Electrolyte, lithium ion battery and electric device

By adjusting the ratio of lithium salt to cyclic ester in the lithium-ion battery electrolyte and adding film-forming additives, the problem of poor storage and circulation performance of lithium-ion batteries at high temperatures is solved, and the high-temperature circulation and storage performance of the battery is improved and the power of the battery is achieved. Performance improvement.

CN118919854APending Publication Date: 2024-11-08CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411210336.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2021-07-22
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Lithium-ion batteries have poor storage and circulation performance under high temperature environments. The ratio of lithium salt to cyclic ester in existing electrolytes is too high, resulting in serious positive electrode oxidation and decomposition, affecting the high-temperature circulation and storage performance of the battery.

Method used

By adjusting the relative content of lithium salts and cyclic ester in the electrolyte, the electrolyte has good conductivity, oxidation resistance and viscosity, and adding film-forming additives to the electrolyte, the formulation of the electrolyte is optimized to improve the negative electrode interface film. The conductivity of the cyclic esters is reduced and the oxidative decomposition of the cyclic esters on the positive electrode surface.

Benefits of technology

The cycling performance, storage performance and power performance of lithium-ion batteries at high temperatures is significantly improved, the high-temperature storage capacity retention rate and cycle capacity retention rate of the battery, while reducing the initial discharge DC resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919854A_ABST
    Figure CN118919854A_ABST
Patent Text Reader

Abstract

The invention provides an electrolyte, a lithium ion battery and an electric device. The electrolyte comprises electrolyte salt and an organic solvent, the electrolyte salt comprises lithium salt, the organic solvent comprises cyclic ester, the mass fraction W1 of the lithium salt in the electrolyte is 2.4%-20.17%, and the mass fraction W2 of the cyclic ester in the electrolyte is 2.93%-46.28%. The lithium ion battery containing the electrolyte has improved high-temperature storage performance and high-temperature cycle performance.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of the Chinese national phase patent application No.: 202180010209.4 of the PCT international application PCT / CN2021 / 107852, whose invention name is "An electrolyte, a lithium-ion battery and an electrical device", filed on July 22, 2021. Technical Field

[0002] The present application relates to the technical field of lithium batteries, and in particular to an electrolyte, a lithium-ion battery, a battery module, a battery pack and an electrical device. Background Art

[0003] In recent years, as the application scope of lithium-ion batteries has become increasingly wider, lithium-ion batteries have been widely used in energy storage power systems such as hydropower, thermal power, wind power and solar power stations, as well as power tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, aerospace and other fields.

[0004] However, when lithium-ion batteries are installed in the above-mentioned electrical devices, the actual working environment temperature of the battery will be higher due to the limitation of the assembly space and the heat release of other components of the electrical devices. Therefore, simply improving the cycle and storage performance of the battery at room temperature cannot effectively improve the cycle and storage performance of the battery in the actual electrical device. Therefore, it is of great practical value to develop and design a lithium-ion battery with excellent high-temperature cycle performance. Summary of the invention

[0005] The present application is made in view of the above-mentioned problems, and its purpose is to provide an electrolyte that can effectively improve the high-temperature storage performance and high-temperature cycle performance of the battery, and to provide lithium-ion batteries, battery modules, battery packs and electrical devices including the electrolyte of the present application.

[0006] In order to achieve the above-mentioned object, the first aspect of the present application provides an electrolyte, wherein the electrolyte comprises an electrolyte salt and an organic solvent, wherein the electrolyte salt comprises a lithium salt, and the organic solvent comprises a cyclic ester, and the mass fraction W1 of the lithium salt in the electrolyte and the mass fraction W2 of the cyclic ester in the electrolyte satisfy

[0007] In any embodiment, in the electrolyte described in the present application, the The range is 0.5~1.06, and can be selected as 0.8~1.0.

[0008] In any embodiment, in the electrolyte of the present application, the mass fraction B of the cyclic ester relative to the mass of the organic solvent is 5% to 18%, and can be optionally 13% to 16%.

[0009] In any embodiment, in the electrolyte of the present application, the lithium salt includes at least one of lithium bis(fluorosulfonyl)imide and lithium hexafluorophosphate, and the cyclic ester includes at least one of ethylene carbonate and propylene carbonate.

[0010] In any embodiment, in the electrolyte of the present application, the sum of the molar concentration C1 of the lithium bis(fluorosulfonyl)imide and the molar concentration C2 of the lithium hexafluorophosphate is 0.86-1.4M.

[0011] In any embodiment, the electrolyte of the present application includes a film-forming additive, and the mass fraction A of the film-forming additive in the electrolyte and the mass fraction W2 of the cyclic ester in the electrolyte satisfy:

[0012] A second aspect of the present application provides a lithium-ion battery, comprising the electrolyte, isolation membrane, negative electrode plate and positive electrode plate described in the first aspect of the present application.

[0013] In any embodiment, the positive electrode sheet includes a positive electrode active material LiNi x Co y Mn z O2, x+y+z=1, the mass fraction W2 of the cyclic ester in the electrolyte and the nickel atomic content x satisfy the relationship:

[0014] In any embodiment, the positive electrode sheet includes a positive electrode active material LiNi x Co y Mn z O2, x+y+z=1. From the perspective of matching the electrolyte of the present application, the nickel atom content x is greater than 0.5 and can be selected as 0.65, 0.8, or 0.96.

[0015] In any embodiment, in the lithium ion battery of the present application, the negative electrode material is 1540.25 mm 2 The loading amount H (in g) on ​​the current collector surface and the mass fraction W2 of the cyclic ester in the electrolyte satisfy the relationship:

[0016] [Beneficial Effects]

[0017] The present application limits the relative ratio of cyclic ester and lithium salt in the electrolyte of lithium-ion battery, so that the electrolyte containing both cyclic ester and lithium salt has good electrical conductivity, oxidation resistance, system stability and suitable viscosity, and can improve the conductivity of the negative electrode interface film, so that the lithium-ion battery containing it has significantly improved high-temperature storage performance and high-temperature cycle performance, and has good power performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 is a schematic diagram of a lithium-ion battery according to one embodiment of the present application.

[0019] Figure 2 yes Figure 1 An exploded view of a lithium-ion battery according to an embodiment of the present application is shown.

[0020] Figure 3 It is a schematic diagram of an electric device using a lithium-ion battery as a power source according to one embodiment of the present application.

[0021] Description of reference numerals:

[0022] 5 lithium-ion battery; 51 housing; 52 electrode assembly; 53 top cover assembly DETAILED DESCRIPTION

[0023] Below, the embodiments of the electrolyte, lithium-ion battery, battery module, battery pack and electrical device of the present application are specifically disclosed with appropriate reference to the accompanying drawings. However, there are cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structures are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following descriptions are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.

[0024] "Scope" disclosed in the present application is limited in the form of lower limit and upper limit, and a given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a special range. The scope limited in this way can be including end values ​​or not including end values, and can be arbitrarily combined, that is, any lower limit can form a scope with any upper limit combination. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values ​​1 and 2 are listed, and if the maximum range values ​​3,4 and 5 are listed, the following scope can be all expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present application, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0025] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0026] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.

[0027] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0028] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.

[0029] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0030] After long-term experience in preparing electrolytes, the inventors of the present application have found that for lithium-ion battery electrolytes, adding cyclic ester solvents to the electrolyte can significantly improve the dissociation function of lithium salts, thereby significantly improving the overall conductivity of the electrolyte, while improving the composition of the negative electrode interface film, effectively preventing further side reactions of the solvent on the negative electrode surface, and playing an important role in improving the electrochemical performance of the battery.

[0031] However, after a large number of experiments, it was found that when this type of cyclic ester solvent is used in the electrolyte, compared with other types of solvents, cyclic ester solvents are easily enriched on the surface of the positive electrode, and the cyclic esters enriched on the surface of the positive electrode are easily oxidized and decomposed, exacerbating the loss of solvent components in the electrolyte and generating a large amount of gas, which ultimately deteriorates the battery's cycle performance and storage performance. Secondly, the viscosity of cyclic esters is significantly higher than that of other types of commonly used solvents, which increases the viscosity of the electrolyte system, is not conducive to lithium ion transmission, and is also detrimental to the electrochemical performance of the battery.

[0032] In addition, the inventors also found that for lithium-ion batteries containing cyclic ester solvents, the storage performance and cycle performance of the batteries in high-temperature environments are significantly deteriorated compared to those in normal temperature environments. After in-depth research and analysis by the inventors, it is speculated that this may be due to the following reasons: high temperature causes the cyclic ester solvents to accumulate on the positive electrode surface more quickly and in larger quantities, and at the same time, high temperature accelerates the decomposition of the cyclic esters accumulated on the positive electrode surface. The high temperature environment ultimately leads to the battery's cycle performance and storage performance.

[0033] Based on this, the inventors have discovered through a large number of experiments that by synergistically adjusting the relative contents of cyclic esters and lithium salts in the electrolyte within a specific range, while fully ensuring that the electrolyte has a high electrical conductivity, the enrichment rate and amount of such cyclic ester solvents in the positive electrode can be significantly improved, the oxidative decomposition of the positive electrode can be slowed down, and the viscosity of the electrolyte system can also be significantly improved. Ultimately, the cycle performance, storage performance and power performance of lithium-ion batteries using cyclic ester solvents at high temperatures are significantly improved.

[0034] The electrolyte formula of the present application is particularly suitable for ternary lithium-ion batteries with high nickel atom content, even ternary lithium-ion batteries with ultra-high nickel atom content.

[0035] The electrolyte formulation of the present application is particularly suitable for improving the cycle performance, storage performance and power performance of lithium-ion batteries at high temperatures.

[0036] [Electrolyte]

[0037] The first aspect of the present application provides an electrolyte solution, wherein the electrolyte solution comprises an electrolyte salt and an organic solvent, wherein the electrolyte salt comprises a lithium salt, and the organic solvent comprises a cyclic ester, and the mass fraction W1 of the lithium salt in the electrolyte solution and the mass fraction W2 of the cyclic ester in the electrolyte solution satisfy

[0038] The lithium salt of the present application can be selected from at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(fluorosulfonyl imide), lithium bis(trifluoromethanesulfonyl imide), lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalatoborate, lithium dioxalatoborate, lithium difluorodioxalatophosphate and lithium tetrafluorooxalatophosphate.

[0039] The cyclic ester of the present application can be selected from one or more of ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), and vinyl ethylene carbonate (VEC). It can be selected from at least one of ethylene carbonate and propylene carbonate.

[0040] It should be noted that, when there is more than one type of lithium salt in the electrolyte, "the mass fraction of the lithium salt in the electrolyte" refers to the mass fraction of the total mass of all types of lithium salts in the electrolyte. Similarly, when there is more than one type of cyclic ester in the electrolyte, "the mass fraction of the cyclic ester in the electrolyte" refers to the mass fraction of the total mass of all types of cyclic esters in the electrolyte.

[0041] This application aims to develop an electrolyte formula that has good conductivity, oxidation resistance, system stability and suitable viscosity, and can improve the conductivity of the negative electrode interface film. After a large number of experiments, it was found that when the cyclic ester content and the lithium salt content in the electrolyte meet a specific matching relationship The developed electrolyte has unexpected beneficial effects. The electrolyte system has good electrical conductivity, oxidation resistance, system stability and suitable viscosity, and improves the conductivity of the negative electrode interface film, improves the enrichment rate and enrichment amount of the cyclic ester solvent in the positive electrode, and slows down the oxidative decomposition of the positive electrode. The corresponding lithium-ion battery has good high-temperature cycle performance and high-temperature storage performance.

[0042] The inventors have found through extensive research that in order to make the lithium-ion battery electrolyte have excellent conductivity, the ratio of lithium salt to cyclic ester in the commercial electrolyte on the market is Usually it is above 1.5. However, in fact, the ratio of lithium salt to cyclic ester is too high. Therefore, the oxidation decomposition reaction at the positive electrode is very serious, which seriously deteriorates the battery performance of high-temperature storage, gas production and high-temperature cycling. After years of development, the lithium-ion battery electrolyte field has not made the ratio of lithium salt to cyclic ester solvent Breakthrough 1.5. After a lot of experiments, this application has developed The electrolyte system significantly improves the high temperature storage performance and high temperature cycle performance of the battery. See Table 1 for details.

[0043] In some embodiments, optionally, in the electrolyte of the present application, the The range is 0.5 to 1.06, and can be selected as 0.8 to 1.0. See Table 1 for details.

[0044] By further limiting The range of can further optimize the composition of the electrolyte, so that the electrolyte forms a good solvation structure, which prompts the electrolyte to form an inorganic-organic composite interface film with better conductivity on the surface of the positive and negative electrodes, which can not only make the battery have significantly improved high-temperature storage performance and high-temperature cycle performance, but also have good power performance.

[0045] Optionally, A numerical range consisting of any specific point value in Table 1 can be selected.

[0046] In some embodiments, optionally, in the electrolyte of the present application, the mass fraction B of the cyclic ester relative to the mass of the organic solvent is 5% to 18%, optionally 13% to 16%.

[0047] After thorough investigation, it was found that in the electrolytes containing cyclic ester solvents on the market, the content of cyclic esters relative to the mass of organic solvents is basically maintained at more than 20%, which easily leads to serious gas production during high-temperature storage and poor high-temperature cycle performance of the battery. This application reduces the content of cyclic esters to 5% to 18% by rationally allocating the specific substance types and contents of the electrolyte, and the high-temperature storage performance, high-temperature cycle performance and power performance of the battery are significantly improved. By further limiting the value of B to within the range of 13% to 16%, the high-temperature cycle performance and high-temperature storage performance of lithium-ion batteries are further improved. See Table 2 for details.

[0048] Optionally, B can be selected from a numerical range consisting of any specific point value in Table 2.

[0049] In some embodiments, optionally, in the electrolyte of the present application, the lithium salt may be at least one of lithium bis(fluorosulfonyl)imide and lithium hexafluorophosphate.

[0050] In some embodiments, the ratio of the molar concentration C1 of the lithium bis(fluorosulfonyl)imide to the molar concentration C2 of the lithium hexafluorophosphate is It is 0.05-5, and can be selected as 1-3.5.

[0051] In this application, due to the restriction of the content of cyclic carbonate, its dissociation ability of lithium salt is subject to certain restrictions, and the conductivity of the electrolyte will be affected to a certain extent. Through a large number of experimental screenings, the inventors found that replacing LiPF6 with lithium bis(fluorosulfonyl)imide (LiFSI) can improve the conductivity of the electrolyte, but LiFSI alone will accelerate the corrosion of aluminum foil. However, the inventors found that using a mixed salt of LiPF6 and LiFSI at the same time, and by increasing the molar concentration C1 of the lithium bis(fluorosulfonyl)imide to the molar concentration C2 of the lithium hexafluorophosphate If the content is limited within a reasonable range, it can not only make up for the electrolyte conductivity loss due to the reduction in the amount of cyclic ester, but also effectively prevent the corrosion of the aluminum foil by the lithium salt, which is beneficial to further improve the high-temperature cycle performance and high-temperature storage performance of the battery. See Table 3 for details.

[0052] Optionally, A numerical range consisting of any specific point value in Table 3 can be selected.

[0053] In some embodiments, optionally, the sum of the molar concentrations of the lithium bis(fluorosulfonyl)imide and the lithium hexafluorophosphate is 0.86-1.4M, optionally 1-1.4M.

[0054] The total concentration of LiFSI and LiPF6 is further limited within an appropriate range because when the lithium salt concentration is too high, the viscosity of the electrolyte is too large, which not only reduces the high-temperature cycle and high-temperature storage performance of the battery, but also reduces the battery power performance; on the contrary, when the total concentration is too low, the content of effectively migrated lithium ions is too small, and the high-temperature cycle performance and high-temperature storage performance of the battery are poor. See Table 4 for details.

[0055] Optionally, the sum of the molar concentrations of lithium bis(fluorosulfonyl)imide and the lithium hexafluorophosphate can be selected from a numerical range consisting of any specific point value in Table 4.

[0056] In some embodiments, optionally, the electrolyte of the present application includes a film-forming additive,

[0057] The mass fraction A of the film-forming additive in the electrolyte and the mass fraction W2 of the cyclic ester in the electrolyte satisfy: The film-forming additive may be at least one of fluoroethylene carbonate (FEC), vinylene carbonate (VC), diethylene sulfate (DTD), and 1,3-propane sultone (PS).

[0058] Cyclic ester solvents will participate in the film formation of the positive and negative electrodes during the formation process of lithium-ion batteries. However, the film quality of cyclic esters alone may be insufficient to maintain good battery cycle performance. The combined use with film-forming additives can improve the film quality.

[0059] After a large number of experimental statistics, when the mass fraction A of the film-forming additive in the electrolyte of the present application and the mass fraction W2 of the cyclic ester in the electrolyte satisfy the relationship of the present application, the electrolyte formed can not only ensure high-quality film formation of the positive and negative electrodes, but also enable the cyclic ester matched therewith to exert its maximum effective effect (improve the overall conductivity of the electrolyte), and the corresponding lithium-ion battery has both good high-temperature cycle performance and high-temperature storage performance, and also has good power performance. See Table 5 for details.

[0060] Optionally, A numerical range consisting of any specific point value in Table 5 can be selected, optionally within the range of 11.9-13.5.

[0061] The lithium-ion battery of the present application further comprises a positive electrode sheet, a separator, and a negative electrode sheet.

[0062] [Positive electrode]

[0063] The positive electrode sheet includes a positive electrode current collector and a positive electrode film layer disposed on at least one surface of the positive electrode current collector, wherein the positive electrode film layer includes a positive electrode active material.

[0064] As an example, the positive electrode current collector has two surfaces opposite to each other in its thickness direction, and the positive electrode film layer is disposed on any one or both of the two opposite surfaces of the positive electrode current collector.

[0065] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base and a metal layer formed on at least one surface of the polymer material base. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0066] In some embodiments, the positive electrode active material may adopt a positive electrode active material for a battery that is well known in the art. As an example, the positive electrode active material may include at least one of the following materials: a lithium-containing phosphate with an olivine structure, a lithium transition metal oxide, and their respective modified compounds. However, the present application is not limited to these materials, and other traditional materials that can be used as positive electrode active materials for batteries may also be used. These positive electrode active materials may be used alone or in combination of two or more. Among them, examples of lithium transition metal oxides may include, but are not limited to, lithium cobalt oxide (such as LiCoO2), lithium nickel oxide (such as LiNiO2), lithium manganese oxide (such as LiMnO2, LiMn2O4), lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide (such as LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (also referred to as NCM 333 )、LiNi 0.5 Co 0.2 Mn 0.3 O2 (also referred to as NCM 523 )、LiNi 0.5 Co 0.25 Mn 0.25 O2 (also referred to as NCM 211 )、LiNi 0.6 Co 0.2 Mn 0.2 O2 (also referred to as NCM 622 )、LiNi 0.8 Co 0.1 Mn 0.1 O2 (also referred to as NCM 811 ), lithium nickel cobalt aluminum oxide (such as LiNi 0.85 Co 0.15 Al0.05 O2) and its modified compounds, etc. Examples of lithium-containing phosphates with an olivine structure may include, but are not limited to, at least one of lithium iron phosphate (such as LiFePO4 (also referred to as LFP)), a composite material of lithium iron phosphate and carbon, lithium manganese phosphate (such as LiMnPO4), a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, and a composite material of lithium iron manganese phosphate and carbon.

[0067] In some embodiments, the positive electrode film layer may further optionally include a binder. As an example, the binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorine-containing acrylate resin.

[0068] In some embodiments, the positive electrode film layer may further include a conductive agent, which may include, for example, at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0069] In some embodiments, the positive electrode sheet can be prepared in the following manner: the components for preparing the positive electrode sheet, such as the positive electrode active material, the conductive agent, the binder and any other components are dispersed in a solvent (such as N-methylpyrrolidone) to form a positive electrode slurry; the positive electrode slurry is coated on the positive electrode collector, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained.

[0070] [Negative electrode]

[0071] The negative electrode sheet includes a negative electrode current collector and a negative electrode film layer disposed on at least one surface of the negative electrode current collector, wherein the negative electrode film layer includes a negative electrode active material.

[0072] As an example, the negative electrode current collector has two surfaces opposite to each other in its thickness direction, and the negative electrode film layer is disposed on any one or both of the two opposite surfaces of the negative electrode current collector.

[0073] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, as the metal foil, a copper foil may be used. The composite current collector may include a polymer material base and a metal layer formed on at least one surface of the polymer material base. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0074] In some embodiments, the negative electrode active material may adopt the negative electrode active material for the battery known in the art. As an example, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, lithium titanate, etc. The silicon-based material may be selected from at least one of elemental silicon, silicon oxide compounds, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. The tin-based material may be selected from at least one of elemental tin, tin oxide compounds, and tin alloys. However, the present application is not limited to these materials, and other traditional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.

[0075] In some embodiments, the negative electrode film layer may further include a binder. The binder may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA) and carboxymethyl chitosan (CMCS).

[0076] In some embodiments, the negative electrode film layer may further include a conductive agent, which may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene and carbon nanofibers.

[0077] In some embodiments, the negative electrode film layer may optionally include other additives, such as a thickener (eg, sodium carboxymethyl cellulose (CMC-Na)).

[0078] In some embodiments, the negative electrode sheet can be prepared in the following manner: the components for preparing the negative electrode sheet, such as the negative electrode active material, the conductive agent, the binder and any other components are dispersed in a solvent (such as deionized water) to form a negative electrode slurry; the negative electrode slurry is coated on the negative electrode collector, and after drying, cold pressing and other processes, the negative electrode sheet can be obtained.

[0079] [Isolation film]

[0080] In some embodiments, the lithium-ion battery further includes a separator. The present application has no particular limitation on the type of separator, and any known porous separator with good chemical stability and mechanical stability can be selected.

[0081] In some embodiments, the material of the isolation membrane can be selected from at least one of glass fiber, non-woven fabric, polyethylene, polypropylene and polyvinylidene fluoride. The isolation membrane can be a single-layer film or a multi-layer composite film, without particular limitation. When the isolation membrane is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.

[0082] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the separator may be formed into an electrode assembly by a winding process or a lamination process.

[0083] [Lithium-ion battery]

[0084] The present application also provides a lithium-ion battery, comprising the electrolyte described in the first aspect of the present application.

[0085] In some embodiments, the lithium-ion battery of the present application comprises a positive electrode sheet and the electrolyte of the first aspect of the present application, wherein the positive electrode sheet comprises a LiNi x Co y Mn z O2, a positive electrode material represented by x+y+z=1; wherein the mass fraction W2 of the cyclic ester in the electrolyte and the nickel atomic content x satisfy the relationship:

[0086] The lithium-ion battery prepared by combining the electrolyte of the present application with the Ni-Co-Mn layered ternary positive electrode active material has significantly improved electrochemical properties, and the amount of cyclic ester in the electrolyte has an adaptive relationship with the nickel atom content x in the ternary positive electrode active material. Generally speaking, the higher the nickel atom content in the ternary positive electrode active material, the stronger the activity of the corresponding ternary positive electrode active material. However, during the use of the battery, the ternary positive electrode active material with a high nickel atom content will aggravate the oxygen release on the positive electrode surface, thereby aggravating the oxidative decomposition of cyclic esters and other solvents. After a large number of experiments, the inventors of the present application found that when the amount of the electrolyte of the present application and the nickel atom content x satisfy a certain adaptive relationship, that is, When the above method is used, it has an unexpected technical effect: it can effectively improve the oxygen release problem of high-nickel batteries and effectively slow down the oxidative decomposition of cyclic esters on the positive electrode surface. The corresponding ternary lithium-ion battery has both excellent cycle performance and power performance. See Table 6 for details.

[0087] In some embodiments, optionally, the nickel atomic content x may be greater than 0.5, and optionally, the nickel atomic content may be 0.5, 0.65, 0.8, or 0.96. See Table 8 for details.

[0088] The electrolyte formula of the present application is particularly suitable for ternary lithium-ion batteries with high nickel atom content. Even ternary lithium-ion batteries with ultra-high nickel atom content have excellent high-temperature storage performance, high-temperature cycle performance and power performance.

[0089] In some embodiments, in the lithium ion battery of the present application, the negative electrode material is 1540.25 mm 2 The loading amount H (in g) on ​​the current collector surface and the mass fraction W2 of the cyclic ester in the electrolyte satisfy the relationship: Optionally,

[0090] After a lot of experiments, the inventors of the present application found that when the amount of cyclic ester in the electrolyte of the present application and the negative electrode material loading H have a synergistic effect, when the two meet a certain adaptation relationship, that is, When the above conditions are met, the overall electrochemical performance of lithium-ion batteries is significantly improved. See Table 7 for details.

[0091] In some embodiments, the lithium ion battery of the present application is a shell battery.

[0092] In some embodiments, the lithium-ion battery may include an outer packaging, which may be used to encapsulate the electrode assembly and the electrolyte.

[0093] In some embodiments, the outer packaging of the lithium ion battery can be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer packaging of the lithium ion battery can also be a soft package, such as a bag-type soft package. The material of the soft package can be plastic, and as the plastic, polypropylene, polybutylene terephthalate, and polybutylene succinate can be listed.

[0094] The present application has no particular limitation on the shape of the lithium-ion battery, which may be cylindrical, square, or any other shape. Figure 1 A lithium-ion battery 5 having a square structure is used as an example.

[0095] In some embodiments, reference Figure 2 , the outer packaging may include a shell 51 and a cover plate 53. Among them, the shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation membrane can form an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is infiltrated in the electrode assembly 52. ​​The number of electrode assemblies 52 contained in the lithium-ion battery 5 can be one or more, and those skilled in the art can choose according to specific actual needs.

[0096] Figure 3 An example of an electric device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle.

[0097] Example

[0098] Hereinafter, the embodiments of the present application will be described. The embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If no specific techniques or conditions are specified in the embodiments, the techniques or conditions described in the literature in the art or the product specifications are used. The reagents or instruments used that do not specify the manufacturer are conventional products that are commonly used in the art and can be obtained commercially. The content of each component in the embodiments of the present application, if not otherwise specified, is based on the mass without crystal water.

[0099] The following descriptive terms: "the electrolyte of Example 1-1" refers to the electrolyte used in the preparation process of the lithium ion battery of Example 1-1; "the positive electrode plate of Example 1-1" refers to the positive electrode plate used in the preparation process of the lithium ion battery of Example 1-1; "the negative electrode plate of Example 1-1" refers to the positive electrode plate used in the preparation process of the lithium ion battery of Example 1-1; "the isolation membrane of Example 1-1" refers to the isolation membrane used in the preparation process of the lithium ion battery of Example 1-1; "the lithium ion battery of Example 1-1" refers to the lithium ion battery prepared by the positive electrode, isolation membrane, negative electrode and electrolyte of Example 1-1.

[0100] The sources of raw materials involved in the embodiments of this application are as follows:

[0101] Nickel-cobalt-manganese ternary material (LiMO2, M is Ni-Co-Mn solid solution, the specific proportion of which is detailed in each embodiment)

[0102] Artificial graphite (Guangdong Kaijin New Energy Technology Co., Ltd.)

[0103] N-Methylpyrrolidone (NMP, CAS: 872-50-4, Shanghai MacLean Biotechnology Co., Ltd.) Polyvinylidene fluoride (CAS: 24937-79-9, Shanghai MacLean Biotechnology Co., Ltd.)

[0104] Acetylene black (Guangdong Kaijin New Energy Technology Co., Ltd.)

[0105] Conductive agent carbon black (Guangdong Kaijin New Energy Technology Co., Ltd.)

[0106] Acrylate (CAS: 25067-02-1, Shanghai MacLean Biotechnology Co., Ltd.)

[0107] Ethylene carbonate (EC, CAS: 96-49-1, Shanghai MacLean Biotechnology Co., Ltd.)

[0108] Dimethyl carbonate (DMC, CAS: 616-38-6, Shanghai MacLean Biotechnology Co., Ltd.) Ethyl methyl carbonate (EMC, CAS: 623-53-0, Shanghai MacLean Biotechnology Co., Ltd.) Lithium hexafluorophosphate (LiPF6, CAS: 21324-40-3, Guangzhou Tianci High-tech Materials Co., Ltd.) Lithium bis(fluorosulfonyl)imide (LiFSI, CAS: 171611-11-3, Guangzhou Tianci High-tech Materials Co., Ltd.)

[0109] Fluorinated Ethylene Carbonate (FEC, CAS: 114435-02-8, Guangzhou Tianci High-tech Materials Co., Ltd.)

[0110] Example 1-1

[0111]

Preparation of electrolyte

[0112] In an argon atmosphere glove box with a water content of <10 ppm, 32.64 g EC, 60.84 g EMC, 6.25 g LiPF6, and 0.15 g LiFSI were added to a beaker, and the electrolyte used in this embodiment was obtained after sufficient stirring and dissolution.

[0113]

Preparation of positive electrode

[0114] The positive electrode active material nickel cobalt manganese ternary material (LiNi 0.8 Co 0.1 Mn 0.1 O2), binder polyvinylidene fluoride, conductive agent acetylene black are mixed in a mass ratio of 8:1:1, solvent NMP is added, and positive electrode slurry is obtained under the action of a vacuum mixer; the positive electrode slurry is 0.28g (dry weight) / 1540.25mm 2 The amount of the coating was evenly coated on the positive electrode current collector aluminum foil with a thickness of 13 μm; the aluminum foil was dried at room temperature and then transferred to a 120°C oven for drying for 1 hour, and then cold pressed and cut to obtain the positive electrode sheet.

[0115]

Preparation of negative electrode sheet

[0116] Artificial graphite, conductive agent carbon black, and binder acrylate were mixed in a mass ratio of 92:2:6, and deionized water was added to obtain negative electrode slurry under the action of a vacuum mixer; the negative electrode slurry was prepared at 0.18 g (dry weight) / 1540.25 mm 2 The amount of the coating was evenly coated on the negative electrode current collector copper foil with a thickness of 8 μm; the copper foil was dried at room temperature and then transferred to a 120°C oven for drying for 1 hour, and then cold pressed and cut to obtain the negative electrode sheet.

[0117]

Isolation film

[0118] The isolation membrane was purchased from Cellgard, model number is cellgard2400.

[0119]

Preparation of lithium-ion batteries

[0120] The positive electrode sheet, the separator, and the negative electrode sheet are stacked in order, so that the separator is placed between the positive and negative electrode sheets to play an isolating role, and then they are wound to obtain a bare battery cell; the bare battery cell with a capacity of 4.3Ah is placed in an outer packaging foil, and the 8.6g electrolyte prepared above is injected into the dried battery. After vacuum packaging, standing, formation, shaping and other processes, a lithium-ion battery is obtained.

[0121] Example 1-2

[0122] The preparation process of the lithium-ion battery as a whole refers to Example 1-1, except that the preparation steps of the electrolyte are as follows: in an argon atmosphere glove box with a water content of <10ppm, 18.17g EC, 72.68g EMC, 9g LiPF6, and 0.15g LiFSI are added to a beaker respectively, and the electrolyte for the example is obtained after sufficient stirring and dissolution.

[0123] Examples 1-3

[0124] The preparation process of the lithium-ion battery as a whole refers to Example 1-1, except that the preparation steps of the electrolyte are as follows: in an argon atmosphere glove box with a water content of <10ppm, 10.10g EC, 81.74g EMC, 8g LiPF6, and 0.15g LiFSI are added to a beaker respectively, and the electrolyte used in this example is obtained after sufficient stirring and dissolution.

[0125] Examples 1-4

[0126] The preparation process of the lithium-ion battery as a whole refers to Example 1-1, except that the preparation steps of the electrolyte are as follows: in an argon atmosphere glove box with a water content of <10ppm, 12.83g EC, 75.648g EMC, 11.38g LiPF6, and 0.15g LiFSI are added to a beaker respectively, and the electrolyte used in this example is obtained after sufficient stirring and dissolution.

[0127] Examples 1-5

[0128] The preparation process of the lithium-ion battery as a whole refers to Example 1-1, except that the preparation steps of the electrolyte are as follows: in an argon atmosphere glove box with a water content of <10ppm, 12.67g EC, 74.68g EMC, 12.5g LiPF6, and 0.15g LiFSI are respectively added to a beaker, and the electrolyte used in this example is obtained after sufficient stirring and dissolution.

[0129] Examples 1-6

[0130] The preparation process of the lithium-ion battery as a whole refers to Example 1-1, except that the preparation steps of the electrolyte are as follows: in an argon atmosphere glove box with a water content of <10ppm, 9.86g EC, 79.74g EMC, 10.25g LiPF6, and 0.15g LiFSI are added to a beaker respectively, and the electrolyte used in this example is obtained after sufficient stirring and dissolution.

[0131] Examples 1-7

[0132] The preparation process of the lithium-ion battery as a whole refers to Example 1-1, except that the preparation steps of the electrolyte are as follows: in an argon atmosphere glove box with a water content of <10ppm, 10.44g EC, 78.03g EMC, 11.38g LiPF6, and 0.15g LiFSI are added to a beaker respectively, and the electrolyte used in this example is obtained after sufficient stirring and dissolution.

[0133] Comparative Example 1

[0134] The preparation process of the lithium-ion battery as a whole refers to Example 1-1, except that the preparation steps of the electrolyte are as follows: in an argon atmosphere glove box with a water content of <10ppm, 82.98g EC, 4.37g EMC, 12.5g LiPF6, and 0.15g LiFSI are added to a beaker respectively, and the electrolyte used in this example is obtained after sufficient stirring and dissolution.

[0135] Example 2-1

[0136] The preparation process of the lithium-ion battery as a whole refers to Example 1-1, except that the preparation steps of the electrolyte are as follows: in an argon atmosphere glove box with a water content of <10ppm, 2.93g PC, 94.67g EMC, 2.25g LiPF6, and 0.15g LiFSI are added to a beaker respectively, and the electrolyte used in this example is obtained after sufficient stirring and dissolution.

[0137] Example 2-2

[0138] The preparation process of the lithium-ion battery as a whole refers to Example 1-1, except that the preparation steps of the electrolyte are as follows: in an argon atmosphere glove box with a water content of <10ppm, 4.80g PC, 91.29g EMC, 3.75g LiPF6, and 0.15g LiFSI are added to a beaker respectively, and the electrolyte used in this example is obtained after sufficient stirring and dissolution.

[0139] Example 2-3

[0140] The preparation process of the lithium-ion battery as a whole refers to Example 1-1, except that the preparation steps of the electrolyte are as follows: in an argon atmosphere glove box with a water content of <10ppm, 7.51g PC, 86.34g EMC, 6gLiPF6, and 0.15gLiFSI are added to a beaker respectively, and the electrolyte used in this example is obtained after sufficient stirring and dissolution.

[0141] Embodiment 2-4

[0142] The preparation process of the lithium-ion battery as a whole refers to Example 1-1, except that the preparation steps of the electrolyte are as follows: in an argon atmosphere glove box with a water content of <10ppm, 9.25g PC, 83.22g EMC, 7.38g LiPF6, and 0.15g LiFSI are added to a beaker respectively, and the electrolyte used in this example is obtained after sufficient stirring and dissolution.

[0143] Embodiment 2-5

[0144] The preparation process of the lithium-ion battery as a whole refers to Example 1-1, except that the preparation steps of the electrolyte are as follows: in an argon atmosphere glove box with a water content of <10ppm, 11.76g PC, 78.71g EMC, 9.38g LiPF6, and 0.15g LiFSI are added to a beaker respectively, and the electrolyte used in this example is obtained after sufficient stirring and dissolution.

[0145] Embodiment 2-6

[0146] The preparation process of the lithium-ion battery as a whole refers to Example 1-1, except that the preparation steps of the electrolyte are as follows: in an argon atmosphere glove box with a water content of <10ppm, 13.38g PC, 75.84g EMC, 10.63g LiPF6, and 0.15g LiFSI are added to a beaker respectively, and the electrolyte used in this example is obtained after sufficient stirring and dissolution.

[0147] Embodiment 2-7

[0148] The preparation process of the lithium-ion battery as a whole refers to Example 1-1, except that the preparation steps of the electrolyte are as follows: in an argon atmosphere glove box with a water content of <10ppm, 15.72g PC, 71.62g EMC, 12.5g LiPF6, and 0.15g LiFSI are added to a beaker respectively, and the electrolyte used in this example is obtained after sufficient stirring and dissolution.

[0149] Embodiment 2-8

[0150] The preparation process of the lithium-ion battery as a whole refers to Example 1-1, except that the preparation steps of the electrolyte are as follows: in an argon atmosphere glove box with a water content of <10ppm, 17.22g PC, 68.88g EMC, 13.75g LiPF6, and 0.15g LiFSI are added to a beaker respectively, and the electrolyte used in this example is obtained after sufficient stirring and dissolution.

[0151] Example 3-1

[0152] The preparation process of the lithium-ion battery as a whole refers to Example 1-1, except that the preparation steps of the electrolyte are as follows: in an argon atmosphere glove box with a water content of <10ppm, 13.92g EC, 73.55g EMC, 12.38g LiPF6, and 0.15g LiFSI are added to a beaker respectively, and the electrolyte used in this example is obtained after sufficient stirring and dissolution.

[0153] Example 3-2

[0154] The preparation process of the lithium-ion battery as a whole refers to Example 1-1, except that the preparation steps of the electrolyte are as follows: in an argon atmosphere glove box with a water content of <10ppm, 14.04g EC, 73.32g EMC, 11.90g LiPF6, and 0.73g LiFSI are added to a beaker respectively, and the electrolyte used in this example is obtained after sufficient stirring and dissolution.

[0155] Example 3-3

[0156] The preparation process of the lithium-ion battery as a whole refers to Example 1-1, except that the preparation steps of the electrolyte are as follows: in an argon atmosphere glove box with a water content of <10ppm, 15.5g EC, 70.55g EMC, 6.25g LiPF6, and 7.7g LiFSI are respectively added to a beaker, and the electrolyte used in this example is obtained after sufficient stirring and dissolution.

[0157] Embodiment 3-4

[0158] The preparation process of the lithium-ion battery as a whole refers to Example 1-1, except that the preparation steps of the electrolyte are as follows: in an argon atmosphere glove box with a water content of <10ppm, 15.82g EC, 69.94g EMC, 5g LiPF6, and 9.24g LiFSI are added to a beaker respectively, and the electrolyte used in this example is obtained after sufficient stirring and dissolution.

[0159] Embodiment 3-5

[0160] The preparation process of the lithium-ion battery as a whole refers to Example 1-1, except that the preparation steps of the electrolyte are as follows: in an argon atmosphere glove box with a water content of <10ppm, 16.04g EC, 69.53g EMC, 4.17g LiPF6, and 10.27g LiFSI are respectively added to a beaker, and the electrolyte used in this example is obtained after sufficient stirring and dissolution.

[0161] Embodiment 3-6

[0162] The preparation process of the lithium-ion battery as a whole refers to Example 1-1, except that the preparation steps of the electrolyte are as follows: in an argon atmosphere glove box with a water content of <10ppm, 16.39g EC, 68.85g EMC, 2.78g LiPF6, and 11.98g LiFSI are added to a beaker respectively, and the electrolyte used in this example is obtained after sufficient stirring and dissolution.

[0163] Embodiment 3-7

[0164] The preparation process of the lithium-ion battery as a whole refers to Example 1-1, except that the preparation steps of the electrolyte are as follows: in an argon atmosphere glove box with a water content of <10ppm, 16.57g EC, 68.51g EMC, 2.08g LiPF6, and 12.83g LiFSI are added to a beaker respectively, and the electrolyte used in this example is obtained after sufficient stirring and dissolution.

[0165] Embodiment 3-8

[0166] The preparation process of the lithium-ion battery as a whole refers to Example 1-1, except that the preparation steps of the electrolyte are as follows: in an argon atmosphere glove box with a water content of <10ppm, 16.62g EC, 68.43g EMC, 1.92g LiPF6, and 13.03g LiFSI are added to a beaker respectively, and the electrolyte used in this example is obtained after sufficient stirring and dissolution.

[0167] Example 4-1

[0168] The preparation process of the lithium-ion battery as a whole refers to Example 1-1, except that the preparation steps of the electrolyte are as follows: in an argon atmosphere glove box with a water content of <10ppm, 10.85g EC, 79.39g EMC, 4.38g LiPF6, and 5.39g LiFSI are added to a beaker respectively, and the electrolyte used in this example is obtained after sufficient stirring and dissolution.

[0169] Example 4-2

[0170] The preparation process of the lithium-ion battery as a whole refers to Example 1-1, except that the preparation steps of the electrolyte are as follows: in an argon atmosphere glove box with a water content of <10ppm, 13.18g EC, 74.97g EMC, 5.31g LiPF6, and 6.55g LiFSI are respectively added to a beaker, and the electrolyte used in this example is obtained after sufficient stirring and dissolution.

[0171] Example 4-3

[0172] The preparation process of the lithium-ion battery as a whole refers to Example 1-1, except that the preparation steps of the electrolyte are as follows: in an argon atmosphere glove box with a water content of <10ppm, 15.5g EC, 70.55g EMC, 6.25g LiPF6, and 7.70g LiFSI are respectively added to a beaker, and the electrolyte used in this example is obtained after sufficient stirring and dissolution.

[0173] Example 4-4

[0174] The preparation process of the lithium-ion battery as a whole refers to Example 1-1, except that the preparation steps of the electrolyte are as follows: in an argon atmosphere glove box with a water content of <10ppm, 21.7g EC, 58.77g EMC, 8.75g LiPF6, and 10.78g LiFSI are added to a beaker respectively, and the electrolyte used in this example is obtained after sufficient stirring and dissolution.

[0175] Embodiment 4-5

[0176] The preparation process of the lithium-ion battery as a whole refers to Example 1-1, except that the preparation steps of the electrolyte are as follows: in an argon atmosphere glove box with a water content of <10ppm, 22.48g EC, 57.3g EMC, 9.06g LiPF6, and 11.17g LiFSI are respectively added to a beaker, and the electrolyte used in this example is obtained after sufficient stirring and dissolution.

[0177] Example 5-1

[0178] The preparation process of the lithium-ion battery as a whole refers to Example 1-1, except that the preparation steps of the electrolyte are as follows: in an argon atmosphere glove box with a water content of <10ppm, 12.30g EC, 72.55g EMC, 11.44g LiPF6, 0.15g LiFSI, and 3.55g FEC are added to a beaker, respectively, and the electrolyte used in this example is obtained after sufficient stirring and dissolution.

[0179] Example 5-2

[0180] The preparation process of the lithium-ion battery as a whole refers to Example 1-1, except that the preparation steps of the electrolyte are as follows: in an argon atmosphere glove box with a water content of <10ppm, 10.35g EC, 75.87g EMC, 9.63g LiPF6, 0.15g LiFSI, and 4g FEC are added to a beaker, respectively, and the electrolyte used in this example is obtained after sufficient stirring and dissolution.

[0181] Example 5-3

[0182] The preparation process of the lithium-ion battery as a whole refers to Example 1-1, except that the preparation steps of the electrolyte are as follows: in an argon atmosphere glove box with a water content of <10ppm, 12.51g EC, 70.89g EMC, 11.75g ​​LiPF6, 0.15g LiFSI, and 4.7g FEC are added to a beaker, respectively, and the electrolyte used in this example is obtained after sufficient stirring and dissolution.

[0183] Example 5-4

[0184] The preparation process of the lithium-ion battery as a whole refers to Example 1-1, except that the preparation steps of the electrolyte are as follows: in an argon atmosphere glove box with a water content of <10ppm, 10.76g EC, 73.31g EMC, 10.13g LiPF6, 0.15g LiFSI, and 5.65g FEC are added to a beaker, respectively, and the electrolyte used in this example is obtained after sufficient stirring and dissolution.

[0185] Example 5-5

[0186] The preparation process of the lithium-ion battery as a whole refers to Example 1-1, except that the preparation steps of the electrolyte are as follows: in an argon atmosphere glove box with a water content of <10ppm, 11.03g EC, 71.29g EMC, 10.63g LiPF6, 0.15g LiFSI, and 6.9g FEC are added to a beaker, respectively, and the electrolyte used in this example is obtained after sufficient stirring and dissolution.

[0187] Embodiment 5-6

[0188] The preparation process of the lithium-ion battery as a whole refers to Example 1-1, except that the preparation steps of the electrolyte are as follows: in an argon atmosphere glove box with a water content of <10ppm, 13.55g EC, 66.17g EMC, 13.13g LiPF6, 0.15g LiFSI, and 7g FEC are added to a beaker, respectively, and the electrolyte used in this example is obtained after sufficient stirring and dissolution.

[0189] Example 6-1

[0190] The preparation process of the lithium-ion battery is generally similar to that of Example 1-1, except that the positive electrode active material ternary material used in this example is LiNi 0.99 Co 0.005 Mn 0.005 In addition, the preparation steps of the electrolyte are as follows: in an argon atmosphere glove box with a water content of <10 ppm, 46.286 g EC, 39.43 g EMC, 4.13 g LiPF6, and 10.16 g LiFSI are added to a beaker, and the mixture is stirred and dissolved to obtain the electrolyte used in this embodiment.

[0191] Example 6-2

[0192] The preparation process of the lithium-ion battery is generally similar to that of Example 1-1, except that the positive electrode active material ternary material used in this example is LiNi 0.69 Co 0.16 Mn 0.15 O2.

[0193] In addition, the preparation steps of the electrolyte are as follows: in an argon atmosphere glove box with a water content of <10 ppm, 34.28 g EC, 51.43 g EMC, 4.13 g LiPF6, and 10.16 g LiFSI are added into a beaker respectively, and the mixture is stirred and dissolved to obtain the electrolyte used in this embodiment.

[0194] Example 6-3

[0195] The preparation process of the lithium-ion battery is generally similar to that of Example 1-1, except that the positive electrode active material ternary material used in this example is LiNi 0.47 Co 0.15 Mn 0.38 O2.

[0196] In addition, the preparation steps of the electrolyte are as follows: in an argon atmosphere glove box with a water content of <10 ppm, 27.86 g EC, 57.85 g EMC, 4.13 g LiPF6, and 10.16 g LiFSI are added into a beaker respectively, and the mixture is stirred and dissolved to obtain the electrolyte used in this embodiment.

[0197] Example 6-4

[0198] The preparation process of the lithium-ion battery is generally similar to that of Example 1-1, except that the positive electrode active material ternary material used in this example is LiNi 0.32 Co 0.19 Mn 0.57 O2.

[0199] In addition, the preparation steps of the electrolyte are as follows: in an argon atmosphere glove box with a water content of <10 ppm, 23.14 g EC, 62.57 g EMC, 4.13 g LiPF6, and 10.16 g LiFSI are respectively added into a beaker, and the mixture is stirred and dissolved to obtain the electrolyte used in this embodiment.

[0200] Example 6-5

[0201] The preparation process of the lithium-ion battery is generally similar to that of Example 1-1, except that the positive electrode active material ternary material used in this example is LiNi 0.25 Co 0.18 Mn 0.57 In addition, the preparation steps of the electrolyte are as follows: in an argon atmosphere glove box with a water content of <10 ppm, 20.06 g EC, 65.65 g EMC, 4.13 g LiPF6, and 10.16 g LiFSI are added to a beaker, and the mixture is stirred and dissolved to obtain the electrolyte used in this embodiment.

[0202] Example 7-1

[0203] The preparation process of the lithium-ion battery is generally similar to that of Example 1-1, except that the negative electrode coating amount of this example is 1.698 mg / 1540.25 mm 2 In addition, the preparation steps of the electrolyte are as follows: in an argon atmosphere glove box with a water content of <10ppm, 30.57g EC, 63.31g EMC, and 6.11g LiPF6 are added to a beaker, and the mixture is stirred and dissolved to obtain the electrolyte used in this embodiment.

[0204] Example 7-2

[0205] The preparation process of the lithium-ion battery is generally similar to that of Example 1-1, except that the negative electrode coating amount of this example is 0.873 mg / 1540.25 mm 2 In addition, the preparation steps of the electrolyte are as follows: in an argon atmosphere glove box with a water content of <10ppm, 17.47g EC, 73.80g EMC, and 8.73g LiPF6 are added into a beaker respectively, and the mixture is stirred and dissolved to obtain the electrolyte for this embodiment.

[0206] Example 7-3

[0207] The preparation process of the lithium-ion battery is generally similar to that of Example 1-1, except that the negative electrode coating amount of this example is 0.192 mg / 1540.25 mm 2In addition, the preparation steps of the electrolyte are as follows: in an argon atmosphere glove box with a water content of <10ppm, 9.61g EC, 82.71g EMC, and 7.69g LiPF6 are added into a beaker respectively, and the mixture is stirred and dissolved to obtain the electrolyte for this embodiment.

[0208] Example 7-4

[0209] The preparation process of the lithium-ion battery is generally similar to that of Example 1-1, except that the negative electrode coating amount of this example is 0.158 mg / 1540.25 mm 2 In addition, the preparation steps of the electrolyte are as follows: in an argon atmosphere glove box with a water content of <10ppm, 12.67g EC, 75.94g EMC, and 11.4g LiPF6 are added to a beaker, and the mixture is stirred and dissolved to obtain the electrolyte used in this embodiment.

[0210] Example 7-5

[0211] The preparation process of the lithium-ion battery is generally similar to that of Example 1-1, except that the negative electrode coating amount of this example is 0.115 mg / 1540.25 mm 2 In addition, the preparation steps of the electrolyte are as follows: in an argon atmosphere glove box with a water content of <10ppm, 12.67g EC, 74.67g EMC, and 12.67g LiPF6 are added into a beaker respectively, and the mixture is stirred and dissolved to obtain the electrolyte for this embodiment.

[0212] Example 7-6

[0213] The preparation process of the lithium-ion battery is generally similar to that of Example 1-1, except that the negative electrode coating amount of this example is 0.09 mg / 1540.25 mm 2 In addition, the preparation steps of the electrolyte are as follows: in an argon atmosphere glove box with a water content of <10ppm, 12.67g EC, 74.67g EMC, and 12.67g LiPF6 are added into a beaker respectively, and the mixture is stirred and dissolved to obtain the electrolyte for this embodiment.

[0214] Example 7-7

[0215] The preparation process of the lithium-ion battery is generally similar to that of Example 1-1, except that the negative electrode coating amount of this example is 0.079 mg / 1540.25 mm 2 In addition, the preparation steps of the electrolyte are as follows: in an argon atmosphere glove box with a water content of <10ppm, 12.67g EC, 74.67g EMC, and 12.67g LiPF6 are added into a beaker respectively, and the mixture is stirred and dissolved to obtain the electrolyte for this embodiment.

[0216] Embodiment 7-8

[0217] The preparation process of the lithium-ion battery is generally similar to that of Example 1-1, except that the negative electrode coating amount of this example is 0.058 mg / 1540.25 mm 2 In addition, the preparation steps of the electrolyte are as follows: in an argon atmosphere glove box with a water content of <10 ppm, 9.61 g EC, 80.3 g EMC, and 10.09 g LiPF6 are added to a beaker, and the mixture is stirred and dissolved to obtain the electrolyte used in this embodiment.

[0218] Example 8-1

[0219] The preparation process of the lithium-ion battery is generally similar to that of Example 1-1, except that the positive electrode active material ternary material used in this example is LiNi 0.5 Co 0.2 Mn 0.3 O2.

[0220] In addition, the preparation steps of the electrolyte are as follows: in an argon atmosphere glove box with a water content of <10 ppm, 16 g EC, 69.6 g EMC, and 14.4 g LiPF6 are respectively added into a beaker, and the electrolyte used in this embodiment is obtained after sufficient stirring and dissolution.

[0221] Example 8-2

[0222] The preparation process of the lithium-ion battery is generally similar to that of Example 1-1, except that the positive electrode active material ternary material used in this example is LiNi 0.65 Co 0.05 Mn 0.3 O2.

[0223] In addition, the preparation steps of the electrolyte are as follows: in an argon atmosphere glove box with a water content of <10 ppm, 16 g EC, 69.6 g EMC, and 14.4 g LiPF6 are respectively added into a beaker, and the electrolyte used in this embodiment is obtained after sufficient stirring and dissolution.

[0224] Example 8-3

[0225] The preparation process of the lithium-ion battery is generally similar to that of Example 1-1, except that the positive electrode active material ternary material used in this example is LiNi 0.85 Co 0.05 Mn 0.1 O2.

[0226] In addition, the preparation steps of the electrolyte are as follows: in an argon atmosphere glove box with a water content of <10 ppm, 16 g EC, 69.6 g EMC, and 14.4 g LiPF6 are respectively added into a beaker, and the electrolyte used in this embodiment is obtained after sufficient stirring and dissolution.

[0227] Example 8-4

[0228] The preparation process of the lithium-ion battery is generally similar to that of Example 1-1, except that the positive electrode active material ternary material used in this example is LiNi 0.96 Co0 .02 Mn 0.02 O2.

[0229] In addition, the preparation steps of the electrolyte are as follows: in an argon atmosphere glove box with a water content of <10 ppm, 16 g EC, 69.6 g EMC, and 14.4 g LiPF6 are respectively added into a beaker, and the electrolyte used in this embodiment is obtained after sufficient stirring and dissolution.

[0230]

Related parameters and battery performance test

[0231] 1. Initial discharge DCR (Direct Current Resistance) test

[0232] At 25°C, the lithium ion batteries of the above embodiments and comparative examples were charged to 4.25V at a charging rate of 1C, then charged at a constant voltage until the current was less than 0.05C, and then discharged at a discharge rate of 1C for 30min, at which time the SOC of the battery was 50%, and the voltage was recorded as V1; then discharged at a discharge rate of 4C (the corresponding current at 4C is I) for 30s, and the voltage was recorded as V2, then the initial discharge DCR of the lithium ion battery = (V1-V2) / I, see Tables 1 to 8 for specific values.

[0233] 2. 60℃ cycle performance test

[0234] At 60°C, charge the battery at 1C constant current to 4.25V, then charge at 4.25V constant voltage to a current of 0.05C, leave for 5 minutes, and then discharge at 1C constant current to 2.5V. The resulting capacity is recorded as the initial capacity C0. Repeat the above steps for the same battery, and start counting at the same time, and record the discharge capacity C0 of the battery after the 300th cycle. 300 , then after 300 cycles, the battery cycle capacity retention rate P = C 300 / C0*100%.

[0235] The lithium-ion batteries of the embodiment and the comparative example were tested according to the above process, and the specific values ​​are shown in Tables 1 to 8.

[0236] 3. 60℃ storage performance test

[0237] At 25°C, the battery was charged at a constant current of 0.5C to 4.25V, then charged at a constant voltage of 4.25V to a current of 0.05C, left for 5 minutes, and then discharged at a constant current of 0.5C to 2.5V. The discharge capacity at this time was recorded as the initial capacity C0.

[0238] The battery is then charged to 4.25V at a constant current of 0.5C, and then charged to a current of 0.05C at a constant voltage of 4.25V. The battery is then placed in a 60°C thermostat and taken out after storage for 60 days. The taken out battery is placed in an atmospheric environment of 25°C. After the temperature of the lithium-ion battery is completely reduced to 25°C, the lithium-ion battery is discharged to 2.5V at a constant current of 0.5C, and then charged to 4.25V at a constant current of 0.5C. Finally, the lithium-ion battery is discharged to 2.5V at a constant current of 0.5V. The discharge capacity at this time is C1. The high temperature storage capacity retention rate of the battery after 60 days of storage is M=C1 / C0×100%.

[0239] Other embodiments and comparative examples were tested according to the above process, and the specific values ​​are shown in Tables 1 to 8.

[0240] Table 1: Effect of the relative ratio of lithium salt to cyclic ester on battery performance

[0241]

[0242] Table 2: Effect of cyclic ester content in organic solvent on battery performance

[0243]

[0244]

[0245] Table 3: Effect of relative content of different lithium salts on battery performance

[0246]

[0247] Table 4: Effect of total lithium salt concentration on battery performance

[0248]

[0249] Table 5: Impact on battery performance

[0250]

[0251]

[0252] Table 6: Effects of other battery parameters on battery performance

[0253]

[0254] Table 7: Effects of other battery parameters on battery performance

[0255]

[0256] Table 8: Effects of other battery parameters on battery performance

[0257]

[0258]

[0259] According to Table 1, the high temperature cycle capacity retention rate and high temperature storage capacity retention rate of the lithium ion batteries corresponding to all the above embodiments are significantly higher than those of Comparative Examples 1-2. At the same time, the initial discharge DCR of all the embodiments is also lower than that of Comparative Examples 1-2.

[0260] Comprehensive comparison of Example 1-1 to Example 1-6, when When the high temperature cycle capacity retention rate of lithium-ion batteries is higher than 75%, the high temperature storage capacity retention rate is higher than 80%, and the initial discharge DCR is also within 20.5mΩ. The high temperature cycle capacity retention, high temperature storage capacity retention and initial discharge DCR of lithium-ion batteries are further improved.

[0261] Comprehensive comparison of Example 2-1 to Example 2-8, When the value of B is constant, when the value of B is in the range of 5% to 18%, the high temperature cycle capacity retention rate of the lithium-ion battery is higher than 75%, the high temperature storage capacity retention rate is higher than 80%, and the initial discharge DCR does not exceed 17.2mΩ. Further, when the value of B is in the range of 13% to 16%, the high temperature cycle capacity retention rate, high temperature storage capacity retention rate and initial discharge DCR of the lithium-ion battery are further improved.

[0262] Comprehensive comparison of Examples 3-1 to 3-8, When the value of C1+C2 is a fixed value, When the value of is in the range of 0.05-5, the high temperature cycle capacity retention rate of lithium-ion batteries is higher than 78.5%, the high temperature storage capacity retention rate is higher than 81%, and the initial discharge DCR does not exceed 17mΩ. When the value of is in the range of 1-3.5, the high temperature cycle capacity retention rate, high temperature storage capacity retention rate and initial discharge DCR of the lithium-ion battery are further improved.

[0263] Comprehensive comparison of Example 4-1 to Example 4-5, When the value of is a constant, when the value of (C1+C2) is in the range of 0.86-1.4M, the high temperature cycle capacity retention rate of the lithium-ion battery is higher than 81.5%, the high temperature storage capacity retention rate is higher than 82.3%, and the initial discharge DCR does not exceed 17mΩ. Further, when the value of (C1+C2) is in the range of 1-1.4, the high temperature cycle capacity retention rate, high temperature storage capacity retention rate and initial discharge DCR of the lithium-ion battery are further improved.

[0264] Comprehensive comparison of Example 5-1 to Example 5-6, when When is a fixed value, When the value of is in the range of 10-16, the high temperature cycle capacity retention rate of the lithium-ion battery is higher than 83%, the high temperature storage capacity retention rate is higher than 84%, and the initial discharge DCR does not exceed 16.5mΩ. When the value of is in the range of 11.9-13.5, the high temperature cycle capacity retention rate, high temperature storage capacity retention rate and initial discharge DCR of the lithium-ion battery are further improved.

[0265] Comprehensive comparison of Example 6-1 to Example 6-5, when When the value is in the range of 0.5-0.72, the high-temperature cycle capacity retention rate of the lithium-ion battery is higher than 81.3%, the high-temperature storage capacity retention rate is higher than 82%, and the initial discharge DCR does not exceed 17mΩ.

[0266] Comprehensive comparison of Example 7-1 to Example 7-8, when When is a fixed value, When the value of is in the range of 20-166, the high temperature cycle capacity retention rate of the lithium-ion battery is higher than 81.5%, the high temperature storage capacity retention rate is no less than 81.3%, and the initial discharge DCR does not exceed 16.9mΩ. Furthermore, when When the value of is in the range of 50-141, the high temperature cycle capacity retention rate, high temperature storage capacity retention rate and initial discharge DCR of the lithium-ion battery are further improved.

[0267] Examples 8-1 to 8-4 illustrate that for current LiNi x Co y Mn z Several commonly used types of O2 ternary positive electrode active materials, namely ternary positive electrode active materials with nickel atomic contents of 0.5, 0.65, 0.85, and 0.96, respectively, have corresponding lithium-ion batteries that have good high-temperature cycle capacity retention, high-temperature storage capacity retention, and initial discharge DCR.

[0268] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples, and the embodiments having the same structure as the technical idea and exerting the same effect within the scope of the technical solution of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the main purpose of the present application, various modifications that can be thought of by those skilled in the art to the embodiments and other methods of combining some of the constituent elements in the embodiments are also included in the scope of the present application.

Claims

1. An electrolyte solution comprising an electrolyte salt and an organic solvent, characterized in that: The electrolyte salt includes a lithium salt, the organic solvent includes a cyclic ester, the mass fraction W1 of the lithium salt in the electrolyte is 2.4%-20.17%, and the mass fraction W2 of the cyclic ester in the electrolyte is 2.93%-46.28%.

2. The electrolyte according to claim 1, characterized in that The mass fraction W1 of the lithium salt in the electrolyte is 9.13%-19.53%, and the mass fraction W2 of the cyclic ester in the electrolyte is 9.61%-23.14%; Optionally, the mass fraction W1 of the lithium salt in the electrolyte is 9.15%-14.95%, and the mass fraction W2 of the cyclic ester in the electrolyte is 15.50%-18.17%; Optionally, the mass fraction W1 of the lithium salt in the electrolyte is 9.15%-13.95%, and the mass fraction W2 of the cyclic ester in the electrolyte is 13.18%-18.17%.

3. The electrolyte according to claim 1 or 2, characterized in that The mass fraction W1 of the lithium salt in the electrolyte and the mass fraction W2 of the cyclic ester in the electrolyte satisfy Optionally, the The range is 0.5 to 1.06, and can be further selected as 0.8 to 1.

0.

4. The electrolyte according to any one of claims 1 to 3, characterized in that The mass fraction B of the cyclic ester relative to the mass of the organic solvent is 5% to 18%, and can be 13% to 16%; Optionally, the organic solvent further comprises methyl ethyl carbonate, and further optionally, the organic solvent comprises methyl ethyl carbonate in an amount of 95%-82%, optionally 87%-84%, by mass relative to the mass of the organic solvent.

5. The electrolyte according to any one of claims 1 to 4, characterized in that The electrolyte salt includes at least one of lithium bis(fluorosulfonyl)imide and lithium hexafluorophosphate, and the cyclic ester includes at least one of ethylene carbonate and propylene carbonate.

6. The electrolyte according to claim 5, characterized in that The electrolyte salt includes or is lithium bis(fluorosulfonyl)imide and lithium hexafluorophosphate, and the ratio of the molar concentration C1 of lithium bis(fluorosulfonyl)imide to the molar concentration C2 of lithium hexafluorophosphate is is 0.05-5, and can be optionally 1-3.5; optionally, the sum of the molar concentrations of the lithium bis(fluorosulfonyl)imide and the lithium hexafluorophosphate (C1+C2) is 0.86-1.4M.

7. The electrolyte according to any one of claims 1 to 6, characterized in that It comprises a film-forming additive, wherein the mass fraction A of the film-forming additive in the electrolyte is 3.55%-7%; optionally, the film-forming additive is at least one of fluoroethylene carbonate, vinylene carbonate, vinyl sulfate and 1,3-propane sultone.

8. A lithium ion battery, characterized in that: The invention comprises a positive electrode sheet, a negative electrode sheet and the electrolyte according to any one of claims 1 to 7.

9. The lithium-ion battery according to claim 8, characterized in that: The positive electrode sheet includes a positive electrode active material LiNi x Co y Mn z O2, x+y+z=1, the nickel atom content x is greater than 0.5, can be selected as 0.5-0.96, and can further be selected as 0.65, 0.8 or 0.

96.

10. The lithium ion battery according to claim 8 or 9, characterized in that: The negative electrode sheet includes a negative electrode current collector and a negative electrode film layer disposed on at least one surface of the negative electrode current collector, wherein the negative electrode film layer is 1540.25 mm 2 The loading amount H on the current collector surface is 0.058 g-1.698 g, and can be optionally 0.079 g-0.192 g; Optionally, the negative electrode film layer includes a negative electrode active material, a conductive agent, a binder, and an optional thickener.

11. An electrical device, characterized in that: A lithium ion battery comprising any one of claims 8 to 10.

Citation Information

Patent Citations

  • Electrolyte for 12V start-stop wide-temperature-band lithium battery of balancing high and low temperature

    CN110233291A

  • Electrolyte, preparation method thereof and lithium ion battery

    CN110752408A

  • High-nickel ternary lithium ion battery electrolyte and lithium ion battery

    CN111834665A