, melting point is -25℃, clearing point is 157℃;

[0075] (4) At a temperature of -25°C, the ionic liquid crystal 1 obtained in step (3) is added between the positive electrode and the solid electrolyte and between the negative electrode material and the solid electrolyte, and cold pressed at 100 MPa for 80 seconds to obtain a solid-state battery 1, wherein in the solid-state battery 1, the thickness of the ionic liquid crystal buffer layer is 0.5 μm.

[0076] Example 2

[0077] (1) 0.1 mol of 1-ethyl-3-methylimidazolium chloride and 1 mol of a 60% aqueous solution of dimethyldiallylammonium chloride were mixed, and stirred at room temperature (25° C.) and a stirring speed of 500 rpm for 10 min;

[0078] (2) adding 6 mol of urea, 12 mol of acetamide and 2 mol of isopropanol to the mixed solution obtained in step (1) in sequence, stirring at a constant temperature of 60° C. for 20 min to obtain a clear and transparent liquid;

[0079] (3) The clear and transparent liquid obtained in step (2) was allowed to stand at room temperature of 25° C. for 24 h to obtain ionic liquid crystal 2. The conductivity of ionic liquid crystal 2 was measured to be 8.79×10 -5 S / cm, viscosity is 2.1Pa·s, elastic modulus is 410Mpa, melting point is -15℃, clearing point is 143℃;

[0080] (4) At a temperature of -15°C, the ionic liquid crystal 2 obtained in step (3) is added between the positive electrode and the solid electrolyte and between the negative electrode material and the solid electrolyte, and cold pressed at 100 MPa for 60 seconds to obtain a solid-state battery 2, wherein in the solid-state battery 2, the thickness of the ionic liquid crystal buffer layer is 0.5 μm.

[0081] Example 3

[0082] (1) 0.1 mol of 1-methyl-3-n-octylimidazolium chloride and 1 mol of a 60% aqueous solution of dimethyldiallylammonium chloride were mixed, and stirred at room temperature (25° C.) and a stirring speed of 500 rpm for 10 min;

[0083] (2) adding 6 mol of urea, 12 mol of acetamide and 2 mol of isopropanol to the mixed solution obtained in step (1) in sequence, stirring at a constant temperature of 60° C. for 20 min to obtain a clear and transparent liquid;

[0084] (3) The clear and transparent liquid obtained in step (2) was allowed to stand at room temperature of 25° C. for 24 h to obtain ionic liquid crystal 3. The conductivity of ionic liquid crystal 3 was measured to be 8.93×10 -6 S / cm, viscosity is 4.17Pa·s, elastic modulus is 539Mpa, melting point is -29℃, clearing point is 164℃;

[0085] (4) At a temperature of -29°C, the ionic liquid crystal 3 obtained in step (3) is added between the positive electrode and the solid electrolyte and between the negative electrode material and the solid electrolyte, and cold pressed at 100 MPa for 120 seconds to obtain a solid-state battery 3, wherein in the solid-state battery 3, the thickness of the ionic liquid crystal buffer layer is 0.6 μm.

[0086] Example 4

[0087] (1) 0.1 mol of 1-octyl-3-methylimidazolium chloride and 1 mol of a 60% aqueous solution of dimethyldiallylammonium chloride were mixed, and stirred at room temperature (25° C.) and a stirring speed of 500 rpm for 10 min;

[0088] (2) adding 6 mol of urea, 12 mol of acetamide and 2 mol of isopropanol to the mixed solution obtained in step (1) in sequence, stirring at a constant temperature of 60° C. for 20 min to obtain a clear and transparent liquid;

[0089] (3) The clear and transparent liquid obtained in step (2) was allowed to stand at room temperature of 25° C. for 24 h to obtain ionic liquid crystal 4. The conductivity of ionic liquid crystal 4 was measured to be 7.59×10 -6 S / cm, viscosity is 4.19Pa·s, elastic modulus is 539Mpa, melting point is -34℃, clearing point is 170℃;

[0090] (4) At a temperature of -34°C, the ionic liquid crystal 4 obtained in step (3) is added between the positive electrode and the solid electrolyte and between the negative electrode material and the solid electrolyte, and cold pressed at 100 MPa for 150 seconds to obtain a solid-state battery 4, wherein the thickness of the ionic liquid crystal buffer layer in the solid-state battery 4 is 0.6 μm.

[0091] Example 5

[0092] (1) 0.1 mol of 1-octyl-3-methylimidazolium chloride and 1 mol of a 60% aqueous solution of diethyldiallylammonium chloride were mixed, and stirred at room temperature (25° C.) and a stirring speed of 500 rpm for 10 min;

[0093] (2) adding 6 mol of urea, 12 mol of acetamide and 2 mol of isopropanol to the mixed solution obtained in step (1) in sequence, stirring at a constant temperature of 60° C. for 20 min to obtain a clear and transparent liquid;

[0094] (3) The clear and transparent liquid obtained in step (2) was allowed to stand at room temperature of 25° C. for 24 h to obtain ionic liquid crystal 5. The conductivity of ionic liquid crystal 5 was measured to be 1.27×10 -6 S / cm, viscosity is 5.16Pa·s, elastic modulus is 627Mpa, melting point is -37℃, clearing point is 181℃;

[0095] (4) At a temperature of -37°C, the ionic liquid crystal 5 obtained in step (3) is added between the positive electrode and the solid electrolyte and between the negative electrode material and the solid electrolyte, and cold pressed at 100 MPa for 180 seconds to obtain a solid-state battery 5, wherein the thickness of the ionic liquid crystal buffer layer in the solid-state battery 5 is 0.6 μm.

[0096] Example 6

[0097] (1) 0.1 mol of 1-octyl-3-methylimidazolium chloride and 1 mol of a 60% aqueous solution of allyldimethylhexadecylammonium bromide were mixed, and stirred at room temperature (25° C.) and a stirring speed of 500 rpm for 10 min;

[0098] (2) adding 6 mol of urea, 12 mol of acetamide and 2 mol of isopropanol to the mixed solution obtained in step (1) in sequence, stirring at a constant temperature of 60° C. for 20 min to obtain a clear and transparent liquid;

[0099] (3) The clear and transparent liquid obtained in step (2) was allowed to stand at room temperature of 25° C. for 24 h to obtain ionic liquid crystal 6. The conductivity of ionic liquid crystal 6 was measured to be 8.97×10 -7 S / cm, viscosity is 6.04Pa·s, elastic modulus is 735Mpa, melting point is -41℃, clearing point is 188℃;

[0100] (4) At a temperature of -41°C, the ionic liquid crystal 6 obtained in step (3) is added between the positive electrode and the solid electrolyte and between the negative electrode material and the solid electrolyte, and cold pressed at 100 MPa for 170 seconds to obtain a solid-state battery 6, wherein the thickness of the ionic liquid crystal buffer layer in the solid-state battery 6 is 0.6 μm.

[0101] Comparative Example 1

[0102] The solid-state battery 7 is prepared by the same method as step (4) of Example 1, except that no ionic liquid crystal buffer layer is added between the positive electrode and the solid electrolyte and between the negative electrode material and the solid electrolyte.

[0103] Comparative Example 2

[0104] The solid-state battery 8 is prepared by the same method as step (4) of Example 1, except that a conductive polymer polyaniline is added between the positive electrode and the solid electrolyte and between the negative electrode material and the solid electrolyte, wherein in the solid-state battery 8, the thickness of the ionic liquid crystal buffer layer is 0.6 μm.

[0105] Figure 1 (1) is a schematic diagram of the state of the interface between the solid electrolyte and the electrode of the solid-state battery 7 at low temperature (0°C) and ion migration; because the battery is cycled at low temperature for a period of time, the interface of the material becomes extremely unstable and easily deformed due to the thermal expansion and contraction effect, which causes the ions to choose the same channel for migration during the migration process, resulting in channel congestion, which is manifested as a decrease in ion conductivity; Figure 1 (2) is a schematic diagram of the state of the interface between the solid electrolyte and the electrode of the solid-state battery 1 prepared in Example 1 of the present invention at low temperature and ion migration; since the ionic liquid crystal buffer layer is in a liquid crystal state at low temperature and has good mechanical properties, it can provide a stable channel for ion migration, so the choice space for ion migration is large, and it migrates in an orderly manner, thereby reducing the interface impedance.

[0106] At 10°C, the solid-state batteries prepared in Examples 1-6 and Comparative Example 1 were subjected to impedance tests using electrochemical impedance spectroscopy (EIS). The test results are as follows: Figure 2 As shown, from Figure 2 It can be seen that under the same conditions, compared with the impedance of the solid-state battery without a buffer layer (2000 ohms), the presence of an ionic liquid crystal buffer layer between the electrolyte and the electrode reduces the impedance of the solid-state battery to less than 2000 ohms, and the impedance values ​​of solid-state batteries 4 and 6 are even lower than 1500 ohms, indicating that the ionic liquid crystal prepared by the present invention enables the solid-state battery to have better ionic conductivity.

[0107] At 10°C, electrochemical cycle tests were performed on the solid-state batteries prepared in Examples 1-6 and Comparative Examples 1 and 2. The test results are as follows: Figure 3 As shown, from Figure 3It can be seen that under the same conditions, after the solid-state battery is cycled and discharged for 50 times, the specific capacity of the solid-state battery using a conductive polymer between the electrolyte and the electrode is reduced from 98mAh / g to 50mAh / g, and the battery specific capacity is reduced by 49%. The solid-state battery using the ionic liquid crystal buffer layer of the present invention has a smaller reduction in battery specific capacity, which is in the range of 15%-35%. Compared with the solid-state battery without a buffer layer, the solid-state battery using the ionic liquid crystal buffer layer of the present invention has a higher battery specific capacity. Therefore, at low temperatures, the ionic liquid crystal prepared by the present invention enables the solid-state battery to have better electrochemical cycle performance.

[0108] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed by the present invention should be covered within the protection scope of the present invention.

Claims

1. A solid-state battery comprising a positive electrode, a solid electrolyte and a negative electrode stacked in sequence, characterized in that: A buffer layer is provided between the positive electrode and the solid electrolyte or / and between the negative electrode and the solid electrolyte, and the material constituting the buffer layer is ionic liquid crystal.

2. The solid-state battery according to claim 1, characterized in that: The conductivity of the ionic liquid crystal is 10 -7 -10 -3 S / cm, viscosity is 10 -2 -10 3 Pa·s; And / or, the elastic modulus of the ionic liquid crystal is 0.01-1000 MPa.

3. The solid-state battery according to claim 1, characterized in that: The melting point of the ionic liquid crystal is (-50)-10°C, and the clearing point is 40-200°C.

4. The solid-state battery according to claim 1, characterized in that: The thickness of the buffer layer is 1%-20% of the thickness of the positive electrode material or the negative electrode material of the solid-state battery.

5. The solid-state battery according to any one of claims 1 to 4, characterized in that: The ionic liquid crystal is prepared from imidazole halides, quaternary ammonium salts containing bisallyl chains and additives.

6. The solid-state battery according to claim 5, characterized in that: The imidazole halide is selected from one or more of 1-methyl-3-decyl imidazole halide, 1-ethyl-3-methyl imidazole halide, 1-butyl-3-methyl imidazole halide, and 1-octyl-3-methyl imidazole halide.

7. The solid-state battery according to claim 5, characterized in that: The quaternary ammonium salt containing a diallyl chain is one or more of dimethyldiallylammonium chloride, diethyldiallylammonium chloride, and allyldimethylalkylammonium bromide.

8. The solid-state battery according to claim 5, characterized in that: The additive is a hydrogen bond donor or a hydrogen bond acceptor.

9. The solid-state battery according to claim 5, characterized in that: The molar ratio of the imidazole halide, the quaternary ammonium salt and the additive is 1:0.001-1000:10-1000.

10. A method for preparing a solid-state battery according to any one of claims 1 to 9, characterized in that: The method comprises: placing the ionic liquid crystal between the solid electrolyte and the positive electrode or / and negative electrode material, and cold pressing; Preferably, the cold pressing temperature is (-200)-(15)°C, the pressure is 10-100 KPa, and the time is 30s-30min.